Particle, affinity particle having ligand for target substance, in vitro diagnostic reagent and kit containing the same, and method for detecting target substance
By using copolymer particles with specific carboxyl density and particle size ratio in the latex agglutination method, combined with chemically reactive functional groups, the problems of non-specific adsorption and electrostatic heterogeneous agglutination are solved, the detection sensitivity and dispersion stability are improved, and it is suitable for latex agglutination. in vitro diagnostics.
Patent Information
- Application Number
- CN202080060786.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-08-30
- Filing Date
- 2020-08-28
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2040-08-28
AI Technical Summary
In the existing latex agglutination method, particles may cause non-specific adsorption and electrostatic heterogeneous agglutination in high-concentration samples, resulting in reduced sensitivity and dispersion stability problems.
Copolymer particles with repeating units A and B are used. The surface contains particles with a carboxyl density of 0.04-0.15/nm3 and a particle size/dry particle size ratio in water of 1.10-1.40. A swelling layer is formed through chemical combination. To reduce non-specific adsorption, and cover the surface with reactive functional groups to improve the reactivity of the ligand with the target substance.
It achieves the reduction of non-specific adsorption and improvement of dispersion stability in latex agglutination method, enhances detection sensitivity and dispersion stability, avoids electrostatic agglutination, and is suitable for in vitro diagnosis and kit applications.
Smart Images

Figure FDA0004936040130000021 
Figure FDA0004936040130000022 
Figure FDA0004936040130000031
Abstract
Description
Technical Field
[0001] The present invention relates to particles, affinity particles comprising a ligand for a target substance, and an in vitro diagnostic reagent and a kit each comprising the affinity particle, and to a method for detecting a target substance. Background Art
[0002] An example of a simple and rapid immunoassay method is the latex agglutination method. In this method, a dispersion of affinity particles obtained by binding particles and a ligand having an affinity for a target substance to each other is mixed with a sample that may contain the target substance. At this time, when the sample contains the target substance, the affinity particles cause an agglutination reaction, and therefore, the presence or absence of a disease can be determined by optically detecting the agglutination reaction as a change in, for example, scattered light intensity, transmitted light intensity, or absorbance.
[0003] A combination of an antibody and an antigen or a combination of an antigen and an antibody is generally used as a combination of a ligand and a target substance. The particles to be used for the latex agglutination method and the affinity particles characterized by including a ligand for a target substance on the particle surface are each expected to show such properties of adsorbing substances other than the target substance (i.e., so-called non-specific adsorption) to a lesser extent, in order to prevent the occurrence of non-specific agglutination reactions not derived from the target substance. In addition, the dispersion of the affinity particles may be stored for several weeks in some detection institutions, so the invention of maintaining the dispersion state of the affinity particles in the dispersion is an extremely important technical issue.
[0004] As a means for reducing nonspecific adsorption of particles or affinity particles, a method involving covering the particle surface with a substance of biological origin such as albumin, casein or gelatin is available. However, the physical properties of such substances of biological origin may vary from one production batch to another. In addition, the following opinions are heard: there is a concern about future biological contamination due to the use of a large amount of such substances.
[0005] The method of covering the surface of particles or affinity particles with amphiphilic polymer compounds is also effective as a method for reducing nonspecific adsorption. However, the adsorption of particles or affinity particles by polymer compounds originates from physical adsorption. Therefore, the compound may be freed by its dilution, and thus nonspecific adsorption may not be fully suppressed in some cases.
[0006] As particles that cause small nonspecific adsorption, particles having polyglycidyl methacrylate arranged on the surface are known. It is believed that since part of the glycidyl groups of the polyglycidyl methacrylate arranged on the surface of the particles undergo ring opening to form diol, nonspecific adsorption is suppressed.
[0007] In Patent Document 1, there is disclosed a case where particles obtained by chemically bonding a ligand via a polyethylene glycol chain to the surface of a particle on which polyglycidyl methacrylate is arranged are applied to biological separation.
[0008] Patent Document 2 discloses that particles obtained by chemically bonding a ligand to the surface of particles on which polyglycidyl methacrylate is arranged are applied to a latex aggregation method.
[0009] Citation List
[0010] Patent Literature
[0011] Patent Document 1: Japanese Patent Application Laid-Open No. 2000-351814
[0012] Patent Document 2: International Publication No. WO2007 / 063616 Summary of the invention
[0013] Problem that the invention aims to solve
[0014] The present inventors have conducted intensive studies and have confirmed that, for example, each particle of Patent Document 1 and Patent Document 2 causes nonspecific adsorption in high-concentration samples, each particle may not show sufficient sensitivity when applied to the latex agglutination method, and there is a concern that electrostatic heteroagglutination may occur under static conditions.
[0015] The present invention has been made in view of such background technology and technical problems. An object of the present invention is to provide a particle that causes little nonspecific adsorption, has a reactive functional group for chemically binding a ligand, and is suitable for a latex agglutination method; and an affinity particle that is excellent in dispersion stability. Another object of the present invention is to provide an in vitro diagnostic reagent and a kit each including the particle or the affinity particle as a particle for a latex agglutination method, and a method for detecting a target substance.
[0016] The present invention relates to particles, affinity particles comprising a ligand for a target substance, in vitro diagnostic reagents and kits each comprising the affinity particles, and a method for detecting a target substance.
[0017] Solutions for solving problems
[0018] That is, the present invention relates to a particle comprising a copolymer having a repeating unit A and a repeating unit B in its surface layer, wherein the repeating unit A has a side chain A and the side chain A has a carboxyl group to be bound to a ligand at its terminal, wherein the repeating unit B has a side chain B and the side chain B has a hydroxyl group at its terminal, wherein the particle is constructed so that when the particle is dispersed in ion exchange water, the surface layer of the particle contains water to form a swollen layer, wherein the density of the carboxyl groups contained in the swollen layer satisfies the formula (1-1), and wherein the dry particle size measured when the particle is dried and the particle size in water measured when the particle is dispersed in ion exchange water satisfy the formula (1-2).
[0019] 0.040≤[Carboxyl density (pcs / nm 3 )]≤0.150…Formula (1-1)
[0020] 1.10≤[particle size in water / dry particle size]≤1.40…Formula (1-2)
[0021] The present invention also relates to an affinity particle, which comprises: a particle; and a ligand bound to the particle.
[0022] The present invention also relates to a reagent for detecting a target substance in a sample by in vitro detection diagnosis, comprising affinity particles, and to a reagent for detecting a target substance in a sample by an agglutination method (latex agglutination method).
[0023] Another embodiment of the present invention relates to an affinity particle, comprising: a particle; and a ligand on the surface of the particle, wherein the area occupied by the ligand relative to the particle surface satisfies the relationship of formula (2-1), wherein the zeta potential of the particle and the ligand satisfies the relationship of formula (2-2), and wherein the particle has a repeating unit A represented by formula (2-3).
[0024] 10≤[Occupancy rate (%)]≤40…Formula (2-1)
[0025] 0≤[||Zeta potential of particles|-|zeta potential of ligand||]≤20…Formula (2-2)
[0026] [Chemical formula 1]
[0027]
[0028] In formula (2-3), R1 represents a methyl group or a hydrogen atom, R2 represents a carboxyl group or a hydrogen atom, and L1 represents an alkylene group having 1 to 15 carbon atoms which may have a substituent or an oxyalkylene group having 1 to 15 carbon atoms which may have a substituent.
[0029] Furthermore, another embodiment of the present invention relates to a reagent for detecting a target substance in a sample by in vitro diagnosis, comprising affinity particles, and to a reagent for detecting a target substance in a sample by an agglutination method (latex agglutination method).
[0030] That is, a first aspect of another embodiment of the present invention relates to a particle comprising a copolymer including a repeating unit A represented by the following formula (3-1), which particle is capable of chemically binding a ligand to its surface with high yield by having a structure including a thioether group in the repeating unit A.
[0031] [Chemical formula 2]
[0032]
[0033] In addition, a second aspect of still another embodiment of the present invention relates to particles for latex agglutination method including a ligand chemically bound via the repeating unit A.
[0034] In addition, a third aspect of another embodiment of the present invention relates to a reagent for detecting a target substance in a sample by in vitro diagnosis comprising particles for latex agglutination method, a kit for detecting a target substance in a sample by in vitro diagnosis comprising at least the reagent, and a detection method comprising mixing particles for latex agglutination method and a sample that may contain the target substance.
[0035] Effects of the Invention
[0036] According to the present invention, particles which cause little nonspecific adsorption, have a reactive functional group for binding a ligand, and are suitable for an agglutination method (latex agglutination method) can be provided.
[0037] Furthermore, according to the present invention, an in vitro diagnostic reagent and a kit each comprising affinity particles formed by binding to a ligand as particles for an agglutination method (latex agglutination method), and a method for detecting a target substance can be provided.
[0038] In addition, according to another embodiment of the present invention, affinity particles that cause little nonspecific adsorption and are excellent in dispersion stability can be provided. According to another embodiment of the present invention, a highly sensitive in vitro diagnostic reagent and a kit, each containing the affinity particles as particles for agglutination method (latex agglutination method), and a method for detecting a target substance can be provided. DETAILED DESCRIPTION
[0039] [First embodiment]
[0040] The first embodiment of the present invention is described below in detail, but the technical scope of the present invention is not limited to the embodiment.
[0041] The particles according to the first embodiment of the present invention are particles comprising, in their surface layer, a copolymer having a repeating unit A having a side chain A having a carboxyl group to be bound to a ligand at its terminal, and a repeating unit B having a side chain B having a hydroxyl group at its terminal.
[0042] The particles to be used for the coagulation method (e.g., latex coagulation method) are preferably excellent in dispersion stability in an aqueous dispersion, so the carboxyl group preferably forms a carboxylate. Examples of carboxylates include: metal salts, such as sodium salts or potassium salts; and organic salts, such as ammonium salts. Considering the reactivity of the carboxyl group and the ligand when combined by a chemical reaction, organic salts are more preferred. Examples of organic bases for forming organic salts with the carboxyl group include ammonia, diethylamine, triethylamine, ethanolamine, and diethylaminoethanol. However, the present invention is not limited thereto. Considering experimental operability such as boiling point or solubility in various solvents, triethylamine is easy to use. The organic base for forming a carboxylate can be used alone or in combination, as long as the purpose of the first embodiment can be achieved. Similarly, a metal base and an organic base can be used in combination.
[0043] When the particles of the first embodiment are dispersed in water or an aqueous solution, the surface layer of the particles contains water to form a hydrogel-like swelling layer. The swelling layer is characterized in that the density of carboxyl groups contained in the swelling layer satisfies the following formula (1-1), and the dry particle size measured when the particles are dried and the particle size in water measured when the particles are dispersed in ion exchange water satisfy the formula (1-2).
[0044] 0.04≤[Carboxyl density (pcs / nm 3 )]≤0.15…Formula (1-1)
[0045] 1.10≤[particle size in water / dry particle size]≤1.40…Formula (1-2)
[0046] When the carboxyl density is less than 0.04 / nm 3 When the reactivity between the particles and the ligand (hereinafter referred to as "sensitization rate") is insufficient. The carboxyl group density is greater than 0.15 / nm 3 The case of is not preferred because the swelling layer has a high water binding force, so when the particles of the first embodiment are applied to the latex agglutination method, osmotic pressure agglutination occurs and a suspected nonspecific adsorption phenomenon is observed. In addition, when the carboxyl group density is greater than 0.15 / nm 3, the zeta potential of the particles increases. Therefore, when the ligand is combined with the particles to provide affinity particles, the electrostatic interaction between the ligand and the particle surface occurs and damages the reactivity between the ligand and the target substance, thereby reducing the detection sensitivity of the latex agglutination method. In addition, as the carboxyl density becomes larger, the zeta potential difference between the particles and the ligand also becomes larger. This means that charges with different signs are given to the affinity particle surfaces obtained by combining the ligand with the particles, thereby promoting the electrostatic agglutination of the affinity particles. Therefore, the zeta potential of the particles of the first embodiment preferably satisfies formula (1-3).
[0047] -30≤[Zeta potential (mV)]≤-10…Formula (1-3)
[0048] As described above, from the viewpoints of sensitization rate, osmotic pressure aggregation, detection sensitivity when affinity particles are applied to latex agglutination method, and electrostatic aggregation of affinity particles, there is a preferred range for carboxyl group density. Therefore, the carboxyl group density is preferably 0.04 / nm 3 Above and 0.15 / nm 3 Below, more preferably 0.10 pieces / nm 3 Above and 0.13 / nm 3 the following.
[0049] Formula (1-2) is related to the thickness of the swelling layer. The smaller the ratio represented by formula (1-2), the thinner the swelling layer is, and the larger the ratio represented by formula (1-2), the thicker the swelling layer is. When the ratio of [particle size in water / dry particle size] is less than 1.10, it may be difficult to expect an inhibitory effect based on nonspecific adsorption of the aqueous swelling layer. In addition, the swelling layer is not sufficiently hydrated, so the mobility of the carboxyl group derived from the repeating unit A of the swelling layer in the aqueous dispersion is not large. Therefore, it may be difficult to achieve a sufficient sensitization rate. In addition, when the ligand is bound to the particle to provide an affinity particle, the mobility of the ligand is inhibited and the reactivity between the ligand and the target substance is impaired, and the impaired reactivity may be the reason for reducing the detection sensitivity of the latex agglutination method. The fact that the ratio of [particle size in water / dry particle size] is greater than 1.10 contributes to the dispersion stability of the particles to a great extent. The particles to be used for the latex agglutination method preferably have excellent dispersion stability in a normal sample or a buffer represented by physiological saline. In this regard, when the ratio of [particle size in water / dry particle size] is 1.10 or more, the swelling layer contains water sufficiently to impart dispersion stability based on the excluded volume effect to the particles. Meanwhile, the case where the ratio of [particle size in water / dry particle size] is greater than 1.40 is not preferred because the swelling layer has a large water binding force, so that when the particles of the first embodiment are applied to the latex agglutination method, osmotic pressure agglutination occurs and a suspected nonspecific adsorption phenomenon is observed.
[0050] As described above, there is a preferred range for the thickness of the swelling layer from the viewpoints of sensitization rate, detection sensitivity when the affinity particles are applied to the latex agglutination method, dispersion stability of the particles, and osmotic pressure aggregation. In view of the foregoing, the ratio of [particle size in water / dry particle size] is preferably 1.10 or more and 1.40 or less, more preferably 1.15 or more and 1.30 or less.
[0051] Preferably, the repeating unit A and the repeating unit B of the copolymer constituting the particle surface layer of the particles of the first embodiment respectively have a side chain A and a side chain B, wherein the side chain A has a carboxyl group at its end to be bound to the ligand, and the side chain B has a hydroxyl group at its end, and the molar number of the repeating unit A and the molar number of the repeating unit B satisfy the formula (1-4).
[0052] 0.05≤[the number of moles of repeating unit A] / [the number of moles of repeating unit B]≤1.00…Formula (1-4)
[0053] When the ratio of [the number of moles of repeating unit A] / [the number of moles of repeating unit B] is less than 0.05, there is a concern about a decrease in the sensitization rate, although the decrease is not fatal. In addition, a decrease in the ratio of repeating unit A relative to the surface layer of the particles is synonymous with a decrease in the amount of carboxyl groups as a negative charge generation source, and an increased difficulty in imparting dispersion stability derived from electrostatic repulsion to the particles may be a potential problem. When the ratio of [the number of moles of repeating unit A] / [the number of moles of repeating unit B] is greater than 1.00, the water restraint force of the swelling layer formed by the water content of the surface layer of the particles becomes greater. Therefore, when the particles are mixed with a high-concentration sample, osmotic pressure aggregation may occur.
[0054] The specific chemical structure of the repeating unit A of the copolymer constituting the particle surface layer of the particle of the first embodiment is described. The repeating unit A is characterized by having a carboxyl group to be bound to a ligand at the end of its side chain, and its chemical structure is not limited within the range that the purpose of the first embodiment can be achieved. However, the side chain structure represented by formula (1-5) is more preferred:
[0055] [Chemical formula 3]
[0056]
[0057] wherein R1 represents a methyl group or a hydrogen atom, R2 represents a carboxyl group or a hydrogen atom, and L1 represents an alkylene group or an oxyalkylene group having 1 to 15 carbon atoms which may be substituted.
[0058] The hydroxyl group adjacent to the ester bond in formula (1-5) is used to reduce nonspecific adsorption of particles. The thioether bond is a chemical structure showing a weak hydrophobic tendency. When the repeating unit A has a side chain structure represented by formula (1-5), the water binding force of the swelling layer formed by the water content of the particle surface layer is moderately weakened. Therefore, it is expected to inhibit osmotic pressure aggregation that may occur when the particles are mixed with a high concentration sample.
[0059] In formula (1-5), L1 preferably represents an alkylene group having 1 carbon atom. The number of carbon atoms of L1 is related to the hydrophilicity or hydrophobicity of the repeating unit A, and when the number of carbon atoms becomes too large, nonspecific adsorption of the target substance to the particles may be promoted.
[0060] From the viewpoint of the sensitization rate of the particles of the first embodiment, R2 in formula (1-5) preferably represents a carboxyl group.
[0061] The specific chemical structure of the repeating unit B of the copolymer constituting the particle surface layer of the particle of the first embodiment is described. The repeating unit B of the first embodiment is characterized by having a side chain B having a hydroxyl group at the terminal, and its chemical structure is not limited within the range that the purpose of the first embodiment can be achieved. However, the side chain structure represented by formula (1-6) is more preferred:
[0062] [Chemical formula 4]
[0063]
[0064] wherein R1 represents a methyl group or a hydrogen atom, L2 represents an alkylene group or an oxyalkylene group having 2 to 15 carbon atoms which may be substituted, and has the relationship of [the number of carbon atoms of L1]+2≥[the number of carbon atoms of L2], and X represents a sulfur atom or a nitrogen atom which may be substituted.
[0065] The hydroxyl group adjacent to the ester bond and the hydroxyl group at the end of the side chain in formula (1-6) are used to reduce the nonspecific adsorption of the particles. X in formula (1-6) can represent any one of a sulfur atom and a nitrogen atom, and more preferably represents a sulfur atom. The thioether bond is a structure showing a weak hydrophobic tendency. When the repeating unit B has a side chain structure represented by formula (1-6), the water constraint force of the swelling layer formed by the water content of the surface layer of the particles is moderately weakened. Therefore, it is expected to inhibit osmotic pressure aggregation that may occur when the particles are mixed with a high concentration sample.
[0066] When comparing formula (1-5) and formula (1-6), the relationship between the number of carbon atoms of L1 in formula (1-5) and the number of carbon atoms of L2 in formula (1-6) is preferably the relationship of formula (1-7). When the relationship of formula (1-7) is not satisfied, the side chain B becomes relatively longer than the side chain A, so the reactivity of the carboxyl group at the end of the side chain A can be suppressed. In view of the foregoing, when L1 in formula (1-5) represents an alkylene group having 1 carbon atom, L2 in formula (1-6) preferably represents an alkylene group having 2 carbon atoms or 3 carbon atoms.
[0067] [The number of carbon atoms of L1] + 2 ≥ [The number of carbon atoms of L2] ... Formula (1-7)
[0068] When L2 in formula (1-6) represents an alkylene group having 3 carbon atoms, a chemical structure in which one hydrogen atom of the alkylene group is substituted with a hydroxyl group is more preferred from the viewpoint of reducing nonspecific adsorption of particles.
[0069] The particles of the first embodiment preferably have at least one selected from the group consisting of styrenes and (meth) acrylates as repeating units C, and more preferably contain repeating units derived from any one of styrenes and (meth) glycidyl acrylate. As described in the "Background Art" section herein, the repeating unit derived from (meth) glycidyl acrylate has the effect of reducing the nonspecific adsorption of particles. At the same time, the reason why the particles preferably contain repeating units derived from any one of styrenes is as follows. When the particles of the first embodiment are purified by methods such as centrifugation or ultrafiltration, the presence of repeating units derived from any one of styrenes having a high glass transition temperature and excellent in mechanical strength helps to inhibit damage to the particles such as cracking or chipping. Examples of styrenes include styrene, α-methylstyrene, β-methylstyrene, o-methylstyrene, m-methylstyrene, p-methylstyrene, 2,4-dimethylstyrene, p-butylstyrene, p-tert-butylstyrene, p-hexylstyrene, p-octylstyrene, p-nonylstyrene, p-decylstyrene, p-dodecylstyrene, p-methoxystyrene, and p-phenylstyrene. However, styrenes are not limited thereto, as long as the purpose of the first embodiment can be achieved. In addition, two or more styrenes can be used in combination. When the mass of the particles is set to 100 parts by mass, the content of styrenes is preferably 10 parts by mass or more and 70 parts by mass or less, because sufficient strength can be given to the particles while reducing nonspecific adsorption.
[0070] The particles of the first embodiment may further include repeating units derived from any one of free radical polymerizable monomers each having crosslinking properties. Examples of free radical polymerizable monomers each having crosslinking properties include diethylene glycol diacrylate, triethylene glycol diacrylate, tetraethylene glycol diacrylate, polyethylene glycol diacrylate, 1,6-hexanediol diacrylate, neopentyl glycol diacrylate, tripropylene glycol diacrylate, polypropylene glycol diacrylate, 2,2′-bis(4-(acryloyloxydiethoxy)phenyl)propane, trimethylolpropane triacrylate, tetramethylolmethane tetraacrylate, ethylene glycol dimethacrylate, diethylene glycol dimethacrylate, triethylene glycol dimethacrylate, Acid, tetraethylene glycol dimethacrylate, polyethylene glycol dimethacrylate, 1,3-butylene glycol dimethacrylate, 1,6-hexanediol dimethacrylate, neopentyl glycol dimethacrylate, polypropylene glycol dimethacrylate, 2,2′-bis(4-(methacryloxydiethoxy)phenyl)propane, 2,2′-bis(4-(methacryloxypolyethoxy)phenyl)propane, trimethylolpropane trimethacrylate, tetramethylolmethane tetramethacrylate, divinylbenzene, divinylnaphthalene, and divinyl ether. However, the monomer class is not limited thereto, as long as the purpose of the first embodiment can be achieved. In addition, two or more free radical polymerizable monomers each having crosslinking properties may be used in combination.
[0071] The particle size of the particles of the first embodiment is preferably 0.05 μm or more and 1.00 μm or less, more preferably 0.05 μm or more and 0.50 μm or less, and still more preferably 0.05 μm or more and 0.30 μm or less in terms of number average particle size. When the particle size is 0.05 μm or more and 0.30 μm or less, the particles are easy to handle, and when the particles are stored for a long time as a dispersion, sedimentation of the particles hardly occurs.
[0072] A typical production method of the particles of the first embodiment is described. However, the production method of the particles of the first embodiment is not limited to the extent that the purpose of the first embodiment can be achieved.
[0073] The method includes step 1 of mixing glycidyl (meth)acrylate, styrene, divinylbenzene, water and a radical polymerization initiator to form a granular copolymer, thereby providing an aqueous dispersion of the granular copolymer. The method includes step 2 of mixing the aqueous dispersion, 3-mercapto-1,2-propanediol and mercaptosuccinic acid to prepare a mixed solution, and then reacting an epoxy group derived from glycidyl (meth)acrylate of the granular copolymer and a thiol group derived from each of 3-mercapto-1,2-propanediol and mercaptosuccinic acid with each other to form particles of the first embodiment. The free radical polymerization initiator is at least one of 4,4′-azobis(4-cyanovaleric acid), 2,2′-azobis[2-methyl-N-(2-hydroxyethyl)propionamide], 2,2′-azobis[N-(2-carboxyethyl)-2-methylpropionamidine] tetrahydrate, 2,2′-azobis(2-methylpropionamidine) dihydrochloride, 2,2′-azobis[2-(2-imidazolin-2-yl)propane], 2,2′-azobis[2-(2-imidazolin-2-yl)propane] dihydrochloride, or 2,2′-azobis[2-(2-imidazolin-2-yl)propane] disulfate dihydrate. The method includes a step of adjusting the pH of the mixed solution in step 2 to an alkaline region using an organic base that does not contain any primary amine. In step 2, the epoxy group derived from glycidyl (meth)acrylate of the granular copolymer is reacted with the thiol group derived from each of 3-mercapto-1,2-propanediol and mercaptosuccinic acid from the surface of the granular copolymer in the depth direction thereof. In order to form a surface layer having a sufficient thickness on the particles of the first embodiment, triethylamine having permeability to the granular copolymer is preferably selected as the organic base.
[0074] The method for forming the granular copolymer is not limited to using free radical polymerization, as long as the purpose of the first embodiment can be achieved. When applying free radical polymerization, preferably use emulsion polymerization, soap-free emulsion polymerization or suspension polymerization, and more preferably use emulsion polymerization or soap-free emulsion polymerization. More preferably use soap-free emulsion polymerization. Usually, emulsion polymerization and soap-free emulsion polymerization can each provide a granular copolymer with a sharper particle size distribution than the granular copolymer provided by suspension polymerization. In addition, when making the particle and the part be combined to provide affinity particles, it is worried that the anionic surfactant or cationic surfactant that is usually used for emulsion polymerization exists as residue and modifies the part. In view of the foregoing, when forming the granular copolymer by emulsion polymerization, it is preferred to use a nonionic surfactant.
