A total dose hardening method for embedded high and low voltage compatible CMOS

By adopting high and low voltage MOS device reinforcement method and floating gate FLASH device reinforcement method in embedded floating gate FLASH process devices, the threshold voltage drift and leakage problems caused by the total dose effect are solved, and the device's radiation resistance is improved.

CN114597174BActive Publication Date: 2024-11-1958TH RES INST OF CETC
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202210237633.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-03-10
Publication Date
2024-11-19
Estimated Expiration
2042-03-10

AI Technical Summary

Technical Problem

The embedded floating gate FLASH process device faces threshold voltage drift and inter-deviation leakage problems under the total dose effect, which affects its radiation resistance.

Method used

The reinforcement method of high and low voltage MOS device is adopted, including STI injection method, high voltage MOS device stacking oxygen technology method, low voltage MOS device stacking oxygen technology method and active region cutoff method, and floating gate type FLASH device reinforcement method, using tunnel oxide layer Reinforcement process and inter-polysilicon dielectric layer processing process enhance the total dose reinforcement capability of the device.

Benefits of technology

It effectively suppresses leakage channels, reduces oxide layer defects and traps, improves the device's radiation resistance and data storage capacity, and improves the radiation resistance of FPGA, CPLD, MCU, and SoC circuits.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114597174B_ABST
    Figure CN114597174B_ABST
Patent Text Reader

Abstract

The present invention discloses an embedded high-low voltage compatible CMOS total dose reinforcement method, belonging to the field of microelectronic integrated circuits. The present invention adopts STI injection method, high-voltage MOS device stacked gate oxygen process method, low-voltage MOS device stacked gate oxygen process method and active area cut-off method to reinforce the total dose of high and low voltage MOS devices, and adopts tunnel oxide layer reinforcement process method and polysilicon inter-dielectric layer reinforcement process method to reinforce the total dose of floating gate FLASH devices, so as to reduce the thermal process, increase the P-type impurity concentration on the surface of the field area, suppress the threshold voltage drift, reduce the leakage between devices and inside the device, and realize the total dose reinforcement of embedded floating gate FLASH process devices.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of microelectronic integrated circuits, and in particular to an embedded high- and low-voltage compatible CMOS total dose reinforcement method. Background Art

[0002] Embedded high and low voltage compatible CMOS integrated circuits have the advantages of high integration, high reliability, mature process technology and low cost.

[0003] Taking embedded floating gate FLASH (eFLASH) process devices as an example, they are the core components of FPGA, CPLD, MCU, SoC and other circuits. Their circuits have the advantages of large data storage capacity and strong data processing capabilities.

[0004] The technical difficulty of total dose reinforcement of embedded floating gate FLASH (eFLASH) process devices lies in the total dose reinforcement of floating gate FLASH process devices and high and low voltage MOS devices: on the one hand, the total dose effect will cause the floating gate FLASH device to emit electrons in the programming state and inject holes in the erased state, which manifests as a narrowing of the erase / write threshold window; on the other hand, the total dose effect will cause the SiO2 dielectric layer in the field area to capture trapped charges, resulting in a decrease in the inversion threshold voltage at the edge of the P substrate field, which manifests as field edge leakage causing source-drain leakage and leakage between devices. Summary of the invention

[0005] The purpose of the present invention is to provide an embedded high-low voltage compatible CMOS total dose reinforcement method to solve the threshold voltage drift, leakage between devices and within the device caused by the total dose effect, thereby improving the radiation resistance of FPGA, CPLD, MCU, and SoC circuits.

[0006] In order to solve the above technical problems, the present invention provides an embedded high-low voltage compatible CMOS total dose reinforcement method, including a high-low voltage MOS device reinforcement method and a floating gate FLASH device reinforcement method; wherein,

[0007] The high and low voltage MOS device reinforcement method comprises an STI injection method, a high voltage MOS device stacked gate oxygen process method, a low voltage MOS device stacked gate oxygen process method and an active area cutoff method;

[0008] The floating gate FLASH device reinforcement method includes a tunnel oxide layer reinforcement process method and a polysilicon inter-dielectric layer processing process method.

