Platinum single atom catalyst, preparation method and application
By loading a platinum single-atom catalyst on a boron-doped or boron-nitrogen-doped substrate, the problem of lead dioxide catalyst contamination in low-voltage electrolytic ozone generators is solved, achieving efficient and environmentally friendly ozone evolution performance and high utilization of platinum precious metals. efficiency, reducing production costs.
Patent Information
- Application Number
- CN202210069902.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-01-21
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2042-01-21
AI Technical Summary
The lead dioxide catalyst used in existing low-voltage electrolytic ozone generators can cause toxic lead ion pollution during the preparation and use process, hindering the commercial promotion and application of this technology. Platinum materials are expensive and difficult to replace.
A platinum single-atom catalyst is supported on a boron-doped or boron-nitrogen-doped substrate, and the platinum single-atom catalyst is prepared through pretreatment, reducing agent treatment and calcination under inert gas protection, which improves the utilization rate and catalytic activity of platinum and reduces the The cost of using precious metals.
Efficient ozone evolution performance is achieved. The environmental friendliness and catalytic performance of the platinum single-atom catalyst are superior to commercial lead dioxide, reducing the amount of platinum used, lowering production costs, and improving ozone evolution efficiency and stability.
Smart Images

Figure CN114606515B_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to the technical field of electrochemical catalysts, and in particular to a platinum single atom catalyst, a preparation method and an application thereof. Background Art
[0002] As a gas disinfectant, ozone has good diffusion, no dead angle, and uniform concentration distribution. The oxides produced during the disinfection process are non-toxic, odorless, and biodegradable substances. The residual ozone can also be quickly decomposed into oxygen, and will not cause secondary pollution. It is a "clean disinfectant". Ozone has a significant inactivation effect on almost all bacteria, viruses, fungi, protozoa, and oocysts. In addition, ozone can oxidize various odorous inorganic or organic substances and remove their odors. It can also be decolorized in wastewater treatment to remove phenols, cyanide and other substances and inorganic metal ions in wastewater. Its application in the fields of advanced oxidation treatment of wastewater, deep purification of drinking water, environmental protection, food processing, medical care, and fruit and vegetable preservation has become more and more extensive.
[0003] At present, the commonly used methods for preparing ozone on the market are mainly corona discharge method and solid polymer membrane (PEM membrane) electrode low-voltage electrolysis method. Among them, the principle of producing ozone by corona discharge method is to generate corona through alternating high-voltage electric field, convert oxygen molecules into oxygen atoms and then combine with oxygen molecules to form ozone molecules; the principle of producing ozone by low-voltage electrolysis method is to use low-voltage direct current to conduct the positive and negative electrodes of solid membrane electrodes to electrolyze deionized water, and water is separated into hydrogen and oxygen molecules in the form of proton exchange at the special anode solution interface. Among them, hydrogen molecules are directly discharged from the cathode solution interface, and oxygen molecules obtain energy at the anode interface due to the electron excitation generated by the high-density current, and polymerize into ozone.
[0004] Compared with the corona discharge method, the low-voltage electrode method for preparing ozone has the advantages of high ozone gas concentration, no carcinogens such as nitrogen oxides, low preparation cost, long membrane electrode service life, and simple equipment installation and maintenance. It has become one of the most competitive ozone preparation methods in the market.
[0005] The low-voltage electrolysis technology of solid polymer membrane (PEM membrane) electrode requires that the anode catalyst material has good electrocatalytic activity and corrosion resistance for ozone precipitation. Graphite, glassy carbon, and platinum materials are anode materials used in early electrochemical synthesis of ozone technology research, but graphite and glassy carbon are easily corroded and consumed during use, and platinum materials are expensive. Low-voltage electrolytic ozone generator products on the current market usually use lead dioxide materials with high electrocatalytic activity, good corrosion resistance, and relatively low prices as the anode catalyst of the membrane electrode. However, as an anode catalyst, lead dioxide cannot actually avoid secondary pollution to the environment caused by toxic lead ions, whether in the preparation of lead dioxide raw materials, the processing of lead dioxide membranes, or in the electrochemical synthesis of ozone, which will hinder the commercial promotion and practical application of PEM membrane electrode low-voltage electrolytic ozone generator products. Therefore, it is urgent to develop cheap, high-performance ozone precipitation anode catalyst electrodes to meet actual use needs. Summary of the invention
[0006] In response to the above technical problems, the present disclosure provides a platinum single atom catalyst, a preparation method and an application, in order to at least partially solve the above technical problems.