[0075] A ligand is a compound that specifically binds to a receptor possessed by a specific target substance. The site where the ligand binds to the target substance is determined, and the ligand has a high affinity for selectivity or specificity to the target substance. Examples of ligands include: antigens and antibodies; enzyme proteins and their substrates; signal substances represented by hormones or neurotransmitters and their receptors; nucleic acids; and avidin and biotin. However, the ligand is not limited thereto, as long as the purpose of the first embodiment can be achieved. Specific examples of ligands include antigens, antibodies, antigen-binding fragments (e.g., Fab, F(ab′)2, F(ab′), Fv or scFv), naturally occurring nucleic acids, artificial nucleic acids, aptamers, peptide aptamers, oligopeptides, enzymes and coenzymes.
[0076] In a first embodiment, the particles of the first embodiment are intended for use as particles for latex agglutination methods that can be applied to latex agglutination methods in immunoassays.
[0077] In the first embodiment, conventionally known methods can be applied as methods for chemical reactions for binding carboxyl groups or carboxylates derived from repeating units A with ligands, as long as the purpose of the first embodiment can be achieved. For example, carbodiimide-mediated reactions or NHS ester activation reactions are suitable examples of the chemical reactions. In addition, the following can be performed: avidin is bound to the carboxyl group, and a biotin-modified ligand is bound to the resultant. However, the method for chemical reactions for binding carboxyl groups or carboxylates derived from repeating units A with ligands is not limited thereto, as long as the purpose of the first embodiment can be achieved.
[0078] In the first embodiment, when an antibody (antigen) is used as a ligand and an antigen (antibody) is used as a target substance, as a method for detecting the target substance in a sample in in vitro diagnosis, the latex agglutination method, which has been widely used in immunoassays in fields such as clinical testing and biochemical research, can be very preferably applied. When ordinary particles are used as particles for the latex agglutination method, the antigen (antibody) as the target substance, or foreign matter in serum or plasma, etc., is non-specifically adsorbed to the particle surface, and therefore, there is a concern that unexpected inter-particle agglutination due to adsorption may impair the accuracy of the immunoassay.
[0079] The reagent for detecting the target substance in the sample by in vitro diagnosis of the first embodiment is characterized in that it contains particles for latex agglutination method. The amount of particles for latex agglutination method contained in the reagent of the first embodiment is preferably 0.001 mass % to 20 mass %, more preferably 0.01 mass % to 10 mass %. In addition to particles for latex agglutination method, the reagent of the first embodiment may also include a third substance such as a solvent or a blocking agent, as long as the purpose of the first embodiment can be achieved. Examples of solvents to be used in the first embodiment include various aqueous buffers, such as phosphate buffer, glycine buffer, Good's buffer, Tris buffer, HEPES buffer, MES buffer and ammonia buffer. However, the solvent contained in the reagent of the first embodiment is not limited thereto.
[0080] The kit for detecting the target substance in the test sample by in vitro diagnosis of the first embodiment is characterized in that it contains at least the reagent of the first embodiment. In addition to the reagent of the first embodiment (hereinafter referred to as "reagent 1"), the kit of the first embodiment preferably further contains a reaction buffer (hereinafter referred to as "reagent 2") containing albumin. Albumin is, for example, serum albumin, and can be treated with protease. As a standard, the amount of albumin contained in reagent 2 is 0.001% by mass to 5% by mass, but the amount of albumin in the kit of the first embodiment is not limited to this. Each of reagent 1 and reagent 2 or one of them may contain a sensitizer for latex agglutination assay. Examples of sensitizers for latex agglutination assay include polyvinyl alcohol, polyvinyl pyrrolidone and alginic acid. However, the sensitizer to be used for the kit of the first embodiment is not limited to this. In addition, in addition to reagent 1 and reagent 2, the kit of the first embodiment may contain, for example, a positive control, a negative control or a serum diluent. In addition to serum or saline containing the target substance that can be measured, a solvent can also be used as a medium for a positive control or a negative control. The kit of the first embodiment can be used for the method for detecting the target substance of the first embodiment in the same manner as a conventional kit for detecting the target substance in a sample by in vitro diagnosis. In addition, the concentration of the target substance can be measured by a conventionally known method, and this method is particularly suitable for detecting the target substance in a sample by latex agglutination method.
[0081] The method for detecting a target substance in a sample by in vitro diagnosis of the first embodiment is characterized in that it includes mixing the affinity particles of the first embodiment with a sample that may contain the target substance. In addition, the affinity particles of the first embodiment and the sample are preferably mixed in the range of pH 3.0 to 11.0. In addition, the mixing temperature falls within the range of 20°C to 50°C, and the mixing time falls within the range of 1 minute to 20 minutes. In addition, in this detection method, a solvent is preferably used. In addition, the concentration of the affinity particles of the first embodiment in the detection method of the first embodiment in the reaction system is preferably 0.001% by mass to 5% by mass, more preferably 0.01% by mass to 1% by mass. The detection method of the first embodiment is characterized in that it includes optical detection of inter-particle agglutination caused by the result of mixing the affinity particles of the first embodiment with the sample. When the inter-particle agglutination is optically detected, the target substance in the sample is detected, and the concentration of the target substance can be measured. As a method for optically detecting agglutination reactions, it is only necessary to use an optical instrument that can detect scattered light intensity, transmitted light intensity, absorbance, etc. to measure the amount of change in these values.
[0082] The method for measuring the dry particle size of the particles in the first embodiment is described. The dry particle size in the first embodiment is a number average particle size, and is measured when the particles are fully dried. Specifically, the particles are dispersed in ion exchange water at a concentration of 5% by mass, and the dispersion is dripped onto an aluminum foil and then dried at 25°C for 48 hours. Thereafter, the dried product is further dried for 24 hours with a vacuum dryer and then measured. A scanning electron microscope and an image processing analyzer are used for the measurement of the dry particle size. Specifically, 100 individual particles are randomly selected from an image of particles in a dry state, the image being obtained using a scanning electron microscope (S-4800: Hitachi High-Technologies Corporation), and their number average particle size is calculated by analyzing the image with an image processing analyzer "Luzex AP" (Nireco Corporation).
[0083] The method for measuring the particle size in water of the particles in the first embodiment is described. The particle size in water in the first embodiment is a number average particle size, and is measured in a state where the particles are dispersed in ion exchange water so that their concentration can be 0.001% by mass. Ion exchange water with an electrical conductivity of 10μS / cm or less is used as ion exchange water. The dynamic light scattering method is applied to the measurement of the particle size in water. Specifically, ZETASIZER (Nano-ZS: Spectris Co., Ltd.) is used for measurement at 25°C. Regarding the analysis parameters, the refractive index of latex (n≈1.59) is selected as the refractive index of the particles, and pure water is selected as the solvent. The measurement is performed 10 times, and the average value of the 10 measured values is adopted as the particle size in water.
[0084] Describes a method for measuring the zeta potential of particles in the first embodiment. The zeta potential in the first embodiment is measured in a state where the particles are dispersed in a 0.01N aqueous potassium solution with a pH of 7.8 so that its concentration can be 0.001% by mass. A solution obtained by appropriately mixing a 0.01N aqueous potassium chloride solution, a 0.01N aqueous potassium hydroxide solution, and a 0.01N aqueous hydrochloric acid solution (each prepared using ion-exchanged water with a conductivity of 10 μS / cm or less) is used as the 0.01N aqueous potassium solution with a pH of 7.8. The measurement is carried out at 25 °C using a ZETASIZER (Nano-ZS: Spectris Co., Ltd.) as the measuring device. Regarding the analysis parameters, the refractive index of latex (n≈1.59) is selected as the refractive index of the particles, and pure water is selected as the solvent. The measurement is carried out 10 times, and the average value of the 10 measurement values is adopted as the zeta potential.
[0085] The carboxyl density in the first embodiment is calculated from the relationship between the amount of carboxyl groups of the particles and the volume of the swelling layer to be formed on the particle surface when the particles are dispersed in ion-exchanged water.
[0086] First, a method for measuring the amount of carboxyl groups of particles is described. The carboxyl groups of the particles are esterified with N-hydroxysuccinimide (NHS) using 1-ethyl-3-(3-dimethylaminopropyl)carbodiimide hydrochloride (EDC / HCl) as a catalyst. Thereafter, the active ester is reacted with aminoethanol to free NHS, and the amount of carboxyl groups per unit particle mass is calculated by measuring the amount of free NHS using a high-performance liquid chromatography device. The unit of the amount of carboxyl groups per unit particle mass is nmol / mg. The following describes the specific method.
[0087] <Active esterification>
[0088] Aqueous dispersion of particles containing 2.5 mg of particles is added to a 1.5 mL microtube, and the particles are separated from the dispersion using a centrifuge. In addition, the particles are redispersed in dimethylformamide (DMF). The foregoing operation is carried out three times. In addition, while the particles are sedimented in the microtube using a centrifuge, DMF is removed from the microtube. Next, 400 μL of DMF, 19.2 mg of EDC·HCl, and 100 μL of a 1 mol / L DMF solution of N-hydroxysuccinimide are added to the microtube, and the mixture is shaken at 25 °C for 2 hours to esterify the carboxyl groups of the particles.
[0089] <Liberation of NHS>
[0090] To remove the excess NHS from the DMF dispersion of the activated esterified particles, the activated esterified particles were separated from the dispersion using a centrifuge, and the particles were redispersed in DMF; the foregoing operation was performed three times. Further, while the activated esterified particles were sedimented in a microtube using a centrifuge, the DMF was removed from the microtube. Next, 500 μL of a 1 mol / L DMF solution of aminoethanol was added to the microtube, and the mixture was shaken at 25 °C for 2 hours to liberate the NHS from the particles.
[0091] <Quantification of NHS>
[0092] The DMF dispersion of the particles containing the liberated NHS was centrifuged, and the DMF solution containing the liberated NHS was recovered while the particles were sedimented in a microtube, and then the amount of the liberated NHS in the DMF solution was quantified using a high performance liquid chromatography apparatus. The amount of carboxyl groups per unit particle mass was calculated using the quantified value.
[0093] The instruments and reagents to be used for the quantification of the amount of carboxyl groups are as described below.
[0094] <Instruments>
[0095] High performance liquid chromatography apparatus: LC20A-FL (Shimadzu Corporation)
[0096] Column: Kinetex 5μm C18 100ALC column 150×4.6 mm (Phenomenex)
[0097] Eluent: 4 mmol / L aqueous ammonium acetate solution
[0098] Flow rate: 1.0 mL / min
[0099] Oven temperature: 40 °C
[0100] Sample injection volume: 1 μL
[0101] When quantifying the amount of the liberated NHS contained in the DMF solution, a calibration curve between the peak area derived from NHS and the amount of NHS was prepared in the range of 0.1 mmol / L to 10 mmol / L, and the amount of the liberated NHS was quantified from the NHS peak area.
[0102] <Reagents>
[0103] EDC / HCl (Dojindo Laboratories)
[0104] NHS (Kishida Chemical Co., Ltd.)
[0105] Aminoethanol (Tokyo Chemical Industry Co., Ltd.)
[0106] DMF(FUJIFILM Wako Pure Chemical Corporation)
[0107] Ammonium acetate (Tokyo Chemical Industry Co., Ltd.)
[0108] Next, a method for calculating the carboxyl group density of the particles is described. In the case where the particles are dispersed in water or an aqueous solution, when calculating the amount of carboxyl groups per unit volume contained in the swelling layer to be formed on the surface layer of the particles (i.e., the carboxyl group density), the values of the particle size in water when the particles are dispersed in ion exchange water and the dry particle size of the particles are used. In addition, the carboxyl group density is calculated by applying formula (1-8), wherein when calculating each of the dry particle size and the particle size in water, the density of the particles is regarded as 1 (g / cm 3 ).
[0109] [Carboxyl density (number / nm 3 )]=Dd 3 / (Dw 3 -Dd 3 )×A×N A ×10 -27 …Formula (1-8)
[0110] In formula (1-8), Dw represents the particle size in water (nm), Dd represents the dry particle size (nm), A represents the amount of carboxyl groups per unit particle mass (nmol / mg), and N A represents Avogadro's constant.
[0111] [Second embodiment]
[0112] The second embodiment of the present invention is described in detail below, but the technical scope of the present invention is not limited to this embodiment.
[0113] The second embodiment relates to an affinity particle, comprising: a particle; and a ligand on the surface of the particle, the affinity particle being characterized in that the area occupied by the ligand relative to the particle surface satisfies the relationship of formula (2-1), the zeta potential of the particle and the ligand satisfies the relationship of formula (2-2), and the particle has a repeating unit A represented by formula (2-3).
[0114] 10≤[Occupancy rate (%)]≤40…Formula (2-1)
[0115] 0≤[||Zeta potential of particles|-|zeta potential of ligand||]≤20…Formula (2-2)
[0116] [Chemical formula 5]
[0117]
[0118] In formula (2-3), R1 represents a methyl group or a hydrogen atom, R2 represents a carboxyl group or a hydrogen atom, and L1 represents an alkylene group having 1 to 15 carbon atoms which may have a substituent or an oxyalkylene group having 1 to 15 carbon atoms which may have a substituent.
[0119] First, the particles are described. In the second embodiment, the particles used to obtain affinity particles by binding with a ligand are simply referred to as "particles".
[0120] The particles have a repeating unit A represented by formula (2-3).
[0121] The hydroxyl group adjacent to the ester bond in formula (2-3) serves to reduce nonspecific adsorption of the affinity particles according to the second embodiment.
[0122] In formula (2-3), L1 preferably represents a methylene group having 1 carbon atom. The number of carbon atoms of L1 is related to the hydrophilicity or hydrophobicity of the repeating unit A, and when the number of carbon atoms of L1 becomes too large, nonspecific adsorption of the target substance to the affinity particles may be promoted.
[0123] Preferably, the surface layer of the particles comprises a copolymer having repeating unit A, and when the particles are dispersed in water or an aqueous solution, the surface layer contains water to form a swelling layer. The thickness of the swelling layer is related to the ratio of the dry particle size of the particles measured when the particles are dried to the particle size in water of the particles measured when the particles are dispersed in ion exchange water, and the dry particle size and the particle size in water preferably satisfy the formula (2-5).
[0124] 1.10≤[particle size in water / dry particle size]≤1.40…Formula (2-5)
[0125] The formation of a swollen layer by the surface layer of the particles containing water in water or an aqueous solution contributes to the following points: namely, the formation contributes to reducing nonspecific adsorption of the target substance to the affinity particles, improving the sensitivity when the affinity particles are applied to particles for agglutination methods (e.g., latex agglutination methods), and improving the dispersion stability of the affinity particles.
[0126] In particular, the fact that the ratio of [particle size in water / dry particle size] is 1.10 or more means that the swelling layer contains water sufficiently to make the particle surface hydrophilic, and thus the nonspecific adsorption of the target substance to the affinity particles is significantly suppressed. In addition, the fact that the ratio of [particle size in water / dry particle size] is 1.10 or more means that the swelling layer contains water sufficiently to improve the mobility of the ligand of the affinity particles, and thus improve the reactivity between the ligand and the target substance. In addition, when the swelling layer contains water sufficiently, dispersion stability based on the excluded volume effect is imparted to the affinity particles.
[0127] In contrast, when the ratio [particle size in water / dry particle size] is greater than 1.40, the swelling layer has a large water binding force, so the affinity particles of the second embodiment may cause osmotic agglutination when applied to the latex agglutination method. It is difficult to distinguish osmotic agglutination from suspected nonspecific agglutination phenomena in the detection mechanism.
[0128] As described above, there is a preferred range for the thickness of the swelling layer from the viewpoints of nonspecific adsorption, sensitivity when the affinity particles are applied to the latex agglutination method, dispersion stability of the affinity particles, and osmotic pressure aggregation. In view of the foregoing, the ratio of [particle size in water / dry particle size] is preferably 1.10 or more and 1.40 or less, more preferably 1.15 or more and 1.30 or less.
[0129] When the particle surface layer contains water in water or an aqueous solution to form a swelling layer, the thioether bond of the repeating unit A represented by the formula (2-3) is a chemical structure showing a weak hydrophobic tendency, so the water binding force of the swelling layer is moderately weakened. Therefore, it is expected to have an inhibitory effect on osmotic pressure aggregation that occurs when the affinity particles according to the second embodiment are mixed with a sample.
[0130] In formula (2-3), R2 preferably represents a carboxyl group. When R2 represents a carboxyl group, the particle surface layer easily contains water or an aqueous solution, and easy water inclusion is conducive to the formation of a swelling layer.
[0131] Next, the ligand is described. The ligand is a compound that specifically binds to the receptor of a specific target substance. The site where the ligand binds to the target substance is determined, and the ligand has a high affinity for the target substance that is selective or specific. Examples of ligands include: antigens and antibodies; enzyme proteins and their substrates; signal substances represented by hormones or neurotransmitters and their receptors; nucleic acids; and avidin and biotin. However, the ligand is not limited to this, as long as the purpose of the second embodiment can be achieved. Specific examples of ligands include antigens, antibodies, antigen-binding fragments (e.g., Fab, F(ab′)2, F(ab′), Fv or scFv), naturally occurring nucleic acids, artificial nucleic acids, aptamers, peptide aptamers, oligopeptides, enzymes and coenzymes.
[0132] Although the method of bonding the particle and the ligand to each other is not limited within the range that the object of the second embodiment can be achieved, it is preferred to bond the ligand to the particle surface via the carboxyl group derived from the repeating unit A represented by formula (2-3) by utilizing a chemical reaction.
[0133] In the second embodiment, conventionally known methods can be applied as a method for chemical reaction for binding the carboxyl group derived from the repeating unit A and the ligand to each other, as long as the purpose of the second embodiment can be achieved. For example, a carbodiimide-mediated reaction or an NHS ester activation reaction is a suitable example. In addition, the following can be performed: avidin is bound to the carboxyl group, and a biotin-modified ligand is bound to the resultant.
[0134] When the carboxyl group derived from repeating unit A is bound to a ligand, a part of the carboxyl group can be converted into another chemical structure by utilizing a chemical reaction. In a second embodiment, such a conversion reaction is referred to as "masking treatment", and the reagent to be used for the masking treatment is referred to as "masking agent". Amines are generally used as masking agents, and trishydroxymethylaminomethane is generally used among amines. In contrast, as a result of the inventor's research, it is recognized that the following will greatly improve the detection sensitivity when the affinity particles according to the second embodiment are applied to the latex agglutination method. That is, the carboxyl group of a part of the repeating unit A is converted by using ethanolamine as a masking agent to provide a chemical structure represented by formula (2-6).
[0135] [Chemical formula 6]
[0136]
[0137] In formula (2-6), R1 represents a methyl group or a hydrogen atom, R2 represents a carboxyl group or a hydrogen atom, and L1 represents an alkylene group having 1 to 15 carbon atoms which may have a substituent or an oxyalkylene group having 1 to 15 carbon atoms which may have a substituent.
[0138] In the second embodiment, when an antibody (antigen) is used as a ligand and an antigen (antibody) is used as a target substance, the latex agglutination method in immunoassay can be applied very preferably. Immunoassay has been widely used in fields such as clinical testing and biochemical research as a detection method for target substances in samples in in vitro diagnosis. When conventional affinity particles are used as particles for latex agglutination, antigens (antibodies) as target substances or foreign matter in serum or plasma are non-specifically adsorbed to the particle surface. In addition, there is a concern that unexpected agglutination between affinity particles due to adsorption may impair the accuracy of immunoassay.
[0139] The relationship between the zeta potential of the particles and the zeta potential of the ligand in the second embodiment is described. The affinity particles according to the second embodiment are characterized in that the zeta potential of the particles and the zeta potential of the ligand satisfy the relationship of formula (2-2).
[0140] 0≤[||Zeta potential of particles (mV)|-|zeta potential of ligand (mV)||]≤20…Formula (2-2)
[0141] The case where the difference between [||Zeta potential of particles (mV)|-|zeta potential of ligand (mV)||] is greater than 20 mV means that charges with different signs are given to the surfaces of the affinity particles obtained by binding the ligand to the particles. In this case, when the affinity particles are stored statically, there is a high possibility of electrostatic heteroagglutination, so care needs to be taken when handling the affinity particles in the detection mechanism. In the second embodiment, when an antibody or an antigen is used as a ligand, the zeta potential of a typical antigen or antibody is about -10 mV, so the zeta potential of the particles is preferably not less than -30 mV and not more than -10 mV.
[0142] The affinity particles according to the second embodiment are characterized in that the occupied area ratio of the ligand with respect to the particle surface satisfies the relationship of formula (2-1).
[0143] 10≤[Occupancy rate (%)]≤40…Formula (2-1)
[0144] The occupied area ratio is described. The occupied area of a ligand is calculated by using a known formula, in which the size of the ligand is approximated as a true sphere and the area of a circle having the same diameter as the sphere is calculated. At the same time, the surface area of each particle is calculated by using a known formula, in which the particle is approximated as a true sphere and the surface area of the true sphere is calculated. The particle size of the particle in water is used as its particle size. At the same time, the sensitizing amount (μg / mg) of the ligand to the particle is quantified by experiment, and the number of ligands per affinity particle is calculated from the quantitative value. Assuming that the affinity particles of the second embodiment are obtained by binding a monolayer of ligands to the particle surface, the occupied area ratio is calculated by applying the monolayer adsorption model. That is, the occupied area ratio is defined as the value calculated by using formula (2-7).
[0145] [Occupancy rate (%)] = [Occupancy area of one ligand (nm 2 )] × [number of ligands per affinity particle (pieces)] / [surface area of each particle (nm 2 )]×100…Formula (2-7)
[0146] When the ligand is an antibody, it is generally considered that the antibody is a true sphere with a diameter of 8 nm, so the specific area of one antibody is determined to be about 50.2 nm.2 An occupied area ratio of 50% means that 50% of the affinity particle surface is occupied by the antibody, and the particle surface corresponding to the remaining 50% serving as a base layer is exposed.
[0147] When the occupied area ratio is less than 10%, when the affinity particles are used as particles for latex agglutination, sufficient detection sensitivity may not be obtained, because the frequency of affinity particles agglutinating each other via the target substance is small. In addition, when the occupied area ratio of the ligand is too small, there is a concern that the heterogeneity of the chemical composition on the surface of the affinity particles may damage the dispersion stability of the affinity particles. At the same time, when the occupied area ratio is greater than 40%, interactions may occur between the ligands to damage the inherent reactivity of the ligands with the target substance. In the second embodiment, the occupied area ratio more preferably falls within the range of 15% or more and less than 30%.
[0148] More preferred forms of particles are described.
[0149] In addition to having a repeating unit A represented by formula (2-3), the particles preferably have a repeating unit B characterized by having a hydroxyl group at the end of the side chain. Affinity particles obtained by binding a ligand to particles having such characteristics significantly suppress nonspecific adsorption. For the purpose of reducing nonspecific adsorption, it is more preferred that the surface layer of the particles contains a copolymer having repeating units A and repeating units B, and when the particles are dispersed in water or an aqueous solution, the surface layer contains water to form a swelling layer.
[0150] The specific chemical structure of repeating unit B is described. Repeating unit B is characterized in that it has a hydroxyl group at its side chain terminal, and its chemical structure is not limited in the range that the purpose of the second embodiment can be achieved. However, a repeating unit having a side chain structure represented by formula (2-4) is more preferred.
[0151] [Chemical formula 7]
[0152]
[0153] In formula (2-4), R1 represents a methyl group or a hydrogen atom, L2 represents an alkylene group having 2 to 15 carbon atoms which may have a substituent or an oxyalkylene group having 2 to 15 carbon atoms which may have a substituent, X represents a sulfur atom or a nitrogen atom which may have a substituent, and L1 in formula (2-3) and L2 in formula (2-4) satisfy the relationship of [the number of carbon atoms of L1] + 2 ≥ [the number of carbon atoms of L2].
[0154] The hydroxyl group adjacent to the ester bond and the hydroxyl group at the end of the side chain in formula (2-4) are used to reduce the nonspecific adsorption of the particles. X in formula (2-4) can represent any one of a sulfur atom and a nitrogen atom, and more preferably represents a sulfur atom. The thioether bond is a structure showing a weak hydrophobic tendency. Therefore, when a swelling layer formed by the surface layer of the particles containing water is formed, the water restraint force of the swelling layer is moderately weakened, and it is expected to inhibit osmotic pressure aggregation that may occur when the particles are mixed with a high concentration sample.
[0155] When comparing formula (2-3) and formula (2-4), the relationship between the number of carbon atoms of L1 in formula (2-3) and the number of carbon atoms of L2 in formula (2-4) preferably satisfies the relationship of formula (2-8). When the relationship of formula (2-8) is not satisfied, the side chain derived from repeating unit B becomes relatively longer than the side chain derived from repeating unit A, and thus may shield the carboxyl group at the end of the side chain of repeating unit A. In view of the foregoing, when L1 in formula (2-3) represents an alkylene group having 1 carbon atom, L2 in formula (2-4) preferably represents an alkylene group having 2 carbon atoms or 3 carbon atoms.
[0156] [The number of carbon atoms of L1] + 2 ≥ [The number of carbon atoms of L2] ... Formula (2-8)
[0157] When L2 in formula (2-4) represents an alkylene group having 3 carbon atoms, a chemical structure in which one hydrogen atom of the alkylene group is substituted with a hydroxyl group is more preferred from the viewpoint of reducing nonspecific adsorption of particles.