[0009] Optionally, providing a P-type silicon substrate, and etching the P-type silicon substrate to form a plurality of isolation grooves thereon;

[0010] The total dose reinforcement is carried out by using STI injection method;

[0011] Using high-density plasma to deposit silicon oxide until the isolation groove is filled to form an isolation body;

[0012] Performing N-type and P-type ion implantation on a P-type silicon substrate to form a deep high-voltage N-well and a high-voltage P-well, wherein a floating gate FLASH device and a high-voltage pMOS device are located in the deep high-voltage N-well, and a high-voltage nMOS device is located in the high-voltage P-well;

[0013] Performing a high-voltage MOS device stacked gate oxide process: forming a high-voltage MOS tube oxide layer on the surface of a deep high-voltage N-well and a high-voltage P-well; removing the high-voltage MOS tube oxide layer in the floating gate FLASH device area in the deep high-voltage N-well, and growing a tunnel oxide layer using a low-temperature thermal oxidation doping N process;

[0014] A polysilicon layer is prepared on the oxide layer of the high-voltage MOS tube; N-type and P-type ion implantation is performed on the P-type silicon substrate to form a low-voltage N-type well and a low-voltage P-type well;

[0015] forming an ONO dielectric layer on the polysilicon layer,

[0016] Performing a low-voltage MOS device stacked gate oxide process: forming an IOMOS tube oxide layer on a low-voltage N-type well and a low-voltage P-type well; using an etching process to remove the IOMOS tube oxide layer on the surface of the low-voltage core MOS tube, and then using a low-temperature wet oxidation process and an N-doping process to form a low-voltage core MOS tube oxide layer;

[0017] After forming the oxide layer of the low-voltage core MOS tube, the active area cutoff method is used to strengthen the total dose of the high and low voltage MOS devices;

[0018] Prepare control gate polysilicon on the ONO dielectric layer, and prepare logic gate polysilicon on the IOMOS tube oxide layer;

[0019] By P-type or N-type ion implantation, lightly doped regions and heavily doped regions are formed in high and low voltage MOS devices and floating gate FLASH devices; a layer of oxide or nitride is deposited on the gate, and sidewalls are formed on both sides of the gate of the high and low voltage MOS devices and floating gate FLASH devices by anisotropic etching;

[0020] The gate interconnection of high-voltage MOS tubes is realized through gate photolithography and etching process, and metal silicide is formed on the heavily doped area and the polysilicon on the top of the gate by metal salicide process;

[0021] A layer of borophosphide silicon glass is formed by chemical vapor deposition to locate the position of the first metal connection port, and a through hole is formed by corrosion; a layer of Ti is formed by chemical vapor deposition, and the first metal connection layer is formed after the metal in the excess area is corroded.

[0022] Optionally, total dose reinforcement using STI injection method includes the following steps:

[0023] Determine the ion implantation area, implantation depth and implantation dose according to the sidewall and bottom structure and size of the isolation trench in the high-voltage P-well and the low-voltage P-well;

[0024] P-type ion implantation is performed on the sidewalls and bottom of the isolation trenches in the high-pressure P-well and low-pressure P-well, with an implantation dose of 5E13atom / cm 2 ~2E14atom / cm 2 , side wall injection dose 1E13atom / cm 2 ~1E14atom / cm 2 ;

[0025] The annealing treatment is carried out in a NO or N2O atmosphere at a temperature of 800°C to 1200°C.

[0026] Optionally, the total dose reinforcement of high and low voltage MOS devices using the active area cutoff method includes the following steps:

[0027] Determine the ion implantation area, implantation depth and implantation dose according to the gate width and insulator size structural parameters of high and low voltage MOS devices;

[0028] Performing P-type ion or inert gas ion implantation in the overlapping region between the gate and the edge of the isolation groove to form a cut-off region;

[0029] An annealing treatment is performed at a temperature of 800°C to 1200°C.