[0007] In order to solve the above technical problems, the technical solutions disclosed in the present invention are as follows:
[0008] A platinum single atom catalyst comprising:
[0009] A boron-doped or boron-nitrogen-doped substrate, and a platinum atom catalyst supported on the substrate in a single-atom state, wherein the substrate comprises at least one of graphene, conductive carbon black, acetylene black, graphite, multi-walled carbon nanotubes and nano-carbon fibers, and the mass percentage of platinum element in the substrate is in the range of 0.01 to 3.5%.
[0010] The present disclosure also provides an application of the above-mentioned platinum single-atom catalyst in ozone evolution reaction.
[0011] The present disclosure also provides a method for preparing the above-mentioned platinum single atom catalyst, comprising:
[0012] pre-treating the substrate to obtain a doped substrate;
[0013] The doped substrate is brought into contact with a platinum source and treated with a reducing agent to obtain a platinum-containing precursor;
[0014] The precursor is calcined under the protection of an inert gas to obtain a platinum single atom catalyst.
[0015] In one embodiment, the preprocessing includes:
[0016] The substrate is treated with a doping agent,
[0017] Alternatively, after treating the substrate with the acidifying agent, the substrate is treated with the doping agent.
[0018] In one embodiment, the doping agent includes at least one of the following: boric acid, melamine, urea;
[0019] The acidifying agent includes at least one of the following: nitric acid, sulfuric acid, perchloric acid, and boric acid.
[0020] In one embodiment, the platinum source includes any one of the following:
[0021] H2PtCl6·6H2O, PtCl4, K2PtCl6, Pt(acac)2.
[0022] In one embodiment, the concentration range of platinum ions in the platinum source includes: 0.01-0.5 mol / L.
[0023] In one embodiment, the reducing agent includes any one of the following: sodium borohydride or formaldehyde.
[0024] In one embodiment, the reaction temperature range of the doped substrate and the platinum source is 10 to 80° C.;
[0025] The time range of the above contact reaction includes: 4 to 48 hours.
[0026] In one embodiment, the calcination temperature range includes: 500-1000°C;
[0027] The above calcination heating rate range includes: 5 to 10°C / min;
[0028] The above calcination and heat preservation time range includes: 1 to 12 hours.
[0029] It can be seen from the above technical solutions that the platinum single atom catalyst, preparation method and application provided by the present disclosure have at least one of the following beneficial effects:
[0030] (1) In the embodiments of the present disclosure, single platinum atoms are loaded on a boron-doped or boron-nitrogen-doped substrate to obtain a platinum single atom catalyst with a high loading rate. The platinum single atom catalyst has the advantages of being environmentally friendly and having a catalytic performance better than commercial lead dioxide.
[0031] (2) In the embodiments of the present disclosure, single platinum atoms are used as catalysts, which reduces the amount of platinum precious metal used, improves the utilization rate of platinum precious metal as a catalyst, and reduces the cost of using precious metal platinum.
[0032] (3) In the embodiments of the present disclosure, a platinum single atom catalyst is used for the ozone evolution reaction. While achieving a higher ozone evolution efficiency, the platinum single atom catalyst also has higher catalytic activity and stability.
[0033] (4) The preparation method of the platinum single atom catalyst provided in the embodiments of the present disclosure is simple. A boron-doped or boron-nitrogen-doped substrate is contacted with a platinum source. A platinum single atom precursor can be obtained after reduction with a reducing agent. After calcination under the protection of an inert gas, a platinum single atom catalyst with high catalytic activity can be obtained. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Figure 1 is a high-angle annular dark field-scanning transmission electron microscope image of the platinum single atom catalyst synthesized in Example 1 of the present disclosure;
[0035] Figure 2 is a transmission electron microscope image of the platinum single atom catalyst synthesized in Example 2 of the present disclosure;
[0036] Figure 3 This is a performance comparison chart of the platinum single atom catalyst in Example 1 of the present disclosure and commercial lead dioxide applied to ozone evolution. DETAILED DESCRIPTION
[0037] In order to make the objectives, technical solutions and advantages of the present disclosure more clearly understood, the present disclosure is further described in detail below in conjunction with embodiments and with reference to the accompanying drawings.
