A low-cost wet processing method for semiconductor photocathode of third-generation image intensifier
Through the combined use of step-by-step etching solution and ultrasonic cleaning machine, the problems of unclean substrate corrosion, poor barrier layer effect and particle problems during the treatment of gallium arsenide photocathode are solved, achieving more efficient surface cleaning and improving imaging quality. .
Patent Information
- Application Number
- CN202210185469.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-02-28
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2042-02-28
AI Technical Summary
During the processing of gallium arsenide photocathode, there are unclean substrate corrosion, residues, poor barrier layer effect, white fog phenomenon and particle problems, which affect the imaging quality and activation sensitivity.
The low-cost third-generation image intensifier semiconductor photocathode wet processing method is used, and the substrate corrosion height is measured with a micrometer. Step-by-step etching liquid and ultrasonic cleaning machine are used to control the corrosion rate and cleaning effect to ensure that the surface is clean and without residue, and through adjustment The chemical reagent ratio and stirring method improve corrosion uniformity and particle removal efficiency.
It solves the problems of substrate residue, uneven barrier layer, white fog phenomenon and particles, improves the cleanliness and imaging quality of the cathode surface, and enhances the electron diffusion length and cathode activation sensitivity.
Smart Images

Figure CN114551189B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of gallium arsenide photocathode preparation methods, and in particular to a low-cost third-generation image intensifier semiconductor photocathode wet processing method. Background Art
[0002] The core component of low-light-level night vision devices is the image intensifier, or image tube for short. Currently, the best practical one is the third-generation image tube. One of its most important features is that it uses the second-generation semiconductor gallium arsenide as the emission layer of the photocathode. Gallium arsenide has the characteristics of high sensitivity, wide light response range, and high electron mobility. It is particularly suitable for making gallium arsenide photocathode electron sources. Gallium arsenide photocathode electron sources mainly include photon absorption, electron transition, electron diffusion, and electron escape. Gallium arsenide photocathode absorbs light of a certain wavelength, such as infrared and ultraviolet light, so that the electrons in the conduction band of gallium arsenide semiconductors obtain the energy of photons. Secondly, due to the large energy, the vibrating electrons break through the constraints of gallium arsenide atoms and become free electrons, which diffuse to the crystal surface in the body. Finally, the electrons escape from the surface of the P-type gallium arsenide photocathode to make a gallium arsenide photocathode electron source. This electron source can realize the conversion of optical signals into electronic signals and is widely used in low-light-level night vision systems.
[0003] During the processing of GaAs epitaxial wafers, there are problems such as unclean substrate corrosion and residue, which leads to unclean and rough surface of the negative side.
[0004] The corrosion depth on the surface of the GaAs photocathode blocking layer is inconsistent, the blocking effect is poor, and the corrosion effect of the subsequent emission layer is affected. There is a white fog phenomenon on the surface of the emission layer, which reduces the surface quality and cathode activation sensitivity.
[0005] During the cleaning process of the GaAs photocathode surface, there are through holes and a large number of particles, which affect the cathode imaging quality. Summary of the invention
[0006] The purpose of the present invention is to provide a low-cost third-generation image intensifier semiconductor photocathode wet processing method, by bonding the gallium arsenide photocathode to the surface of optical glass, thereby achieving a vacuum sealing effect, reducing the potential energy of the gallium arsenide surface, allowing electrons to escape from the gallium arsenide surface and become free electrons, and increasing the diffusion length of electrons.
