A diatom ceramic-based composite material and its preparation method and application

Through the combination of diatom ceramic matrix composite materials and nano-titanium dioxide, the problems of high cost of adsorbent materials and insufficient adsorption capacity in industrial dye wastewater treatment are solved, and efficient and low-cost dye removal effects are achieved.

CN114534778BInactive Publication Date: 2024-10-11江阴金属材料创新研究院有限公司 +1
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202210198249.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-03-02
Publication Date
2024-10-11
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

It is difficult to effectively treat industrial dye wastewater with existing technology, especially due to the high cost of adsorbent materials, complex preparation processes and insufficient adsorption capacity, which limits industrial application.

Method used

Using diatom ceramic matrix composite materials, diatomaceous earth, mullite, molecular sieves, binders and lubricants are used as carriers to load active components, forming a material with high porous structure and selective adsorption capacity, and combined with nano titanium dioxide Compound to improve visible light catalytic performance.

Benefits of technology

It achieves efficient removal of industrial dyes, with an adsorption capacity of more than 256 mg/g and a removal rate of more than 95%. It has high thermal and chemical stability, low cost, and is suitable for industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003528047730000161
    Figure BDA0003528047730000161
Patent Text Reader

Abstract

The invention provides a diatom ceramic-based composite material and a preparation method and application thereof. The composite material comprises a diatom ceramic carrier and an active component; the active component is loaded on the surface of the diatom ceramic carrier; the raw materials of the diatom ceramic carrier comprise, by mass fraction, 40wt%-80wt% of diatomite, 10wt%-30wt% of mullite powder, 8wt%-22wt% of molecular sieve, 1wt%-3wt% of binder and 1wt%-5wt% of lubricant; the composite material adopts diatomite, mullite, molecular sieve, binder and lubricant as carrier raw materials, the active component is loaded on the surface of the composite material, the richness of the pore structure is improved, and the composite material has selective adsorption and flocculation effects on dye molecules in wastewater, thereby improving the dye removal rate; in addition, the preparation method has a simple process, low cost and good industrial application prospect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of environmentally friendly catalyst materials, and specifically relates to a diatom ceramic-based composite material and a preparation method and application thereof. Background Art

[0002] With the rapid development of my country's industry, dye wastewater generated by printing and dyeing, medicine, chemical industry and other industries has become one of the main sources of environmental pollution. Dye wastewater has complex components and is difficult to biodegrade. Discharging it directly into water bodies will pose a great threat to the water ecological balance and the safety of residents' drinking water sources. In particular, dyes such as methyl orange and methylene blue are widely used in industry. These wastewaters are highly toxic and contain carcinogenic, mutagenic and teratogenic substances; they have high chromaticity and inhibit plant photosynthesis in aquatic systems; and they have high COD values ​​and can lead to eutrophication of water bodies. Based on the above hazards, higher requirements are put forward on how to safely, greenly and cheaply treat industrial wastewater.

[0003] Common treatment methods include adsorption, photocatalysis, membrane separation, chemical oxidation, and biological methods. Among them, adsorption and photocatalysis have become research hotspots due to their high treatment efficiency, simple operation, good selectivity, and relatively low investment cost. Adsorption materials and catalysts are important factors that limit the application of adsorption-catalysis. At present, nano-titanium dioxide (TiO2) has the highest catalytic effect among photocatalysts, but it is limited to ultraviolet light, and the utilization rate of sunlight is very low. Studies have reported that nano-TiO2 loaded on porous carriers can change the band gap, red-shift the absorption spectrum of the catalyst, and improve the visible light photocatalytic properties of the catalyst. The commonly used adsorption materials mainly include activated carbon, carbon nanotubes, molecular sieves, chitosan, and metal oxides. Although these adsorption materials show good application potential in the removal of dye wastewater, they all have some common defects, such as secondary pollution, relatively high cost, complex preparation process, lack of raw material resources, and insufficient adsorption capacity, which limit their large-scale application. Therefore, it is of great scientific and practical significance to study low-cost, green, and renewable high-adsorption materials.

[0004] Diatomite is a porous siliceous sedimentary rock formed by the remains of ancient organisms. Its main chemical component is SiO2, and it also contains a small amount of metal oxides and organic matter. Due to its high porosity, light weight, strong adsorption capacity and high chemical stability, it is widely used in filter aids, decolorizers, adsorbent materials, catalyst carriers, etc. The surface of diatomite contains a large number of hydroxyl groups, which can form hydrogen bonds with nitrogen atoms in methylene blue molecules and selectively adsorb such dyes; and the metal oxides in diatomite can easily form flocculants under hydrolysis, and under the combined action of flocculation and adsorption, the fading activity of diatomite on dyes will be further enhanced. Although some patents have been applied for composite materials related to diatomite in recent years, the adsorption effect of these materials on dyes is not ideal.

[0005] CN108358654B discloses a method for preparing high-activity adsorption ceramsite using low-grade diatomite. After hydrothermal treatment with an alcohol solution of soluble metal bicarbonate, the adsorption performance of the ceramsite can be improved. However, the maximum adsorption capacity of the obtained ceramsite for methylene blue is only 4.37 mg / g, which is far below the requirements for industrial dye treatment. In addition, too low an adsorption capacity will also weaken the photocatalytic performance.