[0158] The particles preferably have at least one selected from the group consisting of styrenes and (meth)acrylates as repeating units C, and more preferably contain repeating units derived from any one of styrenes and glycidyl (meth)acrylate. Herein, "(meth)acrylate" refers to "acrylate or methacrylate". As described in the "Background Art" section of this article, the repeating unit derived from glycidyl (meth)acrylate has the effect of reducing the nonspecific adsorption of particles. At the same time, the reason why the particles preferably contain repeating units derived from any one of styrenes is as follows. When the particles are purified by methods such as centrifugation or ultrafiltration, the presence of repeating units derived from any one of styrenes having a high glass transition temperature and excellent in mechanical strength helps to suppress damage to the particles such as cracking or fragmentation. Examples of styrenes include styrene, α-methylstyrene, β-methylstyrene, o-methylstyrene, m-methylstyrene, p-methylstyrene, 2,4-dimethylstyrene, p-butylstyrene, p-tert-butylstyrene, p-hexylstyrene, p-octylstyrene, p-nonylstyrene, p-decylstyrene, p-dodecylstyrene, p-methoxystyrene, and p-phenylstyrene. However, styrenes are not limited thereto, as long as the purpose of the second embodiment can be achieved. In addition, two or more styrenes can be used in combination.
[0159] When the mass of the particles is 100 parts by mass, the content of styrenes is preferably 10 parts by mass or more and 70 parts by mass or less because sufficient strength can be imparted to the particles while reducing nonspecific adsorption.
[0160] The particles may further contain repeating units derived from any one of the free radical polymerizable monomers each having crosslinking properties. Examples of the free radical polymerizable monomers each having crosslinking properties include diethylene glycol diacrylate, triethylene glycol diacrylate, tetraethylene glycol diacrylate, polyethylene glycol diacrylate, 1,6-hexanediol diacrylate, neopentyl glycol diacrylate, tripropylene glycol diacrylate, polypropylene glycol diacrylate, 2,2′-bis(4-(acryloyloxydiethoxy)phenyl)propane, trimethylolpropane triacrylate, tetramethylolmethane tetraacrylate, ethylene glycol dimethacrylate, diethylene glycol dimethacrylate, triethylene glycol dimethacrylate, Ester, tetraethylene glycol dimethacrylate, polyethylene glycol dimethacrylate, 1,3-butylene glycol dimethacrylate, 1,6-hexanediol dimethacrylate, neopentyl glycol dimethacrylate, polypropylene glycol dimethacrylate, 2,2′-bis(4-(methacryloxydiethoxy)phenyl)propane, 2,2′-bis(4-(methacryloxypolyethoxy)phenyl)propane, trimethylolpropane trimethacrylate, tetramethylolmethane tetramethacrylate, divinylbenzene, divinylnaphthalene, and divinyl ether. However, the monomer is not limited thereto, as long as the purpose of the second embodiment can be achieved. In addition, two or more free radical polymerizable monomers each having crosslinking properties may be used in combination.
[0161] The particle size of the particles is preferably 0.05 μm or more and 1.00 μm or less, more preferably 0.05 μm or more and 0.50 μm or less, and even more preferably 0.05 μm or more and 0.30 μm or less in terms of number average particle size. When the particle size is 0.05 μm or more and 0.30 μm or less, the particles are easy to handle, and when the particles are stored for a long time as a dispersion, sedimentation of the particles hardly occurs.
[0162] A typical production method of particles is described. However, the production method of particles is not limited to the extent that the object of the second embodiment can be achieved.
[0163] The method for producing the particles includes step 1 of mixing glycidyl (meth)acrylate, styrene, divinylbenzene, water and a radical polymerization initiator to form a granular copolymer, thereby providing an aqueous dispersion of the granular copolymer.
[0164] In addition, the method for producing particles includes a step 2 of forming particles by the following steps. That is, first, the aqueous dispersion, 3-mercapto-1,2-propanediol and mercaptosuccinic acid are mixed to prepare a mixed solution. Subsequently, the epoxy group derived from glycidyl (meth)acrylate of the granular copolymer and the thiol group derived from each of 3-mercapto-1,2-propanediol and mercaptosuccinic acid are reacted with each other.
[0165] The free radical polymerization initiator is preferably at least one of 4,4′-azobis(4-cyanovaleric acid), 2,2′-azobis[2-methyl-N-(2-hydroxyethyl)propionamide], 2,2′-azobis[N-(2-carboxyethyl)-2-methylpropionamidine] tetrahydrate, 2,2′-azobis(2-methylpropionamidine) dihydrochloride, 2,2′-azobis[2-(2-imidazolin-2-yl)propane], 2,2′-azobis[2-(2-imidazolin-2-yl)propane] dihydrochloride, or 2,2′-azobis[2-(2-imidazolin-2-yl)propane] disulfate dihydrate.
[0166] Furthermore, the method for producing particles includes a step of adjusting the pH of the mixed solution in step 2 to an alkaline region with an organic base that does not contain any primary amine. In step 2, the epoxy group derived from glycidyl (meth)acrylate of the granular copolymer and the thiol group derived from each of 3-mercapto-1,2-propanediol and mercaptosuccinic acid are reacted from the surface of the granular copolymer in the depth direction thereof. In order to form a surface layer having a sufficient thickness on the particles, triethylamine having permeability to the granular copolymer is preferably selected as the organic base.
[0167] The method of forming the particulate copolymer is not limited to using radical polymerization as long as the object of the second embodiment can be achieved.
[0168] When free radical polymerization is applied, it is preferred to use emulsion polymerization, soap-free emulsion polymerization or suspension polymerization, and it is more preferred to use emulsion polymerization or soap-free emulsion polymerization. It is still more preferred to use soap-free emulsion polymerization.
[0169] In general, emulsion polymerization and soap-free emulsion polymerization can each provide a particulate copolymer having a sharper particle size distribution than the particulate copolymer provided by suspension polymerization. In addition, when a ligand is bound to the particle to provide an affinity particle, there is a concern that the anionic or cationic surfactants typically used in the emulsion polymerization are present as residues and modify the ligand. In view of the foregoing, when the particulate copolymer is formed by emulsion polymerization, it is preferred to use a nonionic surfactant.
[0170] The reagent for detecting a target substance in a sample by in vitro diagnosis according to the second embodiment is characterized by containing the affinity particles according to the second embodiment as particles for a latex agglutination method.
[0171] The amount of the particles for latex agglomeration method contained in the reagent is preferably 0.001% by mass or more and 20% by mass or less, and more preferably 0.01% by mass or more and 10% by mass or less.
[0172] The reagent according to the second embodiment may further contain a third substance such as a solvent or a blocking agent in addition to the affinity particles according to the second embodiment, as long as the purpose of the second embodiment can be achieved.
[0173] Examples of the solvent to be used in the second embodiment include various aqueous buffers such as phosphate buffer, glycine buffer, Good's buffer, Tris buffer, HEPES buffer, MES buffer, and ammonia buffer. However, the solvent contained in the reagent according to the second embodiment is not limited thereto.
[0174] A kit for detecting a target substance in a test sample by in vitro diagnosis according to a second embodiment is characterized by comprising at least the reagent according to the second embodiment.
[0175] In addition to the reagent according to the second embodiment (hereinafter referred to as "reagent 1"), the kit according to the second embodiment preferably further contains a reaction buffer containing albumin (hereinafter referred to as "reagent 2"). The albumin is, for example, serum albumin, and may be subjected to protease treatment. As a standard, the amount of albumin contained in reagent 2 is 0.001% by mass or more and 5% by mass or less, but the amount of albumin in the kit according to the second embodiment is not limited thereto.
[0176] Each or one of the reagents 1 and 2 may contain a sensitizer for latex agglutination assay. Examples of the sensitizer for latex agglutination assay include polyvinyl alcohol, polyvinyl pyrrolidone, and alginic acid. However, the sensitizer to be used in the kit according to the second embodiment is not limited thereto.
[0177] In addition, the kit according to the second embodiment may contain, for example, a positive control, a negative control, or a serum dilution in addition to reagents 1 and 2. In addition to serum or saline that does not contain a target substance that can be measured, a solvent may be used as a medium for a positive control or a negative control.
[0178] The kit according to the second embodiment can be used for the method for detecting the target substance in the sample according to the second embodiment in the same manner as a conventional kit for detecting the target substance in the sample by in vitro diagnosis. In addition, the concentration of the target substance can be measured by a conventionally known method, and the method is particularly suitable for detecting the target substance in the sample by latex agglutination method.
[0179] The method for detecting a target substance in a sample by in vitro diagnosis according to the second embodiment is characterized by comprising mixing the affinity particles according to the second embodiment with a sample that may contain the target substance.
[0180] The affinity particles according to the second embodiment and the sample are preferably mixed in the range of pH 3.0 to 11.0. In addition, the mixing temperature falls within the range of 20°C to 50°C, and the mixing time falls within the range of 1 minute to 20 minutes. In addition, in this detection method, a solvent is preferably used. In addition, the concentration of the affinity particles according to the second embodiment in the reaction system in the detection method according to the second embodiment is preferably 0.001% by mass or more and 5% by mass or less, more preferably 0.01% by mass or more and 1% by mass or less. The detection method according to the second embodiment is characterized in that it includes optical detection of inter-particle agglutination caused by the result of mixing the affinity particles according to the second embodiment with the sample. When the inter-particle agglutination is optically detected, the target substance in the sample is detected, and the concentration of the target substance can be measured. As a method for optically detecting agglutination reactions, it is only necessary to use optical instruments that can detect scattered light intensity, transmitted light intensity, and absorbance to measure the amount of change in these values.
[0181] The measuring method of the dry particle size of the particles in the second embodiment is described. The dry particle size in the second embodiment is a number average particle size, and is measured in a state where the particles are fully dried. Specifically, the particles are dispersed in ion exchange water at a concentration of 5% by mass, and the dispersion is dripped onto an aluminum foil and then dried at 25°C for 48 hours. Thereafter, the dried product is further dried for 24 hours with a vacuum dryer and then measured. A scanning electron microscope and an image processing analyzer are used for the measurement of dry particle size. Specifically, for example, 100 single particles are randomly extracted from an image of particles in a dry state, and the image is obtained using a scanning electron microscope (trade name: S-4800, manufactured by Hitachi High-Technologies Corporation), and their number average particle size is calculated by analyzing the image with an image processing analyzer (trade name: Luzex AP, manufactured by Nireco Corporation).
[0182] The method for measuring the particle size in water of the particles in the second embodiment is described. The particle size in water in the second embodiment is a number average particle size, and is measured in a state where the particles are dispersed in ion exchange water so that their concentration can be 0.001% by mass. Ion exchange water with a conductivity of 10μS / cm or less is used as ion exchange water. The dynamic light scattering method is applied to the measurement of the particle size in water. Specifically, ZETASIZER (trade name: Nano-ZS, manufactured by Spectris Co., Ltd.) is used for measurement at 25°C. Regarding the analysis parameters, the refractive index of latex (n≈1.59) is selected as the refractive index of the particles, and pure water is selected as the solvent. The measurement is performed 10 times, and the average value of the 10 measured values is adopted as the particle size in water.
[0183] The method for measuring the particle size in water of the affinity particles in the second embodiment is described. The particle size in water in the second embodiment is the number average particle size, and is measured in a state where the affinity particles are dispersed in a 0.01N potassium aqueous solution at a pH of 7.8 so that their concentration can be 0.001% by mass. A solution obtained by appropriately mixing a 0.01N potassium chloride aqueous solution, a 0.01N potassium hydroxide aqueous solution, and a 0.01N hydrochloric acid aqueous solution (each of which is prepared by using ion exchange water with a conductivity of 10 μS / cm or less) is used as a 0.01N potassium aqueous solution at a pH of 7.8. Dynamic light scattering is applied to the measurement of particle size in water. Specifically, ZETASIZER (trade name: Nano-ZS, manufactured by Spectris Co., Ltd.) is used to measure at 25°C. Regarding the analysis parameters, the refractive index of latex (n≈1.59) is selected as the refractive index of the affinity particles, and pure water is selected as the solvent. The measurement is performed 10 times, and the average value of the 10 measured values is adopted as the particle size in water.
[0184] The method for measuring the zeta potential of the particles or affinity particles in the second embodiment is described. The zeta potential in the second embodiment is measured in a state where the particles are dispersed in a 0.01N potassium aqueous solution at a pH of 7.8 so that its concentration can be 0.001% by mass. A solution obtained by appropriately mixing a 0.01N potassium chloride aqueous solution, a 0.01N potassium hydroxide aqueous solution, and a 0.01N hydrochloric acid aqueous solution (each of which is prepared by using ion exchange water having a conductivity of 10μS / cm or less) is used as a 0.01N potassium aqueous solution at a pH of 7.8. The measurement is performed at 25°C by using ZETASIZER (trade name: Nano-ZS, manufactured by Spectris Co., Ltd.) as a measuring device. Regarding the analysis parameters, the refractive index of latex (n≈1.59) is selected as the refractive index of the particles, and pure water is selected as the solvent. The measurement is performed 10 times, and the average value of the 10 measured values is adopted as the zeta potential.
[0185] The method for measuring the zeta potential of the antibody in the second embodiment is described. The zeta potential of the antibody in the second embodiment is measured in a state where the antibody solution is diluted with a 0.01N potassium aqueous solution having a pH of 7.8 which is at least 10 times the amount of the solution so that the protein concentration is 0.5 mg / mL to 2.0 mg / mL. A solution obtained by appropriately mixing a 0.01N potassium chloride aqueous solution, a 0.01N potassium hydroxide aqueous solution, and a 0.01N hydrochloric acid aqueous solution (each of which is prepared by using ion exchange water having a conductivity of 10 μS / cm or less) is used as a 0.01N potassium aqueous solution having a pH of 7.8. ZETASIZER (trade name: Nano-ZS, manufactured by Spectris Co., Ltd.) is used as a measuring device for measurement at 25°C. With regard to the analysis parameters, the refractive index of the protein (n≈1.4) is selected as the refractive index of the antibody, and pure water is selected as the solvent. The measurement is performed 10 times, and the average value of the 10 measured values is adopted as the zeta potential.
[0186] [Third embodiment]
[0187] The third embodiment of the present invention is described in detail below, but the technical scope of the present invention is not limited to this embodiment. First, the background technology of the third embodiment and the problems to be solved by this embodiment are described.
[0188] (Background Technology of the Third Embodiment and Problems to be Solved by the Embodiment)
[0189] In recent years, research has been widely conducted on the use of affinity particles obtained by chemically bonding a ligand having an affinity for the target substance to particles to purify or quantify the target substance. It is expected that the particles to be used for such purposes will show the property of adsorbing substances other than the target substance to a small extent (i.e., the so-called non-specific adsorption). For example, in Bioseparation using Affinity Latex (1995), pages 11 to 30, resin particles (hereinafter referred to as "SG particles") having a surface covered with polyglycidyl methacrylate obtained by emulsion polymerization of two monomers including styrene and glycidyl methacrylate are disclosed. In addition, in Japanese Patent Application Laid-Open No. 2014-193972, a method for controlling the particle size of SG particles is disclosed.
[0190] In the SG particles, a part of the epoxy groups derived from polyglycidyl methacrylate undergoes ring opening to provide diols, and, as a result of the hydrophilicity of the diols, nonspecific adsorption is suppressed. At the same time, when the ligand is chemically bound to the surface of the SG particles, the epoxy groups derived from polyglycidyl methacrylate can be utilized as they are. However, in general cases, the following method is generally adopted: after going through a process of converting each epoxy group into another reactive functional group such as a carboxyl group, an amino group, or a thiol group, the reactive functional group and the ligand are chemically reacted with each other. Particles obtained by converting the epoxy groups of the SG particles into carboxyl groups among such groups are a preferred form because the particles have the highest versatility when the ligand is chemically bound to the particle surface.
[0191] In addition, in recent years, as a simple and rapid immunoassay method, the immunolatex agglutination assay has attracted attention. In this method, a dispersion of particles obtained by chemically binding an antibody or antigen as a ligand is mixed with a sample that may contain a target substance (antigen or antibody). At this time, when the sample contains the target substance (antigen or antibody), the particles cause an agglutination reaction, so the presence or absence of the disease can be determined by optically detecting the agglutination reaction as a change in, for example, scattered light intensity, transmitted light intensity or absorbance. For the purpose of reducing false positive noise, the particles to be used in the immunolatex agglutination assay preferably have a small nonspecific adsorption and have a reactive functional group for fixing the ligand, such as SG particles.
[0192] The present inventors synthesized SG particles according to Bioseparation using Affinity Latex (1995), pages 11 to 30, and chemically reacted amino acids with epoxy groups derived from glycidyl methacrylate of SG particles to provide particles in which epoxy groups were converted into carboxyl groups. However, the particles obtained as described above were inferior in ability to suppress nonspecific adsorption to SG particles.
[0193] Meanwhile, a method of introducing a carboxyl group into SG particles is known. The carboxyl group-introduced particles are obtained by treating the SG particles with aqueous ammonia; then chemically reacting the treated product with ethylene glycol diglycidyl ether; and chemically reacting an epoxy group derived from the above-mentioned ethylene glycol diglycidyl ether and an amino acid with each other. Although the particles obtained as described above surprisingly suppress nonspecific adsorption, the dispersion stability of the particles is so excellent that the particles hardly agglutinate with each other, so when the particles are used for the immunolatex agglutination method, sufficient sensitivity cannot be obtained in some cases. In addition, the particles obtained as described above involve a problem that the particles are not suitable for industrialization because the chemical reaction requires many processes and the processes are complicated.
[0194] In view of such background technology and problems, the third embodiment is made. The purpose of the third embodiment is to provide a particle that causes little nonspecific adsorption, has a reactive functional group for a chemically bound ligand, and is suitable for a latex agglutination method. Another purpose of the third embodiment is to provide particles for a latex agglutination method obtained by chemically binding a ligand, and an in vitro diagnostic reagent and a kit each containing the particles, and a method for detecting a target substance.
[0195] Specifically, the third embodiment aims to provide a particle having an ability to suppress nonspecific adsorption equivalent to or better than that of SG particles and having a reactive functional group capable of chemically binding a ligand to the particle surface at a high yield. Another object thereof is to provide a novel method for producing the particle simply and at a high yield. Still another object of the third embodiment is to provide an affinity particle obtained by chemically binding an antigen or antibody as a ligand, an in vitro diagnostic reagent and a kit each comprising the particle, and a method for detecting a target substance.
[0196] (Regarding the Effects of the Invention According to the Third Embodiment)
[0197] According to the third embodiment, it is possible to provide particles having an ability to suppress nonspecific adsorption equivalent to or better than that of SG particles and having reactive functional groups for chemically binding a ligand to the particle surface at a high yield, and a novel method for producing the particles simply and at a high yield. In addition, according to the third embodiment, it is possible to provide affinity particles obtained by chemically binding an antigen or antibody as a ligand, an in vitro diagnostic reagent and a kit each containing the particles, and a method for detecting a target substance.
[0198] Details about the particles of the third embodiment are described below.
[0199] The particles according to the third embodiment of the present invention include a copolymer. The repeating unit A in the copolymer has a reactive functional group for chemically bonding a ligand to its side chain. The repeating unit has a carboxyl group as a reactive functional group for chemically bonding a ligand to the side chain. Specifically, the particles according to this embodiment are characterized in that the particles include a copolymer containing "repeating unit A", and the repeating unit A is represented by formula (3-1).
[0200] [Chemical formula 8]
[0201]
[0202] In formula (3-1), R1 represents a methyl group or a hydrogen atom, R2 represents a carboxyl group or a hydrogen atom, and L1 represents an alkylene group having 1 to 15 carbon atoms which may be substituted or an oxyalkylene group having 1 to 15 carbon atoms which may be substituted.
[0203] The "repeating unit A" in the third embodiment has a carboxyl group across a thioether group. The carboxyl group is to be chemically bonded to the ligand, and when the particle has the structure of the repeating unit A, the ligand can be chemically bonded to the particle surface at a high yield. Therefore, when the particle is used for an immunolatex agglutination assay, the target substance can be detected with high sensitivity. Although the details of the foregoing situation are unknown, it is speculated that the foregoing situation is because the side chain of the repeating unit is hardly protonated compared to the case where the repeating unit has a carboxyl group via an amino group, thereby electrostatically stabilizing the particles. In addition, although the details of the mechanism of the foregoing situation are unknown, when the distance between the carboxylic acid and the thioether group is appropriately controlled, the target substance can be detected with high sensitivity.
[0204] In addition, the amount of carboxylic acid per unit mass of the particles of the third embodiment is preferably 5 [nmol / mg] or more, more preferably 100 [nmol / mg] or more. As a result, a large amount of ligands can be chemically bound to the particle surface at a high yield. Therefore, when the particles are used in an immunolatex agglutination assay, the target substance can be detected with high sensitivity. In addition, the amount of carboxylic acid per unit mass of the particles of the third embodiment is preferably 300 [nmol / mg] or less. When the amount of carboxylic acid per unit mass is controlled within this range, nonspecific adsorption of substances other than the target substance can be suppressed.
[0205] In addition, the number average particle size of the particles of the third embodiment is preferably 0.05 μm or more and 1 μm or less. When the number average particle size is controlled within this range, when the particles are used in an immunolatex agglutination assay, both the dispersion stability of the particles when not agglutinated and the turbidity change when agglutinated (i.e., excellent detection sensitivity) can be taken into account.
[0206] Furthermore, the particles of the third embodiment may be expressed in terms of the amount of carboxylic acid per unit area, and in this case, the amount of carboxylic acid per unit area is preferably 0.1 to 20 [molecules / nm 2 ]. The foregoing makes it possible to suppress nonspecific adsorption of substances other than the target substance, and to achieve both dispersion stability of particles when not agglomerated and turbidity change when agglomerated (ie, excellent detection sensitivity).
[0207] In addition, the particles of the third embodiment may contain a "repeating unit B" having a hydrophilic structure for suppressing nonspecific adsorption. A diol structure obtained by ring-opening a part of an epoxy group derived from polyglycidyl methacrylate, or a structure having a thioether group or a secondary amine and two hydroxyl groups on a side chain is preferably used as the "repeating unit B". The presence of these side chains can suppress nonspecific adsorption of substances other than the target substance.
[0208] In addition, from the viewpoint of particle strength and solvent resistance, the particles of the third embodiment may contain a "repeating unit C" having a hydrophobic structure. Although the chemical structure of the "repeating unit C" is not limited within the scope of achieving the purpose of the third embodiment, at least one selected from the group consisting of styrenes and (meth) acrylates is preferred. It is preferred that the repeating unit C is derived from styrene or methyl methacrylate or both of the aforementioned compounds, because the repeating unit C has a high glass transition temperature, so the particles have sufficient strength. The following describes examples of styrenes and (meth) acrylates that can be used for the "repeating unit C", but the "repeating unit C" is not limited thereto. In addition, the hydrophobic "repeating unit C" can use two or more oily free radical polymerizable monomers.
[0209] Examples of styrenes include styrene, α-methylstyrene, β-methylstyrene, o-methylstyrene, m-methylstyrene, p-methylstyrene, 2,4-dimethylstyrene, p-n-butylstyrene, p-tert-butylstyrene, p-n-hexylstyrene, p-n-octylstyrene, p-n-nonylstyrene, p-n-decylstyrene, p-n-dodecylstyrene, p-methoxystyrene, and p-phenylstyrene.
[0210] Examples of the (meth)acrylates include methyl acrylate, ethyl acrylate, n-propyl acrylate, isopropyl acrylate, n-butyl acrylate, isobutyl acrylate, tert-butyl acrylate, n-pentyl acrylate, n-hexyl acrylate, 2-ethylhexyl acrylate, n-octyl acrylate, n-nonyl acrylate, cyclohexyl acrylate, benzyl acrylate, dimethyl phosphate ethyl acrylate, diethyl phosphate ethyl acrylate, dibutyl phosphate ethyl acrylate, 2-benzoyloxyethyl acrylate, methyl methacrylate, ethyl methacrylate, n-propyl methacrylate, isopropyl methacrylate, n-butyl methacrylate, isobutyl methacrylate, tert-butyl methacrylate, n-pentyl methacrylate, n-hexyl methacrylate, 2-ethylhexyl methacrylate, n-octyl methacrylate, n-nonyl methacrylate, diethyl phosphate ethyl methacrylate, and dibutyl phosphate ethyl methacrylate.
[0211] In addition, in the third embodiment, in order to further improve the strength of the particles, a cross-linking free radical polymerizable monomer may be included. The cross-linking free radical polymerizable monomer is a compound having two or more free radical polymerizable groups in the molecule, and examples thereof may include: free radical polymerizable aromatic compounds each having two or more free radical polymerizable groups and an aromatic ring, for example, aromatic divinyl compounds such as divinylbenzene (DVB), divinyltoluene, divinylxylene, divinylanthracene, divinylnaphthalene and divinyldurene, aromatic trivinyl compounds such as trivinylbenzene, and aromatic tetravinyl compounds such as tetravinylbenzene; and free radical polymerizable aliphatic compounds each having two or more free radical polymerizable groups and an aliphatic group, such as pentaerythritol tetraacrylate.
[0212] Furthermore, when the hydrophobic repeating unit C is used, the composition ratio of the repeating units A, B, and C is not limited within the range in which the object of the third embodiment can be achieved.