[0030] Optionally, the method of etching the P-type silicon substrate to form a plurality of isolators thereon includes:

[0031] forming a mask layer having a plurality of openings on the P-type silicon substrate;

[0032] The P-type silicon substrate is etched along the opening of the mask layer to form a plurality of discrete fins on the P-type silicon substrate, with isolation grooves between adjacent fins; wherein the position and size of the opening of the mask layer are the position and size of the isolation grooves formed by etching.

[0033] Optionally, the deep high-voltage N-well surrounds at least one of the isolation bodies, and the deep high-voltage N-well and the high-voltage P-well are separated by the isolation body.

[0034] Optionally, the tunnel oxide layer reinforcement process is: the tunnel oxide layer is formed by a low temperature thermal oxidation N doping process, and its thickness is The growth temperature is 700°C to 850°C, and N2O or NO is used for annealing.

[0035] Optionally, the process temperature for preparing the polysilicon layer is 500° C. to 700° C., and the thickness of the polysilicon layer is

[0036] Optionally, the low-voltage N-well and the low-voltage P-well are separated by an isolation body, and the low-voltage N-well and the high-voltage P-well are separated by another isolation body.

[0037] Optionally, the ONO dielectric layer is composed of bottom oxide, silicon nitride, and top oxide from bottom to top; wherein the thickness of the bottom oxide is The thickness of the silicon nitride is The thickness of the top oxide is The processing technology of the inter-polysilicon dielectric layer is as follows: both the bottom oxide and the top oxide are formed by high-temperature deposition of oxide layers, and annealed with N2O or NO, and the annealing temperature ranges from 700°C to 900°C. The HTO film is prepared by LVCVD equipment, and the preparation temperature is 700 to 800°C, and the preparation gas is N2O and SiH4.

[0038] In the embedded high-low voltage compatible CMOS total dose reinforcement method provided by the present invention, STI injection is used to increase the P-type impurity concentration on the side and bottom surface of STI, thereby effectively increasing the inversion threshold of the side and bottom surface of STI, suppressing the leakage channel, and realizing STI total dose reinforcement; using the high-voltage MOS device stacked gate oxide process and the low-voltage MOS device stacked gate oxide process, the defects and traps in the oxide layer are reduced, and the total dose reinforcement of the high and low voltage MOS devices is realized; using the active area cutoff method to block the leakage channel between the source and drain inside the device, the total dose reinforcement of the high and low voltage MOS devices is realized; using the low-temperature thermal oxidation N-doped process to improve the quality of the thin gate oxide layer, the total dose radiation ionization reinforcement of the floating gate FLASH device and the low voltage MOS device is realized; using the HTO process to reduce the defects and traps in the oxide layer, the polysilicon inter-dielectric layer reinforcement of the floating gate FLASH device is realized. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] Figure 1 A cross-sectional view and a top view after the isolation trench in the P-type substrate is etched for the semiconductor process;

[0040] Figure 2 The cross-sectional view and top view after the P-type ion implantation in the isolation trench is completed for the semiconductor process;

[0041] Figure 3 The cross-sectional view and top view after the semiconductor process completes the isolation trench filling and high-voltage MOS double gate oxide;

[0042] Figure 4 Cross-sectional and top views of semiconductor processes after polysilicon deposition is completed;

[0043] Figure 5 A cross-sectional view and a top view after a low-voltage N-well and a low-voltage P-well are completed for a semiconductor process;

[0044] Figure 6 The cross-sectional view and top view after the ONO layer is completed for the semiconductor process;

[0045] Figure 7 The cross-sectional view and top view of the low-voltage core MOS tube oxide layer after the semiconductor process is completed;

