A method for synthesizing ultrapure copper nanowires

By using a polyol system and a weak reducing agent in the synthesis of copper nanowires under normal pressure, the problem of using toxic hydrazine hydrate and high-pressure conditions in the existing technology is solved, and efficient and simple synthesis and purification of copper nanowires are achieved, which is suitable for Industrial production.

CN114603130BActive Publication Date: 2024-10-25NUOVO FILM SUZHOU CHINA INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210253227.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-03-15
Publication Date
2024-10-25
Estimated Expiration
2042-03-15

AI Technical Summary

Technical Problem

The existing copper nanowire synthesis method uses toxic hydrazine hydrate as a reducing agent in a closed reactor, and it is difficult to achieve large-scale industrial production, and the purification process requires the introduction of organic solvents.

Method used

Using polyol as the solvent system, copper salts, organic protective agents and organic chlorine-containing halides were mixed with weak reducing agents under normal pressure. Through heating and centrifugation, copper nanowires with a high aspect ratio were successfully synthesized, avoiding the need for Simple purification is achieved using toxic hydrazine hydrate and high-pressure conditions, along with centrifugation.

Benefits of technology

It has achieved efficient synthesis of copper nanowires with high aspect ratio and low by-products under normal pressure. The process is simple, suitable for industrial production, and avoids the use of toxic raw materials and high-pressure conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114603130B_ABST
    Figure CN114603130B_ABST
Patent Text Reader

Abstract

The present invention discloses a method for synthesizing ultrapure copper nanowires, comprising the following steps: S1. mixing copper salt, organic protective agent, organic chlorine-containing halide and polyol, stirring until completely dissolved; then adding a weak reducing agent to obtain a mixed solution; S2. introducing nitrogen or inert gas into the mixed solution, heating to discharge water and oxygen therein, and then stopping the introduction of nitrogen; continuing to heat the mixed solution to 160°C to 190°C, and keeping the temperature for 2 to 10 hours; S3. centrifuging the solution obtained in step S2, washing and drying the precipitate, and then obtaining the copper nanowires. The present invention also provides ultrapure copper nanowires prepared by the method. The synthesis method of the present invention has a simple process, can react under normal pressure conditions, has a high product yield, does not require the introduction of other organic solvents during the purification process, and is easy for commercial production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of nanomaterials, and in particular to a method for synthesizing ultrapure copper nanowires. Background Art

[0002] In recent years, one-dimensional nanomaterials have attracted extensive attention in the field of nanoscience due to their excellent optical, electrical, thermal and mechanical properties. In terms of microstructure, these unique properties depend largely on the motion form of electrons; in the nanoscale range, the motion form of electrons directly depends on the type of metal and its specific structure and morphology. At present, the controllable synthesis of one-dimensional nanomaterials is mainly the nanostructure of elements such as gold (Au), silver (Ag), platinum (Pt) and copper (Cu). Among them, the conductivity of copper nanowires (CuNWs) is second only to that of silver nanowires, with a conductivity difference of only 6%. However, in nature, copper reserves are abundant, about 1000 times that of silver, and the price is only one-seventieth of that of silver. Therefore, it has gradually become the best choice for precious metal nanomaterials such as Au and Ag. CuNWs with high aspect ratio have good ductility and conductivity, and have broad application prospects in many fields such as touch screens, organic light-emitting diodes, solar cells, lithium-ion batteries, smart windows and implantable medical devices.

[0003] At present, the method for preparing copper nanowires by liquid phase reduction is mainly to use hydrazine hydrate as a reducing agent or to form a stable emulsion of copper salt and alkane fatty amine in a mixed solvent to synthesize copper nanowires in an aqueous phase or an oil amine system. Although these methods have the advantages of controllable morphology and adjustable aspect ratio, these reactions are usually prepared in a closed reactor. At the same time, hydrazine hydrate has certain toxicity and is harmful to the environment, so it is not suitable for large-scale commercial production. For example, Chinese patent CN107103945A discloses a method of synthesizing copper nanowires with a high aspect ratio using an electric pressure cooker as a reaction vessel, but this method uses a high-temperature pressure vessel and is difficult to achieve large-scale industrial mass production. Chinese patent CN103212721B discloses a method of synthesizing copper nanowires with a high aspect ratio in an oil amine system, but the method needs to introduce n-hexane or acetone to remove residual organic matter in the synthesis process during the purification process. Summary of the invention

[0004] The technical problem to be solved by the present invention is to provide a method for synthesizing ultrapure copper nanowires. The synthesis method has a simple process, can react under normal pressure conditions, has a high product yield, does not require the introduction of other organic solvents during the purification process, and is easy for commercial production.