[0213] The particle size of the particles of the third embodiment is 0.05 μm or more and 1 μm or less, preferably 0.1 μm or more and 0.5 μm or less, and more preferably 0.15 μm or more and 0.3 μm or less in terms of number average particle size in water. When the particle size is 0.15 μm or more and 0.3 μm or less, the particles are excellent in operability in centrifugal operation, and the large specific surface area that is a characteristic of the particles becomes prominent. The number average particle size of the particles of the third embodiment is evaluated by a dynamic light scattering method.
[0214] Furthermore, the third embodiment relates to affinity particles obtained by chemically bonding a carboxyl group of the “repeating unit A” derived from the particles of the third embodiment and a ligand to each other.
[0215] A ligand is a compound that specifically binds to a receptor possessed by a specific target substance. The site where the ligand binds to the target substance is determined, and the ligand has a high affinity that is selective or specific for the target substance. Examples of ligands include: antigens and antibodies; enzyme proteins and their substrates; signal substances such as hormones or neurotransmitters and their receptors; nucleic acids; and avidin and biotin. However, the ligand is not limited to this. Specific examples of ligands include antigens, antibodies, antigen-binding fragments (e.g., Fab, F(ab')2, F(ab'), Fv or scFv), naturally occurring nucleic acids, artificial nucleic acids, aptamers, peptide aptamers, oligopeptides, enzymes and coenzymes. The affinity particles in the third embodiment mean particles that have a high affinity that is selective or specific for the target substance.
[0216] In the third embodiment, conventionally known methods can be applied as methods for chemical reactions for chemically binding carboxyl groups of "repeating unit A" of particles derived from the third embodiment and ligands to each other, as long as the purpose of the third embodiment can be achieved. For example, carbodiimide-mediated reactions or NHS ester activation reactions are frequently used chemical reaction methods. In addition, the following method is available: binding avidin to the carboxyl groups of particles, and binding a biotin-modified ligand to avidin. However, the method for chemical reactions for chemically binding carboxyl groups of "repeating unit A" of particles derived from the third embodiment and ligands to each other is not limited thereto.
[0217] When an antibody (antigen) is used as a ligand and an antigen (antibody) is used as a target substance, the affinity particles of the third embodiment can be preferably applied to the immunolatex agglutination assay which has been widely used in fields such as clinical testing and biochemical research. When conventional particles are applied to the immunolatex agglutination assay, there is a problem that the antigen (antibody) as the target substance or foreign matter in the serum is nonspecifically adsorbed to the particle surface, and unexpected particle agglutination caused by the adsorption is detected, thereby preventing accurate measurement.
[0218] Therefore, for the purpose of reducing false positive noise, etc., particles coated with biologically derived substances such as albumin are generally used as blocking agents, so that nonspecific adsorption to the particle surface can be suppressed. However, the properties of such biologically derived substances vary slightly from batch to batch, so the ability of particles coated with such substances to suppress nonspecific adsorption varies depending on the coating treatment. Therefore, there is a problem in stably supplying particles with the same level of ability to suppress nonspecific adsorption. In addition, the biologically derived substances coated on the particle surface may become hydrophobic when modified, and therefore may not necessarily be excellent in the ability to suppress nonspecific adsorption. Biological contamination is also a problem.
[0219] In patent document 2, an affinity particle for in vitro diagnosis is disclosed, characterized in that the particle is coated with a polymer having a repeating unit with a sulfenyl group on the side chain, and the polymer is used as a blocking agent. However, the polymer having a repeating unit with a sulfenyl group on the side chain is water-soluble and covers the particle surface by physical adsorption, so, in essence, it is worried that the copolymer will be free due to its dilution. In addition, the inventors evaluated the ability of the SG particles obtained by the method described in Bioseparation using Affinity Latex (1995) pages 11 to 30 and the particles obtained by adsorbing the polymer in chyle to the polystyrene particles obtained by the method described in Japanese Patent Application Laid-Open No. 2014-153140 to inhibit nonspecific adsorption.
[0220] In the particles obtained by the method described in Japanese Patent Application Laid-Open No. 2014-153140, a polymer having a repeating unit having a sulfide group on a side chain is obtained by soap-free emulsion polymerization.
[0221] As a result, although there is a possibility that Bioseparation using Affinity Latex (1995) pages 11 to 30 cannot be completely reproduced, the SG particles are more excellent in the ability to suppress nonspecific adsorption than the particles obtained by the method described in Japanese Patent Application Laid-Open No. 2014-153140. Herein, the SG particles are particles obtained by converting epoxy groups derived from glycidyl methacrylate into diols by heating in an acidic aqueous solution.
[0222] The reagent for detecting a target substance in a sample by in vitro diagnosis of the third embodiment is characterized in that it contains the affinity particles of the third embodiment. The amount of the affinity particles of the third embodiment contained in the reagent of the third embodiment is preferably 0.001 mass % to 20 mass %, more preferably 0.01 mass % to 10 mass %. In addition to the affinity particles of the third embodiment, the reagent of the third embodiment may also contain a third substance such as a solvent or a blocking agent, as long as the purpose of the third embodiment can be achieved. The reagent may contain two or more third substances such as a solvent and a blocking agent in combination. Examples of the solvent to be used in the third embodiment include various buffers, such as phosphate buffer, glycine buffer, Tris buffer, ammonia buffer, and МES (2-morpholinoethanesulfonic acid), ADA (N-(2-acetamido)iminodiacetic acid), PIPES (piperazine-1,4-bis(2-ethanesulfonic acid)), ACES (N-(2-acetamido)-2-aminoethanesulfonic acid), cholestyrene chloride, BES (N,N-bis(2-hydroxyethyl)-2-aminoethanesulfonic acid), TES (N-tris(hydroxymethyl)methyl-2-aminoethanesulfonic acid), HEPES (2-[4-(2-hydroxyethyl)-1-piperazinyl]ethanesulfonic acid), acetylaminoglycine, tris(hydroxymethyl)methylglycine (tricine), glycineamide, and Good's buffer of N,N-dihydroxyethylglycine (bicine). However, the solvent contained in the reagent of the third embodiment is not limited thereto.
[0223] The kit for detecting the target substance in the test specimen by in vitro diagnosis of the third embodiment is characterized in that it contains at least the reagent of the third embodiment. In addition to the reagent of the third embodiment (hereinafter referred to as "reagent 1"), the kit of the third embodiment preferably further contains a reaction buffer containing albumin (hereinafter referred to as "reagent 2"). Albumin is, for example, serum albumin, and can be treated with protease. As a standard, the amount of albumin contained in reagent 2 is 0.001% by mass to 5% by mass, but the amount of albumin in the kit of the third embodiment is not limited to this. Each of reagent 1 and reagent 2 or one of them can contain a sensitizer for latex agglutination determination. Examples of sensitizers for latex agglutination determination include polyvinyl alcohol, polyvinyl pyrrolidone and alginic acid. However, the sensitizer to be used for the kit of the third embodiment is not limited to this. In addition, in addition to reagent 1 and reagent 2, the kit of the third embodiment can contain, for example, a positive control, a negative control or a serum diluent. In addition to serum or saline containing the target substance that can be measured, a solvent can also be used as a medium for a positive control or a negative control. The kit of the third embodiment can be used for the method for detecting the target substance in the third embodiment in the same manner as a conventional kit for detecting the target substance in a sample by in vitro diagnosis. In addition, the concentration of the target substance can be measured by a conventionally known method, and the method is particularly suitable for detecting the target substance in a sample by agglutination method, particularly latex agglutination method.
[0224] The method for detecting the target substance in the sample by in vitro diagnosis of the third embodiment is characterized in that it includes mixing the affinity particles of the third embodiment with a sample that may contain the target substance, and can be used for agglutination method. In addition, the affinity particles of the third embodiment and the sample are preferably mixed in the range of pH 3.0 to 11.0. In addition, the mixing temperature falls within the range of 20°C to 50°C, and the mixing time falls within the range of 1 minute to 20 minutes. In addition, in this detection method, a solvent is preferably used. In addition, the concentration of the affinity particles of the third embodiment in the detection method of the third embodiment in the reaction system is preferably 0.001% by mass to 5% by mass, more preferably 0.01% by mass to 1% by mass. The detection method of the third embodiment is characterized in that it includes optical detection of the agglutination reaction caused by the result of mixing the affinity particles of the third embodiment with the sample. When the agglutination reaction is optically detected, the target substance in the sample is detected, and the concentration of the target substance can be measured. As a method for optically detecting agglutination reaction, it is only necessary to use an optical instrument that can detect scattered light intensity, transmitted light intensity, absorbance, etc. to measure the change in these values.
[0225] Next, a preferred method for producing the particles of the third embodiment is described.
[0226] The third embodiment is a method for producing particles, the method being characterized by comprising: step 1 of mixing glycidyl (meth)acrylate, styrene or methyl (meth)acrylate, water and a radical polymerization initiator to form a granular copolymer, thereby providing an aqueous dispersion of the granular copolymer; and step 2 of mixing the aqueous dispersion with mercaptosuccinic acid or mercaptopropionic acid to prepare a mixed solution, and then reacting an epoxy group derived from glycidyl (meth)acrylate of the granular copolymer and a thiol group derived from mercaptosuccinic acid or mercaptopropionic acid with each other.
[0227] First, operation 1 is described. Operation 1 is a process for forming a granular copolymer, but the method for forming the granular copolymer is not limited to free radical polymerization, as long as the purpose of the third embodiment can be achieved. Among various free radical polymerizations, it is preferred to use emulsion polymerization, soap-free emulsion polymerization or suspension polymerization, and it is more preferred to use emulsion polymerization or soap-free emulsion polymerization. It is also more preferred to use soap-free emulsion polymerization. Usually, emulsion polymerization and soap-free emulsion polymerization can each provide a granular copolymer with a sharper particle size distribution than the granular copolymer provided by suspension polymerization. In addition, when the particles are chemically bonded to the ligand, it is feared that the presence of such anionic surfactants that are usually used for emulsion polymerization will modify the ligand. Therefore, the method for forming the granular copolymer is most preferably soap-free emulsion polymerization.
[0228] The free radical polymerization initiator preferably used in step 1 is one of 4,4′-azobis(4-cyanovaleric acid), 2,2′-azobis[2-methyl-N-(2-hydroxyethyl)propionamide], 2,2′-azobis[N-(2-carboxyethyl)-2-methylpropionamidine] tetrahydrate, 2,2′-azobis(2-methylpropionamidine) dihydrochloride, 2,2′-azobis[2-(2-imidazolin-2-yl)propane], 2,2′-azobis[2-(2-imidazolin-2-yl)propane] dihydrochloride and 2,2′-azobis[2-(2-imidazolin-2-yl)propane] disulfate dihydrate. Among them, it is more preferred to use one of 2,2′-azobis[2-(2-imidazolin-2-yl)propane] dihydrochloride, 2,2′-azobis[2-(2-imidazolin-2-yl)propane] disulfate dihydrate, 2,2′-azobis(2-methylpropionamidine) dihydrochloride, and 2,2′-azobis[2-(2-imidazolin-2-yl)propane]. This is because in step 1 of providing an aqueous dispersion of a granular copolymer, it is necessary to prevent the ring opening of the epoxy group derived from glycidyl (meth)acrylate. For example, when potassium persulfate is used as a free radical polymerization initiator, the free radical polymerization reaction field becomes acidic under the influence of the initiator residue, so the epoxy group derived from glycidyl (meth)acrylate can react with water to form a diol. In addition, when ammonium persulfate is used as a free radical polymerization initiator, the epoxy group derived from glycidyl (meth)acrylate and ammonia can react with each other. In addition, when an anionic free radical polymerization initiator having a carboxyl group is used as a free radical polymerization initiator, the epoxy group derived from glycidyl (meth)acrylate and the carboxyl group derived from the polymerization initiator react with each other to agglomerate the particles of the granular copolymer. A possible means for avoiding agglomeration is as follows: the granular copolymer is formed at a temperature significantly lower than the 10-hour half-life temperature of the free radical polymerization initiator. However, this means is not suitable for industrialization because a large amount of free radical polymerization initiator is required and the free radical polymerization time becomes long.
[0229] In addition, in step 1, it is preferred that a cross-linking free radical polymerizable monomer is further contained in addition to glycidyl (meth)acrylate and styrene or methyl (meth)acrylate. The inclusion of a cross-linking free radical polymerizable monomer makes the obtained granular copolymer physically strong, and therefore, there is no need to worry about the copolymer being broken or fragmented even when centrifugation is repeated during purification.
[0230] The following lists examples of crosslinkable free radical polymerizable monomers that can be used in the third embodiment, but the third embodiment is not limited thereto. In addition, two or more oily free radical polymerizable monomers can be used. Among the exemplified free radical polymerizable monomers, divinylbenzene is preferably used due to its excellent operability during free radical polymerization, although the reason why divinylbenzene is excellent in operability is unknown.
[0231] Examples of the crosslinkable free radical polymerizable monomer include diethylene glycol diacrylate, triethylene glycol diacrylate, tetraethylene glycol diacrylate, polyethylene glycol diacrylate, 1,6-hexanediol diacrylate, neopentyl glycol diacrylate, tripropylene glycol diacrylate, polypropylene glycol diacrylate, 2,2′-bis(4-(acryloxydiethoxy)phenyl)propane, trimethylolpropane triacrylate, tetramethylolmethane tetraacrylate, ethylene glycol dimethacrylate, diethylene glycol dimethacrylate, triethylene glycol dimethacrylate, Tetraethylene glycol dimethacrylate, polyethylene glycol dimethacrylate, 1,3-butanediol dimethacrylate, 1,6-hexanediol dimethacrylate, neopentyl glycol dimethacrylate, polypropylene glycol dimethacrylate, 2,2′-bis(4-(methacryloxydiethoxy)phenyl)propane, 2,2′-bis(4-(methacryloxypolyethoxy)phenyl)propane, trimethylolpropane trimethacrylate, tetramethylolmethane tetramethacrylate, divinylbenzene, divinylnaphthalene, and divinyl ether.
[0232] In addition, step 1 preferably further comprises a step of further mixing glycidyl (meth)acrylate into the mixture during the formation of the granular copolymer to cover the surface of the granular copolymer with polyglycidyl (meth)acrylate. Herein, the state in which the surface is coated with the polymer may be any bonding state. That is, the polymer does not necessarily need to cover the entire particle, and may cover a portion of the particle, and the layer covering the polymer may not be uniform.
[0233] Next, the step 2 is described. The step 2 is a step of reacting an epoxy group derived from glycidyl (meth)acrylate of the particulate copolymer and a thiol group derived from mercaptosuccinic acid or mercaptopropionic acid with each other to introduce a carboxyl group via a thioether group.
[0234] In step 2, an alkaline component may be added to adjust the pH of the mixed solution. Although there is no particular limitation on the alkaline component, an organic base having a secondary amine or a tertiary amine is preferably used. For example, pyridine, triethylamine, diazabicycloundecene or 1,8-bis(dimethylamino)naphthalene is preferably used as the organic base having a secondary amine or a tertiary amine, and triethylamine is more preferably used. Two or more organic bases may be used in combination.
[0235] Furthermore, in step 2, the amount of carboxylic acid can be controlled by adjusting the pH of the mixed solution. In particular, when the pH is adjusted to a range greater than 9.0, a large amount of carboxylic acid can be added to the particles to be produced. Furthermore, it is more preferable to set the pH to greater than 10.0 because a larger amount of carboxylic acid can be added to the particles to be produced.
[0236] <Carboxylic acid quantitative analysis method>
[0237] First, a method for measuring the amount of carboxyl groups on particles is described. By using 1-ethyl-3-(3-dimethylaminopropyl)carbodiimide hydrochloride (EDC / HCl) as a catalyst, the carboxyl groups on the particles are esterified with N-hydroxysuccinimide (NHS) to make them active. Thereafter, the active ester is reacted with aminoethanol to liberate NHS, and the amount of carboxyl groups per unit particle mass is calculated by measuring the amount of free NHS using a high-performance liquid chromatography device. The unit of the amount of carboxyl groups per unit particle mass is nmol / mg. The specific method is described below.
[0238] <Active esterification>
[0239] Aqueous dispersion of particles containing 2.5 mg of particles is added to a 1.5 mL microtube, and the particles are separated from the dispersion using a centrifuge. In addition, the particles are redispersed in dimethylformamide (DMF). The above operations are performed three times. In addition, while the particles are sedimented in the microtube using a centrifuge, the DMF is removed from the microtube. Next, 400 μL of DMF, 19.2 mg of EDC·HCl, and 100 μL of a 1 mol / L DMF solution of N-hydroxysuccinimide are added to the microtube, and the mixture is shaken at 25 °C for 2 hours to esterify the carboxyl groups on the particles to make them active.
[0240] <Liberation of NHS>
[0241] To remove the excess NHS from the DMF dispersion of the active-esterified particles, the active-esterified particles are separated from the dispersion using a centrifuge, and the particles are redispersed in DMF; the above operations are performed three times. In addition, while the active-esterified particles are sedimented in the microtube using a centrifuge, the DMF is removed from the microtube. Next, 500 μL of a 1 mol / L DMF solution of aminoethanol is added to the microtube, and the mixture is shaken at 25 °C for 2 hours to liberate NHS from the particles.
[0242] <Quantification of NHS>
[0243] The DMF dispersion of the particles containing free NHS is centrifuged, and the DMF solution containing free NHS is recovered while the particles are sedimented in the microtube, and then the amount of free NHS in the DMF solution is quantified using a high-performance liquid chromatography device. The amount of carboxyl groups per unit particle mass is calculated using the quantified value.
[0244] The instruments and reagents to be used for the quantification of the amount of carboxyl groups are described below.
[0245] <Instruments>
[0246] High performance liquid chromatography equipment: LC20A-FL (Shimadzu Corporation)
[0247] Column: Kinetex 5μm C18 100ALC column 150×4.6mm (Phenomenex)
[0248] Eluent: 4 mmol / L ammonium acetate aqueous solution
[0249] Flow rate: 1.0mL / min
[0250] Oven temperature: 40℃
[0251] Sample injection volume: 1μL
[0252] When the amount of free NHS contained in the DMF solution was quantified, a calibration curve between the peak area derived from NHS and the amount of NHS was prepared in the range of 0.1 mmol / L to 10 mmol / L, and the amount of free NHS was quantified from the NHS peak area.
[0253] <Reagents>
[0254] EDC / HCl(Dojindo Laboratories)
[0255] NHS(Kishida Chemical Co.,Ltd.)
[0256] Aminoethanol (Tokyo Chemical Industry Co., Ltd.)
[0257] DMF(FUJIFILM Wako Pure Chemical Corporation)
[0258] Ammonium acetate (Tokyo Chemical Industry Co., Ltd.)
[0259] Example
[0260] Hereinafter, the present invention is described in detail by way of examples corresponding to the first embodiment. However, the present invention is not limited to these examples.
[0261] [Example 1-1]
[0262] (Synthesis of Granular Copolymer 1-1)
[0263] 22.7 g of styrene (St: Kishida Chemical Co., Ltd.), 33.9 g of glycidyl methacrylate (GMA: Tokyo Chemical Industry Co., Ltd.), 0.86 g of divinylbenzene (DVB: Kishida Chemical Co., Ltd.) and 2,168.6 g of ion exchange water were weighed in a 2L four-necked separable flask to provide a mixed solution. Thereafter, the mixed solution was maintained at 70°C while stirring at 200 rpm, and nitrogen was allowed to flow at a flow rate of 200 mL / min to remove oxygen from the inside of the four-necked separable flask. Next, a separately prepared solution obtained by dissolving 1.13 g of V-50 (FUJIFILM Wako Pure Chemical Corporation) in 30 g of ion exchange water was added to the mixed solution to initiate soap-free emulsion polymerization. Two hours after the start of the polymerization, 5.8 g of GMA was added to the four-necked separable flask, and the mixture was maintained at 70°C while stirring at 200 rpm for 22 hours. Thus, an aqueous dispersion containing the granular copolymer 1-1 was obtained. After the dispersion was gradually cooled to room temperature, a portion of the dispersion was collected, and its polymerization conversion was evaluated by using proton NMR, gas chromatography and gel permeation chromatography. As a result, it was confirmed that the polymerization conversion was substantially 100%. The dry particle size of the granular copolymer 1-1 was 196.6 nm and the particle size in water was 206.9 nm. The granular copolymer 1-1 was concentrated by ultrafiltration or diluted by adding ion exchange water to become a 2.5 wt % aqueous dispersion, and the dispersion was stored at 4° C. under light-shielding conditions.
[0264] [Example 1-2]
[0265] (Synthesis of Granular Copolymer 1-2)
[0266] Except that 22.7g St was changed to 12.0g, 33.9g GMA was changed to 17.9g, 0.86g divinylbenzene was changed to 0.45g, and the amount of GMA to be added to the four-necked separable flask after 2 hours of the polymerization was changed from 5.8g to 3.1g in Example 1-1, an aqueous dispersion of granular copolymer 2 was obtained in the same manner as in Example 1-1. After the dispersion was gradually cooled to room temperature, a portion of the dispersion was collected, and its polymerization conversion was evaluated by using proton NMR, gas chromatography and gel permeation chromatography. As a result, it was confirmed that the polymerization conversion was substantially 100%. The dry particle size of granular copolymer 1-2 was 151.4nm and the particle size in water was 160.2nm. Granular copolymer 1-2 was concentrated by ultrafiltration or diluted by adding ion exchange water to become a 2.5wt% aqueous dispersion, and the dispersion was stored at 4°C under light-shielding conditions.
[0267] [Examples 1-3]
[0268] (Synthesis of Granular Copolymer 1-3)
[0269] Except that 22.7 g of St was changed to 5.0 g, 33.9 g of GMA was changed to 7.5 g, 0.86 g of divinylbenzene was changed to 0.19 g, and the amount of GMA to be added to the four-necked separable flask after 2 hours of the polymerization was changed from 5.8 g to 1.3 g in Example 1-1, an aqueous dispersion of granular copolymer 1-3 was obtained in the same manner as in Example 1-1. After the dispersion was gradually cooled to room temperature, a portion of the dispersion was collected, and its polymerization conversion was evaluated by using proton NMR, gas chromatography and gel permeation chromatography. As a result, it was confirmed that the polymerization conversion was substantially 100%. The dry particle size of granular copolymer 1-3 was 96.8 nm and the particle size in water was 105.2 nm. Granular copolymer 1-3 was concentrated by ultrafiltration or diluted by adding ion exchange water to become a 2.5 wt % aqueous dispersion, and the dispersion was stored at 4° C. under light-shielding conditions.
[0270] [Examples 1-4]
[0271] (Synthesis of Particle 1-1)
[0272] 24 g of a 2.5 wt% aqueous dispersion of the granular copolymer 1-1, 3.3 g of ion exchange water, 40 mg (0.26 mmol) of mercaptosuccinic acid (FUJIFILM Wako Pure Chemical Corporation) and 0.214 mL (2.34 mmol) of 3-mercapto-1,2-propanediol (FUJIFILM Wako Pure Chemical Corporation) were weighed in a 100 ml round-bottom flask, and triethylamine (Kishida Chemical Co., Ltd.) was added to the mixture to adjust its pH to 10. Next, the contents of the round-bottom flask were heated to 70° C. while stirring the contents at 200 rpm. In addition, the contents were kept in this state for 4 hours to provide a dispersion of particles 1-1. The particles 1-1 were separated from the dispersion with a centrifugal separator, and the particles 1-1 were redispersed in ion exchange water; this operation was repeated 8 times to purify the particles 1-1, and the concentration of the particles 1-1 was finally adjusted to 1.0 wt% in the state of an aqueous dispersion. The storage condition was set to 4° C. under light-shielding conditions. Table 1-1 summarizes the particle properties of the particles 1-1.
[0273] [Examples 1-5]
[0274] (Synthesis of Particles 1-2)
[0275] A 1.0 wt % aqueous dispersion of Granules 1-2 was obtained in the same manner as in Example 1-4 except that the holding time after heating the contents of the round-bottom flask to 70° C. was changed from 4 hours to 6 hours. Table 1-1 summarizes the particle properties of Granules 1-2.
[0276] [Examples 1-6]
[0277] (Synthesis of Particles 1-3)
[0278] A 1.0 wt % aqueous dispersion of Granules 1-3 was obtained in the same manner as in Example 1-4 except that the holding time after heating the contents of the round-bottom flask to 70° C. was changed from 4 hours to 8 hours. Table 1-1 summarizes the particle properties of Granules 1-3.
[0279] [Examples 1-7]
[0280] (Synthesis of Particles 1-4)
[0281] A 1.0 wt % aqueous dispersion of Granules 1-4 was obtained in the same manner as in Example 1-4 except that the holding time after heating the contents of the round-bottom flask to 70° C. was changed from 4 hours to 12 hours. Table 1-1 summarizes the particle properties of Granules 1-4.
[0282] [Examples 1-8]
[0283] (Synthesis of Particles 1-5)
[0284] A 1.0 wt % aqueous dispersion of Granules 1-5 was obtained in the same manner as in Example 1-4 except that the holding time after heating the contents of the round-bottom flask to 70° C. was changed from 4 hours to 18 hours. Table 1-1 summarizes the particle properties of Granules 1-5.
[0285] [Examples 1-9]
[0286] (Synthesis of Particles 1-6)
[0287] A 1.0 wt% aqueous dispersion of Granules 1-6 was obtained in the same manner as in Example 1-8 except that Granules Copolymer 1-1 of Example 1-8 was changed to Granules Copolymer 1-2. Table 1-1 summarizes the particle properties of Granules 1-6.