[0006] CN113274972A discloses a composite modified diatomite and its preparation method and application. The composite modified diatomite is obtained by compounding diatomite and biopolymerized ferric sulfate. The removal rate of dyes is as high as 98.6%, but the adsorption amount is only 0.197 mg / g, indicating that this composite material is only suitable for treating wastewater with low concentration of dyes.

[0007] CN106512701A discloses a composite diatomite air purifier, which is made of the following components: 20-50 parts of adsorbent, 15-25 parts of activator, 30-40 parts of strong oxidant, 10-18 parts of adhesive, 1-3 parts of nanoparticle powder and 10-20 parts of deionized water. The composite material is used to adsorb harmful substances such as formaldehyde and benzene in the air, but is not suitable for adsorption and purification of wastewater.

[0008] CN106582513A discloses a composite adsorption material for heavy metal wastewater treatment and a preparation method thereof, wherein the composite adsorption material for heavy metal wastewater treatment is composed of the following raw materials in parts by weight: 20-30 parts of diatomaceous earth, 15-25 parts of shell powder, 10-20 parts of zeolite powder, 20-40 parts of mesoporous molecular sieve, 40-60 parts of ethylenediaminetetraacetic acid metal sodium salt, 70-80 parts of zinc chloride, and 30-50 parts of magnesium chloride. A variety of metal oxides are added to the composite material, which is costly and prone to secondary pollution.

[0009] In summary, the development of a porous adsorption material with high adsorption capacity, long service life and low comprehensive cost is of great significance for the treatment of industrial dye wastewater. Summary of the invention

[0010] In view of the problems existing in the prior art, the purpose of the present invention is to provide a diatom ceramic-based composite material and a preparation method and application thereof. The composite material uses diatomaceous earth, mullite, molecular sieve, binder and lubricant as carrier raw materials, and its surface is loaded with active components, which improves its pore structure richness while enabling it to selectively adsorb and flocculate dye molecules in wastewater, thereby improving the dye removal rate; in addition, the preparation method has a simple process, low cost, and good industrial application prospects.

[0011] To achieve this object, the present invention adopts the following technical solutions:

[0012] In a first aspect, the present invention provides a diatom ceramic-based composite material, the composite material comprising a diatom ceramic carrier and an active component; the active component is loaded on the surface of the diatom ceramic carrier;

[0013] The raw materials of the diatom ceramic carrier include, by mass ratio, 40wt% to 80wt% of diatomaceous earth, for example, 40wt%, 50wt%, 60wt%, 70wt% or 80wt%, etc.; 10wt% to 30wt% of mullite powder, for example, 10wt%, 15wt%, 20wt%, 25wt% or 30wt%, etc.; 8wt% to 22wt% of molecular sieve, for example, 8wt%, 10wt%, 14wt%, 18wt% or 22wt%, etc.; 1wt% to 3wt% of binder and 1wt% to 5wt% of lubricant, for example, 1wt%, 2wt%, 3wt%, 14wt% or 5wt%, etc. The selection of the above numerical values ​​is not limited to the listed numerical values, and other unlisted numerical values ​​within the numerical range are also applicable.

[0014] The present invention adopts diatomite, mullite, molecular sieve, binder and lubricant as carrier raw materials, and forms the composite material by loading active components. The obtained composite material has rich pore structure, has selective adsorption effect on organic dye molecules, and has high catalytic performance under visible light and high removal efficiency. In addition, the diatom ceramic carrier has high porosity, large contact area, fast adsorption rate, high thermal stability and chemical stability, high compressive strength, high recycling rate, and is conducive to industrial production.

[0015] In the present invention, in order to ensure the quality of the composite material obtained, its composition content needs to be controlled. If the diatomite content is too high, the ceramic strength will be reduced; if the diatomite content is too low, the adsorption amount of the product will drop sharply. If the molecular sieve content is too high, the ceramic strength will be reduced; if the molecular sieve content is too low, the ceramic strength will also be reduced.

[0016] The following are preferred technical solutions of the present invention, but are not intended to be limitations of the technical solutions provided by the present invention. Through the following technical solutions, the technical objectives and beneficial effects of the present invention can be better achieved and realized.

[0017] As a preferred technical solution of the present invention, the active component includes nano titanium dioxide.

[0018] Preferably, the crystal form of the nano titanium dioxide includes rutile or anatase.

[0019] As a preferred technical solution of the present invention, the mesh number of the mullite powder includes any one of 200 mesh, 500 mesh, 800 mesh or 1000 mesh or a combination of at least two of them. Typical but non-limiting examples of the combination include: a combination of 200 mesh and 500 mesh, a combination of 200 mesh and 800 mesh, a combination of 500 mesh, 800 mesh and 1000 mesh, etc.

[0020] As a preferred technical solution of the present invention, the molecular sieve includes any one of 4A molecular sieve, 5A molecular sieve or 13X molecular sieve, or a combination of at least two of them. Typical but non-limiting examples of the combination include: a combination of 4A molecular sieve and 5A molecular sieve, a combination of 5A molecular sieve and 13X molecular sieve, a combination of 4A molecular sieve, 5A molecular sieve and 13X molecular sieve, etc.