[0007] In order to achieve the above object, the present invention adopts the following technical solutions:
[0008] A low-cost third-generation image intensifier semiconductor photocathode wet processing method, S1, using a micrometer to measure the height h1 of the cathode assembly substrate before corrosion, and quantitatively judging the end time of substrate corrosion through the height change difference;
[0009] S2. Use an ultrasonic cleaning machine at a frequency of 40KHz to degrease and clean the gallium arsenide cathode assembly with K9 glass as the window glass using isopropyl alcohol and deionized water respectively;
[0010] S3. Store the cleaned cathode assembly in deionized water at a temperature of 25±1°C for no more than 30 minutes;
[0011] S4. The cathode component substrate is etched in a step-by-step manner, with the principle of fast first and slow later. First, ammonia: hydrogen peroxide: water = 1:10:10~1:10:20 volume ratio etching solution is used, and then ammonia + hydrogen peroxide etching solution is used to achieve the purpose of uniform corrosion of the cathode component substrate, clean surface, and no residue;
[0012] S5. The cathode assembly substrate etching solution 1 is prepared according to the volume ratio of ammonia water: hydrogen peroxide: water = 1:10:10~1:10:20, and the temperature of the substrate etching solution 1 is controlled at 25±1℃;
[0013] S6, cathode assembly 1 substrate corrosion;
[0014] S7, after etching the cathode assembly once with substrate etching solution 1, take out the cathode assembly, rinse it with deionized water for 30 seconds, and blow dry the surface moisture with nitrogen;
[0015] S8. After the cathode assembly is qualified for the first substrate corrosion, take out the cathode assembly, rinse it with deionized water for 30 seconds, and store it in deionized water for no more than 30 minutes;
[0016] S9, cathode assembly substrate etching solution 2 is prepared according to the volume ratio of ammonia water: hydrogen peroxide = 1:10~1:20;
[0017] S10, cathode assembly secondary substrate corrosion;
[0018] S11, after the cathode assembly is etched twice with substrate etching solution 2, the substrate is evenly and completely etched to the barrier layer. At this time, the cathode assembly surface is black, which is qualified; if it does not turn black, return to the previous step and continue etching;
[0019] S12. After the cathode assembly is etched twice, take out the cathode assembly, rinse it with deionized water for 30 seconds, and store it in deionized water for no more than 30 minutes.
[0020] S13, cathode component barrier layer corrosion solution preparation: potassium hydroxide + hydrogen peroxide + water = 0.02 ~ 0.06 mol + 10 ~ 20 ml + 300 ml;
[0021] S14, cathode assembly barrier layer corrosion: using barrier layer corrosion liquid to corrode the cathode assembly barrier layer;
[0022] S15. After the cathode assembly barrier layer is corroded, the cathode assembly is taken out and rinsed with deionized water for 30 seconds. Then, it is placed in a 200 ml culture dish and 150 ml of deionized water is poured into it. A megasonic cleaning machine is used with a frequency of 1000 KHz to remove particles smaller than 0.2 µm. The cleaning time is 2 minutes.
[0023] S16, cathode component emission layer etching solution preparation: potassium hydroxide + hydrogen peroxide + water = 0.02 ~ 0.06mol + 10 ~ 20ml + 600ml, use a bubbler to stir, at the same time, the temperature of the etching solution is controlled at 25 ± 1 ° C;
[0024] S17, cathode assembly emission layer corrosion: the emission layer of the cathode assembly is corroded by using an emission layer corrosion liquid;
[0025] S18. After the cathode assembly emitter layer is corroded, take out the cathode assembly, rinse it with deionized water for 30 seconds, and then place it in a 200 ml culture dish and pour 150 ml of deionized water;
[0026] S19. The cathode component rinsing liquid is prepared according to the volume ratio of hydrochloric acid: isopropanol = 1:10~1:20 to remove metal impurities adsorbed on the surface of the cathode component. Magnetic stirring is used and the rinsing liquid temperature is controlled at 25±1℃;
[0027] S20, cathode assembly rinsing: using an emission layer rinsing liquid to rinse the emission layer of the cathode assembly, stirring with a magnetic stirrer at a stirring rate of 500 rpm;
[0028] S21. After the cathode assembly is rinsed, high-purity isopropanol is used to rinse the rinsed cathode assembly for 30 seconds, then it is blown dry with nitrogen and transferred to a vacuum box for storage.
[0029] Furthermore, the cathode assembly substrate was etched once using substrate etching solution 1, stirred by magnetic stirring heating, with a stirring rate of 500 rpm, and the working temperature of the etching solution was controlled at 28-32°C for rapid etching, and the substrate etching rate was controlled at 5-10 µm / min, with a etching time of 40±5 min, thereby obtaining a clean, bright, and uniform surface.
[0030] Furthermore, the height h2 of the cathode assembly is measured at this time. When (h1-h2) / h1=0.04~0.06 is satisfied, it is clean and has no residue, and the next step is carried out. When (h1-h2) / h1<0.04 is satisfied, the cathode assembly is subjected to one more substrate etching operation until it is qualified. When (h1-h2) / h1>0.06 is satisfied, the cathode assembly is recovered.