[0046] Figure 8 Cross-sectional and top-down views of semiconductor processes after polysilicon deposition, sidewalls and metal nitrides are completed;

[0047] Fig. 9 Cross-sectional and top views after borophosphide silicon glass coverage for semiconductor processing;

[0048] Fig.10 Cross-sectional and top-down views of the semiconductor process after titanium deposition. DETAILED DESCRIPTION

[0049] The following is a further detailed description of an embedded high and low voltage compatible CMOS total dose reinforcement method proposed by the present invention in combination with the accompanying drawings and specific embodiments. The advantages and features of the present invention will become clearer according to the following description and claims. It should be noted that the drawings are all in a very simplified form and are not in precise proportions, and are only used to conveniently and clearly assist in explaining the purpose of the embodiments of the present invention.

[0050] like Figure 1 As shown, a mask layer having a plurality of openings is formed on a P-type silicon substrate 1, and the positions and sizes of the openings are the positions and sizes of isolation grooves to be formed subsequently; the P-type silicon substrate 1 is etched along the positions and sizes of the openings to form a plurality of discrete fins on the P-type silicon substrate 1, and isolation grooves are provided between adjacent fins.

[0051] like Figure 2 As shown, in order to achieve total dose reinforcement of eFLASH process devices, the present invention adopts STI injection method to reinforce the total dose of high and low voltage MOS devices. The specific steps of total dose reinforcement of STI injection method are as follows:

[0052] Step S1, determining the ion implantation area, implantation depth and implantation dose according to the sidewall and bottom structure and size of the isolation trench (STI) in the high-voltage P-well and the low-voltage P-well;

[0053] Step S2: P-type ion implantation is performed on the sidewalls and bottom of the isolation trench (STI) in the high-voltage P-well and low-voltage P-well. The ion implantation position is shown by the dotted line. The implantation dose at the bottom of the trench is 5E13atom / cm 2 ~2E14atom / cm 2 , side wall injection dose 1E13atom / cm 2 ~1E14atom / cm2 ; P-type ions can be boron or indium;

[0054] Step S3, performing annealing in a NO or N2O atmosphere at a temperature of 800°C to 1200°C;

[0055] like Figure 3 As shown, high-density plasma is used to deposit silicon oxide until the isolation groove is filled to form an isolation body 2, and then annealing is performed at a temperature of 800°C to 1200°C.

[0056] N-type and P-type ion implantation are performed on a P-type silicon substrate 1 to form a deep high-voltage N-well 3 and a high-voltage P-well 4, wherein the deep high-voltage N-well 3 surrounds at least one of the isolators 2, and the deep high-voltage N-well 3 and the high-voltage P-well 4 are separated by the isolator 2, wherein a floating gate FLASH device and a high-voltage pMOS device are located in the deep high-voltage N-well 3, and a high-voltage nMOS device is located in the high-voltage P-well 4.

[0057] A high temperature oxide deposition process (HTO) is used to deposit oxide to a specified thickness on the surface of the deep high voltage N well 3 and the high voltage P well 4, and the temperature range is 700°C to 800°C to form a high voltage MOS tube oxide layer 5; an etching process is used to remove the high voltage MOS tube oxide layer in the floating gate type FLASH device area in the deep high voltage N well 3, and a tunnel oxide layer 6 is grown by a low temperature thermal oxidation doping N process, and the thickness is The growth temperature is 700°C to 850°C, and N2O or NO is used for annealing; the stacked gate oxide of the high-voltage MOS device is a high-voltage MOS tube oxide layer formed by a high-temperature deposited oxide layer process (HTO) and a low-temperature thermal oxidation doped N process.

