Electrolyte additive, electrolyte and lithium secondary battery
By using electrolyte additives containing thiazolyl, amino and nitrile groups in lithium-ion batteries, a stable positive electrode surface film is formed, which solves the problems of electrolyte decomposition and transition metal ion precipitation at high voltage and high temperature, and improves the battery resistance High voltage, high temperature resistance and cycling performance.
Patent Information
- Application Number
- CN202210143682.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-02-16
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2042-02-16
AI Technical Summary
Existing lithium-ion batteries have problems with electrolyte decomposition and transition metal ion precipitation under high voltage and high temperature conditions, resulting in a decline in battery performance, and the application of high-voltage positive electrode materials is limited by insufficient electrolyte stability.
Develop an electrolyte additive containing thiazolyl, amino and nitrile groups. By forming a film on the surface of the positive electrode, the HF content is reduced, the interface stability between the positive electrode and the electrolyte is enhanced, the electrolyte decomposition and the precipitation of transition metal ions are inhibited, and the battery is improved. High voltage resistance, high temperature resistance and cycle performance.
It effectively improves the high-temperature storage and high voltage performance of lithium-ion batteries, extends the cycle life, enhances the high voltage and high temperature performance of the battery, forms a denser film structure, and improves the overall performance of the battery.
Smart Images

Figure CN114583271B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of lithium ion batteries, and in particular to an electrolyte additive containing thiazole groups, amino groups and cyano groups, and an electrolyte and a lithium ion battery containing the additive. Background Art
[0002] Since its introduction in 1990, lithium-ion batteries have become one of the internationally recognized ideal secondary batteries for their high energy density, long cycle life, low environmental pollution and no memory effect, and have been widely used in electronic devices such as mobile communications, laptops, and electric bicycles. With the increasing development of hybrid electric vehicles and pure electric vehicles, lithium-ion batteries, as an ideal power source for power vehicles, are facing unprecedented challenges - improving battery safety performance and energy density.
[0003] Improving the working voltage of the battery is one of the effective ways to increase the energy density of lithium-ion batteries. Currently, the negative electrode of commercial lithium-ion batteries mainly uses graphite materials, which have a lithium insertion potential of 0.1V (vs. Li / Li + ) is very close to the theoretical lithium insertion potential of metallic lithium. Therefore, the only way to increase the operating voltage of lithium-ion batteries is to increase the lithium insertion / extraction potential of the positive electrode material. Several major high-voltage positive electrode materials that have been reported include LiCoPO4 (4.8V), LiNi 0.5 Mn 1.5 O4 (4.7V), ternary material LiNi 1-x-y Co x Mn y O2 (0≤x, y≤1, x+y≤1) and lithium-rich. These high-voltage cathode materials have not yet been applied to actual production. The biggest reason is that the electrochemical stability window of the carbonate-based electrolyte currently used in business is low. When the battery voltage reaches 4.5V (vs. Li / Li + ) or so, the electrolyte begins to undergo violent oxidative decomposition reactions, resulting in the battery's lithium insertion and extraction reactions being unable to proceed normally. Secondly, some positive electrode materials, such as LiNi0.5Mn1.5O4 materials, will undergo dissolution of metal Mn and Ni ions under high voltage conditions, destroying the material structure and causing serious battery capacity decay. This shows that improving the stability of the battery's electrode / electrolyte (especially the positive electrode / electrolyte) interface is a basic prerequisite for the development of high-voltage lithium-ion batteries.
[0004] At present, a simple, easy-to-operate and low-cost method for improving the battery electrode / electrolyte interface has been reported - the development and application of a new type of elegant electrolyte system or high-voltage film-forming additive. Generally speaking, additives containing thiazole and amino groups have the effect of reducing the HF content under high voltage due to their weak alkalinity, thereby reducing the precipitation of transition metal ions in the positive electrode of lithium-ion batteries and enhancing the stability of the interface film between the positive electrode and the electrolyte, so as to improve the high-temperature storage and high-voltage performance of the battery; cyanide can complex the transition metal of the positive electrode of lithium-ion batteries and form a film on the surface of the positive electrode. This interface film can effectively inhibit the decomposition of the electrolyte and reduce the precipitation of transition metal ions, so it can improve the cycle performance of the high-voltage system.