[0031] Furthermore, a bubbler was used for stirring, with a power of 10w and a gas output of 5L / min, and the temperature of the etching solution was controlled at 25±1°C.
[0032] Furthermore, the cathode assembly substrate was etched twice using substrate etching solution 2, and a bubbler was used for stirring, with a power of 10w and a gas output of 5L / min to make the stirring more uniform. At the same time, the working temperature of the etching solution was controlled at 25±1°C, and slow etching was performed to control the substrate etching rate at 3~5µm / min and the etching time at 5~10min.
[0033] Furthermore, a bubbler is used for stirring, and the temperature of the etching solution is controlled at 25±1°C.
[0034] Furthermore, the working temperature of the etching liquid is controlled at 25±1°C, and a bubbler is used for stirring, with a power of 10w and a gas output of 5L / min. At the same time, the etching rate is controlled at 15~30nm / s and the etching time is 60~100s, so that the cathode assembly barrier layer is completely corroded to the emission layer, and the black surface disappears.
[0035] Furthermore, a bubbler is used for stirring, with a power of 10w and a gas output of 5L / min. At the same time, the working temperature of the etching solution is controlled at 25±1℃. At the same time, the etching rate is controlled at 5~15nm / s and the etching time is 15~30s, so that the emission layer of the cathode assembly is thinned to an appropriate thickness, with no white fog on the surface, and it is clean and bright.
[0036] Furthermore, a megasonic cleaning machine with a frequency of 1000 KHz was used to further remove particles smaller than 0.2 µm, and the cleaning time was 2 min.
[0037] Furthermore, the working temperature of the rinsing solution is controlled at 25±1°C, and at the same time, the corrosion rate is controlled at 0.2~0.4nm / min, and the rinsing time is 10s.
[0038] The present invention has the following beneficial effects:
[0039] 1. By adjusting the chemical reagent ratio and the temperature of the etching solution during the etching process, the etching rate is controlled and the etching is uniform, which can solve the problems of substrate residue and incomplete etching. At the same time, the etching rate is controlled in sections to appropriately speed up the efficiency of wet processing of GaAs epitaxial wafers, improve the productivity rate, and solve the problems of unclean etching and residue of GaAs epitaxial wafer substrates, unclean surface, and rough surface.
[0040] 2. Using a bubbler instead of magnetic stirring as the stirring method has the advantage of high stirring efficiency and solves the problem of inconsistent corrosion depth and poor blocking effect on the surface of the gallium arsenide photocathode barrier layer.
[0041] 3. Adjust the ratio of etching solution, alkali and hydrogen peroxide to make the etching solution more selective, so as to achieve uniform etching of GaAs photocathode without white marks, and solve the problem of white fog on the surface of GaAs photocathode emission layer. The white fog is caused by uneven etching of GaAs.
[0042] 4. Using megasonic cleaning machine instead of ultrasonic cleaning machine can reduce the damage in the cleaning process. At the same time, megasonic wave can better clean fine particles on the surface, and has better cleaning effect on particles below 0.2μm, improves cathode imaging quality, and solves the problem of through holes and more particles on the surface during the cleaning process of gallium arsenide photocathode.
[0043] 5. Use hydrochloric acid and isopropyl alcohol to clean the gallium arsenide emission layer, which has the effect of removing metal particles and metal ion residues, making the cathode surface cleaner and solving the problem of alkali metal residues on the surface of the gallium arsenide photocathode. BRIEF DESCRIPTION OF THE DRAWINGS
[0044] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without paying any creative work.