[0005] In order to solve the above technical problems, the present invention provides the following technical solutions:

[0006] In a first aspect, the present invention provides a method for synthesizing ultrapure copper nanowires, comprising the following steps:

[0007] S1. Mix the copper salt, organic protective agent, organic chlorine-containing halide and polyol, and stir until completely dissolved; then add a weak reducing agent to obtain a mixed solution;

[0008] S2. Nitrogen or an inert gas is introduced into the mixed solution, heated to discharge water and oxygen therein, and then the introduction of nitrogen is stopped; the mixed solution is heated to 160°C to 190°C and kept warm for 2 to 10 hours;

[0009] S3. The solution obtained in step S2 is centrifuged, and the precipitate is washed and dried to obtain the copper nanowires.

[0010] Furthermore, the copper salt is selected from one or more of copper nitrate, copper carboxylate, copper sulfate, copper acetylacetonate, copper acetate, and copper chloride.

[0011] Furthermore, the organic protective agent is selected from one or more of polyvinyl pyrrolidone and polyvinyl alcohol.

[0012] Furthermore, the organic chlorine-containing halide is selected from one or more of hexadecyltrimethylammonium chloride, octadecyltrimethylammonium chloride, tetrabutylammonium chloride, and tetrapropylammonium chloride.

[0013] Furthermore, the polyol is ethylene glycol, propylene glycol or glycerol.

[0014] Furthermore, the weak reducing agent is selected from one or more of glucose, sorbitol, glycerol, tripropylene glycol, triethylene glycol, propylene glycol, phenylethyl alcohol, diethylene glycol, ascorbic acid, sodium ascorbate, and polyphenols.

[0015] Furthermore, in the mixed solution, the molar ratio of copper ions, chloride ions and organic protective agent is 1:0.1 to 1:1 to 8.

[0016] Furthermore, in the mixed solution, the molar ratio of copper ions to weak reducing agent is 1:0.1-0.5.

[0017] In a second aspect, the present invention also provides ultrapure copper nanowires prepared by the method.

[0018] Compared with the prior art, the present invention has the following beneficial effects:

[0019] 1. The present invention uses polyol as a solvent system and introduces an environmentally friendly weak reducing agent to successfully synthesize copper nanowires with a high aspect ratio and low by-products under normal pressure. Compared with the existing synthesis method of copper nanowires, the present invention does not require the use of toxic hydrazine hydrate as a reducing agent, nor does it require high-pressure reaction conditions. At the same time, the prepared copper nanowires have less particulate matter and low by-product content.

[0020] 2. The preparation method of the copper nanowires of the present invention has a simple process and a simple subsequent purification treatment. It does not require the introduction of an organic solvent and only requires centrifugation, and is suitable for industrial production. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 The scanning electron microscope images of the copper nanowires prepared in Example 1 at different magnifications. DETAILED DESCRIPTION

[0022] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.

[0023] As described in the background art, the method for preparing copper nanowires by liquid phase reduction in the prior art is mainly to use hydrazine hydrate as a reducing agent or to form a stable emulsion of copper salt and alkane fatty amine in a mixed solvent in an aqueous phase or an oil amine system to synthesize copper nanowires. However, these reactions are usually prepared in a closed reactor, and hydrazine hydrate has certain toxicity and is harmful to the environment, so it is not suitable for large-scale commercial production.

[0024] In order to solve this technical problem, the present invention provides a method for synthesizing ultrapure copper nanowires, comprising the following steps:

[0025] S1. Mix the copper salt, organic protective agent, organic chlorine-containing halide and polyol, and stir until completely dissolved; then add a weak reducing agent to obtain a mixed solution;

[0026] S2. Nitrogen or an inert gas is introduced into the mixed solution, heated to discharge water and oxygen therein, and then the introduction of nitrogen is stopped; the mixed solution is heated to 160°C to 190°C and kept warm for 2 to 10 hours;

[0027] S3. The solution obtained in step S2 is centrifuged, and the precipitate is washed and dried to obtain the copper nanowires.