[0058] like Figure 4 As shown, the polysilicon layer 7 is prepared by an in-situ POCL3 doped polysilicon process, wherein the process temperature is 500°C to 700°C, and the thickness of the polysilicon layer 7 is

[0059] like Figure 5 As shown, N-type and P-type ion implantation is performed on a P-type silicon substrate 1 to form a low-voltage N-type well 8 and a low-voltage P-type well 9. The low-voltage N-well 8 and the low-voltage P-well 9 are separated by an isolation body 2, and the low-voltage N-well 8 and the high-voltage P-well 4 are separated by another isolation body 2.

[0060] like Figure 6 As shown, an ONO (silicon dioxide-silicon nitride-silicon dioxide) dielectric layer 10 is formed by depositing an oxide layer and silicon nitride on the polysilicon layer 7. The ONO dielectric layer 10 is composed of a bottom oxide, silicon nitride, and a top oxide from bottom to top. The thickness of the bottom oxide is The thickness of silicon nitride is The thickness of the top oxide is The bottom oxide and the top oxide are both made by HTO process and annealed by N2O or NO at a temperature range of 700°C to 900°C, wherein the HTO film is prepared by LVCVD equipment at a preparation temperature of 700 to 800°C and the preparation gases are N2O and SiH4.

[0061] like Figure 7 As shown, a low-temperature wet oxidation process and an N-doping process are used to grow an oxide layer to form an IOMOS tube oxide layer 11; an etching process is used to remove the IOMOS tube oxide layer on the surface of the low-voltage core MOS tube, and then a low-temperature wet oxidation process and an N-doping process are used to grow a low-voltage core MOS tube oxide layer 12; the IOMOS tube stacked gate oxide is formed by two low-temperature wet oxidation processes and an N-doping process.

[0062] In order to avoid the reduction of P-type impurity concentration on the surface between the isolator 2 and the P-well 1 caused by the sacrificial oxidation process before gate oxidation, the stacked gate oxide process and the polycrystalline in-situ doping high temperature process, after the logic gate oxide (i.e., after the stacked gate oxide process of the low-voltage MOS device), the active area cutoff method is used to strengthen the total dose of the high and low voltage MOS devices. The specific steps are as follows:

[0063] Step S1, determining the ion implantation area, implantation depth and implantation dose according to structural parameters such as gate width and insulator size;

[0064] Step S2, performing P-type ion or inert gas ion implantation in the overlapping region between the gate and the STI edge to form a cut-off region 13;

[0065] Step S3, performing annealing treatment at a temperature of 800°C to 1200°C.

[0066] like Figure 8 As shown, the control gate polysilicon 14 is prepared on the ONO dielectric layer 10 by ion implantation doping process, and the logic gate polysilicon 15 is prepared on the IOMOS tube oxide layer 11, wherein the process temperature is 500° C. to 700° C., and the thickness of the control gate polysilicon 14 and the logic gate polysilicon 15 are both The ion doping type is N-type, such as phosphorus, and then the doping is activated by high temperature annealing.

[0067] By P-type or N-type ion implantation, a lightly doped region 16 and a heavily doped region 18 are formed in the high and low voltage MOS devices and the floating gate FLASH devices; a layer of oxide or nitride is deposited on the gate, and sidewalls 17 are formed on both sides of the gate of the high and low voltage MOS devices and the floating gate FLASH devices by anisotropic etching.

[0068] like Fig. 9As shown, the gate interconnection of the high-voltage MOS tube is realized by gate photolithography and etching process, and a metal salicide process is used to form a metal silicide 19, such as Co, on the heavily doped region and the top polysilicon of the gate, and the annealing temperature is 450°C to 900°C;

[0069] A layer of borophosphide silicon glass 20 is deposited on the substrate after the above steps by chemical vapor deposition, the position of the first layer of metal connection port is located, and a through hole is formed by etching.

[0070] like Fig.10 As shown, a layer of Ti21 is deposited on the borophosphide silicon glass 20 by chemical vapor deposition, and the first metal connection layer is formed after the metal in the redundant area is etched.