[0045] Figure 1 This is a block diagram of the overall structure of the present invention. DETAILED DESCRIPTION
[0046] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention. Example
[0047] Reference Figure 1 ,A low-cost third-generation image intensifier semiconductor photocathode wet processing method, S1, using a micrometer to measure the height h1 of the cathode assembly substrate before corrosion, and quantitatively determine the end time of substrate corrosion through the height change difference;
[0048] S2. Use an ultrasonic cleaning machine at a frequency of 40KHz to degrease and clean the gallium arsenide cathode assembly with K9 glass as the window glass using isopropyl alcohol and deionized water respectively;
[0049] S3. Store the cleaned cathode assembly in deionized water at a temperature of 25±1°C for no more than 30 minutes;
[0050] S4. The cathode component substrate is etched in a step-by-step manner, with the principle of fast first and slow later. First, ammonia: hydrogen peroxide: water = 1:10:10~1:10:20 volume ratio etching solution is used, and then ammonia + hydrogen peroxide etching solution is used to achieve the purpose of uniform corrosion of the cathode component substrate, clean surface, and no residue;
[0051] S5. The cathode assembly substrate etching solution 1 is prepared according to the volume ratio of ammonia water: hydrogen peroxide: water = 1:10:10~1:10:20, and the temperature of the substrate etching solution 1 is controlled at 25±1℃;
[0052] S6, cathode assembly 1 substrate corrosion;
[0053] S7, after etching the cathode assembly once with substrate etching solution 1, take out the cathode assembly, rinse it with deionized water for 30 seconds, and blow dry the surface moisture with nitrogen;
[0054] S8. After the cathode assembly is qualified for the first substrate corrosion, take out the cathode assembly, rinse it with deionized water for 30 seconds, and store it in deionized water for no more than 30 minutes;
[0055] S9, cathode assembly substrate etching solution 2 is prepared according to the volume ratio of ammonia water: hydrogen peroxide = 1:10~1:20;
[0056] S10, cathode assembly secondary substrate corrosion;
[0057] S11, after the cathode assembly is etched twice with substrate etching solution 2, the substrate is evenly and completely etched to the barrier layer. At this time, the cathode assembly surface is black, which is qualified; if it does not turn black, return to the previous step and continue etching;
[0058] S12. After the cathode assembly is etched twice, take out the cathode assembly, rinse it with deionized water for 30 seconds, and store it in deionized water for no more than 30 minutes.
[0059] S13, cathode component barrier layer corrosion solution preparation: potassium hydroxide + hydrogen peroxide + water = 0.02 ~ 0.06 mol + 10 ~ 20 ml + 300 ml;
[0060] S14, cathode assembly barrier layer corrosion: using barrier layer corrosion liquid to corrode the cathode assembly barrier layer;
[0061] S15. After the cathode assembly barrier layer is corroded, the cathode assembly is taken out and rinsed with deionized water for 30 seconds. Then, it is placed in a 200 ml culture dish and 150 ml of deionized water is poured into it. A megasonic cleaning machine is used with a frequency of 1000 KHz to remove particles smaller than 0.2 µm. The cleaning time is 2 minutes.
[0062] S16, cathode component emission layer etching solution preparation: potassium hydroxide + hydrogen peroxide + water = 0.02 ~ 0.06mol + 10 ~ 20ml + 600ml, use a bubbler to stir, at the same time, the temperature of the etching solution is controlled at 25 ± 1 ° C;
[0063] S17, cathode assembly emission layer corrosion: the emission layer of the cathode assembly is corroded by using an emission layer corrosion liquid;
[0064] S18. After the cathode assembly emitter layer is corroded, take out the cathode assembly, rinse it with deionized water for 30 seconds, and then place it in a 200 ml culture dish and pour in 150 ml of deionized water;
[0065] S19. The cathode component rinsing liquid is prepared according to the volume ratio of hydrochloric acid: isopropanol = 1:10~1:20 to remove metal impurities adsorbed on the surface of the cathode component. Magnetic stirring is used and the rinsing liquid temperature is controlled at 25±1℃;
[0066] S20, cathode assembly rinsing: using an emission layer rinsing liquid to rinse the emission layer of the cathode assembly, stirring with a magnetic stirrer at a stirring rate of 500 rpm;
[0067] S21. After the cathode assembly is rinsed, high-purity isopropanol is used to rinse the rinsed cathode assembly for 30 seconds, then it is blown dry with nitrogen and transferred to a vacuum box for storage.
[0068] The cathode assembly substrate was etched once using substrate etching solution 1, stirred by magnetic stirring heating, with a stirring rate of 500 rpm, and the working temperature of the etching solution was controlled at 28°C. Rapid etching was performed, and the substrate etching rate was controlled at 5µm / min, and the etching time was 35min, thereby obtaining a clean, bright and uniform surface.