[0021] As a preferred technical solution of the present invention, the binder includes any one of starch, water-based polyurethane, polyvinyl alcohol or dextrin, or a combination of at least two of them. Typical but non-limiting examples of the combination include: a combination of starch and water-based polyurethane, a combination of starch and dextrin, a combination of water-based polyurethane and polyvinyl alcohol, etc.

[0022] As a preferred technical solution of the present invention, the lubricant includes any one of oleic acid, silicone oil or paraffin, or a combination of at least two of them. Typical but non-limiting examples of the combination include: a combination of oleic acid and silicone oil, a combination of silicone oil and paraffin, a combination of oleic acid and paraffin, etc.

[0023] In a second aspect, this statement further provides a method for preparing the diatom ceramic-based composite material as described in the first aspect, the preparation method comprising the following steps:

[0024] (1) diatomaceous earth, mullite powder, molecular sieve, binder, lubricant and water are mixed in proportion to obtain a wet material;

[0025] Dispersing the active components to obtain a dispersion;

[0026] (2) subjecting the wet material obtained in step (1) to aging and vacuum refining to obtain a clay blank;

[0027] (3) molding, drying and sintering the clay obtained in step (2) to obtain a diatom ceramic carrier;

[0028] (4) The diatom ceramic carrier obtained in step (3) is impregnated into the dispersion liquid described in step (1), and then dried and sintered in sequence to obtain a diatom ceramic-based composite material.

[0029] In the present invention, the preparation method sequentially prepares the diatom ceramic-based composite material through mixing, kneading, molding, drying, sintering and loading, has a simple production process, low cost, and has a strong value for application and promotion of dye treatment.

[0030] As a preferred technical solution of the present invention, the mixing temperature in step (1) is 30-70°C, for example, 30°C, 40°C, 50°C, 60°C or 70°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0031] Preferably, the mixing time in step (1) is 1 to 3 hours, such as 1 hour, 1.5 hours, 2 hours, 2.5 hours or 3 hours, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0032] Preferably, the ratio of the water to the sum of the mass of diatomaceous earth, mullite powder, molecular sieve, binder and lubricant in step (1) is (0.2-0.6):1, for example, 0.2:1, 0.3:1, 0.4:1, 0.5:1 or 0.6:1, etc., but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0033] Preferably, in the dispersion of step (1), the mass fraction of the active component is 0.5wt% to 5wt%, for example, 0.5wt%, 1wt%, 2wt%, 3wt%, 4wt% or 5wt%, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0034] Preferably, the vacuum pressure of the vacuum mud refining in step (2) is -0.25 to -0.06 MPa, for example, -0.25 MPa, -0.20 MPa, -0.16 MPa, -0.12 MPa, -0.10 MPa, -0.08 MPa or -0.06 MPa, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0035] Preferably, the vacuum sludge refining time in step (2) is 1 to 3 hours, for example, 1 hour, 1.5 hours, 2 hours, 2.5 hours or 3 hours, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0036] Preferably, the dry material rate of the clay in step (2) is 50% to 80%, for example 50%, 55%, 60%, 65%, 70%, 75% or 80%, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0037] The dry material rate of the clay blank in the preparation process of the present invention has a certain influence on the final product. If the material rate is too low, the ceramic strength will be reduced, the pores will be larger, and the adsorption capacity will be reduced; if the material rate is too high, the ceramic porosity will be reduced.

[0038] Preferably, the molding in step (3) is carried out in a vacuum extruder.

[0039] Preferably, the molding temperature in step (3) is 10-50°C, for example, 10°C, 20°C, 30°C, 40°C or 50°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0040] In the present invention, the molding temperature should not be too high, otherwise it will cause the water in the ceramic body to evaporate too quickly and break.

[0041] Preferably, the vacuum pressure of the molding in step (3) is -0.25 to -0.06 MPa, for example, -0.25 MPa, -0.20 MPa, -0.16 MPa, -0.12 MPa, -0.10 MPa, -0.08 MPa or -0.06 MPa, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0042] Preferably, the drying temperature in step (3) is 80-150°C, for example 80°C, 90°C, 100°C, 110°C, 120°C, 130°C, 140°C or 150°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0043] Preferably, the drying time in step (3) is 12 to 36 hours, for example, 12 hours, 16 hours, 20 hours, 24 hours, 28 hours, 32 hours or 36 hours, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0044] Preferably, the sintering temperature in step (3) is 600-1200°C, for example 600°C, 700°C, 800°C, 900°C, 1000°C, 1100°C or 200°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0045] Preferably, the sintering time in step (3) is 2 to 6 hours, for example 2 hours, 3 hours, 4 hours, 5 hours or 6 hours, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0046] Preferably, the morphology of the diatom ceramic carrier in step (3) includes any one of columnar, tubular or honeycomb shapes, or a combination of at least two of them. Typical but non-limiting examples of the combination include: a combination of columnar and tubular shapes, a combination of columnar and honeycomb shapes, a combination of tubular and honeycomb shapes, etc.