[0288] [Examples 1-10]
[0289] (Synthesis of Particles 1-7)
[0290] A 1.0 wt% aqueous dispersion of Granules 1-7 was obtained in the same manner as in Example 1-8 except that Granules Copolymer 1-1 of Example 1-8 was changed to Granules Copolymer 1-3. Table 1-1 summarizes the particle properties of Granules 1-7.
[0291] [Examples 1-11]
[0292] (Synthesis of Particles 1-8)
[0293] 24 g of a 2.5 wt% aqueous dispersion of the granular copolymer 1-1, 3.3 g of ion exchanged water, 0.046 mL (0.52 mmol) of mercaptopropionic acid (FUJIFILM Wako Pure Chemical Corporation) and 0.190 mL (2.08 mmol) of 3-mercapto-1,2-propanediol (FUJIFILM Wako Pure Chemical Corporation) were weighed in a 100 ml round-bottom flask, and triethylamine (Kishida Chemical Co., Ltd.) was added to the mixture to adjust its pH to 10. Next, the contents of the round-bottom flask were heated to 70° C. while stirring the contents at 200 rpm. Furthermore, the contents were kept in this state for 18 hours to provide a dispersion of particles 1-8. Particles 1-8 were separated from the dispersion using a centrifugal separator, and the particles 1-8 were redispersed in ion exchange water; this operation was repeated 8 times to purify the particles 1-8, and stored in the state of an aqueous dispersion in which the concentration of the particles 1-8 was finally adjusted to 1.0 wt%. The storage conditions were set to 4° C. under light shielding conditions. Table 1-1 summarizes the particle properties of particles 1-8.
[0294] [Examples 1-12]
[0295] (Synthesis of Particles 1-9)
[0296] A 1.0 wt% aqueous dispersion of Particles 1-9 was obtained in the same manner as in Example 1-4, except that the pH was changed from pH 10 to pH 11 and the holding time after the content of the round-bottom flask was heated to 70° C. was changed from 4 hours to 18 hours. Table 1-1 summarizes the particle properties of Particles 1-9.
[0297] [Examples 1-13]
[0298] (Synthesis of Particles 1-10)
[0299] A 1.0 wt% aqueous dispersion of Granules 1-10 was obtained in the same manner as in Example 1-4, except that the pH was changed from pH 10 to pH 11 and the holding time after the temperature of the contents of the round-bottom flask was raised to 70° C. was changed from 4 hours to 30 hours. Table 1-1 summarizes the particle properties of Granules 1-10.
[0300] [Examples 1-14]
[0301] (Synthesis of Particles 1-11)
[0302] A 1.0 wt% aqueous dispersion of particles 1-11 was obtained in the same manner as in Example 1-4, except that the pH was changed from pH 10 to pH 11 and the holding time after the content of the round-bottom flask was heated to 70° C. was changed from 4 hours to 48 hours. Table 1-1 summarizes the particle properties of particles 1-11.
[0303] [Examples 1-15]
[0304] (Synthesis of Particles 1-12)
[0305] A 1.0 wt% aqueous dispersion of Particles 1-12 was obtained in the same manner as in Example 1-11, except that mercaptopropionic acid was changed to 323 mg (2.08 mmol) of mercaptosuccinic acid and the amount of 3-mercapto-1,2-propanediol was changed to 0.047 mL (0.52 mmol). Table 1-1 summarizes the particle properties of Particles 1-12.
[0306] [Examples 1-16]
[0307] (Synthesis of Particles 1-13)
[0308] A 1.0 wt% aqueous dispersion of Particles 1-13 was obtained in the same manner as in Example 1-15, except that the amount of mercaptosuccinic acid was changed to 282 mg (1.82 mmol) and the amount of 3-mercapto-1,2-propanediol was changed to 0.071 mL (0.78 mmol). Table 1-1 summarizes the particle properties of Particles 1-13.
[0309] [Example 1-17]
[0310] (Synthesis of Particles 1-14)
[0311] A 1.0 wt% aqueous dispersion of Granules 1-14 was obtained in the same manner as in Example 1-15, except that the amount of mercaptosuccinic acid was changed to 242 mg (1.56 mmol) and the amount of 3-mercapto-1,2-propanediol was changed to 0.095 mL (1.04 mmol). Table 1-1 summarizes the particle properties of Granules 1-14.
[0312] [Examples 1-18]
[0313] (Synthesis of Particles 1-15)
[0314] A 1.0 wt% aqueous dispersion of Granules 1-15 was obtained in the same manner as in Example 1-15, except that the amount of mercaptosuccinic acid was changed to 202 mg (1.30 mmol) and the amount of 3-mercapto-1,2-propanediol was changed to 0.119 mL (1.30 mmol). Table 1-1 summarizes the particle properties of Granules 1-15.
[0315] [Example 1-19]
[0316] (Synthesis of Particles 1-16)
[0317] A 1.0 wt% aqueous dispersion of Particles 1-16 was obtained in the same manner as in Example 1-15, except that the amount of mercaptosuccinic acid was changed to 81 mg (0.52 mmol) and the amount of 3-mercapto-1,2-propanediol was changed to 0.191 mL (2.08 mmol). Table 1-1 summarizes the particle properties of Particles 1-16.
[0318] [Examples 1-20]
[0319] (Synthesis of Particles 1-17)
[0320] A 1.0 wt% aqueous dispersion of Particles 1-17 was obtained in the same manner as in Example 1-15, except that the amount of mercaptosuccinic acid was changed to 20 mg (0.13 mmol) and the amount of 3-mercapto-1,2-propanediol was changed to 0.225 mL (2.47 mmol). Table 1-1 summarizes the particle properties of Particles 1-17.
[0321] [Comparative Example 1-1]
[0322] (Synthesis of Particles 1-18)
[0323] A 1.0 wt % aqueous dispersion of Granules 1-18 was obtained in the same manner as in Example 1-4 except that the holding time after heating the contents of the round-bottom flask to 70° C. was changed from 4 hours to 3 hours. Table 1-1 summarizes the particle properties of Granules 1-18.
[0324] [Comparative Example 1-2]
[0325] (Synthesis of Particles 1-19)
[0326] A 1.0 wt% aqueous dispersion of Particles 1-19 was obtained in the same manner as in Example 1-4, except that the pH was changed from pH 10 to pH 11 and the holding time after the content of the round-bottom flask was heated to 70° C. was changed from 4 hours to 60 hours. Table 1-1 summarizes the particle properties of Particles 1-19.
[0327] [Comparative Examples 1-3]
[0328] (Synthesis of Particles 1-20)
[0329] A 1.0 wt % aqueous dispersion of Granules 1-20 was obtained in the same manner as in Example 1-15, except that the amount of mercaptosuccinic acid was changed to 403 mg (2.60 mmol) and 3-mercapto-1,2-propanediol was not used. Table 1-1 summarizes the particle properties of Granules 1-20.
[0330] [Comparative Examples 1-4]
[0331] (Synthesis of Particles 1-21)
[0332] A 1.0 wt% aqueous dispersion of Particles 1-21 was obtained in the same manner as in Example 1-15, except that the amount of mercaptosuccinic acid was changed to 8 mg (0.05 mmol) and the amount of 3-mercapto-1,2-propanediol was changed to 0.232 mL (2.55 mmol). Table 1-1 summarizes the particle properties of Particles 1-21.
[0333] [Comparative Examples 1-5]
[0334] (Synthesis of Particles 1-22)
[0335] The 2.5wt% aqueous dispersion of the granular copolymer 1-1 obtained in Example 1-1 was concentrated to a 10wt% aqueous dispersion with a centrifugal separator to obtain a concentrated dispersion. 20g of the concentrated dispersion was weighed in a 200ml round-bottom flask. While the concentrated dispersion was maintained at 4°C, 28% ammonia water (Kishida Chemical Co., Ltd.) was added thereto at 50 times the theoretical amount of epoxy groups derived from GMA contained in the 20g concentrated dispersion, and the pH of the mixture was adjusted to 11 by using a 2N aqueous hydrochloric acid solution and a 2N aqueous sodium hydroxide solution. Thereafter, the contents of the round-bottom flask were heated to 70°C while the contents were stirred at 100rpm. The contents were kept in this state for 24 hours to provide a dispersion of particles 1-22-1. The particles 1-22-1 were separated from the dispersion liquid by a centrifugal separator, and the particles 1-22-1 were dispersed in ion exchange water again; this operation was repeated 8 times to purify the particles 1-22-1, and the particles 1-22-1 were stored in the state of an aqueous dispersion liquid in which the concentration of the particles 1-22-1 was finally adjusted to 10 wt%. The storage conditions were set to 4° C. under light shielding conditions.
[0336] 6.3 g of a 10 wt% aqueous dispersion of particles 1-22-1 and 3.81 g of ethylene glycol diglycidyl ether (Tokyo Chemical Industry Co., Ltd.) were weighed in a 50 ml round-bottom flask, and the pH of the mixture was adjusted to 9 by using a 0.1 N aqueous hydrochloric acid solution and a 0.1 N aqueous sodium hydroxide solution. Thereafter, the contents of the round-bottom flask were heated to 30° C. while stirring the contents at 100 rpm. The contents were kept in this state for 24 hours to provide a dispersion of particles 1-22-2. Particles 1-22-2 were separated from the dispersion using a centrifugal separator, and particles 1-22-2 were redispersed in ion exchange water; this operation was repeated 8 times to purify particles 1-22-2, and stored in a state of an aqueous dispersion in which the concentration of particles 1-22-2 was finally adjusted to 10 wt%. The storage conditions were set to 4° C. under light-shielding conditions.
[0337] 6.0 g of a 10 wt% aqueous dispersion of particles 1-22-2 and a 28% aqueous ammonia solution of 10 times the mole relative to the theoretical amount of epoxy groups derived from ethylene glycol diglycidyl ether of the particles contained in the aqueous dispersion (assuming that 100% of the epoxy groups derived from glycidyl methacrylate of the particulate copolymer 1-1 react with ammonia to be converted into primary amines, and further assuming that 100% of the primary amines react with one of the epoxy groups at both ends of ethylene glycol diglycidyl ether) were added to a 50 ml round-bottom flask, and the pH of the mixture was adjusted to 11 by using a 1N aqueous hydrochloric acid solution and a 1N aqueous sodium hydroxide solution. Thereafter, the content of the round-bottom flask was heated to 70° C. while stirring the content at 100 rpm. The content was kept in this state for 24 hours to provide a dispersion of particles 1-22-3. The particles 1-22-3 were separated from the dispersion using a centrifugal separator, and the particles 1-22-3 were dispersed in ion exchange water again; this operation was repeated 8 times to purify the particles 1-22-3, and the particles 1-22-3 were stored in the state of an aqueous dispersion in which the concentration of the particles 1-22-3 was finally adjusted to 10 wt%. The storage conditions were set to 4° C. under light shielding conditions.
[0338] Particles 1-22-3 were separated from a 10 wt % aqueous dispersion of particles 1-22-3 using a centrifugal separator, and particles 1-22-3 were redispersed in methanol; this operation was repeated three times to prepare a methanol dispersion of particles 1-22-3 in which the concentration of particles 1-22-3 was finally adjusted to 1 wt %. 63 g of the methanol dispersion of particles 1-22-3 and 2.77 g of succinic anhydride (Tokyo Chemical Industry Co., Ltd.) were weighed in a 200 ml round-bottom flask. Thereafter, the contents of the round-bottom flask were heated to 30° C. while stirring the contents at 100 rpm. The contents were kept in this state for 5 hours to provide a dispersion of particles 1-22. Particles 1-22 were separated from the dispersion using a centrifugal separator, and Particles 1-22 were dispersed again in ion-exchanged water; this operation was repeated 8 times to purify Particles 1-22, which were stored in the state of an aqueous dispersion in which the concentration of Particles 1-22 was finally adjusted to 1.0 wt%.
[0339] [Comparative Examples 1-6]
[0340] (Synthesis of Particles 1-23)
[0341] The 2.5wt% aqueous dispersion of the granular copolymer 1-1 obtained in Example 1-1 was concentrated to a 10wt% aqueous dispersion with a centrifugal separator to obtain a concentrated dispersion. 20g of the concentrated dispersion was weighed in a 200ml round-bottom flask. While the concentrated dispersion was maintained at 4°C, 10 times the molar amount of glycine (Kishida Chemical Co., Ltd.) relative to the theoretical amount of epoxy groups derived from GMA contained in the 20g concentrated dispersion was added thereto, and the pH of the mixture was adjusted to 11 by using 0.1N aqueous hydrochloric acid solution and 0.1N aqueous sodium hydroxide solution. Thereafter, the contents of the round-bottom flask were heated to 70°C while the contents were stirred at 100rpm. The contents were kept in this state for 24 hours to provide a dispersion of particles 1-23. The particles 1-23 were separated from the dispersion using a centrifugal separator, and the particles 1-23 were dispersed in ion exchange water again; this operation was repeated 8 times to purify the particles 1-23, and the particles 1-23 were stored in the state of an aqueous dispersion in which the concentration of the particles 1-23 was finally adjusted to 10 wt%. The storage conditions were set to 4° C. under light shielding conditions.
[0342] [Example 1-21]
[0343] (Evaluation of nonspecific adsorption to particles)
[0344] Particles 1-1 to 1-23 were each dispersed in a phosphate buffer (containing 0.01% Tween 20) at 0.1 wt% to prepare a dispersion (P solution). Next, 51 μL of a sample diluent (Q solution) formed by a normal human sample (serum sample, 1 μL) and a phosphate buffer (50 μL) was added to 50 μL of each dispersion, and the absorbance of the mixed solution at a wavelength of 572 nm was measured immediately after stirring. The spectrophotometer GeneQuant 1300 manufactured by Biochrom was used for absorbance measurement. Then, each mixed solution was allowed to stand at 37°C for 5 minutes, and then its absorbance at a wavelength of 572 nm was measured again, and then the value of the change in absorbance ΔABS×10,000 was calculated. The results are summarized in Table 1-1. It should be understood that as this value becomes larger, nonspecific adsorption occurs to a greater extent. However, when particles with a larger carboxyl density or particles with a larger value of [particle size in water / dry particle size] have a large value, the particles can detect osmotic pressure agglutination rather than agglutination caused by nonspecific adsorption. In any case, when particles with a larger value of the absorbance change ΔABS×10,000 in this evaluation are used as particles for the latex agglutination method in sample detection, there is a concern that the normal sample will be interpreted as a false positive due to noise. The case where the Q liquid contains 1μL of a normal human sample is expressed as "human normal sample concentration×1". The case where the Q liquid contains 2.5μL of a normal human sample is expressed as "human normal sample concentration×2.5". The case where the Q liquid contains 5μL of a normal human sample is expressed as "human normal sample concentration×5". The normal sample amounts are 1 times, 2.5 times and 5 times, respectively. The thresholds for excellent, good, fair and poor in Table 1-1 are benchmarks determined by the noise risk when detecting low concentrations of target substances by the latex agglutination method.
[0345] [Example 1-22]
[0346] (Production of affinity particles by antibody sensitization of the particles)
[0347] 0.1 mL (1 mg of particles) of a particle dispersion (1.0 wt% solution, 10 mg / mL) of each of particles 1-1 to 1-23 was transferred to a microtube (volume: 1.5 mL), 0.12 mL of activation buffer (25 mM MES, pH: 6.0) was added thereto, and the mixture was centrifuged at 4°C and 15,000 rpm (20,400 g) for 5 minutes. After centrifugation, the supernatant was discarded. 0.12 mL of activation buffer (25 mM MES, pH: 6.0) was added to the residue, and the particles were redispersed with ultrasound. Centrifugation and redispersion were repeated once.
[0348] Next, 60 μL of a WSC solution (a solution obtained by dissolving 50 mg of WSC in 1 mL of an activation buffer, the term "WSC" means 1-[3-(dimethylaminopropyl)-3-ethylcarbodiimide] hydrochloride) and a Sulfo NHS solution (a solution obtained by dissolving 50 mg of Sulfo NHS in 1 mL of an activation buffer, the term "Sulfo NHS" means sulfo-N-hydroxysuccinimide) were each added to the resultant, and dispersed with ultrasonic waves. The dispersion was stirred at room temperature for 30 minutes to convert the carboxyl groups of its particles into active esters. The resultant was centrifuged at 4°C and 15,000 rpm (20,400 g) for 5 minutes, and the supernatant was discarded. 0.2 mL of an immobilization buffer (25 mM MES, pH: 5.0) was added to the residue, and the particles were dispersed with ultrasonic waves. The dispersion was centrifuged at 4°C and 15,000 rpm (20,400 g) for 5 minutes, and the supernatant was discarded. 50 μL of immobilization buffer was added to the residue, and the carboxyl-activated particles were dispersed using ultrasound.
[0349] 50 μL antibody solution (a solution obtained by diluting anti-CRP antibody with immobilization buffer to make its concentration 25 μg / 50 μL) is added to the solution of 50 μL carboxyl activated particles, and the particles are dispersed with ultrasound. The amount of antibody loaded is 25 μg (25 μg / mg) per 1 mg particle. The final antibody concentration is 0.25 mg / mL, and the final particle concentration is 10 mg / mL. The contents in the microtube are stirred at room temperature for 60 minutes to bind the antibody to the carboxyl of the particles. Next, the resultant is centrifuged at 4 ° C and 15,000 rpm (20,400 g) for 5 minutes, and the supernatant is discarded. 0.24 mL masking buffer (buffer obtained by including 0.1% Tween 20 in 1M Tris at pH 8.0) is added to the residue, and the particles are dispersed with ultrasound. The dispersion is stirred at room temperature for 1 hour, and then left to stand overnight at 4 ° C to bind Tris to the residual activated carboxyl. Next, the resultant was centrifuged at 4°C and 15,000rpm (20,400g) for 5 minutes, and the supernatant was discarded. 0.2mL washing buffer (10mM HEPES, pH: 7.9) was added to the residue, and the particles were dispersed with ultrasound. The washing operation (centrifugation and redispersion) using washing buffer (10mM HEPES, pH: 7.9) was repeated once. A washing operation was performed using 0.2mL preservation buffer (10mM HEPES, pH: 7.9, containing 0.01% Tween 20). 1.0mL preservation buffer was added to the washed product, and the particles were dispersed with ultrasound. The particle concentration of the dispersion eventually became 0.1wt% (1mg / mL). The dispersion was stored in a refrigerator. Hereinafter, the name of the affinity particle directly follows the particle name, expressed as "affinity particle 1-1" and the like.
[0350] [Example 1-23]
[0351] (Evaluation of Antibody Sensitization Rate of Affinity Particles)
[0352] The antibody sensitization rate (%) of the affinity particles produced in Examples 1-21 was determined by protein quantification. Herein, the term "antibody sensitization rate (%)" means the ratio of the amount of antibody bound to the particles relative to the amount of antibody used in the reaction with the particles (antibody loading amount). The following describes an evaluation example of protein quantification.
[0353] First, 7 mL of LA liquid and 140 μL of B liquid of PROTEIN ASSAY BCA KIT (Wako Pure Chemical Industries, Ltd.) were mixed, and the prepared liquid was used as AB liquid. Next, 25 μL (particle amount: 25 μg) of a dispersion of affinity particles (0.1% solution) was taken and placed in a 1.5 mL tube. Next, 200 μL of AB liquid was added to the dispersion (25 μL), and the mixture was incubated at 60°C for 30 minutes. The resulting solution was centrifuged at 4°C and 15,000 rpm (20,400 g) for 5 minutes, and 200 μL of the supernatant was loaded into a 96-well microwell with a pipette. The absorbance of the supernatant at 562 nm was measured using an ELISA reader together with a standard sample (several samples were obtained by diluting the antibody with 10 mM HEPES so that its concentration fell within the range of 0 μg / mL to 200 μg / mL). The antibody amount was calculated from the standard curve. The antibody sensitization amount of the particles (antibody binding amount per particle weight (μg / mg)) was determined by dividing the calculated antibody amount by the particle weight (herein, 0.025mg). Finally, the sensitization rate was calculated. When the antibody loading was 25μg per 1mg particle, the sensitization rate was 50% when the antibody sensitization amount was 12.5μg / mg. The results are summarized in Table 1-1.
[0354] [Example 1-24]
[0355] (Evaluation of Latex Agglutination Sensitivity of Affinity Particles)
[0356] 1 μL of human CRP (Denka Seiken Co., Ltd., C-reactive protein, derived from human plasma, 40 μg / ml) and 50 μL of buffer (PBS containing 0.01% Tween 20) were mixed to prepare a mixed solution (hereinafter referred to as R1+), and incubated at 37°C. In addition, 1 μL of physiological saline and 50 μL of buffer (PBS containing 0.01% Tween 20) were mixed to prepare a mixed solution (hereinafter referred to as R1-) as a control, and also incubated at 37°C. Next, 50 μL of a solution containing each affinity particle prepared in Examples 1-21 (particle concentration: 0.1 wt%, referred to as R2) was mixed with R1+ or R1-, and the absorbance of the mixed solution (volume: 101 μL) at a wavelength of 572 nm was measured immediately after stirring. A spectrophotometer GeneQuant 1300 manufactured by Biochrom was used for absorbance measurement. Then, the mixed solution was allowed to stand at 37°C for 5 minutes, and then its absorbance at a wavelength of 572nm was measured again, and then the value of the change in absorbance ΔABS×10,000 was calculated. This series of evaluations was performed for each of the following: R2 immediately after preparation in Example 1-21; R2 after 24 hours after preparation; and R2 after 72 hours after preparation. The results are summarized in Table 1-1. The larger the value of R- in Table 1-1, the more agglutination or osmotic pressure agglutination caused by nonspecific adsorption occurs in the affinity particles. Therefore, when the particles are used as particles for latex agglutination in sample detection, there is a concern that normal samples will be interpreted as false positives due to noise. At the same time, it is expected that affinity particles with larger R+ values in Table 1-1 can detect target substances with higher sensitivity when used as particles for latex agglutination in sample detection. The thresholds of excellent, good, medium and poor R- in Table 1-1 are benchmarks determined by the noise risk when detecting low concentrations of target substances by latex agglutination. In addition, the threshold values of excellent, good, fair, and poor of R+ are determined with reference to the following values obtained by using CRP-L Auto "TBA" manufactured by Denka Seiken Co., Ltd as a CRP detection kit and CRP standard liquid "TBA" for latex.
[0357] ΔABS of 0 μg / ml (normal saline) × 10,000: -80
[0358] 5 μg / ml ΔABS × 10,000: 1,410
[0359] 20 μg / ml ΔABS × 10,000: 3,530
[0360] 40 μg / ml ΔABS × 10,000: 5,130
[0361] 160 μg / ml ΔABS × 10,000: 9,750
[0362] 320 μg / ml ΔABS × 10,000: 12,150
[0363]
[0364]
[0365]
[0366] [Example 1-25]
[0367] (Production of affinity particles for KL-6)
[0368] Particles 1-5, 1-6, and 1-7 were sensitized with anti-KL-6 antibodies in the same manner as in Example 1-22, except that the antibody in Example 1-22 was changed from anti-CRP antibody to anti-KL-6 antibody and the amount of antibody loaded was changed from 25 to 100. The resulting affinity particles for KL-6 were respectively indicated as "affinity particles 1-5K", "affinity particles 1-6K", and "affinity particles 1-7K".
[0369] The antibody sensitization rates of affinity particles 1-5K, affinity particles 1-6K, and affinity particles 1-7K were evaluated in the same manner as in Example 1-23. As a result, the antibody sensitization rates were found to be 93%, 100%, and 94%, respectively.
[0370] [Example 1-26]
[0371] (Evaluation of latex aggregation sensitivity of KL-6)
[0372] The latex agglutination sensitivity of the affinity particles 1-5K, 1-6K, and 1-7K was evaluated in the same manner as in Example 1-24 except that the human CRP of Example 1-24 was changed to human KL-6.
[0373] The absorbance change (ΔABS×10,000) obtained with affinity particles 1-5K is shown below.
[0374] 0U / mL (normal saline): -140
[0375] 500U / mL: 410
[0376] 1,000 U / mL: 1,380
[0377] 2,000 U / mL: 4,840
[0378] 5,000 U / mL: 7,520
[0379] The absorbance change (ΔABS×10,000) obtained with affinity particles 1-6K is shown below.
[0380] 0U / mL (normal saline): -240
[0381] 500U / mL: -90
[0382] 1,000 U / mL: 480
[0383] 2,000 U / mL: 3,320
[0384] 5,000 U / mL: 6,160
[0385] The absorbance change (ΔABS×10,000) obtained with affinity particles 1-7K is shown below.
[0386] 0U / mL (normal saline): -320
[0387] 500U / mL: -50
[0388] 1,000U / mL: -340
[0389] 2,000 U / mL: 550
[0390] 5,000 U / mL: 1,200
[0391] All particles showed a linear absorbance change relative to the concentration of KL-6. It was found that when the concentration of KL-6 was constant, the absorbance change increased as the particle size became larger. The latex aggregation sensitivity can be controlled by controlling the particle size.
[0392] [Example 1-27]
[0393] (Effect of sensitizer on latex aggregation sensitivity)
[0394] The latex agglutination sensitivity of affinity particles 1-5K and affinity particles 1-6K was evaluated in the same manner as in Example 1-24, except that the human CRP of Example 1-24 was changed to human KL-6 and the buffer (PBS containing 0.01% Tween 20) was changed to a buffer containing a sensitizer (PBS containing 0.58% PVP K90 or 0.68% sodium alginate 80-120 and 0.01% Tween 20).