[0069] Measure the height h2 of the cathode assembly at this time. When (h1-h2) / h1=0.04~0.06 is satisfied, it is clean and has no residue, and proceed to the next step. When (h1-h2) / h1<0.04 is satisfied, perform another substrate etching operation on the cathode assembly until it is qualified. When (h1-h2) / h1>0.06 is satisfied, the cathode assembly is recovered.
[0070] The aerator was used for stirring, the power was 10w, the gas output was 5L / min, and the temperature of the corrosive liquid was controlled at 24℃.
[0071] The cathode assembly substrate was etched twice using substrate etching solution 2, and a bubbler was used for stirring with a power of 10w and a gas output of 5L / min to make the stirring more uniform. At the same time, the working temperature of the etching solution was controlled at 24°C for slow etching, and the substrate etching rate was controlled at 3µm / min for 5min.
[0072] A bubbler is used for stirring, and the temperature of the etching solution is controlled at 25±1℃.
[0073] The working temperature of the etching liquid is controlled at 24°C, and a bubbler is used for stirring. The power is 10w and the gas output is 5L / min. At the same time, the etching rate is controlled at 15nm / s and the etching time is 60s, so that the cathode assembly barrier layer is completely corroded to the emission layer, and the black surface disappears.
[0074] A bubbler is used for stirring, with a power of 10w and a gas output of 5L / min. At the same time, the working temperature of the etching solution is controlled at 24°C. At the same time, the etching rate is controlled at 5nm / s and the etching time is 15s, so that the emission layer of the cathode component is thinned to an appropriate thickness, with no white fog on the surface, and it is clean and bright.
[0075] A megasonic cleaning machine with a frequency of 1000 KHz was used to further remove particles smaller than 0.2 µm, and the cleaning time was 2 min.
[0076] The working temperature of the rinsing solution was controlled at 24°C. At the same time, the corrosion rate was controlled at 0.2 nm / min and the rinsing time was 10 s. Example
[0077] A low-cost third-generation image intensifier semiconductor photocathode wet processing method, S1, using a micrometer to measure the height h1 of the cathode assembly substrate before corrosion, and quantitatively judging the end time of substrate corrosion through the height change difference;
[0078] S2. Use an ultrasonic cleaning machine at a frequency of 40KHz to degrease and clean the gallium arsenide cathode assembly with K9 glass as the window glass using isopropyl alcohol and deionized water respectively;
[0079] S3. Store the cleaned cathode assembly in deionized water at a temperature of 25±1°C for no more than 30 minutes;
[0080] S4. The cathode component substrate is etched in a step-by-step manner, with the principle of fast first and slow later. First, ammonia: hydrogen peroxide: water = 1:10:10~1:10:20 volume ratio etching solution is used, and then ammonia + hydrogen peroxide etching solution is used to achieve the purpose of uniform corrosion of the cathode component substrate, clean surface, and no residue;
[0081] S5. The cathode assembly substrate etching solution 1 is prepared according to the volume ratio of ammonia water: hydrogen peroxide: water = 1:10:10~1:10:20, and the temperature of the substrate etching solution 1 is controlled at 25±1℃;
[0082] S6, cathode assembly 1 substrate corrosion;
[0083] S7, after etching the cathode assembly once with substrate etching solution 1, take out the cathode assembly, rinse it with deionized water for 30 seconds, and blow dry the surface moisture with nitrogen;
[0084] S8. After the cathode assembly is qualified for the first substrate corrosion, take out the cathode assembly, rinse it with deionized water for 30 seconds, and store it in deionized water for no more than 30 minutes;
[0085] S9, cathode assembly substrate etching solution 2 is prepared according to the volume ratio of ammonia water: hydrogen peroxide = 1:10~1:20;
[0086] S10, cathode assembly secondary substrate corrosion;
[0087] S11, after the cathode assembly is etched twice with substrate etching solution 2, the substrate is evenly and completely etched to the barrier layer. At this time, the cathode assembly surface is black, which is qualified; if it does not turn black, return to the previous step and continue etching;
[0088] S12. After the cathode assembly is etched twice, take out the cathode assembly, rinse it with deionized water for 30 seconds, and store it in deionized water for no more than 30 minutes.