[0005] Based on this background, it is of great significance to utilize the synergistic effect of the above three groups to develop an additive with better high voltage resistance, high temperature resistance and excellent cycle performance. Summary of the invention
[0006] One of the purposes of the present invention is to provide an electrolyte additive for lithium ion battery electrolyte which can form a film on the positive electrode, reduce the HF content in the electrolyte, and enhance the stability of the interface film between the positive electrode and the electrolyte.
[0007] The second object of the present invention is to provide an electrolyte for lithium ion batteries containing the above electrolyte additive and having high voltage resistance, high temperature resistance and excellent cycle performance.
[0008] The third object of the present invention is to provide a lithium ion battery containing the above-mentioned electrolyte and having high voltage resistance, high temperature resistance and excellent cycle performance.
[0009] To achieve the above object, the present invention provides an electrolyte additive, comprising a compound having a structure shown in structural formula (I):
[0010]
[0011] The present invention also provides an electrolyte comprising a lithium salt, a solvent and an additive, wherein the additive comprises the electrolyte additive mentioned above.
[0012] Preferably, the mass percentage of the electrolyte additive of the present invention to the total mass of the lithium salt and the solvent is 0.1%-5.0%. Preferably, the amount of the additive can be selected to be 0.5%-5.0%; more preferably, the amount of the additive can be selected to be: 0.5%, 1.0%, 2.0%, 5.0%.
[0013] Preferably, the lithium salt of the electrolyte of the present invention is selected from the conductive lithium salt, which is at least one of lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium bis(oxalatoborate) (LiBOB), lithium difluorooxalatoborate (LiODFB), lithium bis(fluorosulfonyl)imide (LiFSI), and lithium bis(trifluoromethylsulfonyl)imide (LiTFSI).
[0014] Preferably, the concentration of the lithium salt in the electrolyte of the present invention is 0.5M to 1.5M. Specifically, the concentration of the lithium salt in the electrolyte of the present invention may be, but is not limited to, 0.5M, 0.75M, 1M, 1.25M, or 1.5M.
[0015] Preferably, the solvent is selected from one or more of chain and cyclic carbonates and carboxylates. Cyclic carbonate solvents refer to ethylene carbonate (EC), fluoroethylene carbonate (FEC) or propylene carbonate (PC); chain carbonate solvents refer to dimethyl carbonate (DMC), diethyl carbonate (DEC) or ethyl methyl carbonate (EMC); carboxylates solvents refer to propyl acetate (PA), ethyl acetate (EA) or propyl propionate (PP).
[0016] In the present invention, preferably, an auxiliary additive is further included, and the auxiliary additive is one or both of 1,3-propane sultone and tris(trimethylsilyl)borate.
[0017] Preferably, the mass percentage of the auxiliary additive to the total mass of the lithium salt and the solvent is 0.1-2%.
[0018] The present invention also provides a lithium secondary battery, the lithium secondary battery comprising a positive electrode, a negative electrode and a lithium secondary battery electrolyte as described above, wherein: the positive electrode material is selected from lithium transition metal oxides, wherein the lithium transition metal oxide is LiCoO2, LiMn2O4, LiMnO2, Li2MnO4, LiFePO4, Li 1+a Mn 1-x M x O2、LiCo 1-x M x O2、LiFe 1- x M x PO4、Li2Mn 1-x O4, wherein M is one or more selected from Ni, Co, Mn, Al, Cr, Mg, Zr, Mo, V, Ti, B, F, 0≤a<0.2, 0≤x<1; the negative electrode material is selected from at least one of graphite, silicon-carbon composite material, and lithium titanate.
[0019] Compared with the prior art, the electrolyte additive of the present invention contains thiazole and amino groups, both of which are weakly alkaline, so it has the effect of reducing the HF content under high voltage, thereby improving the high-temperature storage and high-voltage performance of the battery; secondly, it contains a nitrile group, which complexes the transition metal of the positive electrode of the lithium-ion battery and forms a film on the surface of the positive electrode. The interface film can effectively inhibit the decomposition of the electrolyte and reduce the precipitation of transition metal ions, so it can improve the cycle performance of the high-voltage system, thereby exerting a synergistic effect and better improving the high-voltage resistance, high-temperature resistance and cycle performance of the battery. DETAILED DESCRIPTION
[0020] The present invention will be further described below in conjunction with the embodiments, but it does not constitute any limitation to the present invention. Any limited number of modifications made within the scope of the claims of the present invention are still within the scope of the claims of the present invention.