[0395] In the case of using alginic acid as a sensitizer, the amount of absorbance change (ΔABS×10,000) obtained with affinity particles 1-5K is shown below.
[0396] 0U / mL (normal saline): -240
[0397] 500 U / mL: 1,090
[0398] 1,000 U / mL: 2,780
[0399] 2,000 U / mL: 9,960
[0400] 5,000 U / mL: 11,520
[0401] In the case of using alginic acid as a sensitizer, the amount of absorbance change (ΔABS×10,000) obtained with affinity particles 1-6K is shown below.
[0402] 0U / mL (normal saline): -50
[0403] 500U / mL: 420
[0404] 1,000 U / mL: 1,260
[0405] 2,000 U / mL: 6,590
[0406] 5,000 U / mL: 8,720
[0407] In the case of using PVP as a sensitizer, the absorbance change (ΔABS×10,000) obtained with affinity particles 1-5K is shown below.
[0408] 0U / mL (normal saline): -70
[0409] 500U / mL: 480
[0410] 1,000 U / mL: 1,020
[0411] 2,000 U / mL: 3,860
[0412] 5,000 U / mL: 5,970
[0413] In the case of using PVP as a sensitizer, the amount of absorbance change (ΔABS×10,000) obtained with affinity particles 1-6K is shown below.
[0414] 0U / mL (normal saline): -280
[0415] 500U / mL: -60
[0416] 1,000 U / mL: 670
[0417] 2,000 U / mL: 4,080
[0418] 5,000 U / mL: 6,820
[0419] The sensitizing effects of PVP and alginic acid were confirmed for the affinity particles 1-5K and 1-6K. In particular, it was found that alginic acid had a high sensitizing effect.
[0420] [Example 1-28]
[0421] (Production of affinity particles for IgE)
[0422] Particles 1-5 were sensitized with anti-IgE antibody in the same manner as in Example 1-22, except that the antibody in Example 1-22 was changed from anti-CRP antibody to anti-IgE antibody and the amount of loaded antibody was changed from 25 to 100. The resulting affinity particles for IgE are designated as "affinity particles 1-5I".
[0423] The antibody sensitization rate of affinity particle 1-5I was evaluated in the same manner as in Example 1-23. As a result, the antibody sensitization rate was found to be 80%.
[0424] [Example 1-29]
[0425] (Evaluation of latex agglutination sensitivity to IgE)
[0426] The latex agglutination sensitivity of affinity particles 1-5I was evaluated in the same manner as in Example 1-24, except that human CRP of Example 1-24 was changed to human IgE. The sample volume was set to 1.5 μL, the amount of the sample diluent (Good's buffer, LT Auto Wako IgE, Wako Pure Chemical Industries, Ltd.) was set to 75 μL, and the amount of the affinity particle dispersion was set to 25 μL.
[0427] The absorbance change (ΔABS×10,000) obtained with affinity particles 1-5I is shown below.
[0428] 0IU / mL (normal saline): -60
[0429] 100IU / mL: -50
[0430] 300 IU / mL: 100
[0431] 1,000 IU / mL: 200
[0432] 2,000 IU / mL: 510
[0433] 3,000 IU / mL: 1,790
[0434] Affinity particles 1-5I showed a linear absorbance change with respect to the IgE concentration. In addition, the latex agglutination sensitivity of affinity particles 1-5I was evaluated in the same manner as in Example 1-27 using a buffer containing a sensitizer (Good's buffer containing 0.045% alginic acid was used as a sample diluent).
[0435] In the case of using alginic acid as a sensitizer, the amount of absorbance change (ΔABS×10,000) obtained with affinity particles 1-5K is shown below.
[0436] 0IU / mL (normal saline): 30
[0437] 100 IU / mL: 140
[0438] 300IU / mL: 300
[0439] 1,000 IU / mL: 1,130
[0440] 2,000 IU / mL: 3,870
[0441] 3,000 IU / mL: 5,910
[0442] Regarding affinity particle 1-5I, the sensitizing effect of alginic acid was confirmed.
[0443] Now, the present invention will be described in detail by way of examples corresponding to the second embodiment. However, the present invention is not limited to these examples.
[0444] (Example 2-1: Synthesis of granular copolymer)
[0445] The following materials were weighed in a 2 L four-necked separable flask to provide a mixed solution.
[0446] 22.7 g styrene (St, manufactured by Kishida Chemical Co., Ltd.)
[0447] 33.9 g of glycidyl methacrylate (GMA, manufactured by Tokyo Chemical Industry Co., Ltd.)
[0448] 0.86 g divinylbenzene (DVB, manufactured by Kishida Chemical Co., Ltd.)
[0449] 2,168.6 g ion exchange water
[0450] Thereafter, the mixed solution was maintained at 70°C while stirring at 200 rpm, and nitrogen was passed at a flow rate of 200 mL / min to remove oxygen from the inside of the four-necked separable flask. Next, a separately prepared solution obtained by dissolving 1.13 g of a polymerization initiator (trade name: V-50, manufactured by FUJIFILM Wako Pure Chemical Corporation) in 30 g of ion exchange water was added to the mixed solution to initiate soap-free emulsion polymerization. After 2 hours from the start of polymerization, 5.8 g of GMA was added to the four-necked separable flask, and the mixture was maintained at 70°C while stirring at 200 rpm for 22 hours. Thus, an aqueous dispersion containing granular copolymer 2-1 was obtained.
[0451] After the dispersion was gradually cooled to room temperature, a portion of the dispersion was collected and its polymerization conversion was evaluated by using proton NMR, gas chromatography and gel permeation chromatography. As a result, it was confirmed that the polymerization conversion was substantially 100%. The dry particle size of the granular copolymer was 196.6 nm and the particle size in water was 206.9 nm.
[0452] The particulate copolymer was concentrated by ultrafiltration or diluted by adding ion-exchanged water to obtain a 2.5 mass % aqueous dispersion, and the dispersion was stored at 4° C. under light-shielding conditions.
[0453] (Example 2-2: Synthesis of Particle 2-1)
[0454] The following materials were weighed in a 100 ml round-bottom flask, and triethylamine (manufactured by Kishida Chemical Co., Ltd.) was added to the mixture to adjust its pH to 10.
[0455] 24 g of a 2.5 mass % aqueous dispersion of the granular copolymer 2-1
[0456] 3.3g ion exchange water
[0457] 202 mg (1.30 mmol) mercaptosuccinic acid (manufactured by FUJIFILM Wako Pure Chemical Corporation)
[0458] 0.119 mL (1.30 mmol) 3-mercapto-1,2-propanediol (manufactured by FUJIFILM Wako Pure Chemical Corporation)
[0459] Next, the content of the round-bottom flask was heated to 70°C while stirring the content at 200 rpm. Furthermore, the content was kept in this state for 18 hours to provide a dispersion of particles 2-1. Particles 2-1 were separated from the dispersion using a centrifugal separator, and particles 2-1 were redispersed in ion exchange water; this operation was repeated 8 times to purify particles 2-1, and stored in a state of an aqueous dispersion in which the concentration of particles 2-1 was finally adjusted to 1.0% by mass. The storage conditions were set to 4°C under light-shielding conditions. Table 2-1 summarizes the particle properties of particles 2-1.
[0460] (Example 2-3: Synthesis of Particle 2-2)
[0461] The following materials were weighed in a 100 ml round-bottom flask, and triethylamine (manufactured by Kishida Chemical Co., Ltd.) was added to the mixture to adjust its pH to 10.
[0462] 24 g of a 2.5 mass % aqueous dispersion of the granular copolymer 2-1
[0463] 3.3g ion exchange water
[0464] 40 mg (0.26 mmol) mercaptosuccinic acid (manufactured by FUJIFILM Wako Pure Chemical Corporation)
[0465] 0.214 mL (2.34 mmol) 3-mercapto-1,2-propanediol (manufactured by FUJIFILM Wako Pure Chemical Corporation)
[0466] Next, the content of the round-bottom flask was heated to 70°C while stirring the content at 200 rpm. Furthermore, the content was kept in this state for 6 hours to provide a dispersion of particles 2-2. Particles 2-2 were separated from the dispersion using a centrifugal separator, and particles 2-2 were redispersed in ion exchange water; this operation was repeated 8 times to purify particles 2-2, and stored in a state of an aqueous dispersion in which the concentration of particles 2-2 was finally adjusted to 1.0% by mass. The storage conditions were set to 4°C under light-shielding conditions. Table 2-1 summarizes the particle properties of particles 2-2.
[0467] (Example 2-4: Synthesis of Particles 2-3)
[0468] The following materials were weighed in a 100 ml round-bottom flask, and triethylamine (manufactured by Kishida Chemical Co., Ltd.) was added to the mixture to adjust its pH to 10.
[0469] 24 g of a 2.5 mass % aqueous dispersion of the granular copolymer 2-1
[0470] 3.3g ion exchange water
[0471] 40 mg (0.26 mmol) mercaptosuccinic acid (manufactured by FUJIFILM Wako Pure Chemical Corporation)
[0472] 0.214 mL (2.34 mmol) 3-mercapto-1,2-propanediol (manufactured by FUJIFILM Wako Pure Chemical Corporation)
[0473] Next, the content of the round-bottom flask was heated to 70°C while stirring the content at 200 rpm. Furthermore, the content was kept in this state for 8 hours to provide a dispersion of particles 2-3. Particles 2-3 were separated from the dispersion using a centrifugal separator, and particles 2-3 were redispersed in ion exchange water; this operation was repeated 8 times to purify particles 2-3, and stored in a state of an aqueous dispersion in which the concentration of particles 2-3 was finally adjusted to 1.0% by mass. The storage conditions were set to 4°C under light-shielding conditions. Table 2-1 summarizes the particle properties of particles 2-3.
[0474] (Example 2-5: Synthesis of Particles 2-4)
[0475] The following materials were weighed in a 100 ml round-bottom flask, and triethylamine (manufactured by Kishida Chemical Co., Ltd.) was added to the mixture to adjust its pH to 10.
[0476] 24 g of a 2.5 mass % aqueous dispersion of the granular copolymer 2-1
[0477] 3.3g ion exchange water
[0478] 40 mg (0.26 mmol) mercaptosuccinic acid (manufactured by FUJIFILM Wako Pure Chemical Corporation)
[0479] 0.214 mL (2.34 mmol) 3-mercapto-1,2-propanediol (manufactured by FUJIFILM Wako Pure Chemical Corporation)
[0480] Next, the content of the round-bottom flask was heated to 70°C while stirring the content at 200 rpm. Furthermore, the content was kept in this state for 12 hours to provide a dispersion of particles 2-4. Particles 2-4 were separated from the dispersion using a centrifugal separator, and particles 2-4 were redispersed in ion exchange water; this operation was repeated 8 times to purify particles 2-4, which were stored in the state of an aqueous dispersion in which the concentration of particles 2-4 was finally adjusted to 1.0% by mass. The storage conditions were set to 4°C under light-shielding conditions. Table 2-1 summarizes the particle properties of particles 2-4.
[0481] (Example 2-6: Synthesis of Particles 2-5)
[0482] The following materials were weighed in a 100 ml round-bottom flask, and triethylamine (manufactured by Kishida Chemical Co., Ltd.) was added to the mixture to adjust its pH to 10.
[0483] 24 g of a 2.5 mass % aqueous dispersion of the granular copolymer 2-1
[0484] 3.3g ion exchange water
[0485] 40 mg (0.26 mmol) mercaptosuccinic acid (manufactured by FUJIFILM Wako Pure Chemical Corporation)
[0486] 0.214 mL (2.34 mmol) 3-mercapto-1,2-propanediol (manufactured by FUJIFILM Wako Pure Chemical Corporation)
[0487] Next, the content of the round-bottom flask was heated to 70°C while stirring the content at 200 rpm. Furthermore, the content was kept in this state for 18 hours to provide a dispersion of particles 2-5. Particles 2-5 were separated from the dispersion using a centrifugal separator, and particles 2-5 were redispersed in ion exchange water; this operation was repeated 8 times to purify particles 2-5, and stored in a state of an aqueous dispersion in which the concentration of particles 2-5 was finally adjusted to 1.0% by mass. The storage conditions were set to 4°C under light-shielding conditions. Table 2-1 summarizes the particle properties of particles 2-5.
[0488] (Example 2-7: Synthesis of Particles 2-6)
[0489] The following materials were weighed in a 100 ml round-bottom flask, and triethylamine (manufactured by Kishida Chemical Co., Ltd.) was added to the mixture to adjust its pH to 11.
[0490] 24 g of a 2.5 mass % aqueous dispersion of the granular copolymer 2-1
[0491] 3.3g ion exchange water
[0492] 40 mg (0.26 mmol) mercaptosuccinic acid (manufactured by FUJIFILM Wako Pure Chemical Corporation)
[0493] 0.214 mL (2.34 mmol) 3-mercapto-1,2-propanediol (manufactured by FUJIFILM Wako Pure Chemical Corporation)
[0494] Next, the content of the round-bottom flask was heated to 70°C while stirring the content at 200 rpm. Furthermore, the content was kept in this state for 30 hours to provide a dispersion of particles 2-6. Particles 2-6 were separated from the dispersion using a centrifugal separator, and particles 2-6 were redispersed in ion exchange water; this operation was repeated 8 times to purify particles 2-6, which were stored in the state of an aqueous dispersion in which the concentration of particles 2-6 was finally adjusted to 1.0% by mass. The storage conditions were set to 4°C under light-shielding conditions. Table 2-1 summarizes the particle properties of particles 2-6.
[0495] (Example 2-8: Synthesis of Particles 2-7)
[0496] The following materials were weighed in a 100 ml round-bottom flask, and triethylamine (manufactured by Kishida Chemical Co., Ltd.) was added to the mixture to adjust its pH to 10.
[0497] 24 g of a 2.5 mass % aqueous dispersion of the granular copolymer 2-1
[0498] 3.3g ion exchange water
[0499] 81 mg (0.52 mmol) mercaptosuccinic acid (manufactured by FUJIFILM Wako Pure Chemical Corporation)
[0500] 0.191 mL (2.08 mmol) 3-mercapto-1,2-propanediol (manufactured by FUJIFILM Wako Pure Chemical Corporation)
[0501] Next, the content of the round-bottom flask was heated to 70°C while stirring the content at 200 rpm. Furthermore, the content was kept in this state for 18 hours to provide a dispersion of particles 2-7. Particles 2-7 were separated from the dispersion using a centrifugal separator, and particles 2-7 were redispersed in ion exchange water; this operation was repeated 8 times to purify particles 2-7, which were stored in the state of an aqueous dispersion in which the concentration of particles 2-7 was finally adjusted to 1.0% by mass. The storage conditions were set to 4°C under light-shielding conditions. Table 2-1 summarizes the particle properties of particles 2-7.
[0502] (Example 2-9: Synthesis of Particles 2-8)
[0503] The following materials were weighed in a 100 ml round-bottom flask, and triethylamine (manufactured by Kishida Chemical Co., Ltd.) was added to the mixture to adjust its pH to 10.
[0504] 24 g of a 2.5 mass % aqueous dispersion of the granular copolymer 2-1
[0505] 3.3g ion exchange water
[0506] 323 mg (2.08 mmol) mercaptosuccinic acid (manufactured by FUJIFILM Wako Pure Chemical Corporation)
[0507] 0.047 mL (0.52 mmol) 3-mercapto-1,2-propanediol (manufactured by FUJIFILM Wako Pure Chemical Corporation)
[0508] Next, the content of the round-bottom flask was heated to 70°C while stirring the content at 200 rpm. Furthermore, the content was kept in this state for 18 hours to provide a dispersion of particles 2-8. Particles 2-8 were separated from the dispersion using a centrifugal separator, and particles 2-8 were redispersed in ion-exchanged water; this operation was repeated 8 times to purify particles 2-8, and stored in a state of an aqueous dispersion in which the concentration of particles 2-8 was finally adjusted to 1.0% by mass. The storage conditions were set to 4°C under light-shielding conditions. Table 2-1 summarizes the particle properties of particles 2-8.
[0509] (Example 2-10: Synthesis of Particles 2-9)
[0510] The following materials were weighed in a 100 ml round-bottom flask, and triethylamine (manufactured by Kishida Chemical Co., Ltd.) was added to the mixture to adjust its pH to 10.
[0511] 24 g of a 2.5 mass % aqueous dispersion of the granular copolymer 2-1
[0512] 3.3g ion exchange water
[0513] 282 mg (1.82 mmol) mercaptosuccinic acid (manufactured by FUJIFILM Wako Pure Chemical Corporation)
[0514] 0.071 mL (0.78 mmol) 3-mercapto-1,2-propanediol (manufactured by FUJIFILM Wako Pure Chemical Corporation)
[0515] Next, the content of the round-bottom flask was heated to 70°C while stirring the content at 200 rpm. Furthermore, the content was kept in this state for 18 hours to provide a dispersion of particles 2-9. Particles 2-9 were separated from the dispersion using a centrifugal separator, and particles 2-9 were redispersed in ion exchange water; this operation was repeated 8 times to purify particles 2-9, which were stored in the state of an aqueous dispersion in which the concentration of particles 2-9 was finally adjusted to 1.0% by mass. The storage conditions were set to 4°C under light-shielding conditions. Table 2-1 summarizes the particle properties of particles 2-9.
[0516] (Example 2-11: Synthesis of Particles 2-10)
[0517] The following materials were weighed in a 100 ml round-bottom flask, and triethylamine (manufactured by Kishida Chemical Co., Ltd.) was added to the mixture to adjust its pH to 10.
[0518] 24 g of a 2.5 mass % aqueous dispersion of the granular copolymer 2-1
[0519] 3.3g ion exchange water
[0520] 242 mg (1.56 mmol) mercaptosuccinic acid (manufactured by FUJIFILM Wako Pure Chemical Corporation)
[0521] 0.095 mL (1.04 mmol) 3-mercapto-1,2-propanediol (manufactured by FUJIFILM Wako Pure Chemical Corporation)
[0522] Next, the content of the round-bottom flask was heated to 70°C while stirring the content at 200 rpm. Furthermore, the content was kept in this state for 18 hours to provide a dispersion of particles 2-10. Particles 2-10 were separated from the dispersion using a centrifugal separator, and particles 2-10 were redispersed in ion exchange water; this operation was repeated 8 times to purify particles 2-10, and stored in a state of an aqueous dispersion in which the concentration of particles 2-10 was finally adjusted to 1.0% by mass. The storage conditions were set to 4°C under light-shielding conditions. Table 2-1 summarizes the particle properties of particles 2-10.
[0523] (Example 2-12: Production of affinity particles 2-1 to 2-6 by antibody sensitization of particles)
[0524] 0.1 mL (1 mg of particles) of the particle dispersion (1.0 mass % solution, 10 mg / mL) of each of particles 2-1 to 2-6 was transferred to a microtube (volume: 1.5 mL). Thereafter, 0.12 mL of activation buffer (25 mM MES, pH: 6.0) was added thereto, and the mixture was centrifuged at 4 ° C and 15,000 rpm (20,400 g) for 5 minutes. After centrifugation, the supernatant was discarded. 0.12 mL of activation buffer (25 mM MES, pH: 6.0) was added to the residue, and the particles were redispersed with ultrasound. Centrifugation and redispersion were repeated once.
[0525] Next, 60 μL of each of the following materials was added to the resultant, and dispersed therein with ultrasonic waves.
[0526] 1-[3-(Dimethylaminopropyl)-3-ethylcarbodiimide] hydrochloride (WSC) solution (a solution obtained by dissolving 50 mg of WSC in 1 mL of activation buffer)
[0527] Sulfo-N-hydroxysuccinimide (SulfoNHS) solution (a solution obtained by dissolving 50 mg of SulfoNHS in 1 mL of activation buffer)
[0528] The dispersion was stirred at room temperature for 30 minutes to convert the carboxyl groups of its particles into active esters. The resulting product was centrifuged at 4 ° C and 15,000 rpm (20,400 g) for 5 minutes, and the supernatant was discarded. 0.2 mL of immobilization buffer (25 mM MES, pH: 5.0) was added to the residue, and the particles were dispersed with ultrasound. The dispersion was centrifuged at 4 ° C and 15,000 rpm (20,400 g) for 5 minutes, and the supernatant was discarded. 50 μL of immobilization buffer was added to the residue, and the carboxyl-activated particles were dispersed with ultrasound.
[0529] 50 μL antibody solution (a solution obtained by diluting anti-C reactive protein (CRP) antibody with immobilization buffer to make its concentration 25 μg / 50 μL) is added to 50 μL of carboxyl activated particles, and the particles are dispersed with ultrasound. The amount of antibody loaded is 25 μg (25 μg / mg) per 1 mg of particles. The final concentration of the antibody is 0.25 mg / mL, and the final concentration of the particles is 10 mg / mL. The contents of the test tube are stirred at room temperature for 60 minutes to bind the antibody to the carboxyl group of the particles.
[0530] Next, the resultant was centrifuged at 4°C and 15,000rpm (20,400g) for 5 minutes, and the supernatant was discarded. 0.24mL of masking buffer (buffer obtained by including 0.1% Tween 20 in 1M Tris at pH 8.0) was added to the residue, and the particles were dispersed with ultrasound. The dispersion was stirred at room temperature for 1 hour, and then allowed to stand overnight at 4°C to allow trishydroxymethylaminomethane (Tris) to bind to the residual activated carboxyl groups. Next, the resultant was centrifuged at 4°C and 15,000rpm (20,400g) for 5 minutes, and the supernatant was discarded. 0.2mL of washing buffer (10mM hydroxyethylpiperazineethanesulfonic acid (HEPES), pH: 7.9) was added to the residue, and the particles were dispersed with ultrasound. The washing operation (centrifugation and redispersion) using washing buffer (10mM HEPES, pH: 7.9) was repeated once. The washing operation was performed once with 0.2 mL of storage buffer (10 mM HEPES, pH: 7.9, containing 0.01% Tween 20). 1.0 mL of storage buffer was added to the washed product, and the particles were dispersed with ultrasound. The particle concentration of the dispersion liquid finally became 0.1 mass % (1 mg / mL). The obtained dispersion liquid of the particles was stored in a refrigerator.
[0531] The affinity particles obtained in this example are named as follows. When the particles used are particles 2-1, the affinity particles are expressed as affinity particles 2-1. In addition, when the particles used are particles 2-2, the affinity particles are expressed as affinity particles 2-2. When the particles used are particles 2-3, the affinity particles are expressed as affinity particles 2-3. When the particles used are particles 2-4, the affinity particles are expressed as affinity particles 2-4. When the particles used are particles 2-5, the affinity particles are expressed as affinity particles 2-5. When the particles used are particles 2-6, the affinity particles are expressed as affinity particles 2-6. Table 2-1 summarizes the particle properties of affinity particles 2-1 to 2-6.
[0532] (Example 2-13: Production of affinity particles 2-7 to 2-12 by antibody sensitization of particles)
[0533] The particles used were changed to particles 2-5, and the amount of antibody loaded in Example 2-12 was changed from 25 μg / mg to 48 μg / mg, 41 μg / mg, 31 μg / mg, 25 μg / mg, 18 μg / mg and 11 μg / mg, respectively. In addition, 0.1 mass % aqueous dispersions of affinity particles 2-7, affinity particles 2-8, affinity particles 2-9, affinity particles 2-10, affinity particles 2-11 and affinity particles 2-12 were obtained in the same manner as in Example 2-12. Table 2-1 summarizes the particle properties of affinity particles 2-7 to 2-12.
[0534] (Example 2-14: Production of affinity particles 2-13 by antibody sensitization of particles)
[0535] A 0.1 mass % aqueous dispersion of affinity particles 2-13 was obtained in the same manner as in Example 2-12 except that the particles used were changed to particles 2-7 and the amount of antibody loaded in Example 2-12 was changed from 25 μg / mg to 54 μg / mg. Table 2-1 summarizes the particle properties of affinity particles 2-13.
[0536] (Example 2-15: Production of affinity particles 2-14 by antibody sensitization of particles)
[0537] The particles used were changed to particles 2-5, the antibody of Example 2-12 was changed from anti-CRP antibody to anti-prostate specific antigen (PSA) antibody, and the amount of antibody loaded in Example 2-12 was changed from 25 μg / mg to 20 μg / mg. In addition, a 0.1% by mass aqueous dispersion of affinity particles 2-14 was obtained in the same manner as in Example 2-12. Table 2-1 summarizes the particle properties of affinity particles 2-14.
[0538] (Example 2-16: Production of affinity particles 2-15 by antibody sensitization of particles)
[0539] The particles used were changed to particles 2-5, the antibody of Example 2-12 was changed from anti-CRP antibody to anti-bovine serum albumin (BSA) antibody, and the amount of antibody loaded in Example 2-12 was changed from 25 μg / mg to 23 μg / mg. In addition, a 0.1% by mass aqueous dispersion of affinity particles 2-15 was obtained in the same manner as in Example 2-12. Table 2-1 summarizes the particle properties of affinity particles 2-15.
[0540] (Comparative Example 2-1: Production of affinity particles 2-16 to 2-18 by antibody sensitization of particles)
[0541] 0.1 mass % aqueous dispersions of affinity particles 2-16, 2-17 and 2-18 were obtained in the same manner as in Example 2-12 except that the particles used in Example 2-12 were changed to particles 2-8, 2-9 and 2-10, respectively. Table 2-1 summarizes the particle properties of affinity particles 2-16 to 2-18.