[0089] S13, cathode component barrier layer corrosion solution preparation: potassium hydroxide + hydrogen peroxide + water = 0.02 ~ 0.06 mol + 10 ~ 20 ml + 300 ml;
[0090] S14, cathode assembly barrier layer corrosion: using barrier layer corrosion liquid to corrode the cathode assembly barrier layer;
[0091] S15. After the cathode assembly barrier layer is corroded, the cathode assembly is taken out and rinsed with deionized water for 30 seconds. Then, it is placed in a 200 ml culture dish and 150 ml of deionized water is poured into it. A megasonic cleaning machine is used with a frequency of 1000 KHz to remove particles smaller than 0.2 µm. The cleaning time is 2 minutes.
[0092] S16, cathode component emission layer etching solution preparation: potassium hydroxide + hydrogen peroxide + water = 0.02 ~ 0.06mol + 10 ~ 20ml + 600ml, use a bubbler to stir, at the same time, the temperature of the etching solution is controlled at 25 ± 1 ° C;
[0093] S17, cathode assembly emission layer corrosion: the emission layer of the cathode assembly is corroded by using an emission layer corrosion liquid;
[0094] S18. After the cathode assembly emitter layer is corroded, take out the cathode assembly, rinse it with deionized water for 30 seconds, and then place it in a 200 ml culture dish and pour 150 ml of deionized water;
[0095] S19. The cathode component rinsing liquid is prepared according to the volume ratio of hydrochloric acid: isopropanol = 1:10~1:20 to remove metal impurities adsorbed on the surface of the cathode component. Magnetic stirring is used and the rinsing liquid temperature is controlled at 25±1℃;
[0096] S20, cathode assembly rinsing: using an emission layer rinsing liquid to rinse the emission layer of the cathode assembly, stirring with a magnetic stirrer at a stirring rate of 500 rpm;
[0097] S21. After the cathode assembly is rinsed, high-purity isopropanol is used to rinse the rinsed cathode assembly for 30 seconds, then it is blown dry with nitrogen and transferred to a vacuum box for storage.
[0098] Through S6, the cathode assembly substrate is etched once using substrate etching solution 1, stirred by magnetic stirring heating, with a stirring rate of 500 rpm, the working temperature of the etching solution controlled at 32°C, and rapid etching is performed to control the substrate etching rate at 10µm / min, and the etching time is 455min, thereby obtaining a clean, bright and uniform surface.
[0099] Through S7, the height h2 of the cathode assembly is measured at this time. When (h1-h2) / h1=0.06 is satisfied, it is clean and has no residue, and the next step is carried out; when (h1-h2) / h1<0.04 is satisfied, the cathode assembly is subjected to one more substrate etching operation until it is qualified; when (h1-h2) / h1>0.06 is satisfied, the cathode assembly is recovered.
[0100] Through S9, a bubbler is used for stirring, the power is 10w, the gas output is 5L / min, and the temperature of the etching liquid is controlled at 26℃.
[0101] Through S10, the cathode assembly substrate is etched twice using substrate etching solution 2, and a bubbler is used for stirring, with a power of 10w and a gas output of 5L / min to make the stirring more uniform. At the same time, the working temperature of the etching solution is controlled at 26°C, and slow etching is performed to control the substrate etching rate at 5µm / min, and the etching time is 10min.
[0102] Through S13, a bubbler is used for stirring, and at the same time, the temperature of the etching solution is controlled at 26°C.
[0103] Through S14, the working temperature of the etching liquid is controlled at 26°C, and a bubbler is used for stirring, with a power of 10w and a gas output of 5L / min. At the same time, the etching rate is controlled at 30nm / s and the etching time is 100s, so that the cathode assembly barrier layer is completely corroded to the emission layer, and the black surface disappears.
[0104] Through S17, a bubbler is used for stirring, the power is 10w, the gas output is 5L / min, and at the same time, the working temperature of the etching liquid is controlled at 26°C. At the same time, the etching rate is controlled at 15nm / s, and the etching time is 30s, so that the emission layer of the cathode assembly is thinned to an appropriate thickness, and the surface is free of white fog, clean and bright.