[0028] In the present invention, polyol is used as the solvent system, and copper nanowires can be obtained by reaction at normal pressure. Compared with the prior art, the reaction does not need to be carried out under high pressure, and no toxic hydrazine hydrate needs to be used as a reducing agent. At the same time, the prepared copper nanowires contain less particulate matter and low by-product content.

[0029] In the present invention, the copper salt may be a copper salt commonly used in the art, including but not limited to one or more selected from copper nitrate, copper carboxylate, copper sulfate, copper acetylacetonate, copper acetate, copper chloride and other copper salt compounds with organic silver ions.

[0030] In the present invention, the organic protective agent plays the role of a capping agent in the reaction. Preferably, the organic protective agent can be selected from one or more of polyvinyl pyrrolidone and polyvinyl alcohol.

[0031] In the present invention, the organic chlorine-containing halide will form copper chloride with the copper salt, thereby promoting the growth of copper nanowires. The generated copper chloride is equivalent to crystals, which will affect the diameter of the copper nanowires. Preferably, the organic chlorine-containing halide is selected from one or more of hexadecyltrimethylammonium chloride, octadecyltrimethylammonium chloride, tetrabutylammonium chloride, and tetrapropylammonium chloride.

[0032] In the present invention, polyols are used as solvents because they have certain reducing properties. For example, ethylene glycol can generate glyoxal under heating conditions. The aldehyde group has reducing properties and can promote the reduction of divalent copper ions into elemental copper. The polyols include but are not limited to ethylene glycol, propylene glycol, and glycerol.

[0033] In the present invention, the weak reducing agent is preferably an environmentally friendly reducing agent, including but not limited to one or more of glucose, sorbitol, glycerol, tripropylene glycol, triethylene glycol, propylene glycol, phenylethyl alcohol, diethylene glycol, ascorbic acid, sodium ascorbate, and polyphenols. In addition, the type of reducing agent has a great influence on the length and diameter of the prepared copper nanowires. Therefore, by controlling the type of reducing agent, the aspect ratio of the copper nanowires can be regulated.

[0034] In the present invention, in the mixed solution, the molar ratio of copper ions, chloride ions and organic protective agent is preferably 1:0.1-1:1-8.

[0035] In the present invention, in the mixed solution, the molar ratio of copper ions to weak reducing agent is preferably 1:0.1-0.5.

[0036] In the present invention, the heating temperature of the mixed solution is preferably 180° C., and the insulation time is preferably 8 h.

[0037] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments so that those skilled in the art can better understand the present invention and implement it, but the embodiments are not intended to limit the present invention.

[0038] Unless otherwise specified, the experimental methods used in the following examples are all conventional methods, and the materials, reagents, etc. used are all available from commercial sources unless otherwise specified.

[0039] Example 1

[0040] This embodiment provides a method for synthesizing copper nanowires, which specifically includes the following steps:

[0041] 1) 8 g of polyvinyl pyrrolidone and 1 g of hexadecyl trimethyl ammonium chloride were dissolved in a three-necked round-bottom container filled with 500 ml of ethylene glycol, and then 2 ml of phenylethanol was added;

[0042] 2) nitrogen was introduced into the mixed solution, and the solution was heated to 170°C and maintained at this temperature for 5 minutes to fully remove water and oxygen, and then the nitrogen was turned off;

[0043] 3) Continue heating the mixed solution to 180°C and keep it at this temperature for 8 hours;

[0044] 4) Stop heating, wait for the solution temperature to cool to room temperature, dilute the original solution with water in a ratio of 1:1, process it through a centrifuge at 3600r / min for 30min, pour off the supernatant, and finally wash and dry the obtained precipitate to obtain copper nanowires with a diameter of 60nm and a length of 60um.

[0045] See also Figure 1 In this embodiment, ethylene glycol is used as the solvent system to successfully prepare copper nanowires with high aspect ratio and low by-products, and the nanowires have uniform morphology and good dispersibility.