[0047] As a preferred technical solution of the present invention, the immersion time in step (4) is 4 to 12 hours, for example 4 hours, 6 hours, 8 hours, 10 hours or 12 hours, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0048] Preferably, the drying temperature in step (4) is 100-200°C, for example, 100°C, 120°C, 140°C, 160°C, 180°C or 200°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0049] Preferably, the drying time in step (4) is 12 to 36 hours, for example, 12 hours, 16 hours, 20 hours, 24 hours, 28 hours, 32 hours or 36 hours, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0050] Preferably, the sintering temperature in step (4) is 400-800°C, for example 400°C, 500°C, 600°C, 700°C or 800°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0051] Preferably, the sintering time in step (4) is 2 to 6 hours, for example 2 hours, 3 hours, 4 hours, 5 hours or 6 hours, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0052] In a third aspect, the present invention further provides an application of the diatom ceramic-based composite material as described in the first aspect, wherein the diatom ceramic-based composite material is used for treating organic dyes in industrial wastewater.

[0053] Compared with the prior art, the present invention has the following beneficial effects:

[0054] (1) The diatom ceramic carrier of the present invention has a rich pore structure, a porosity of ≥50%, a large number of hydroxyl groups and a small amount of metal oxides, and has a selective adsorption and flocculation effect on dye molecules in wastewater, with high adsorption and removal efficiency. The adsorption amount of methylene blue by the obtained diatom ceramic carrier is ≥256 mg·g -1 ;

[0055] (2) The diatom ceramic carrier of the present invention is porous and three-dimensional, has a large contact area with the organic dye, a fast adsorption rate, and has high thermal and chemical stability, high compressive strength, and high recycling rate;

[0056] (3) The composite material of the present invention, which combines the diatom ceramic carrier with nano-TiO2, can solve the shortcoming that TiO2 can only absorb ultraviolet light, and still has high catalytic performance under visible light, with a dye removal rate of ≥95%;

[0057] (4) The preparation method of the diatom ceramic-based composite material of the present invention has a simple production process, low raw material cost, and great application and promotion value in industrial wastewater treatment. DETAILED DESCRIPTION

[0058] In order to better illustrate the present invention and facilitate understanding of the technical solution of the present invention, the present invention is further described in detail below. However, the following embodiments are only simple examples of the present invention and do not represent or limit the scope of protection of the present invention. The scope of protection of the present invention shall be subject to the claims.

[0059] The following are typical but non-limiting embodiments of the present invention:

[0060] Embodiment 1:

[0061] This embodiment provides a diatom ceramic-based composite material and a preparation method thereof, wherein the composite material comprises a diatom ceramic carrier and rutile nano-titanium dioxide; the rutile nano-titanium dioxide is loaded on the surface of the diatom ceramic carrier;

[0062] The raw materials of the diatom ceramic carrier include, by mass fraction, 60 wt% of diatomite, 30 wt% of 500-mesh mullite powder, 8 wt% of 5A molecular sieve, 1 wt% of starch and 1 wt% of oleic acid.

[0063] The preparation method of the diatom ceramic-based composite material comprises the following steps:

[0064] (1) diatomaceous earth, mullite powder, 5A molecular sieve, starch and oleic acid are mixed with water in proportion and kneaded for 2 hours to obtain a wet material; wherein the ratio of the mass of water to the sum of the mass of diatomaceous earth, mullite powder, 5A molecular sieve, starch and oleic acid is 0.6:1;

[0065] Dispersing rutile nano-titanium dioxide in water to obtain a dispersion, wherein the mass fraction of rutile nano-titanium dioxide in the dispersion is 0.5wt%;

[0066] (2) kneading the wet material in step (1) under vacuum conditions, controlling the vacuum pressure of the kneading to be -0.15 MPa, and kneading time to be 1 h, to obtain a clay blank with a dry material rate of 50%;

[0067] (3) Extruding the clay obtained in step (2) into a honeycomb blank in a vacuum extruder, wherein the vacuum pressure during molding is controlled at -0.25 MPa and the molding temperature is 30° C.; drying the honeycomb blank at 80° C. for 24 h, and then sintering at 900° C. for 6 h to obtain a diatom ceramic carrier;

[0068] (4) The diatom ceramic carrier obtained in step (3) is immersed in the dispersion for 12 hours, then dried at 200° C. for 36 hours, and then sintered at 400° C. for 6 hours to obtain a diatom ceramic-based composite material.

[0069] Embodiment 2:

[0070] This embodiment provides a diatom ceramic-based composite material and a preparation method thereof, wherein the composite material comprises a diatom ceramic carrier and rutile nano-titanium dioxide; the rutile nano-titanium dioxide is loaded on the surface of the diatom ceramic carrier;

[0071] The raw materials of the diatom ceramic carrier include, by mass fraction, 60 wt% of diatomite, 30 wt% of 500-mesh mullite powder, 8 wt% of 5A molecular sieve, 1 wt% of starch and 1 wt% of oleic acid.

[0072] The preparation method of the diatom ceramic-based composite material is similar to the preparation method in Example 1, with the only difference being that the time for mud kneading in step (2) is controlled to be 1 hour to obtain a mud blank with a dry material rate of 60%.