[0105] Through S18, a megasonic cleaning machine with a frequency of 1000KHz is used to further remove particles below 0.2µm, and the cleaning time is 2min.
[0106] Through S20, the working temperature of the rinsing liquid is controlled at 26°C, and at the same time, the corrosion rate is controlled at 0.4nm / min, and the rinsing time is 10s.
[0107] The above shows and describes the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments. The above embodiments and descriptions only describe the principles of the present invention. The present invention may be subject to various changes and improvements without departing from the spirit and scope of the present invention. These changes and improvements fall within the scope of the present invention. The scope of protection claimed by the present invention is defined by the attached claims and their equivalents.
Claims
1. A low-cost wet processing method for semiconductor photocathode of third-generation image intensifier, Features: S1. Use a micrometer to measure the height h1 of the cathode assembly substrate before corrosion, and quantitatively determine the end time of substrate corrosion based on the height change difference; S2. Use an ultrasonic cleaning machine at a frequency of 40KHz to degrease and clean the gallium arsenide cathode assembly with K9 glass as the window glass using isopropyl alcohol and deionized water respectively; S3. Store the cleaned cathode assembly in deionized water at a temperature of 25±1°C for no more than 30 minutes; S4. The cathode component substrate is etched in a step-by-step manner, with the principle of fast first and slow later. First, ammonia: hydrogen peroxide: water = 1:10:10~1:10:20 volume ratio etching solution is used, and then ammonia + hydrogen peroxide etching solution is used to achieve the purpose of uniform corrosion of the cathode component substrate, clean surface, and no residue; S5. The cathode assembly substrate etching solution 1 is prepared according to the volume ratio of ammonia water: hydrogen peroxide: water = 1:10:10~1:10:20, and the temperature of the substrate etching solution 1 is controlled at 25±1℃; S6, cathode assembly 1 substrate corrosion; S7, after etching the cathode assembly once with substrate etching solution 1, take out the cathode assembly, rinse it with deionized water for 30 seconds, and blow dry the surface moisture with nitrogen; S8. After the cathode assembly is qualified for the first substrate corrosion, take out the cathode assembly, rinse it with deionized water for 30 seconds, and store it in deionized water for no more than 30 minutes; S9, cathode assembly substrate etching solution 2 is prepared according to the volume ratio of ammonia water: hydrogen peroxide = 1:10~1:20; S10, cathode assembly secondary substrate corrosion; S11, after the cathode assembly is etched twice with substrate etching solution 2, the substrate is evenly and completely etched to the barrier layer. At this time, the cathode assembly surface is black, which is qualified; if it does not turn black, return to the previous step and continue etching; S12. After the cathode assembly is etched twice, take out the cathode assembly, rinse it with deionized water for 30 seconds, and store it in deionized water for no more than 30 minutes. S13, cathode component barrier layer corrosion solution preparation: potassium hydroxide + hydrogen peroxide + water = 0.02 ~ 0.06 mol + 10 ~ 20 ml + 300 ml; S14, cathode assembly barrier layer corrosion: using barrier layer corrosion liquid to corrode the cathode assembly barrier layer; S15. After the cathode assembly barrier layer is corroded, the cathode assembly is taken out and rinsed with deionized water for 30 seconds. Then, it is placed in a 200 ml culture dish and 150 ml of deionized water is poured into it. A megasonic cleaning machine is used with a frequency of 1000 KHz to remove particles smaller than 0.2 µm. The cleaning time is 2 minutes. S16, cathode component emission layer etching solution preparation: potassium hydroxide + hydrogen peroxide + water = 0.02 ~ 0.06mol + 10 ~ 20ml + 600ml, use a bubbler to stir, at the same time, the temperature of the etching solution is controlled at 25 ± 1 ° C; S17, cathode assembly emission layer corrosion: the cathode assembly emission layer corrosion liquid is used to corrode the cathode assembly emission layer; S18. After the cathode assembly emitter layer is corroded, take out the cathode assembly, rinse it with deionized water for 30 seconds, and then place it in a 200 ml culture dish and pour in 150 ml of deionized water; S19. The cathode component rinsing liquid is prepared according to the volume ratio of hydrochloric acid: isopropanol = 1:10~1:20 to remove metal impurities adsorbed on the surface of the cathode component. Magnetic stirring is used and the rinsing liquid temperature is controlled at 25±1℃; S20, cathode assembly rinsing: using an emission layer rinsing liquid to rinse the emission layer of the cathode assembly, stirring with a magnetic stirrer at a stirring rate of 500 rpm; S21. After the cathode assembly is rinsed, high-purity isopropanol is used to rinse the rinsed cathode assembly for 30 seconds, then it is blown dry with nitrogen and transferred to a vacuum box for storage.