[0038] According to an embodiment of the present disclosure, a platinum single atom catalyst includes: a boron-doped or boron-nitrogen-doped substrate, and a platinum atom catalyst supported on the substrate in a single atom state.
[0039] According to an embodiment of the present disclosure, a mass ratio of the doping amount of boron to nitrogen in a boron-doped or boron-nitrogen-doped substrate includes 1:3.
[0040] According to an embodiment of the present disclosure, the substrate includes at least one of graphene, conductive carbon black, acetylene black, graphite, multi-walled carbon nanotubes and nano-carbon fibers, wherein the thickness of the graphene is 1 to 3 layers; the particle size of the conductive carbon black, acetylene black, and graphite is 50 to 200 nm; the diameter of the nano-carbon fiber is 100 to 200 nm; and the diameter of the multi-walled carbon nanotube is 5 to 30 nm.
[0041] According to an embodiment of the present disclosure, the mass percentage of platinum element in the substrate is in the range of 0.01 to 3.5%, wherein the range can be selected as 0.01%, 0.1%, 0.5%, 1.0%, 1.5%, 2.0%, 2.5%, 3.0%, 3.5%.
[0042] According to the embodiments of the present disclosure, the mass percentage of platinum element in the substrate is in the range of 0.01 to 3.5%, and platinum exists in the form of single atoms. The platinum element will not form platinum nanoparticles and agglomerate, thereby ensuring the formation of platinum single atom catalysts.
[0043] According to an embodiment of the present disclosure, a platinum single atom catalyst can be applied to an ozone evolution reaction.
[0044] According to an embodiment of the present disclosure, a method for preparing a platinum single-atom catalyst comprises: pretreating a substrate to obtain a doped substrate; contacting the doped substrate with a platinum source and obtaining a platinum-containing precursor after treatment with a reducing agent; and calcining the precursor under the protection of an inert gas to obtain a platinum single-atom catalyst.
[0045] According to an embodiment of the present disclosure, the pretreatment includes: treating the substrate with a doping agent, or treating the substrate with a doping agent after treating the substrate with an acidifying agent.
[0046] According to an embodiment of the present disclosure, the doping agent includes at least one of the following: boric acid, melamine, urea; the acidifying agent includes at least one of the following: nitric acid, sulfuric acid, perchloric acid, boric acid.
[0047] Through the embodiments of the present disclosure, acid treatment of the substrate material can increase the oxygen-containing groups in the substrate material, thereby increasing the loading of single platinum atoms on the substrate; boron doping or boron-nitrogen doping of the acid-treated substrate material can further increase the active sites of the substrate material, facilitate the subsequent attachment of platinum atoms, and increase the loading amount of platinum atoms.
[0048] According to an embodiment of the present disclosure, the platinum source includes any one of the following: H2PtCl6·6H2O, PtCl4, K2PtCl6, Pt(acac)2.
[0049] According to an embodiment of the present disclosure, the concentration range of platinum ions in the platinum source includes: 0.01 to 0.5 mol / L, wherein the concentration of platinum ions can be selected as 0.01, 0.05, 0.1, 0.15, 0.2, 0.25, 0.3, 0.35, 0.4, 0.45, 0.5 mol / L, etc.
[0050] Through the embodiments of the present disclosure, the concentration range of platinum ions is controlled within 0.01 to 0.5 mol / L, which can effectively prevent the platinum ions from becoming platinum nanoparticles due to excessively high platinum ion concentration when the platinum source is mixed with the doped substrate to form a platinum-containing precursor, causing the particles to agglomerate and unable to form platinum single atoms, thereby affecting the preparation of single-atom catalysts.
[0051] According to an embodiment of the present disclosure, the reducing agent includes any one of the following: sodium borohydride or formaldehyde.
[0052] According to the embodiments of the present disclosure, platinum ions in a platinum source can be reduced to single platinum atoms using sodium borohydride or formaldehyde, thereby avoiding the formation of platinum nanoparticles.