[0073] Embodiment 3:

[0074] This embodiment provides a diatom ceramic-based composite material and a preparation method thereof, wherein the composite material comprises a diatom ceramic carrier and rutile nano-titanium dioxide; the rutile nano-titanium dioxide is loaded on the surface of the diatom ceramic carrier;

[0075] The raw materials of the diatom ceramic carrier include, by mass fraction, 60 wt% of diatomite, 30 wt% of 500-mesh mullite powder, 8 wt% of 5A molecular sieve, 1 wt% of starch and 1 wt% of oleic acid.

[0076] The preparation method of the diatom ceramic-based composite material is similar to the preparation method in Example 1, with the only difference being that the time for mud kneading in step (2) is controlled to be 2.2 hours to obtain a mud blank with a dry material rate of 70%.

[0077] Embodiment 4:

[0078] This embodiment provides a diatom ceramic-based composite material and a preparation method thereof, wherein the composite material comprises a diatom ceramic carrier and rutile nano-titanium dioxide; the rutile nano-titanium dioxide is loaded on the surface of the diatom ceramic carrier;

[0079] The raw materials of the diatom ceramic carrier include, by mass fraction, 60 wt% of diatomite, 30 wt% of 500-mesh mullite powder, 8 wt% of 5A molecular sieve, 1 wt% of starch and 1 wt% of oleic acid.

[0080] The preparation method of the diatom ceramic-based composite material is similar to the preparation method in Example 1, with the only difference being that the time for mud kneading in step (2) is controlled to be 3 hours to obtain a mud blank with a dry material rate of 80%.

[0081] Embodiment 5:

[0082] This embodiment provides a diatom ceramic-based composite material and a preparation method thereof, wherein the composite material comprises a diatom ceramic carrier and rutile nano-titanium dioxide; the rutile nano-titanium dioxide is loaded on the surface of the diatom ceramic carrier;

[0083] The raw materials of the diatom ceramic carrier include, by mass fraction, 60 wt% of diatomite, 30 wt% of 500-mesh mullite powder, 8 wt% of 5A molecular sieve, 1 wt% of starch and 1 wt% of oleic acid.

[0084] The preparation method of the diatom ceramic-based composite material is similar to the preparation method in Example 1, with the only difference being that the time for mud kneading in step (2) is controlled to be 0.3 h, and a mud blank with a dry material rate of 20% is obtained.

[0085] Embodiment 6:

[0086] This embodiment provides a diatom ceramic-based composite material and a preparation method thereof, wherein the composite material comprises a diatom ceramic carrier and rutile nano-titanium dioxide; the rutile nano-titanium dioxide is loaded on the surface of the diatom ceramic carrier;

[0087] The raw materials of the diatom ceramic carrier include, by mass fraction, 60 wt% of diatomite, 30 wt% of 500-mesh mullite powder, 8 wt% of 5A molecular sieve, 1 wt% of starch and 1 wt% of oleic acid.

[0088] The preparation method of the diatom ceramic-based composite material is similar to the preparation method in Example 1, with the only difference being that the time for mud kneading in step (2) is controlled to be 3.8 hours to obtain a mud blank with a dry material rate of 90%.

[0089] Embodiment 7:

[0090] This embodiment provides a diatom ceramic-based composite material and a preparation method thereof, wherein the composite material comprises a diatom ceramic carrier and anatase-type nano-titanium dioxide; the anatase-type nano-titanium dioxide is loaded on the surface of the diatom ceramic carrier;

[0091] The raw materials of the diatom ceramic carrier include, by mass fraction, 40 wt% of diatomite, 30 wt% of 500-mesh mullite powder, 22 wt% of 13X molecular sieve, 3 wt% of dextrin and 5 wt% of silicone oil.

[0092] The preparation method of the diatom ceramic-based composite material comprises the following steps:

[0093] (1) diatomaceous earth, mullite powder, 13X molecular sieve, dextrin and silicone oil are mixed with water in proportion and kneaded for 3 hours to obtain a wet material; wherein the ratio of the mass of water to the sum of the mass of diatomaceous earth, mullite powder, 13X molecular sieve, dextrin and silicone oil is 0.4:1;

[0094] Dispersing anatase nano-titanium dioxide in water to obtain a dispersion, wherein the mass fraction of anatase nano-titanium dioxide in the dispersion is 1 wt %;

[0095] (2) kneading the wet material in step (1) under vacuum conditions, controlling the vacuum pressure of the kneading to be -0.15 MPa, and kneading time to be 1 h, to obtain a clay blank with a dry material rate of 60%;

[0096] (3) Extruding the clay obtained in step (2) into a columnar blank in a vacuum extruder, wherein the vacuum pressure during molding is controlled at -0.25 MPa and the molding temperature is 20° C.; drying the honeycomb blank at 150° C. for 12 h, and then sintering at 600° C. for 2 h to obtain a diatom ceramic carrier;

[0097] (4) The diatom ceramic carrier obtained in step (3) is immersed in the dispersion for 4 hours, then dried at 150° C. for 12 hours, and then sintered at 400° C. for 4 hours to obtain a diatom ceramic-based composite material.