[0071] In summary, the present invention is aimed at embedded high and low voltage compatible CMOS process devices, taking embedded floating gate FLASH (eFLASH) process devices as an example, and proposes a total dose reinforcement method including two parts: high and low voltage MOS devices and floating gate FLASH devices. The total dose reinforcement method of high and low voltage MOS devices includes STI injection method, high voltage MOS device stacked gate oxygen process method, low voltage MOS device stacked gate oxygen process method and active area cutoff method (PA); the total dose reinforcement process method of floating gate FLASH devices includes tunnel oxide layer reinforcement process method and inter-polysilicon dielectric layer (IPD) reinforcement process method.

[0072] The above description is only a description of the preferred embodiments of the present invention, and is not intended to limit the scope of the present invention. Any changes or modifications made by a person skilled in the art in the field of the present invention based on the above disclosure shall fall within the scope of protection of the claims.

Claims

1. An embedded high and low voltage compatible CMOS total dose reinforcement method, characterized in that: It includes high and low voltage MOS device reinforcement method and floating gate FLASH device reinforcement method; wherein, The high and low voltage MOS device reinforcement method comprises an STI injection method, a high voltage MOS device stacked gate oxygen process method, a low voltage MOS device stacked gate oxygen process method and an active area cutoff method; The floating gate FLASH device reinforcement method includes a tunnel oxide layer reinforcement process and a polysilicon inter-dielectric layer processing process; The embedded high and low voltage compatible CMOS total dose reinforcement method specifically includes: Providing a P-type silicon substrate, and etching the P-type silicon substrate to form a plurality of isolation grooves thereon; The total dose reinforcement is carried out by using STI injection method; Using high-density plasma to deposit silicon oxide until the isolation groove is filled to form an isolation body; Performing N-type and P-type ion implantation on a P-type silicon substrate to form a deep high-voltage N-well and a high-voltage P-well, wherein a floating gate FLASH device and a high-voltage pMOS device are located in the deep high-voltage N-well, and a high-voltage nMOS device is located in the high-voltage P-well; Performing a high-voltage MOS device stacked gate oxide process: forming a high-voltage MOS tube oxide layer on the surface of a deep high-voltage N-well and a high-voltage P-well; removing the high-voltage MOS tube oxide layer in the floating gate FLASH device area in the deep high-voltage N-well, and growing a tunnel oxide layer using a low-temperature thermal oxidation doping N process; A polysilicon layer is prepared on the oxide layer of the high-voltage MOS tube; N-type and P-type ion implantation is performed on the P-type silicon substrate to form a low-voltage N-type well and a low-voltage P-type well; forming an ONO dielectric layer on the polysilicon layer, Performing a low-voltage MOS device stacked gate oxide process: forming an IO MOS tube oxide layer on a low-voltage N-type well and a low-voltage P-type well; using an etching process to remove the IO MOS tube oxide layer on the surface of the low-voltage core MOS tube, and then using a low-temperature wet oxidation process and an N-doping process to form a low-voltage core MOS tube oxide layer; After forming the oxide layer of the low-voltage core MOS tube, the active area cutoff method is used to strengthen the total dose of the high and low voltage MOS devices; Prepare control gate polysilicon on the ONO dielectric layer, and prepare logic gate polysilicon on the IO MOS tube oxide layer; By P-type or N-type ion implantation, lightly doped regions and heavily doped regions are formed in high and low voltage MOS devices and floating gate FLASH devices; a layer of oxide or nitride is deposited on the gate, and sidewalls are formed on both sides of the gate of the high and low voltage MOS devices and floating gate FLASH devices by anisotropic etching; The gate interconnection of high-voltage MOS tubes is realized through gate photolithography and etching process, and metal silicide is formed on the heavily doped area and the polysilicon on the top of the gate by metal salicide process; A layer of borophosphide silicon glass is formed by chemical vapor deposition to locate the position of the first metal connection port, and a through hole is formed by corrosion; a layer of Ti is formed by chemical vapor deposition, and the first metal connection layer is formed after the metal in the excess area is corroded.