[0053] According to the embodiments of the present disclosure, the reaction temperature range of the doped substrate in contact with the platinum source includes: 10-80°C, wherein the contact temperature can be selected as 10, 20, 30, 40, 50, 60, 70, 80°C, etc.; the time range of the contact reaction includes: 4-48h, wherein it can be selected as 4, 8, 12, 16, 18, 24, 28, 32, 36, 40, 44, 48h.
[0054] According to an embodiment of the present disclosure, the contact between the doped substrate and the platinum source can be carried out under ultrasound or stirring, wherein the ultrasound frequency is 40 KHz, the time is 10 to 30 minutes, and the stirring is 10 minutes to 180 minutes.
[0055] According to the embodiments of the present disclosure, the contact reaction time is within 4 to 48 hours, which can allow the platinum source and the doped substrate to fully react, thereby ensuring a certain platinum loading amount.
[0056] According to an embodiment of the present disclosure, the precursor is calcined under the protection of an inert gas to obtain a platinum single atom catalyst, wherein the inert gas may be nitrogen or argon.
[0057] According to the embodiments of the present disclosure, the calcination temperature range includes: 500-1000°C, wherein the calcination temperature can be selected as 500, 600, 700, 800, 900, 1000°C, etc.; the calcination heating rate range includes: 5-10°C / min, wherein the heating rate can be selected as 5, 6, 7, 8, 9, 10°C / min; the calcination insulation time range includes: 1-12h, wherein it can be selected as 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12h.
[0058] According to the embodiments of the present disclosure, a precursor containing single platinum atoms is calcined under an inert gas, so that the precursor can be transformed into a stable catalyst, and the catalytic activity of the catalyst prepared from the precursor containing single platinum atoms can be improved during application.
[0059] In order to make the purpose, technical solutions and advantages of the present disclosure clearer, the present disclosure is illustrated below in conjunction with specific embodiments. The embodiments are only used to explain the present disclosure and are not used to limit the scope of the present disclosure.
[0060] Example 1
[0061] Weigh 1g of graphene and put it into a 100mL mixed solution of concentrated sulfuric acid: concentrated nitric acid = 1:3, and ultrasonically disperse it for 30min to make the graphene evenly dispersed. Then heat and reflux at 90℃ for 2h to obtain graphene rich in oxygen-containing groups. Then, weigh 100mg of acid-treated graphene, ultrasonically disperse it in 50mL deionized water, add 0.2g boric acid and 1.0g melamine, and ultrasonically disperse it for 30min. Then seal the mixture in a 100mL high-pressure reactor and keep it at 180℃ for 12h. After natural cooling, wash the obtained sample with ultrapure water and dry it to obtain boron-nitrogen-doped graphene.
[0062] 518 mg of H2PtCl6·6H2O was added to 100 mL of deionized water and ultrasonicated in an ultrasonic machine for 15 min to obtain a uniformly dispersed platinum source.
[0063] Next, 100 mg of boron-nitrogen-doped graphene was added to 20 mL of deionized water and ultrasonicated for 10 minutes, and then stirred for 2 hours to further evenly disperse the boron-nitrogen-doped graphene in the water. After that, 1.8 mL of a platinum source prepared by H2PtCl6·6H2O was added, and after stirring at room temperature for 24 hours, 0.3 M NaBH4 was added dropwise under ice bath conditions and stirred continuously for 2 hours to convert platinum ions into platinum single atoms. After filtration, the precipitate was washed with deionized water to pH = 7, placed in a vacuum drying oven and dried at 60°C for 12 hours to obtain a precursor of boron-nitrogen-doped graphene containing platinum single atoms.
[0064] The above-mentioned precursor containing single platinum atoms is placed in a tubular furnace, and the temperature is heated to 800°C at a heating rate of 5°C / min in an argon atmosphere with a flow rate of 100 ml / min, and is kept at this temperature for 2 hours. After the heating is completed, it is taken out after natural cooling to obtain a platinum single atom catalyst.
[0065] Figure 1 This is a high-angle annular dark field-scanning transmission electron microscopy (HAADF-STEM) image of the platinum single atom catalyst synthesized in Example 1 of the present disclosure.
[0066] like Figure 1 As shown, platinum exists in the form of single atoms and is uniformly dispersed in the boron-nitrogen-doped graphene, and platinum does not aggregate to form platinum nanoparticles.