[0021] In order to explain the technical content of the present invention in detail, further description is given below in conjunction with the implementation modes.
[0022] Embodiment 1
[0023] 1. Preparation of electrolyte: Ethylene carbonate (EC), diethyl carbonate (DEC) and ethyl methyl carbonate (EMC) are mixed in a mass ratio of EC:DEC:EMC=1:1:1, and 1 mol of lithium hexafluorophosphate (LiPF6) is added after mixing. After the lithium salt is completely dissolved, 0.5% of the additive shown in structural formula I is added.
[0024] 2. Preparation of positive electrode: LiNi 0.6 Co 0.2 Mn 0.2 O2, conductive agent SuperP, adhesive PVDF and carbon nanotubes (CNT) are mixed evenly in a mass ratio of 97.5:1.5:1:1 to form a lithium-ion battery positive electrode slurry with a certain viscosity, which is coated on the aluminum foil for current collector. The coating amount is 324g / m 2 , dried at 85°C and then cold pressed; then trimmed, cut into pieces, and slit, and after slitting, dried at 85°C under vacuum conditions for 4 hours, and the tabs were welded to make lithium-ion battery positive electrodes that meet the requirements.
[0025] 3. Preparation of negative electrode sheet: artificial graphite, conductive agent SuperP, thickener CMC, adhesive SBR (styrene-butadiene rubber latex) are mixed in a mass ratio of 95:1.5:1.0:2.5 to make a slurry, mix them evenly, apply the mixed slurry on both sides of the copper foil, dry and roll to obtain the negative electrode sheet, and make a lithium-ion battery negative electrode sheet that meets the requirements.
[0026] 4. Preparation of lithium-ion batteries: The positive electrode sheet, negative electrode sheet and separator prepared according to the above process are stacked to form a lithium-ion battery with a thickness of 4.7 mm, a width of 55 mm, and a length of 60 mm. The capacity is 1800 mAh. The battery is vacuum-baked at 85°C for 48 hours, and the above electrolyte is injected to complete the battery production.
[0027] Embodiments 2 to 4
[0028] The preparation of the electrolyte, the positive electrode sheet, the negative electrode sheet and the lithium-ion battery are consistent with those in Example 1, but the contents of the additives shown in Structural Formula I are 1.0%, 2.0% and 5.0% respectively.
[0029] Embodiment 5
[0030] The preparation of the electrolyte, the positive electrode sheet, the negative electrode sheet and the lithium-ion battery are consistent with those in Example 1, but the content of the additive shown in structural formula I is 0.7%; in addition, 0.3% of 1,3-propane sultone is also added in this example.
[0031] Embodiment 6
[0032] The preparation of the electrolyte, the positive electrode sheet, the negative electrode sheet and the lithium-ion battery are consistent with those in Example 1, except that the content of the additive shown in structural formula I is 0.7%; in addition, 0.2% of 1,3-propane sultone and 0.1% of tris(trimethylsilyl)borate are added in this example.
[0033] Embodiment 7
[0034] 1. Preparation of electrolyte: Ethylene carbonate (EC), diethyl carbonate (DEC) and ethyl methyl carbonate (EMC) are mixed in a mass ratio of EC:DEC:EMC=1:1:1, and 1 mol of lithium hexafluorophosphate (LiPF6) is added after mixing. After the lithium salt is completely dissolved, 0.5% of the additive shown in structural formula I is added.
[0035] 2. Preparation of positive electrode sheet: LiCoO2, a cobalt oxide material, SuperP, a binder PVDF and carbon nanotubes (CNT) are mixed evenly at a mass ratio of 97.5:1.5:1:1 to form a lithium-ion battery positive electrode slurry with a certain viscosity, which is then coated on the aluminum foil for current collector. The coating amount is 316 g / m 2 , dried at 85°C and then cold pressed; then trimmed, cut into pieces, and slit, and after slitting, dried at 85°C under vacuum conditions for 4 hours, and the tabs were welded to make lithium-ion battery positive electrodes that meet the requirements.