[0098] Embodiment 8:

[0099] This embodiment provides a diatom ceramic-based composite material and a preparation method thereof, wherein the composite material comprises a diatom ceramic carrier and rutile nano-titanium dioxide; the rutile nano-titanium dioxide is loaded on the surface of the diatom ceramic carrier;

[0100] The raw materials of the diatom ceramic carrier include, by mass fraction, 80 wt% of diatomite, 10 wt% of 500-mesh mullite powder, 8 wt% of 13X molecular sieve, 1 wt% of polyvinyl alcohol and 1 wt% of paraffin.

[0101] The preparation method of the diatom ceramic-based composite material comprises the following steps:

[0102] (1) diatomaceous earth, mullite powder, 13X molecular sieve, polyvinyl alcohol and paraffin are mixed with water in proportion and kneaded for 3 hours to obtain a wet material; wherein the ratio of the mass of water to the sum of the mass of diatomaceous earth, mullite powder, 13X molecular sieve, polyvinyl alcohol and paraffin is 0.3:1;

[0103] Dispersing rutile nano-titanium dioxide in water to obtain a dispersion, wherein the mass fraction of rutile nano-titanium dioxide in the dispersion is 1 wt %;

[0104] (2) kneading the wet material in step (1) under vacuum conditions, controlling the vacuum pressure of the kneading to be -0.15 MPa, and kneading time to be 1 h, to obtain a clay blank with a dry material rate of 70%;

[0105] (3) Extruding the clay obtained in step (2) into a tubular green billet in a vacuum extruder, wherein the vacuum pressure during molding is controlled at -0.25 MPa and the molding temperature is 50° C.; drying the honeycomb green billet at 150° C. for 12 h, and then sintering at 1200° C. for 4 h to obtain a diatom ceramic carrier;

[0106] (4) The diatom ceramic carrier obtained in step (3) is immersed in the dispersion for 12 hours, then dried at 200° C. for 36 hours, and then sintered at 600° C. for 2 hours to obtain a diatom ceramic-based composite material.

[0107] Embodiment 9:

[0108] This embodiment provides a diatom ceramic-based composite material and a preparation method thereof, wherein the composite material comprises a diatom ceramic carrier and rutile nano-titanium dioxide; the rutile nano-titanium dioxide is loaded on the surface of the diatom ceramic carrier;

[0109] The raw materials of the diatom ceramic carrier include, by mass fraction, 60 wt% of diatomite, 30 wt% of 500-mesh mullite powder, 8 wt% of 5A molecular sieve, 1 wt% of starch and 1 wt% of oleic acid.

[0110] The preparation method of the diatom ceramic-based composite material is similar to the preparation method in Example 1, with the only difference being that the molding temperature in step (3) is 60°C.

[0111] Comparative Example 1:

[0112] This comparative example provides a diatom ceramic-based composite material and a preparation method thereof. The composite material refers to the composite material in Example 7, except that:

[0113] The raw materials of the diatom ceramic carrier include 30wt% diatomite by mass fraction, and the reduced part is added to other components in proportion to ensure that 100wt% is met, namely, 30wt% diatomite, 35wt% 500-mesh mullite powder, 25.7wt% 13X molecular sieve, 3.5wt% dextrin and 5.8wt% silicone oil.

[0114] The preparation method of the diatom ceramic-based composite material is similar to the preparation method in Example 7, except that the raw materials for preparing the diatom ceramic carrier in step (1) are mixed according to the contents of this comparative example.

[0115] Comparative Example 2:

[0116] This comparative example provides a diatom ceramic-based composite material and a preparation method thereof. The composite material refers to the composite material in Example 8, except that:

[0117] The raw materials of the diatom ceramic carrier include 90wt% diatomite by mass fraction, and the increased part is obtained by reducing other components in proportion to ensure that 100wt% is met, that is, it includes 90wt% diatomite, 5wt% 500-mesh mullite powder, 4wt% 13X molecular sieve, 0.5wt% polyvinyl alcohol and 0.5wt% paraffin.

[0118] The preparation method of the diatom ceramic-based composite material is similar to the preparation method in Example 8, except that the raw materials for preparing the diatom ceramic carrier in step (1) are mixed according to the contents of this comparative example.

[0119] Comparative Example 3:

[0120] This comparative example provides a diatom ceramic-based composite material and a preparation method thereof. The composite material refers to the composite material in Example 7, except that:

[0121] The raw materials of the diatom ceramic carrier include 28wt% of 13X molecular sieve by mass fraction, and the increased part is obtained by reducing other components in proportion to ensure that 100wt% is met, that is, it includes 36.9wt% of diatomaceous earth, 27.7wt% of 500-mesh mullite powder, 28wt% of 13X molecular sieve, 2.8wt% of dextrin and 4.6wt% of silicone oil.

[0122] The preparation method of the diatom ceramic-based composite material is similar to the preparation method in Example 7, except that the raw materials for preparing the diatom ceramic carrier in step (1) are mixed according to the contents of this comparative example.

[0123] Comparative Example 4:

[0124] This comparative example provides a diatom ceramic-based composite material and a preparation method thereof. The composite material refers to the composite material in Example 8, except that:

[0125] The raw materials of the diatom ceramic carrier are calculated by mass fraction, 4wt% of 13X molecular sieve, and the reduced part is proportionally added to other ingredients to ensure that 100wt% is met, namely, 83.5wt% of diatomaceous earth, 10.4wt% of 500-mesh mullite powder, 4wt% of 13X molecular sieve, 1.05wt% of polyvinyl alcohol and 1.05wt% of paraffin.