2. The embedded high and low voltage compatible CMOS total dose reinforcement method according to claim 1, characterized in that: The total dose reinforcement using STI injection method includes the following steps: Determine the ion implantation area, implantation depth and implantation dose according to the sidewall and bottom structure and size of the isolation trench in the high-voltage P-well and the low-voltage P-well; P-type ion implantation is performed on the sidewalls and bottom of the isolation trenches in the high-pressure P-well and low-pressure P-well, with an implantation dose of 5E13atom / cm 2 ~2E14 atoms / cm 2 , side wall injection dose 1E13 atom / cm 2 ~1E14 atoms / cm 2 ; The annealing treatment is carried out in a NO or N2O atmosphere at a temperature of 800°C to 1200°C.

3. The embedded high and low voltage compatible CMOS total dose reinforcement method according to claim 1, characterized in that: The total dose hardening of high and low voltage MOS devices using the active area cutoff method includes the following steps: Determine the ion implantation area, implantation depth and implantation dose according to the gate width and insulator size structural parameters of high and low voltage MOS devices; Performing P-type ion or inert gas ion implantation in the overlapping region between the gate and the edge of the isolation groove to form a cut-off region; An annealing treatment is performed at a temperature of 800°C to 1200°C.

4. The embedded high and low voltage compatible CMOS total dose reinforcement method according to claim 1, characterized in that: The method of etching the P-type silicon substrate to form a plurality of isolators thereon comprises: forming a mask layer having a plurality of openings on the P-type silicon substrate; The P-type silicon substrate is etched along the opening of the mask layer to form a plurality of discrete fins on the P-type silicon substrate, with isolation grooves between adjacent fins; wherein the position and size of the opening of the mask layer are the position and size of the isolation grooves formed by etching.

5. The embedded high and low voltage compatible CMOS total dose reinforcement method according to claim 1, characterized in that: The deep high-voltage N-well surrounds at least one of the isolation bodies, and the deep high-voltage N-well and the high-voltage P-well are separated by the isolation body.

6. The embedded high and low voltage compatible CMOS total dose reinforcement method according to claim 1, characterized in that: The tunnel oxide layer reinforcement process is as follows: the tunnel oxide layer is formed by a low-temperature thermal oxidation N-doping process, the thickness of the tunnel oxide layer is 85Å~105Å, the growth temperature is 700℃~850℃, and N2O or NO is used for annealing.

7. The embedded high and low voltage compatible CMOS total dose reinforcement method according to claim 1, characterized in that: The process temperature for preparing the polysilicon layer is 500°C to 700°C, and the thickness of the polysilicon layer is 1000Å to 3000Å.

8. The embedded high and low voltage compatible CMOS total dose reinforcement method according to claim 1, characterized in that: The low-voltage N-well and the low-voltage P-well are separated by an isolation body, and the low-voltage N-well and the high-voltage P-well are separated by another isolation body.

9. The embedded high and low voltage compatible CMOS total dose reinforcement method according to claim 1, characterized in that: The ONO dielectric layer is composed of bottom oxide, silicon nitride and top oxide from bottom to top; the thickness of the bottom oxide is 40Å~100Å, the thickness of the silicon nitride is 40Å~100Å, and the thickness of the top oxide is 40Å~100Å; the processing method of the dielectric layer between polysilicon is: the bottom oxide and the top oxide are both deposited by high-temperature oxide layer process, and annealed by N2O or NO, and the annealing temperature range is 700℃~900℃, wherein the HTO film is prepared by LVCVD equipment, the preparation temperature is 700~800℃, and the preparation gas is N2O and SiH4.

Citation Information

Patent Citations

  • Semiconductor device and method of manufacturing the same

    JP2015041626A

  • Method for manufacturing eeprom equipment

    KR1020000014093A

  • Semiconductor device and its manufacture method