[0067] 8 mg of catalyst, 100 uL of Nafion solution and 900 uL of ethanol were ultrasonicated for 30 min to obtain a uniform suspension. The mixed solution was then slowly dripped onto a 2*2 cm carbon paper and the performance of ozone precipitation was tested by linear scanning cyclic voltammetry in a saturated potassium sulfate electrolyte. The test results are shown in Figure 2. Figure 3 shown.
[0068] Figure 3 This is a performance comparison chart of the platinum single atom catalyst in Example 1 of the present disclosure and commercial lead dioxide applied to ozone evolution.
[0069] When the same current density is applied to the catalyst for water electrolysis, since ozone and oxygen evolution reactions occur simultaneously in the reaction and these two reactions are competitive reactions, the higher the potential generated by the catalyst, the more favorable it is for the ozone evolution reaction to occur. Figure 3 As shown, when the catalyst prepared by the method in Example 1 and commercial lead dioxide (β-PbO2) are used to electrolyze water at the same time, at the same current density, the higher the potential generated by the catalyst in Example 1, the stronger the ozone release performance. The ozone release performance of the catalyst in Example 1 is much higher than that of the commercial lead dioxide catalyst, indicating that the platinum single atom catalyst in the disclosed embodiment is expected to replace the commercial lead dioxide catalyst to prepare ozone.
[0070] Example 2
[0071] Weigh 100 mg of multi-walled carbon nanotubes with a diameter of 30 nm, and ultrasonically disperse them in a 100 mL mixed solution of concentrated sulfuric acid: concentrated nitric acid = 1:3 for 30 minutes to make the multi-walled carbon nanotubes evenly dispersed. Then, heat and reflux at 90 ° C for 2 hours, and then wash it with deionized water until it is neutral to obtain multi-walled carbon nanotubes rich in oxygen-containing groups. After that, add the acid-treated multi-walled carbon nanotubes to 50 mL deionized water for ultrasonic dispersion for 20 minutes, then add 0.2 g boric acid and 1.0 g melamine, and ultrasonically disperse for 30 minutes. Then seal the mixture in a 100 mL high-pressure reactor and keep it at 180 ° C for 12 hours. After natural cooling, wash the obtained sample with deionized water and dry it to obtain boron-nitrogen doped carbon nanotubes.
[0072] 518 mg H2PtCl6·6H2O was added into 100 mL deionized water and ultrasonicated for 15 min to obtain a uniformly dispersed platinum source.
[0073] Next, 100 mg of boron-nitrogen-doped carbon nanotubes were added to 20 mL of deionized water and ultrasonicated for 10 minutes, and then stirred for 2 hours to further evenly disperse the boron-nitrogen-doped carbon nanotubes in the water. After that, 1.8 mL of a platinum source prepared by H2PtCl6·6H2O was added, and stirred in an 80°C oil bath for 2 hours. While stirring, formaldehyde solution was slowly added dropwise to reduce platinum ions to platinum single atoms using formaldehyde. After filtration, the precipitate was washed three times with deionized water, placed in a vacuum drying oven and dried at 60°C for 12 hours to obtain a precursor of boron-nitrogen-doped carbon nanotubes loaded with platinum single atoms.
[0074] The above-mentioned precursor containing single platinum atoms is placed in a tubular furnace, and the temperature is heated to 800°C at a heating rate of 5°C / min in an argon atmosphere with a flow rate of 100 ml / min, and the heat preservation time at this temperature is 2 hours. After the heating is completed, it is taken out after natural cooling to obtain a platinum single atom catalyst.
[0075] Figure 2 It is a transmission electron microscope (TEM) image of the platinum single atom catalyst synthesized in Example 2 of the present disclosure.
[0076] like Figure 2 As shown, no aggregation of platinum particles was observed in the TEM image, indicating that platinum in the catalyst prepared by the method in Example 2 exists in the form of single atoms.
[0077] Example 3
[0078] Weigh 50 mg of multi-walled carbon nanotubes with a tube diameter of 30 nm, then add them to 20 mL of 0.01 M boric acid solution for ultrasonic dispersion for 30 min, and then freeze-dry. Then put the freeze-dried product into a tube furnace, and heat it to 900 ° C at a heating rate of 5 ° C / min in a mixed gas containing 5% H2 / Ar at a flow rate of 100 ml / min, and keep it at this temperature for 3 hours. After natural cooling, boron-doped multi-walled carbon nanotubes can be obtained.