[0126] The preparation method of the diatom ceramic-based composite material is similar to the preparation method in Example 8, except that the raw materials for preparing the diatom ceramic carrier in step (1) are mixed according to the contents of this comparative example.

[0127] Comparative Example 5:

[0128] This comparative example provides a diatom ceramic-based composite material and a preparation method thereof, the preparation method comprising the following steps:

[0129] (1) dispersing rutile nano-titanium dioxide in water to obtain a dispersion, wherein the mass fraction of rutile nano-titanium dioxide in the dispersion is 0.5 wt %;

[0130] 60wt% of diatomaceous earth, 30wt% of 500-mesh mullite powder, 8wt% of 5A molecular sieve, 1wt% of starch and 1wt% of oleic acid were mixed with the dispersion and kneaded for 2h to obtain a wet material; wherein the ratio of the mass of the dispersion to the sum of the mass of the diatomaceous earth, mullite powder, 5A molecular sieve, starch and oleic acid was 0.6:1;

[0131] (2) kneading the wet material in step (1) under vacuum conditions, controlling the vacuum pressure of the kneading to be -0.15 MPa, and kneading time to be 1 h, to obtain a clay blank with a dry material rate of 50%;

[0132] (3) Extruding the clay obtained in step (2) into a honeycomb blank in a vacuum extruder, wherein the vacuum pressure during molding is controlled at -0.25 MPa and the molding temperature is 30° C.; drying the honeycomb blank at 80° C. for 24 h, and then sintering it at 900° C. for 6 h to obtain a diatom ceramic-based composite material.

[0133] The porosity and static saturated adsorption capacity of the diatom ceramic-based composite materials obtained in the above Examples 1-9 and Comparative Examples 1-5 were tested, and the testing method was as follows:

[0134] Porosity: measured by the boiling method disclosed in the national standard GB / T 1966-1996 "Test method for apparent porosity and bulk density of porous ceramics";

[0135] Saturated adsorption capacity: measured according to the method disclosed in the national standard GB / T 12496.10-1999 "Test method for wood activated carbon - Determination of methylene blue adsorption value";

[0136] Photocatalytic performance test of dye wastewater: first prepare a methylene blue dye solution with a concentration of 200 mg / L for storage. Weigh 1g of diatom ceramic-based composite material and place it in the prepared 1L dye solution, control the speed to 300r / min for stirring, the temperature is 20℃, pH=6, and place it in a dark environment and a visible light environment for irradiation. After a period of reaction time, take a sample and use an ultraviolet spectrophotometer to measure the absorbance at the maximum absorption wavelength = 664nm, and calculate the dye removal rate. All test results are shown in Table 1.

[0137] Table 1

[0138]

[0139] The diatom ceramic-based composite materials prepared by the preparation method of the present invention in Examples 1-4 and 7-8 have a pore structure of windproof clothing, a porosity of more than 50%, and selective adsorption and flocculation of dye molecules in wastewater, and an adsorption rate of methylene blue of 256 mg·g -1 As shown above, under visible light environment, the dye removal rate can reach more than 95%; in Example 5, the dry material rate of the clay blank is too low during the preparation process, resulting in too large pores in the ceramic carrier, which cannot selectively adsorb the dye; in Example 6, the dry material rate of the clay blank is too high during the preparation process, which affects the porosity, and the porosity decreases, and the adsorption amount also decreases. In Example 9, the molding temperature is too high, resulting in too fast evaporation of water in the ceramic blank, resulting in fracture, so even if subsequent operations are performed, a good dye removal effect cannot be achieved.

[0140] In Comparative Example 1, too little diatomaceous earth was added, resulting in fewer effective pores, thereby reducing the fuel removal rate; in Comparative Example 2, too much diatomaceous earth was added, the ceramic strength was low and could not be formed, so even if subsequent operations were performed, a good dye removal effect could not be achieved; in Comparative Example 3, too much molecular sieve was added, and the strength of the ceramic would decrease; in Comparative Example 4, too little molecular sieve was added, and the effective ingredients for adsorbing dyes were reduced, resulting in a decrease in the dye removal rate; in Comparative Example 5, the active component and the carrier raw material were mixed and prepared simultaneously, resulting in the active component not being evenly and massively loaded on the carrier surface, affecting the contact area between the active component and the dye, resulting in a greatly reduced removal rate.

[0141] Based on the above embodiments and comparative examples, it can be seen that, in the first aspect, the diatom ceramic carrier of the present invention has a rich pore structure, a porosity of ≥50%, a large number of hydroxyl groups and a small amount of metal oxides, and has selective adsorption and flocculation effects on dye molecules in wastewater, and has high adsorption and removal efficiency. The adsorption amount of methylene blue by the obtained diatom ceramic carrier is ≥256 mg·g -1 ; Secondly, the diatom ceramic carrier is porous and three-dimensional, with a large contact area with the organic dye, a fast adsorption rate, high thermal stability and chemical stability, high compressive strength, and high recycling rate; Thirdly, the composite material, which combines the diatom ceramic carrier with nano-TiO2, can solve the shortcoming that TiO2 can only absorb ultraviolet light, and still has high catalytic performance under visible light, with a dye removal rate of ≥95%; Fourthly, the preparation method of the diatom ceramic-based composite material has a simple production process, low raw material cost, and great value for application and promotion of industrial wastewater treatment.