[0046] Example 2

[0047] This embodiment provides a method for synthesizing copper nanowires, which is different from Embodiment 1 only in that diethylene glycol is used as a reducing agent.

[0048] Example 3

[0049] This embodiment provides a method for synthesizing copper nanowires, which is different from Embodiment 1 only in that triethylene glycol is used as a reducing agent.

[0050] Example 4

[0051] This embodiment provides a method for synthesizing copper nanowires, which is different from Embodiment 1 only in that glucose is used as a reducing agent.

[0052] Example 5

[0053] This embodiment provides a method for synthesizing copper nanowires, which is different from Embodiment 1 only in that sodium ascorbate is used as a reducing agent.

[0054] Table 1 shows the wire length and wire diameter of the copper nanowires prepared in Examples 1-5.

[0055] Table 1

[0056] reducing agent Line length Wire diameter Example 1 Phenylethyl alcohol 60μm 60nm Example 2 Diethylene glycol 40μm 70nm Example 3 Triethylene glycol 50μm 55nm Example 4 glucose 10μm 150nm Example 5 Sodium Ascorbate 20μm 200nm

[0057] It can be seen from Table 1 that when different reducing agents are used, the prepared copper nanowires have different wire lengths and wire diameters. Therefore, the wire length and wire diameter of the copper nanowire can be controlled by controlling the type of reducing agent.

[0058] In summary, the present invention introduces an environmentally friendly reducing agent into the polyol system, and successfully synthesizes copper nanowires with a high aspect ratio and low by-products under normal pressure. Compared with the prior art, the synthesis process of the present invention does not require the use of toxic raw materials such as hydrazine hydrate, and does not need to be carried out under high pressure. The process is simple, the subsequent purification treatment is simple, and no organic solvent is required. It only needs centrifugation treatment, which is suitable for industrial production.

[0059] The above-described embodiments are only preferred embodiments for fully illustrating the present invention, and the protection scope of the present invention is not limited thereto. Equivalent substitutions or changes made by those skilled in the art based on the present invention are within the protection scope of the present invention. The protection scope of the present invention shall be subject to the claims.

Claims

1. A method for synthesizing ultrapure copper nanowires, characterized in that: The following steps are involved: S1. Mix the copper salt, organic protective agent, organic chlorine-containing halide and polyol, and stir until completely dissolved; then add a weak reducing agent to obtain a mixed solution; S2. Nitrogen or an inert gas is introduced into the mixed solution, heated to discharge water and oxygen therein, and then the introduction of nitrogen is stopped; the mixed solution is heated to 160°C to 190°C and kept warm for 2 to 10 hours; S3. The solution obtained in step S2 is centrifuged, and the precipitate is washed and dried to obtain the copper nanowires; The weak reducing agent is selected from one or more of glucose, sorbitol, glycerol, tripropylene glycol, triethylene glycol, propylene glycol, phenylethyl alcohol, diethylene glycol, ascorbic acid, sodium ascorbate, and polyphenols.

2. The method for synthesizing ultrapure copper nanowires according to claim 1, characterized in that: The copper salt is selected from one or more of copper nitrate, copper carboxylate, copper sulfate, copper acetylacetonate, copper acetate, and copper chloride.

3. The method for synthesizing ultrapure copper nanowires according to claim 1, characterized in that: The organic protective agent is selected from one or more of polyvinyl pyrrolidone and polyvinyl alcohol.

4. The method for synthesizing ultrapure copper nanowires according to claim 1, characterized in that: The organic chlorine-containing halide is selected from one or more of hexadecyltrimethylammonium chloride, octadecyltrimethylammonium chloride, tetrabutylammonium chloride and tetrapropylammonium chloride.

5. The method for synthesizing ultrapure copper nanowires according to claim 1, characterized in that: The polyol is ethylene glycol, propylene glycol or glycerol.

6. The method for synthesizing ultrapure copper nanowires according to claim 1, characterized in that: In the mixed solution, the molar ratio of copper ions, chloride ions and organic protective agent is 1:0.1 to 1:1 to 8.

7. The method for synthesizing ultrapure copper nanowires according to claim 1, characterized in that: In the mixed solution, the molar ratio of copper ions to weak reducing agent is 1:0.1-0.

5.

8. The copper nanowire prepared according to the method according to any one of claims 1 to 7.