[0542] (Comparative Example 2-2: Production of affinity particles 2-19 by antibody sensitization of particles)
[0543] A 0.1 mass % aqueous dispersion of affinity particles 2-19 was obtained in the same manner as in Example 2-12 except that the particles used were changed to particles 2-5 and the amount of antibody loaded in Example 2-12 was changed from 25 μg / mg to 5 μg / mg. Table 2-1 summarizes the particle properties of affinity particles 2-19.
[0544] (Comparative Example 2-3: Production of affinity particles 2-20 and 2-21 by antibody sensitization of particles)
[0545] A 0.1 mass % aqueous dispersion of affinity particles 2-20 and 2-21 was obtained in the same manner as in Example 2-12, except that the particles used were changed to particles 2-5 and the amount of antibody loaded in Example 2-12 was changed from 25 μg / mg to 64 μg / mg and 56 μg / mg, respectively. Table 2-1 summarizes the particle properties of affinity particles 2-20 and 2-21.
[0546] (Example 2-17: Evaluation of Antibody Sensitization Rate of Affinity Particles)
[0547] The antibody sensitization rate (%) of the affinity particles 2-1 to 2-21 produced in Examples 2-12 to 2-16 and Comparative Examples 2-1 to 2-3 was determined by protein quantification. Herein, the term "antibody sensitization rate (%)" means the ratio of the amount of antibody bound to the particle relative to the amount of antibody used in the reaction with the particle (antibody loading amount). The evaluation example of protein quantification is described below.
[0548] First, 7 mL of A solution and 140 μL of B solution of PROTEIN ASSAY BCA KIT (manufactured by FUJIFILM Wako Pure Chemical Corporation) were mixed, and the prepared liquid was used as AB solution. Next, 25 μL (particle amount: 25 μg) of the dispersion liquid (0.1% solution) of the affinity particles was taken and loaded into a 1.5 mL tube. Next, 200 μL of AB liquid was added to the dispersion liquid (25 μL), and the mixture was incubated at 60°C for 30 minutes. The resulting solution was centrifuged at 4°C and 15,000 rpm (20,400 g) for 5 minutes, and 200 μL of the supernatant was loaded into a 96-well microwell with a pipette. The absorbance of the supernatant at a wavelength of 562nm was measured using an ELISA instrument and a standard sample (by diluting the antibody with 10mM HEPES so that its concentration falls within the range of 0μg / mL to 200μg / mL to obtain several samples). The antibody amount was calculated by the standard curve. The antibody sensitization amount of the particle (antibody binding amount per particle weight (μg / mg)) was determined by dividing the calculated antibody amount by the particle weight (herein, 0.025mg). Finally, the sensitization rate was calculated. When the antibody loading was 25μg per 1mg particle, the sensitization rate was 50% when the antibody sensitization amount was 12.5μg / mg. The results are summarized in Table 2-1.
[0549] (Example 2-18: Evaluation of nonspecific adsorption to affinity particles using chylomicron)
[0550] Affinity particles 2-1 to 2-21 were each dispersed in a phosphate buffer at 0.1 mass % to prepare a dispersion (liquid A). Next, 60 μL of chylomicron (liquid B) formed by triolein, lecithin, free fatty acids, bovine albumin and Tris buffer was added to 30 μL of each dispersion, and the absorbance of the mixed solution immediately after stirring at a wavelength of 572 nm was measured. The spectrophotometer GeneQuant 1300 manufactured by Biochrom was used for absorbance measurement. Then, each mixed solution was left to stand at 37°C for 5 minutes, and then its absorbance at a wavelength of 572 nm was measured again, and then the value of the change in absorbance ΔABS×10,000 was calculated. The results are summarized in Table 2-1.
[0551] It should be understood that as this value becomes larger, nonspecific adsorption occurs to a greater extent. However, osmotic pressure agglutination rather than agglutination caused by nonspecific adsorption may be detected. In any case, when affinity particles having a large value of the absorbance change ΔABS×10,000 in this evaluation are used as particles for the latex agglutination method in sample detection, there is a concern that normal samples may be interpreted as false positives due to noise. The thresholds of excellent, good, fair, and poor in Table 2-1 are benchmarks determined by the noise risk when detecting low concentrations of target substances by the latex agglutination method.
[0552] (Example 2-19: Evaluation of dispersion stability of affinity particles)
[0553] Affinity particles 2-1 to 2-21 were each fully dispersed with ultrasound and then stored at 4°C. The sedimentation of the particles was visually observed over time. The results are summarized in Table 2-1. As described in the embodiment, affinity particles having a small zeta potential difference or an area occupied by antibodies falling within an appropriate range have satisfactory dispersion stability. The thresholds of excellent, good, neutral and poor in Table 2-1 are benchmarks determined by the storage period and particle size of the reagent to be used for the latex agglutination method (this is because, in the case of the solution composition of this embodiment, the particles inevitably undergo natural sedimentation, albeit slowly).
[0554] (Example 2-20: Evaluation 1 of latex aggregation sensitivity of affinity particles)
[0555] 1 μL of human CRP (manufactured by Denka Seiken Co., Ltd., derived from human plasma, 40 μg / ml) and 50 μL of buffer (phosphate buffered saline (PBS) containing 0.01% Tween 20) were mixed to prepare a mixed solution (hereinafter referred to as R1+), and incubated at 37°C. In addition, 1 μL of physiological saline and 50 μL of buffer (PBS containing 0.01% Tween 20) were mixed to prepare a mixed solution (hereinafter referred to as R1-) as a control, and also incubated at 37°C. Next, 50 μL of a solution each containing affinity particles 2-1 to 2-13 and affinity particles 2-16 to 2-21 prepared in each embodiment and comparative example (particle concentration: 0.1% by mass, referred to as R2) was mixed with R1+ or R1-, and the mixture was stirred. The absorbance of the mixed solution (volume: 101 μL) immediately after mixing and stirring at a wavelength of 572 nm was measured. A spectrophotometer GeneQuant 1300 manufactured by Biochrom was used for absorbance measurement. Then, the mixed solution was allowed to stand at 37°C for 5 minutes, and then its absorbance at a wavelength of 572nm was measured again, and then the value of the change in absorbance ΔABS×10,000 was calculated. This series of evaluations was performed for each of the following: R2 immediately after preparation in each embodiment and comparative example; R2 after 24 hours after preparation; and R2 after 72 hours after preparation. The results are summarized in Table 2-1. The larger the value of R- in Table 2-1, the more agglutination or osmotic pressure agglutination caused by nonspecific adsorption occurs in the affinity particles. Therefore, when the particles are used as particles for latex agglutination method in sample detection, there is a concern that normal samples will be interpreted as false positives due to noise. At the same time, it is expected that affinity particles with larger R+ values in Table 2-1 can detect target substances with higher sensitivity when used as affinity particles for latex agglutination method in sample detection. The threshold values of excellent, good, neutral, and poor for R- in Table 2-1 are benchmarks determined by the noise risk when detecting low concentrations of target substances by latex agglutination method. In addition, the threshold values of excellent, good, neutral, and poor for R+ are benchmarks determined by referring to the following values obtained by using CRP-L Auto "TBA" manufactured by Denka Seiken Co., Ltd as a CRP detection kit and CRP standard solution "TBA" for latex.
[0556] ΔABS of 0 μg / ml (normal saline) × 10,000: -80
[0557] 5 μg / ml ΔABS × 10,000: 1,410
[0558] 20 μg / ml ΔABS × 10,000: 3,530
[0559] 40 μg / ml ΔABS × 10,000: 5,130
[0560] 160 μg / ml ΔABS × 10,000: 9,750
[0561] 320 μg / ml ΔABS × 10,000: 12,150
[0562] (Example 2-21: Evaluation 2 of latex aggregation sensitivity of affinity particles)
[0563] The latex agglutination sensitivity of affinity particle 2-14 was evaluated in the same manner as in Example 2-20 except that human CRP of Example 2-20 was changed to PSA and the affinity particle was changed to affinity particle 2-14. The results are shown in Table 2-1. It was found that affinity particle 2-14 was an affinity particle with high sensitivity to PSA, just as affinity particles 2-1 to 2-13 had high sensitivity to CRP.
[0564] (Example 2-22: Evaluation 3 of latex aggregation sensitivity of affinity particles)
[0565] The latex agglutination sensitivity of affinity particle 2-15 was evaluated in the same manner as in Example 2-20 except that human CRP of Example 2-20 was changed to BSA and the affinity particle was changed to affinity particle 2-15. The results are shown in Table 2-1. It was found that affinity particle 2-15 was an affinity particle with high sensitivity to BSA, just as affinity particles 2-1 to 2-13 had high sensitivity to CRP.
[0566]
[0567]
[0568]
[0569] (Example 2-23: Synthesis of Particles 2-23)
[0570] Except that 22.7g St was changed to 12.0g, 33.9g GMA was changed to 17.9g, 0.86g divinylbenzene was changed to 0.45g, and the amount of GMA to be added to the four-necked separable flask after 2 hours of the polymerization was changed from 5.8g to 3.1g in Example 2-1, an aqueous dispersion of granular copolymer 2-2 was obtained in the same manner as in Example 2-1. After the dispersion was gradually cooled to room temperature, a portion of the dispersion was collected, and its polymerization conversion was evaluated by using proton NMR, gas chromatography and gel permeation chromatography. As a result, it was confirmed that the polymerization conversion was substantially 100%. The dry particle size of granular copolymer 2-2 was 151.4nm and the particle size in water was 160.2nm. Granular copolymer 2-2 was concentrated by ultrafiltration or diluted by adding ion exchange water to become a 2.5wt% aqueous dispersion, and the dispersion was stored at 4°C under light-shielding conditions.
[0571] A 1.0 wt% aqueous dispersion of Particle 2-23 was obtained in the same manner as in Example 2-6 except that Particle Copolymer 2-1 of Example 2-6 was changed to Particle Copolymer 2-2. Particle 2-23 had a dry particle size of 161.6 nm, a particle size in water of 202 nm, and a zeta potential of -16 mV.
[0572] (Example 2-24: Synthesis of Particles 2-24)
[0573] Except that 22.7g St was changed to 5.0g, 33.9g GMA was changed to 7.5g, 0.86g divinylbenzene was changed to 0.19g, and the amount of GMA to be added to the four-necked separable flask was changed from 5.8g to 1.3g 2 hours after the start of polymerization in Example 2-1, an aqueous dispersion of granular copolymer 2-3 was obtained in the same manner as in Example 2-1. After the dispersion was gradually cooled to room temperature, a portion of the dispersion was collected, and its polymerization conversion was evaluated by using proton NMR, gas chromatography and gel permeation chromatography. As a result, it was confirmed that the polymerization conversion was substantially 100%. The dry particle size of granular copolymer 2-3 was 96.8nm and the particle size in water was 105.2nm. Granular copolymer 2-3 was concentrated by ultrafiltration or diluted by adding ion exchange water to become a 2.5wt% aqueous dispersion, and the dispersion was stored at 4°C under light-shielding conditions.
[0574] A 1.0 wt% aqueous dispersion of Particle 2-24 was obtained in the same manner as in Example 2-6 except that Particle Copolymer 2-1 of Example 2-6 was changed to Particle Copolymer 2-3. Particle 2-24 had a dry particle size of 119 nm, a particle size in water of 144 nm, and a zeta potential of -15 mV.
[0575] (Example 2-25: Production of affinity particles 2-5K to 2-7K by antibody sensitization of particles with anti-KL-6 antibodies)
[0576] Except that the particles used in Example 2-12 are changed to particles 2-5, particles 2-23 and particles 2-24, respectively, and the antibody of Example 2-12 is changed from anti-CRP antibody to anti-KL-6 antibody, particles 2-5, particles 2-23 and particles 2-24 are sensitized with anti-KL-6 antibody in the same manner as in Example 2-12. The resulting affinity particles for KL-6 are respectively referred to as affinity particles 2-5K, affinity particles 2-6K and affinity particles 2-7K. The antibody sensitization rates of affinity particles 2-5K, affinity particles 2-6K and affinity particles 2-7K are evaluated in the same manner as in Example 2-17. As a result, it was found that the antibody sensitization rates were 93%, 100% and 94%, respectively. The occupied area rates of the antibodies were 20.3%, 17.3% and 12.4%, respectively. The zeta potential of the anti-KL-6 antibody is -14mV. Therefore, the zeta potential differences (mV) of affinity particles 2-5K, affinity particles 2-6K, and affinity particles 2-7K are 2, 2, and 1, respectively.
[0577] (Example 2-26: Evaluation of the latex aggregation sensitivity of affinity particles to KL-6)
[0578] The latex agglutination sensitivity of the affinity particles 2-5K, 2-6K, and 2-7K was evaluated in the same manner as in Example 2-20 except that the human CRP of Example 2-20 was changed to human KL-6.
[0579] The absorbance change (ΔABS×10,000) obtained with affinity particles 2-5K is shown below.
[0580] 0U / mL (normal saline): -140
[0581] 500U / mL: 410
[0582] 1,000 U / mL: 1,380
[0583] 2,000 U / mL: 4,840
[0584] 5,000 U / mL: 7,520
[0585] The absorbance change (ΔABS×10,000) obtained with affinity particles 2-6K is shown below.
[0586] 0U / mL (normal saline): -240
[0587] 500U / mL: -90
[0588] 1,000 U / mL: 480
[0589] 2,000 U / mL: 3,320
[0590] 5,000 U / mL: 6,160
[0591] The absorbance change (ΔABS×10,000) obtained with affinity particles 2-7K is shown below.
[0592] 0U / mL (normal saline): -320
[0593] 500U / mL: -50
[0594] 1,000U / mL: -340
[0595] 2,000 U / mL: 550
[0596] 5,000 U / mL: 1,200
[0597] All particles showed a linear absorbance change relative to the concentration of KL-6. It was found that when the concentration of KL-6 was constant, the absorbance change increased as the particle size became larger. The latex aggregation sensitivity can be controlled by controlling the particle size.
[0598] (Example 2-27: Effect of sensitizer on latex aggregation sensitivity)
[0599] The latex agglutination sensitivity of affinity particles 2-5K and affinity particles 2-6K was evaluated in the same manner as in Example 2-20, except that the human CRP of Example 2-20 was changed to human KL-6 and the buffer (PBS containing 0.01% Tween 20) was changed to a buffer containing a sensitizer (PBS containing 0.58% PVP K90 or 0.68% sodium alginate 80-120 and 0.01% Tween 20).
[0600] In the case of using alginic acid as a sensitizer, the amount of absorbance change (ΔABS×10,000) obtained with affinity particles 2-5K is shown below.
[0601] 0U / mL (normal saline): -240
[0602] 500 U / mL: 1,090
[0603] 1,000 U / mL: 2,780
[0604] 2,000 U / mL: 9,960
[0605] 5,000 U / mL: 11,520
[0606] In the case of using alginic acid as a sensitizer, the amount of absorbance change (ΔABS×10,000) obtained with the affinity particles 2-6K is shown below.
[0607] 0U / mL (normal saline): -50
[0608] 500U / mL: 420
[0609] 1,000 U / mL: 1,260
[0610] 2,000 U / mL: 6,590
[0611] 5,000 U / mL: 8,720
[0612] In the case of using PVP as a sensitizer, the absorbance change (ΔABS×10,000) obtained with affinity particles 2-5K is shown below.
[0613] 0U / mL (normal saline): -70
[0614] 500U / mL: 480
[0615] 1,000 U / mL: 1,020
[0616] 2,000 U / mL: 3,860
[0617] 5,000 U / mL: 5,970
[0618] In the case of using PVP as a sensitizer, the amount of absorbance change (ΔABS×10,000) obtained with affinity particles 2-6K is shown below.
[0619] 0U / mL (normal saline): -280
[0620] 500U / mL: -60
[0621] 1,000 U / mL: 670
[0622] 2,000 U / mL: 4,080
[0623] 5,000 U / mL: 6,820
[0624] The sensitizing effects of PVP and alginic acid were confirmed for the affinity particles 2-5K and 2-6K. In particular, it was found that alginic acid had a high sensitizing effect.
[0625] (Example 2-28: Production of affinity particles 2-5I by antibody sensitization of particles with anti-IgE antibodies)
[0626] Particles 2-5 were sensitized with anti-IgE antibody in the same manner as in Example 2-12, except that the antibody in Example 2-12 was changed from anti-CRP antibody to anti-IgE antibody. The resulting affinity particles for IgE were referred to as affinity particles 2-5I.
[0627] The antibody sensitization rate of affinity particle 2-5I was evaluated in the same manner as in Example 2-17. As a result, it was found that the antibody sensitization rate was 80%. The area occupied by the antibody was 18%. The zeta potential of the anti-IgE antibody was -6 mV. Therefore, the zeta potential difference (mV) of affinity particle 2-5I was 10.
[0628] (Example 2-29: Evaluation of the latex agglutination sensitivity of affinity particles to IgE)
[0629] The latex agglutination sensitivity of affinity particles 2-5I was evaluated in the same manner as in Example 2-20, except that human CRP in Example 2-20 was changed to human IgE. The sample volume was set to 1.5 μL, the amount of the sample diluent (Good's buffer, LT Auto Wako IgE, Wako Pure Chemical Industries, Ltd.) was set to 75 μL, and the amount of the affinity particle dispersion was set to 25 μL.
[0630] The absorbance change (ΔABS×10,000) obtained using affinity particles 2-5I is shown below.
[0631] 0IU / mL (normal saline): -60
[0632] 100IU / mL: -50
[0633] 300 IU / mL: 100
[0634] 1,000 IU / mL: 200
[0635] 2,000 IU / mL: 510
[0636] 3,000 IU / mL: 1,790
[0637] The absorbance change of affinity particle 2-5I was linear with respect to the concentration of IgE.
[0638] Furthermore, the latex agglutination sensitivity of the affinity particle 2-5I was evaluated in the same manner as in Example 2-27 using a buffer containing a sensitizer (Good's buffer containing 0.045% alginic acid was used as a sample diluent).
[0639] In the case of using alginic acid as a sensitizer, the amount of absorbance change (ΔABS×10,000) obtained with affinity particles 2-5K is shown below.
[0640] 0IU / mL (normal saline): 30
[0641] 100 IU / mL: 140
[0642] 300IU / mL: 300
[0643] 1,000 IU / mL: 1,130
[0644] 2,000 IU / mL: 3,870
[0645] 3,000 IU / mL: 5,910
[0646] Regarding the affinity particle 2-5I, the sensitizing effect of alginic acid was confirmed.
[0647] (Example 2-30: Production of affinity particles 2-22 by antibody sensitization of particles and evaluation thereof)
[0648] Except that 1M Tris in the masking buffer of Example 2-12 is changed to 1M ethanolamine, the particle 2-5 is sensitized with the anti-CRP antibody in the same manner as in Example 2-12. The resulting affinity particle for CRP is called affinity particle 2-22. The difference from affinity particle 2-5 is that a part of the carboxyl group of the repeating unit A is Tris in affinity particle 2-5, while it is ethanolamine in affinity particle 2-22. Therefore, affinity particle 2-22 is the same as affinity particle 2-5 in terms of antibody sensitization rate and antibody occupied area rate.
[0649] The latex aggregation sensitivity of affinity particles 2-22 was evaluated in the same manner as in Example 2-20.
[0650] The relative value of the absorbance change amount (ΔABS×10,000) obtained with affinity particles 2-22 to that with affinity particles 2-5 is shown below.
[0651] 5μg / mL: 1.11
[0652] 20μg / mL: 1.17
[0653] 40 μg / mL: 1.13
[0654] 160 μg / mL: 1.09
[0655] 320 μg / mL: 1.10
[0656] It was found that affinity particle 2-22 increased the amount of absorbance change compared to affinity particle 2-5. The latex agglutination sensitivity to CRP can be controlled by changing the masking chemical structure to ethanolamine.
[0657] Hereinafter, the present invention is described in detail by way of examples corresponding to the third embodiment. However, the present invention is not limited to these examples.
[0658] (Example 3-1: Synthesis of Particle 3-1)
[0659] 1.2 g of styrene (Kishida Chemical Co., Ltd.), 1.8 g of glycidyl methacrylate (Kishida Chemical Co., Ltd.), 0.04 g of divinylbenzene (Kishida Chemical Co., Ltd.) and 100 g of ion exchange water were weighed in a 200 mL flask to provide a mixed solution. Thereafter, the mixed solution was maintained at 40° C. while stirring at 200 rpm, and nitrogen bubbling was performed for 30 minutes. Next, the nitrogen bubbling was replaced with a nitrogen stream. Then, a separately prepared solution obtained by dissolving 0.06 g of V-50 (Wako Pure Chemical Industries, Ltd.) in 3 g of ion exchange water was added to the mixed solution to initiate free radical polymerization (soap-free emulsion polymerization). Two hours after the start of the polymerization, 0.3 g of glycidyl methacrylate was added to the free radical polymerization reaction field, and the mixture was maintained at 70° C. while stirring at 200 rpm for 8 hours, and then gradually cooled to room temperature to provide a particle dispersion (process 1). At this time, the contents of the 200 mL flask were sampled, and their free radical polymerization conversions were evaluated by using proton NMR, gas chromatography, and gel permeation chromatography. As a result, it was confirmed that the free radical polymerization conversion was substantially 100%. While the particle dispersion obtained in step 1 was cooled in an ice bath and stirred, an aqueous solution obtained by adding 2.2 g of mercaptosuccinic acid (Wako Pure Chemical Industries, Ltd.: the total number of moles of mercaptosuccinic acid is equal to the number of moles of glycidyl methacrylate) and 3.0 g of triethylamine to 40 g of ion exchange water was prepared and added dropwise to the particle dispersion. After completion of the dropwise addition, the pH of the reaction solution was adjusted to 10.3 by using triethylamine and a 2N hydrochloric acid aqueous solution. Thereafter, the resultant was heated to 70° C. and maintained for 4 hours while stirring, so that the epoxy group derived from glycidyl methacrylate and the thiol group derived from mercaptosuccinic acid were chemically reacted to provide particles 3-1 having a carboxyl group as a reactive functional group (step 2). Agglomerates and the like did not appear during the chemical reaction. Particles 3-1 were purified by centrifugation, and, before storage, the dispersion medium was replaced with pure water (replacement of the dispersion medium was also performed by centrifugation). Particles 3-1 were evaluated by using dynamic light scattering (DLS-8000: Otsuka Electronics Co., Ltd.) to find that their number average particle diameter was 214 nm. In addition, their carboxyl group amount per unit mass was quantified and was 130 [nmol / mg].
[0660] (Example 3-2: Synthesis of Particle 3-2)
[0661] Except that the pH of the reaction solution in step 2 of Example 3-1 was changed from 10.3 to 10.7, particles 3-2 having carboxyl groups as reactive functional groups were obtained by the same experimental operation as in Example 3-1. The purification and storage methods were also the same. The particle size of particles 3-2 was evaluated by using a dynamic light scattering method (DLS-8000: Otsuka Electronics Co., Ltd.) and found that their number average particle size was 226 nm. In addition, the amount of carboxyl groups per unit mass was quantified and was 200 [nmol / mg].
[0662] (Example 3-3: Synthesis of Particle 3-3)
[0663] Particles 3-3 having a carboxyl group as a reactive functional group were obtained by the same experimental operation as in Example 3-1, except that 2.2 g of mercaptosuccinic acid in step 2 of Example 3-1 was changed to 1.6 g of mercaptopropionic acid (Wako Pure Chemical Industries, Ltd.: the number of moles of mercaptopropionic acid is equal to the number of moles of glycidyl methacrylate) and the amount of triethylamine to be added to the aqueous solution was changed to 1.6 g. As in Example 3-1, no agglomerates or the like appeared during the chemical reaction. The purification and storage methods were also the same. The particle size of particles 3-3 was evaluated by using a dynamic light scattering method (DLS-8000: Otsuka Electronics Co., Ltd.) and their number average particle size was found to be 211 nm. In addition, their carboxyl group amount per unit mass was quantified and was 120 [nmol / mg].
[0664] (Example 3-4: Synthesis of Particles 3-4)
[0665] Except that the reaction was carried out without adding triethylamine in step 2 of Example 3-1, particles 3-4 having a carboxyl group as a reactive functional group were obtained by the same experimental operation as in Example 3-1. The purification and storage methods were also the same. The particle size of particles 3-4 was evaluated by using a dynamic light scattering method (DLS-8000: Otsuka Electronics Co., Ltd.) and found that their number average particle size was 209 nm. In addition, the amount of carboxyl groups per unit mass was quantified and was 20 [nmol / mg].
[0666] (Example 3-5: Synthesis of Particles 3-5)
[0667] Except that the pH of the reaction solution in step 2 of Example 3-1 was changed from 10.3 to 9.9, particles 3-5 having a carboxyl group as a reactive functional group were obtained by the same experimental operation as in Example 3-1. The purification and storage methods were also the same. The particle size of particles 3-5 was evaluated by using a dynamic light scattering method (DLS-8000: Otsuka Electronics Co., Ltd.) and found that their number average particle size was 216 nm. In addition, the amount of carboxyl groups per unit mass was quantified and was 80 [nmol / mg].