[0142] The applicant declares that the present invention illustrates the products and detailed methods of the present invention through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned products and detailed methods, that is, it does not mean that the present invention must rely on the above-mentioned products and detailed methods to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of the operation of the present invention, addition of auxiliary operations, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

Claims

1. Application of a diatom ceramic-based composite material in treating methylene blue in industrial wastewater, characterized in that: The composite material comprises a diatom ceramic carrier and an active component; the active component is loaded on the surface of the diatom ceramic carrier; The raw materials of the diatom ceramic carrier are composed of 40wt% to 80wt% of diatomite, 10wt% to 30wt% of mullite powder, 8wt% to 22wt% of molecular sieve, 1wt% to 3wt% of binder and 1wt% to 5wt% of lubricant, calculated by mass fraction; The active component is nano titanium dioxide; The crystal form of the nano titanium dioxide is rutile or anatase; The lubricant is oleic acid and / or silicone oil; The molecular sieve includes any one of 4A molecular sieve, 5A molecular sieve or 13X molecular sieve or a combination of at least two thereof; The diatom ceramic-based composite material is prepared by the following method, which comprises the following steps: (1) diatomaceous earth, mullite powder, molecular sieve, binder, lubricant and water are mixed in proportion to obtain a wet material; Dispersing the active components to obtain a dispersion; (2) subjecting the wet material obtained in step (1) to aging and vacuum refining to obtain a clay blank; (3) molding, drying and sintering the clay obtained in step (2) to obtain a diatom ceramic carrier; (4) impregnating the diatom ceramic carrier obtained in step (3) into the dispersion liquid described in step (1), and then drying and sintering in sequence to obtain a diatom ceramic-based composite material; The ratio of the water to the sum of the mass of diatomaceous earth, mullite powder, molecular sieve, binder and lubricant in step (1) is (0.2-0.6):1; The vacuum sludge refining time in step (2) is 1 to 3 hours; The dry material rate of the clay blank in step (2) is 70% to 80%; The molding temperature in step (3) is 10 to 50° C. The adsorption capacity of methylene blue by the diatom ceramic carrier is ≥256 mg·g -1 .

2. The use according to claim 1, characterized in that: The mesh size of the mullite powder includes any one of 200 mesh, 500 mesh, 800 mesh or 1000 mesh, or a combination of at least two of them.

3. The use according to claim 1, characterized in that: The binder includes any one of starch, waterborne polyurethane, polyvinyl alcohol or dextrin, or a combination of at least two of them.

4. The use according to claim 1, characterized in that: The mixing temperature in step (1) is 30-70°C.

5. The use according to claim 1, characterized in that: The mixing time in step (1) is 1 to 3 hours.

6. The use according to claim 1, characterized in that: In the dispersion of step (1), the mass fraction of the active component is 0.5wt% to 5wt%.

7. The use according to claim 1, characterized in that: The vacuum pressure of the vacuum mud refining in step (2) is -0.25 to -0.06 MPa.

8. The use according to claim 1, characterized in that: The molding in step (3) is carried out in a vacuum extruder.

9. The use according to claim 1, characterized in that: The vacuum pressure of the molding in step (3) is -0.25 to -0.06 MPa.

10. The use according to claim 1, characterized in that: The drying temperature in step (3) is 80-150°C.

11. The use according to claim 1, characterized in that: The drying time in step (3) is 12 to 36 hours.

12. The use according to claim 1, characterized in that: The sintering temperature in step (3) is 600-1200°C.

13. The use according to claim 1, characterized in that: The sintering time in step (3) is 2 to 6 hours.

14. The use according to claim 1, characterized in that: The shape of the diatom ceramic carrier in step (3) includes any one of columnar, tubular or honeycomb shapes or a combination of at least two of them.

15. The use according to claim 1, characterized in that: The immersion time in step (4) is 4 to 12 hours.

16. The use according to claim 1, characterized in that: The drying temperature in step (4) is 100-200°C.

17. The use according to claim 1, characterized in that: The drying time in step (4) is 12 to 36 hours.

18. The use according to claim 1, characterized in that: The sintering temperature in step (4) is 400-800°C.

19. The use according to claim 1, characterized in that: The sintering time in step (4) is 2 to 6 hours.

Citation Information

Patent Citations

  • Compound kieselguhr air cleaning agent and preparation method thereof

    CN106512701A

  • Composite adsorption material for treatment of heavy metal wastewater and preparation method thereof

    CN106582513A

  • A method for preparing highly active adsorbent ceramsite using low-grade diatomaceous earth

    CN108358654B

  • Composite modified diatomite as well as preparation method and application thereof

    CN113274972A

  • Kieselguhr-based porous ceramics and method for loading Ag doped with nano TiO2 on same

    CN101891497A