[0036] 3. Preparation of negative electrode sheet: artificial graphite, conductive agent SuperP, thickener CMC, adhesive SBR (styrene-butadiene rubber latex) are mixed in a mass ratio of 95:1.5:1.0:2.5 to make a slurry, mix them evenly, apply the mixed slurry on both sides of the copper foil, dry and roll to obtain the negative electrode sheet, and make a lithium-ion battery negative electrode sheet that meets the requirements.
[0037] 4. Preparation of lithium-ion batteries: The positive electrode sheet, negative electrode sheet and separator prepared according to the above process are stacked to form a lithium-ion battery with a thickness of 4.7 mm, a width of 55 mm, and a length of 60 mm. The capacity is 2000 mAh. The battery is vacuum-baked at 85°C for 48 hours, and the above electrolyte is injected to complete the battery production.
[0038] Embodiments 8 to 10
[0039] The preparation of the electrolyte, the positive electrode sheet, the negative electrode sheet and the lithium ion battery are the same as those in Example 5, but the contents of the additives shown in Structural Formula I are 1.0%, 2.0% and 5.0% respectively.
[0040] Comparative Examples 1 to 4
[0041] The electrolyte preparation method and battery preparation method refer to Examples 1 to 4, where no additives are added, and for Comparative Compounds 1 to 3, the additive addition amount is 1.0%.
[0042] Comparative Example 5
[0043] Comparative compounds 1 to 3 were added, each at 1.0% and the total amount was 3%.
[0044] Comparative Example 6
[0045] The preparation of the electrolyte, the positive electrode sheet, the negative electrode sheet and the lithium-ion battery are consistent with those in Example 1, but do not contain the additive shown in structural formula I; in addition, this example also adds 1% of 1,3-propane sultone.
[0046] Comparative Examples 7 to 10
[0047] The electrolyte preparation method and battery preparation method refer to Examples 5 to 8, where no additives are added, and for Comparative Compounds 1 to 3, the additive addition amount is 1.0%.
[0048] Comparative Example 11
[0049] Comparative compounds 1 to 3 were added, and the additives were all 1.0%.
[0050] Comparative compounds 1 to 3 are as follows:
[0051]
[0052] The electrolyte components and battery systems of the above examples and comparative examples are shown in Table 1.
[0053] Table 1: Electrolyte compositions and battery systems of the embodiments and comparative examples.
[0054]
[0055]
[0056] Application experiments of embodiments and comparative examples
[0057] 25℃ 1.0C / 1.0C normal temperature cycle test: Charge at 25℃ with 1.0C constant current to 4.5V, charge at 4.5V constant voltage to cut-off current 0.05C, then discharge at 1.0C constant current, discharge capacity is recorded as C0, repeat the charge and discharge steps for 1000 cycles, and obtain the 1000th cycle discharge capacity C 1000 , capacity retention rate = C 1000 / C0*100%.
[0058] 45℃ 1.0C / 1.0C high temperature cycle test: Charge at 45℃ with 1.0C constant current to 4.5V, charge at constant voltage to cut-off current 0.05C, then discharge at 1.0C constant current, discharge capacity is recorded as C0, repeat the charge and discharge steps for 1000 cycles, and obtain the 1000th cycle discharge capacity C 1000 , capacity retention rate = C 1000 / C0*100%
[0059] Capacity retention rate after 14-day storage at 60°C: After the battery is cycled 3 times at a charge and discharge rate of 1C, it is stored at 60°C for 14 days under full charge and then discharged. The obtained discharge capacity is divided by the discharge capacity of the first cycle to obtain the capacity retention rate after high-temperature storage.
[0060] -20℃ low temperature discharge test: At 25℃, charge to 4.5V at 1.0C constant current, charge to 0.05C at 4.5V constant voltage, and then discharge the battery at 0.5C constant current. The discharge capacity is recorded as C0. At 25℃, charge to 4.5V at 1.0C constant current, charge to 0.05C at 4.5V constant voltage, and then transfer the battery to -20℃ for 240min, and then discharge the battery at 0.5C constant current. The discharge capacity is recorded as C1. -20℃ discharge rate = C1 / C0*100%.