[0079] 518 mg H2PtCl6·6H2O was added into 100 mL deionized water and ultrasonicated for 15 min to obtain a uniformly dispersed platinum source.
[0080] Next, 100 mg of boron-doped multi-walled carbon nanotubes were added to 20 mL of deionized water and ultrasonicated for 10 minutes, and then stirred for 2 hours to further evenly disperse the boron-doped multi-walled carbon nanotubes in the water. After that, 1.8 mL of a platinum source prepared by H2PtCl6·6H2O was added, and after stirring at room temperature for 2 hours, 0.3 M NaBH4 was added dropwise under ice bath conditions and stirred continuously for 2 hours, and NaBH4 was used to convert platinum ions into platinum single atoms. After filtering, the obtained precipitate was washed with deionized water to pH = 7, placed in a vacuum drying oven and dried at 60°C for 12 hours to obtain a precursor of boron-doped multi-walled carbon nanotubes containing platinum single atoms.
[0081] The above-mentioned precursor containing single platinum atoms is placed in a tubular furnace, and the temperature is heated to 800°C at a heating rate of 5°C / min in an argon atmosphere with a flow rate of 100 ml / min, and is kept at this temperature for 2 hours. After the heating is completed, it is taken out after natural cooling to obtain a platinum single atom catalyst.
[0082] The specific embodiments described above further illustrate the purpose, technical solutions and beneficial effects of the present disclosure. It should be understood that the above description is only a specific embodiment of the present disclosure and is not intended to limit the present disclosure. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present disclosure should be included in the protection scope of the present disclosure.
Claims
1. Application of a platinum single atom catalyst in an electrocatalytic ozone evolution reaction, comprising: Platinum single-atom catalyst is used to electrolyze water to produce ozone; Wherein, the platinum single atom catalyst comprises: A boron-nitrogen doped substrate, and a platinum atom catalyst supported on the substrate in a single-atom state, wherein the substrate is graphene or multi-walled carbon nanotubes, and the mass percentage of platinum element in the substrate is in the range of 0.01 to 3.5%; Wherein, the platinum single atom catalyst is obtained by the following method: Pre-treating the substrate to obtain a doped substrate, wherein the pre-treatment includes treating the substrate with a doping agent or treating the substrate with a doping agent after treating the substrate with an acidifying agent, and the doping agent is boric acid and melamine or boric acid and urea; The doped substrate is contacted with a platinum source, and a platinum-containing precursor is obtained after treatment with a reducing agent; calcining the precursor under the protection of an inert gas to obtain a platinum single atom catalyst; Wherein, the concentration range of platinum ions in the platinum source includes: 0.01-0.5 mol / L; The reaction temperature range of the doped substrate and the platinum source solution is 10-80° C.; the time range of the contact reaction is 4-48 hours.
2. The use according to claim 1, wherein: The acidifying agent includes at least one of the following: nitric acid, sulfuric acid, perchloric acid, and boric acid.
3. The use according to claim 1, wherein: The platinum source includes any one of the following: H2PtCl6·6H2O, PtCl4, K2PtCl6, Pt(acac)2.
4. The use according to claim 1, wherein the reducing agent comprises any one of the following: sodium borohydride or formaldehyde.
5. The use according to claim 1, wherein: The calcination temperature range is: 500~1000℃; The calcination heating rate range is: 5~10℃ / min; The calcination holding time ranges from 1 to 12 hours.
Citation Information
Patent Citations
Catalyst with dispersed single platinum atoms and preparation method of catalyst
CN105529475A
Catalyst based on platinum oxide alloy loaded boron and nitrogen doped diamond as well as preparation method and application thereof
CN109112571A
Preparation method of monolithic nitrogen-doped mesoporous carbon atom-scale active site catalyst loaded with transition metal
CN110433838A
Boron and nitrogen doped carbon porous nanosheet loaded transition metal nanoparticle material catalyst and preparation method and application thereof
CN110639592A
Supported monatomic rhodium-based catalyst and preparation method and application thereof
CN111036262A
Cited By
Gasification slag-based monatomic catalyst as well as preparation method and application thereof
CN122538211A