2. A low-cost third-generation image intensifier semiconductor photocathode wet processing method according to claim 1, It is characterized in that Through S6, the cathode assembly substrate is etched once using substrate etching solution 1, stirred by magnetic stirring heating, with a stirring rate of 500rpm, and the working temperature of substrate etching solution 1 is controlled at 28~32℃, and rapid etching is performed, and the substrate etching rate is controlled at 5~10µm / min, and the etching time is 40±5min, so as to obtain a clean, bright and uniform surface.
3. A low-cost third-generation image intensifier semiconductor photocathode wet processing method according to claim 1, It is characterized in that Through S7, the height h2 of the cathode assembly is measured at this time. When (h1-h2) / h1=0.04~0.06 is satisfied, it is clean and has no residue, and the next step is carried out; when (h1-h2) / h1<0.04 is satisfied, the cathode assembly is subjected to one more substrate etching operation until it is qualified; when (h1-h2) / h1>0.06 is satisfied, the cathode assembly is recovered.
4. A low-cost third-generation image intensifier semiconductor photocathode wet processing method according to claim 1, It is characterized in that Through S9, a bubbler is used for stirring, the power is 10w, the gas output is 5L / min, and the temperature of the substrate etching solution 2 is controlled at 25±1℃.
5. A low-cost third-generation image intensifier semiconductor photocathode wet processing method according to claim 1, It is characterized in that Through S10, the cathode assembly substrate is etched twice using substrate etching solution 2, and a bubbler is used for stirring, with a power of 10w and a gas output of 5L / min to make the stirring more uniform. At the same time, the working temperature of the etching solution is controlled at 25±1℃, and slow etching is performed to control the substrate etching rate at 3~5µm / min and the etching time is 5~10min.
6. A low-cost third-generation image intensifier semiconductor photocathode wet processing method according to claim 1, It is characterized in that Through S13, a bubbler is used for stirring, and at the same time, the temperature of the barrier layer etching solution is controlled at 25±1°C.
7. A low-cost third-generation image intensifier semiconductor photocathode wet processing method according to claim 1, It is characterized in that Through S14, the working temperature of the barrier layer etching liquid is controlled at 25±1℃, and a bubbler is used for stirring, with a power of 10w and a gas output of 5L / min. At the same time, the corrosion rate is controlled at 15~30nm / s and the corrosion time is 60~100s, so that the cathode assembly barrier layer is completely corroded until the black color on the surface of the emission layer disappears.
8. A low-cost third-generation image intensifier semiconductor photocathode wet processing method according to claim 1, It is characterized in that Through S17, a bubbler is used for stirring, the power is 10w, the gas output is 5L / min, and at the same time, the working temperature of the emission layer etching solution is controlled at 25±1℃. At the same time, the corrosion rate is controlled at 5~15nm / s, and the corrosion time is 15~30s, so that the emission layer of the cathode assembly is thinned to an appropriate thickness, with no white fog on the surface, clean and bright.
9. A low-cost third-generation image intensifier semiconductor photocathode wet processing method according to claim 1, It is characterized in that Through S18, a megasonic cleaning machine with a frequency of 1000KHz is used to remove particles below 0.2µm, and the cleaning time is 2min.
10. A low-cost third-generation image intensifier semiconductor photocathode wet processing method according to claim 1, It is characterized in that Through S20, the working temperature of the rinsing solution is controlled at 25±1°C, and at the same time, the corrosion rate is controlled at 0.2~0.4nm / min, and the rinsing time is 10s.
Citation Information
Patent Citations
Nitride-based compound semiconductor, method of cleaning a compound semiconductor, method of producing the same, and substrate
CN1866476A
Method of manufacturing 3-5 group compound semiconductor
JP2005039237A