[0061] After the electrolytes in the above embodiments and comparative examples were made into lithium-ion batteries, the room temperature cycle energy absorption, high temperature cycle performance, high temperature storage performance, and low temperature discharge performance of the lithium-ion batteries were tested. The results are shown in Table 2:
[0062] Table 2: Lithium-ion battery performance test results
[0063]
[0064] In the high voltage system, by comparing Examples 1 to 4 and Examples 6 to 9, it is found that the optimal dosage of the target additive is 1.0%. When the addition amount is 0.5%, the density of the film formed at the positive electrode is not enough due to the small amount of addition, so the overall performance is worse than 1.0%. When the addition amount exceeds 1.0%, its normal temperature cycle, high temperature cycle and high temperature storage performance are equivalent to 1.0%, indicating that when the addition amount is 1.0%, the film formed is dense enough, and when the addition amount is exceeded, the effect is not significant. Adding the target additive can slightly improve the low temperature performance. This is because the three work together to better inhibit the dissolution of transition metal ions, avoid their deposition at the negative electrode, catalyze the decomposition of the electrolyte, and form a thinner film than when not added. When the addition amount exceeds 1.0%, the low temperature performance may be slightly worse than 1.0% because the density of the film formed at the positive electrode is too dense. By comparing the examples with the comparative examples, it is found that the normal temperature, high temperature cycle and high temperature storage performance of the additive containing a single thiazole group, an amino group and a cyano group is better than that without the additive, but the three have little effect on the low temperature performance. The best performance is the additive containing a nitrile group. When the three are used at the same time, the overall performance of the battery is improved, but there is still a big gap compared with the target additive, which proves that an additive containing three groups at the same time will better play a synergistic role and improve the overall performance of the battery.
[0065] At the same time, it can be found from Examples 5 and 6 that when the electrolyte additive of the present invention and 1,3-propane sultone are matched with each other, the normal temperature and high temperature cycle, high temperature storage and low temperature performance of the electrolyte additive of the present invention can be better exerted.
Claims
1. An electrolyte comprising a lithium salt, a solvent and an additive, characterized in that: The additive comprises the electrolyte additive as described in structural formula (I); the mass percentage of the electrolyte additive to the total mass of the lithium salt and the solvent is 0.1%-5.0%; ; Structural formula (Ⅰ).
2. The electrolyte according to claim 1, characterized in that The lithium salt is selected from at least one of lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate, lithium bis(oxalato)borate, lithium difluorooxalato)borate, lithium bis(fluorosulfonyl)imide salt, and lithium bis(trifluoromethyl)sulfonyl imide.
3. The electrolyte according to claim 1, characterized in that The concentration of the lithium salt in the electrolyte is 0.5M to 1.5M.
4. The electrolyte according to claim 1, characterized in that The solvent is selected from one or more of chain and cyclic carbonates and carboxylic acid ester solvents; the cyclic carbonate solvent is one or more of ethylene carbonate, fluoroethylene carbonate, and propylene carbonate; the chain carbonate solvent is dimethyl carbonate, diethyl carbonate, and ethyl methyl carbonate; the carboxylic acid ester solvent is one or more of propyl acetate, ethyl acetate, and propyl propionate.
5. The electrolyte according to any one of claims 1 to 3, characterized in that: The invention also comprises auxiliary additives, which are one or two of 1,3-propane sultone and tris(trimethylsilyl)borate.
6. The electrolyte according to claim 5, characterized in that The mass percentage of the auxiliary additive to the total mass of the lithium salt and the solvent is 0.1-2%.
7. A lithium secondary battery, characterized in that: The lithium secondary battery comprises a positive electrode, a negative electrode and an electrolyte according to any one of claims 1 to 6, wherein the positive electrode material is selected from lithium transition metal oxides, wherein the lithium transition metal oxide is LiCoO2, LiMn2O4, LiMnO2, Li2MnO4, LiFePO4, Li1 +a Mn 1-x MxO2、LiCo 1-x M x O2、LiFe 1-x M x PO4、Li2Mn 1-x O4, wherein M is one or more selected from Ni, Co, Mn, Al, Cr, Mg, Zr, Mo, V, Ti, B, F, 0≤a<0.2, 0≤x<1; the negative electrode material is selected from at least one of graphite, silicon-carbon composite material, and lithium titanate.