[0668] (Example 3-6: Synthesis of Particles 3-6)
[0669] While the particles 3-5 obtained in Example 3-5 were cooled in an ice bath and stirred, an aqueous solution obtained by adding 0.9 g of aminoethanol (Wako Pure Chemical Industries, Ltd.: the total mole number of aminoethanol is equal to the mole number of glycidyl methacrylate) and 0.6 g of sodium hydroxide (Kishida Chemical Co., Ltd.: in an amount equal to the mole number of aminoethanol) to 40 g of ion exchange water was prepared and dropped into the particle dispersion. After the dropwise addition was completed, the pH of the reaction liquid was adjusted to 10.0 by using sodium hydroxide and 1N hydrochloric acid. Thereafter, the resultant was heated to 70°C and maintained for 4 hours while stirring, so that the epoxy group derived from glycidyl methacrylate and the amino group derived from aminoethanol were chemically reacted to provide particles 3-6 in which the epoxy group was ring-opened. Agglomerates and the like did not appear during the chemical reaction. Particles 3-6 were purified by centrifugal operation, and, before storage, the dispersion medium was replaced with pure water (the replacement of the dispersion medium was also performed by centrifugal operation). Particles 3 to 6 were evaluated by using dynamic light scattering (DLS-8000: Otsuka Electronics Co., Ltd.) to find that their number average particle diameter was 214 nm. In addition, their carboxyl group amount per unit mass was quantified and was 80 [nmol / mg].
[0670] (Example 3-7: Synthesis of Particles 3-7)
[0671] While the particles 3-5 obtained in Example 3-5 were cooled in an ice bath and stirred, an aqueous solution obtained by adding 1.4 g of 3-mercapto-1-propanol (Wako Pure Chemical Industries, Ltd.: the total number of moles of mercaptopropanol is equal to the number of moles of glycidyl methacrylate) and 1.5 g of triethylamine (Kishida Chemical Co., Ltd.: in an amount equal to the number of moles of 3-mercapto-1-propanol) to 40 g of ion exchange water was prepared and dropped into the particle dispersion. After the dropwise addition was completed, the pH of the reaction liquid was adjusted to 10.0 by using triethylamine and 1N hydrochloric acid. Thereafter, the resultant was heated to 70°C and maintained for 4 hours while stirring to allow the epoxy group derived from glycidyl methacrylate and the mercapto group derived from mercaptopropanol to chemically react to provide particles 3-7 in which the epoxy group was ring-opened. Agglomerates and the like did not occur during the chemical reaction. Particles 3-7 were purified by centrifugation, and before storage, the dispersion medium was replaced with pure water (the replacement of the dispersion medium was also performed by centrifugation). Particles 3-7 were evaluated by dynamic light scattering (DLS-8000: Otsuka Electronics Co., Ltd.) to find that their number average particle size was 220 nm. In addition, their carboxyl group amount per unit mass was quantified and was 80 [nmol / mg].
[0672] (Comparative Example 3-1: Synthesis of Modified SG Particles 3-1)
[0673] Modified SG particles 3-1 having a carboxyl group as a reactive functional group were obtained by the same experimental operation as in Example 3-1, except that 2.2 g of mercaptosuccinic acid in step 2 of Example 3-1 was changed to 1.1 g of glycine (Wako Pure Chemical Industries, Ltd.: the number of moles of glycine is equal to the number of moles of glycidyl methacrylate) and the amount of triethylamine to be added to the aqueous solution was changed to 1.6 g. As in Example 3-1, no agglomerates or the like appeared during the chemical reaction. The purification and storage methods were also the same. The particle size of the modified SG particles 3-1 was evaluated by using a dynamic light scattering method (DLS-8000: Otsuka Electronics Co., Ltd.) and their number average particle size was found to be 211 nm. In addition, their carboxyl group amount per unit mass was quantified and was 120 [nmol / mg].
[0674] (Synthesis of affinity particles: Binding of antibodies)
[0675] Each of particles 3-1 to 3-7 and modified SG particles 3-1 was dispersed in MES buffer at 1.0wt% to prepare 1 μL of each dispersion. The solution obtained by dissolving 0.055mg 1-[3-(dimethylaminopropyl)-3-ethylcarbodiimide] (Wako PureChemical Industries, Ltd.) in 10 μL of phosphate buffer was added to each of these dispersions. Thereafter, 5 μL of 4.9mg / mL dispersion of clone C5 (Funakoshi Co., Ltd.) of monoclonal mouse anti-human C-reactive protein (hereinafter referred to as CRP antibody) and 5 μL of 5.8mg / mL dispersion of clone C6 (Funakoshi Co., Ltd.) thereof were added to the mixture. Then, the mixture was shaken at room temperature for 180 hours to synthesize affinity particles. Next, the affinity particles were purified by centrifugal purification (15,000rpm) three times, and finally stored in a state dispersed in 1mL of phosphate buffer. The affinity particles obtained from particles 3-1 to 3-7 are hereinafter referred to as affinity particles 3-1 to 3-7, respectively. In addition, the affinity particles obtained from modified SG particles 3-1 are referred to as CRP-immobilized modified SG particles 3-1.
[0676] The sensitization rates of affinity particles 3-1 to 3-7 and CRP-immobilized modified SG particle 3-1 were evaluated based on the following indices. The results are shown in Table 3-1.
[0677] A: More than 80%
[0678] B: 60% or more and less than 80%
[0679] C: less than 60%
[0680] (Evaluation of Antigen-Antibody Reactivity to Human CRP Antigen)
[0681] 1 μL of human CRP (C4063 manufactured by Sigma-Aldrich, C-reactive protein, derived from human plasma, 32 mg / dl) and 50 μL of buffer (buffer (R-1) of CRP-L Auto "TBA", Denka Seiken Co., Ltd.) were mixed to obtain a mixed solution, and the mixed solution was warmed at 37°C for 5 minutes. Next, 50 μL of each dispersion of the affinity particles obtained in Examples 3-1 to 3-7 and Comparative Example 3-1 was mixed with the mixed solution, and the absorbance of the dispersion immediately after stirring at a wavelength of 572 nm was measured. A spectrophotometer GeneQuant 1300 manufactured by Biochrom was used for absorbance measurement. Then, the dispersion was allowed to stand at 37°C for 5 minutes, and then its absorbance at a wavelength of 572 nm was measured again, and then the change in absorbance ΔABS×10,000 was calculated. Regarding the value of the amount of change in absorbance ΔABS×10,000, affinity particles 3-1 to 3-7 and CRP-immobilized modified SG particle 3-1 were evaluated based on the following indices, respectively. The results are shown in Table 3-1.
[0682] A: The change is 10,000 or more.
[0683] B: The amount of change is 5,000 or more and less than 10,000.
[0684] C: The change is less than 5,000.
[0685] (Nonspecific adsorption evaluation)
[0686] In addition, the nonspecific adsorption was evaluated by performing the evaluation in the same manner except that physiological saline was used instead of adding 1 μL of human CRP (C4063 manufactured by Sigma-Aldrich, C-reactive protein, derived from human plasma, 32 mg / dl), and the amount of change in absorbance ΔABS×10,000 was calculated. For the value of the amount of change in absorbance ΔABS×10,000, affinity particles 3-1 to 3-7 and CRP-immobilized modified SG particles 3-1 were evaluated based on the following indicators, respectively. The results are shown in Table 3-1.
[0687] A: The change is less than 1,000.
[0688] B: The amount of change is 1,000 or more.
[0689] [Table 3-1]
[0690] Table 3-1
[0691]
[0692] As described above, the following particles can be provided, which have a structure having a carboxyl group in the side chain via a thioether group, and therefore have excellent ability to suppress nonspecific adsorption, have highly sensitive sensitization in the immunolatex agglutination method, and chemically bind ligands to the particle surface with high yield.
[0693] (Example 3-8: Synthesis of Particles 3-8 Having Small Particle Size)
[0694] In Example 3-1, the amount of styrene was changed to 0.5 g, the amount of glycidyl methacrylate was changed to 0.8 g, the amount of divinylbenzene was changed to 0.02 g, and the amount of GMA to be added to the four-necked separable flask 2 hours after the start of polymerization was changed to 0.13 g. A particle dispersion was obtained in the same manner as in step 1 of Example 3-1. Particles 3-8 having a carboxyl group as a reactive functional group were obtained by the same experimental operation as in step 2 of Example 3-1, except that the pH of the reaction solution in step 2 of Example 3-1 was changed from 10.3 to 10.7. The particles were centrifuged and purified, and then, before storage, the dispersion medium was replaced with pure water. Particles 3-8 were evaluated by using dynamic light scattering (DLS-8000: Otsuka Electronics Co., Ltd.) and found that their number average particle size was 184 nm. In addition, their carboxyl group amount per unit mass was quantified and was 215 [nmol / mg].
[0695] (Example 3-9: Synthesis of Particles 3-9 with Different Amounts of Carboxyl Groups and Small Particle Sizes)
[0696] Except that the pH of the reaction solution in step 2 of Example 3-8 was changed from 10.3 to 9.98, particles 3-9 having a carboxyl group as a reactive functional group were obtained by the same experimental operation as in Example 3-8. The purification and storage methods were also the same. The particle size of particles 3-9 was evaluated by using a dynamic light scattering method (DLS-8000: Otsuka Electronics Co., Ltd.) and found that their number average particle size was 153 nm. In addition, the amount of carboxyl groups per unit mass was quantified and was 96 [nmol / mg].
[0697] (Example 3-10: Synthesis of Particles 3-10 with Different Amounts of Carboxyl Groups and Small Particle Sizes)
[0698] Except that the pH of the reaction solution in step 2 of Example 3-8 is changed from 10.3 to 2.3 (without using triethylamine), particles 3-10 having a carboxyl group as a reactive functional group are obtained by the same experimental operation as in Example 3-8. The purification and storage methods are also the same. The particle size of particles 3-10 was evaluated by using a dynamic light scattering method (DLS-8000: Otsuka Electronics Co., Ltd.) and found that their number average particle size was 149 nm. In addition, the amount of carboxyl groups per unit mass was quantified and was 22 [nmol / mg].
[0699] (Example 3-11: Synthesis of Particles 3-11 Having Large Particle Size)
[0700] In Example 3-1, the amount of styrene was changed to 2.27 g, the amount of glycidyl methacrylate was changed to 3.4 g, the amount of divinylbenzene was changed to 0.08 g, and the amount of GMA to be added to the four-necked separable flask 2 hours after the start of polymerization was changed to 0.56 g. A particle dispersion was obtained in the same manner as in step 1 of Example 3-1. Particles 3-11 having a carboxyl group as a reactive functional group were obtained by the same experimental operation as in step 2 of Example 3-1, except that the pH of the reaction solution in step 2 of Example 3-1 was changed from 10.3 to 11.3. The particles were centrifuged and purified, and then, before storage, the dispersion medium was replaced with pure water. Particles 3-11 were evaluated by using dynamic light scattering (DLS-8000: Otsuka Electronics Co., Ltd.) and found that their number average particle size was 309 nm. In addition, their carboxyl group amount per unit mass was quantified and was 266 [nmol / mg].
[0701] (Example 3-12: Synthesis of Particles 3-12 with Large Particle Sizes Having Different Amounts of Carboxyl Groups)
[0702] Except that the pH of the reaction solution in step 2 of Example 3-11 is changed from 11.3 to 11.0, particles 3-12 having carboxyl groups as reactive functional groups are obtained by the same experimental operation as in Example 3-11. The purification and storage methods are also the same. The particle size of particles 3-12 was evaluated by using a dynamic light scattering method (DLS-8000: Otsuka Electronics Co., Ltd.) and found that their number average particle size was 280 nm. In addition, the amount of carboxyl groups per unit mass was quantified, which was 239 [nmol / mg].
[0703] (Example 3-13: Synthesis of Particles 3-13 with Large Particle Sizes Having Different Amounts of Carboxyl Groups)
[0704] Except that the pH of the reaction solution in step 2 of Example 3-11 is changed from 11.3 to 2.4 (without using triethylamine), particles 3-13 having a carboxyl group as a reactive functional group are obtained by the same experimental operation as in Example 3-11. The purification and storage methods are also the same. The particle size of particles 3-13 was evaluated by using a dynamic light scattering method (DLS-8000: Otsuka Electronics Co., Ltd.) and found that their number average particle size was 247nm. In addition, the amount of carboxyl groups per unit mass was quantified and was 16 [nmol / mg].
[0705] (Example 3-14: Synthesis of affinity particles)
[0706] 0.1 mL (particle 1 mg) of each of particles 3-8 to 3-13 (solution with a concentration of 1.0 wt%, 10 mg / mL) was transferred to a microtube (volume: 1.5 mL), 0.12 mL of activation buffer (25 mM MES, pH: 6.0) was added thereto, and the mixture was centrifuged at 4°C and 15,000 rpm (20,400 g) for 5 minutes. After centrifugation, the supernatant was discarded. 0.12 mL of activation buffer (25 mM MES, pH: 6.0) was added to the residue, and the particles were redispersed with ultrasound. Centrifugation and redispersion were repeated once.
[0707] Next, 60 μL of a WSC solution (a solution obtained by dissolving 50 mg of WSC in 1 mL of an activation buffer, the term "WSC" means 1-[3-(dimethylaminopropyl)-3-ethylcarbodiimide] hydrochloride) and a Sulfo NHS solution (a solution obtained by dissolving 50 mg of Sulfo NHS in 1 mL of an activation buffer, the term "Sulfo NHS" means sulfo-N-hydroxysuccinimide) were each added to the resultant, and dispersed with ultrasonic waves. The dispersion was stirred at room temperature for 30 minutes to convert the carboxyl groups of its particles into active esters. The resultant was centrifuged at 4° C. and 15,000 rpm (20,400 g) for 5 minutes, and the supernatant was discarded. 0.2 mL of an immobilization buffer (25 mM MES, pH: 5.0) was added to the residue, and the particles were dispersed with ultrasonic waves. The dispersion was centrifuged at 4° C. and 15,000 rpm (20,400 g) for 5 minutes, and the supernatant was discarded. 50 μL of immobilization buffer was added to the residue, and the carboxyl-activated particles were dispersed using ultrasound.
[0708] 50 μL antibody solution (a solution obtained by diluting anti-CRP antibody with immobilization buffer to make its concentration 25 μg / 50 μL) is added to the solution of 50 μL carboxyl activated particles, and the particles are dispersed with ultrasound. The amount of antibody loaded is 25 μg (25 μg / mg) per 1 mg particle. The final antibody concentration is 0.25 mg / mL, and the final particle concentration is 10 mg / mL. The contents in the microtube are stirred at room temperature for 60 minutes to bind the antibody to the carboxyl of the particles. Next, the resultant is centrifuged at 4 ° C and 15,000 rpm (20,400 g) for 5 minutes, and the supernatant is discarded. 0.24 mL masking buffer (buffer obtained by including 0.1% Tween 20 in 1M Tris at pH 8.0) is added to the residue, and the particles are dispersed with ultrasound. The dispersion is stirred at room temperature for 1 hour, and then left to stand overnight at 4 ° C to bind Tris to the residual activated carboxyl. Next, the resultant was centrifuged at 4°C and 15,000rpm (20,400g) for 5 minutes, and the supernatant was discarded. 0.2mL washing buffer (10mM HEPES, pH: 7.9) was added to the residue, and the particles were dispersed with ultrasound. The washing operation (centrifugation and redispersion) using washing buffer (10mM HEPES, pH: 7.9) was repeated once. The washing operation was performed once with 0.2mL preservation buffer (10mM HEPES, pH: 7.9, containing 0.01% Tween 20). 1.0mL preservation buffer was added to the washed product, and the particles were dispersed with ultrasound. The particle concentration of the dispersion eventually became 0.1wt% (1mg / mL). The dispersion was stored in a refrigerator. The affinity particles obtained from particles 3-8 to 3-13 are hereinafter referred to as affinity particles 3-8 to 3-13, respectively.
[0709] (Example 3-15: Evaluation of Antigen-Antibody Reactivity of Affinity Particles 3-8 to 3-13)
[0710] The antigen-antibody reactivity to human CRP antigen was evaluated in the same manner as in the above example. The values of the change in absorbance ΔABS×10,000 of affinity particles 3-8 to 3-13 relative to human CRP (32 mg / dl) were 3,430, 4,330, 6,930, 2,250, 6,750, and 12,400, respectively. Antigen-antibody reactivity to human CRP antigen was confirmed in all particles.
[0711] (Example 3-16: Evaluation of nonspecific adsorption of affinity particles 3-8 to 3-13)
[0712] The evaluation of nonspecific adsorption using physiological saline was performed in the same manner as in the above-mentioned Example. The values of the absorbance variation ΔABS×10,000 of affinity particles 3-8 to 3-13 were 40, 80, 120, -240, 0, and 260, respectively. No nonspecific adsorption was found in any of the particles.
[0713] (Example 3-17: Synthesis of affinity particles with increased antibody binding capacity)
[0714] In addition to changing the amount of loaded antibody to 200 μg per 1 mg of particles (200 μg / mg), affinity particles 3-14 with increased antibody binding amount were synthesized by binding anti-CRP antibodies to particles 3-8 in the same manner as in Example 3-14. The antigen-antibody reactivity of the obtained affinity particles 3-14 to human CRP antigen was evaluated. As a result, it was found that the value of the change in absorbance ΔABS×10,000 of affinity particles 3-14 relative to human CRP (32 mg / dl) was 10,440. An evaluation of nonspecific adsorption using physiological saline was performed. As a result, it was found that the value of the change in absorbance ΔABS×10,000 of affinity particles 3-14 was 600. It was found that the change in absorbance, that is, sensitivity, can be increased by increasing the amount of antibody bound to the particles.
[0715] (Example 3-18: Evaluation of non-specific adsorption of human serum samples to particles)
[0716] 51 μL of a sample dilution formed by a human serum sample (1 μL, NHS-9, Tennessee Blood Services) and a phosphate buffer (50 μL) was added to a 50 μL dispersion of each of particles 3-8 to 3-12, and the absorbance of the mixed solution immediately after stirring at a wavelength of 572 nm was measured. A spectrophotometer GeneQuant 1300 manufactured by Biochrom was used for absorbance measurement. Then, each mixed solution was allowed to stand at 37°C for 5 minutes, and then its absorbance at a wavelength of 572 nm was measured again, and then the value of the change in absorbance ΔABS×10,000 was calculated. It should be understood that as the value becomes larger, more nonspecific adsorption occurs. The values of the change in absorbance ΔABS×10,000 of particles 3-8 to 3-12 were -70, -20, 60, -50 and 40, respectively. No nonspecific adsorption to human serum samples was found in any of the particles.
[0717] The present invention is not limited to the above-described embodiments, and various changes and modifications may be made without departing from the spirit and scope of the present invention. Therefore, the following claims are attached hereto to disclose the scope of the present invention.
[0718] This application claims priority based on Japanese Patent Application No. 2019-158952 filed on August 30, 2019, Japanese Patent Application No. 2019-158962 filed on August 30, 2019, and Japanese Patent Application No. 2019-158138 filed on August 30, 2019, and the entire contents of which are incorporated herein by reference.
Claims
1. An affinity particle for latex agglutination method, comprising: A particle comprising a copolymer having a repeating unit A and a repeating unit B in a surface layer thereof, and a ligand bound to the particle, It is characterized in that the repeating unit A has a side chain A, and the side chain A has a carboxyl group to be bound to the ligand at its end, wherein the repeating unit B has a side chain B, and the side chain B has a hydroxyl group at its terminal, wherein the particles are constituted so that when the particles are dispersed in ion exchange water, the surface layer of the particles contains water to form a swelling layer, wherein the density of the carboxyl groups contained in the swelling layer satisfies the formula (1-1), and wherein the dry particle size measured when the particles are dried and the particle size in water measured when the particles are dispersed in ion exchange water satisfy formula (1-2), 0.04≤[Carboxyl group density]≤0.15···Formula (1-1) 1.10≤[particle size in water / dry particle size]≤1.40···Formula (1-2) The unit of carboxyl density is / nm 3 .
2. The affinity particle according to claim 1, wherein the zeta potential of the particle satisfies formula (1-3), -30≤[Zeta potential]≤-10···Formula (1-3) The unit of Zeta potential is mV.
3. The affinity particle according to claim 1 or 2, wherein the number of moles of the repeating unit A and the number of moles of the repeating unit B satisfy formula (1-4), 0.05≤[the number of moles of repeating unit A] / [the number of moles of repeating unit B]≤1.00···Formula (1-4).
4. The affinity particle according to claim 1 or 2, wherein the repeating unit A is represented by formula (1-5): wherein R1 represents a methyl group or a hydrogen atom, R2 represents a carboxyl group or a hydrogen atom, and L1 represents an optionally substituted alkylene group having 1 to 15 carbon atoms or an optionally substituted oxyalkylene group having 1 to 15 carbon atoms.
5. The affinity particle according to claim 4, wherein the repeating unit B is represented by formula (1-6): wherein R1 represents a methyl group or a hydrogen atom, L2 represents an optionally substituted alkylene group or oxyalkylene group having 2 to 15 carbon atoms, and has the relationship of [the number of carbon atoms of L1]+2≥[the number of carbon atoms of L2], and X represents a sulfur atom or an optionally substituted nitrogen atom. 6 . The affinity particle according to claim 4 , wherein L1 in the formula (1-5) represents an alkylene group having 1 carbon atom. 7 . The affinity particle according to claim 5 , wherein L 2 in the formula (1-6) represents an alkylene group having 2 carbon atoms.
8. The affinity particle according to claim 5, wherein in the formula (1-6), X represents a sulfur atom, L2 represents an alkylene group having 3 carbon atoms, and one hydrogen atom of the alkylene group is substituted with a hydroxyl group. 9 . The affinity particles according to claim 1 , wherein the particles have, as a repeating unit C, at least one selected from the group consisting of styrenes and (meth)acrylates.
10. The affinity particle according to claim 1 or 2, wherein the ligand is an antibody or an antigen.
11. An affinity particle for latex agglutination method, characterized in that: It includes: Particles; and The ligands on the particle surface, The area ratio of the ligand to the particle surface satisfies the relationship of formula (2-1), The zeta potentials of the particles and the ligands satisfy the relationship of formula (2-2), and wherein the particles have a repeating unit A represented by formula (2-3): 10≤[occupancy rate]≤40…Formula (2-1) 0≤[||Zeta potential of particles|-|zeta potential of ligand||]≤20…Formula (2-2) The unit of area occupancy is %, and the unit of zeta potential is mV. In the formula (2-3), R1 represents a methyl group or a hydrogen atom, R2 represents a carboxyl group or a hydrogen atom, and L1 represents an optionally substituted alkylene group having 1 to 15 carbon atoms or an optionally substituted oxyalkylene group having 1 to 15 carbon atoms. 12 . The affinity particle according to claim 11 , wherein the particle has a repeating unit B having a hydroxyl group at a terminal of a side chain thereof. 13 . The affinity particle according to claim 11 , wherein L1 in the formula (2-3) represents a methylene group.
14. The affinity particle according to claim 11 or 12, wherein R2 in the formula (2-3) represents a carboxyl group.
15. The affinity particle according to claim 12, wherein the repeating unit B is represented by formula (2-4): In the formula (2-4), R1 represents a methyl group or a hydrogen atom, L2 represents an alkylene group having 2 to 15 carbon atoms which may be substituted or an oxyalkylene group having 2 to 15 carbon atoms which may be substituted, X represents a sulfur atom or a nitrogen atom which may be substituted, and L1 in the formula (2-3) and L2 in the formula (2-4) satisfy the relationship of [the number of carbon atoms of L1] + 2 ≥ [the number of carbon atoms of L2]. 16 . The affinity particle according to claim 15 , wherein L2 in the formula (2-4) represents an alkylene group having 2 carbon atoms.
17. The affinity particle according to claim 15, wherein X in the formula (2-4) represents a sulfur atom, L2 in the formula (2-4) represents an alkylene group having 3 carbon atoms, and one hydrogen atom of the alkylene group represented by L2 is substituted with a hydroxyl group.
18. The affinity particle according to claim 12, wherein a surface layer of the particle comprises a copolymer having the repeating unit A and the repeating unit B, and when the particle is dispersed in an aqueous solution, the surface layer contains water to form a swelling layer.
19. The affinity particle according to claim 11 or 12, wherein the dry particle size of the particle measured when the particle is dry and the particle size of the particle in water measured when the particle is dispersed in ion exchange water satisfy the formula (2-5), 1.1≤[particle size in water / particle size in dry state]≤1.4…Formula (2-5).
20. The affinity particle according to claim 11 or 12, wherein the affinity particle has a chemical structure represented by formula (2-6) obtained by converting a part of the carboxyl group of the repeating unit A by using a chemical reaction: In the formula (2-6), R1 represents a methyl group or a hydrogen atom, R2 represents a carboxyl group or a hydrogen atom, and L1 represents an optionally substituted alkylene group having 1 to 15 carbon atoms or an optionally substituted oxyalkylene group having 1 to 15 carbon atoms.
21. The affinity particles according to claim 11 or 12, wherein the particles have, as a repeating unit C, at least one selected from the group consisting of styrenes and (meth)acrylates.
22. The affinity particle according to claim 11 or 12, wherein the ligand is an antibody or an antigen.
23. A reagent for detecting a target substance in a sample by in vitro diagnosis, characterized in that: The reagent comprises the affinity particle according to any one of claims 1 to 22.
24. A kit for detecting a target substance in a sample by in vitro diagnosis, characterized in that: The kit comprises at least the reagent according to claim 23.