Additive manufacturing method for achieving three-dimensional components with excellent properties

By using functionalized photocuring compositions and controlling their polymerization conditions, the problem of insufficient mechanical performance of energy polymerized resins in the manufacture of three-dimensional components by a single reaction mechanism is solved, and the high thermal deformation temperature and mechanical properties are improved, which is suitable for a variety of increase Material manufacturing technology.

CN114616087BActive Publication Date: 2024-11-01HENKEL KGAA
View PDF 40 Cites 0 Cited by

Patent Information

Application Number
CN202080072557.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-10-17
Filing Date
2020-10-19
Publication Date
2024-11-01
Estimated Expiration
2040-10-19

AI Technical Summary

Technical Problem

The existing single reaction mechanism energy polymeric resins have insufficient mechanical properties in the manufacturing of three-dimensional components, especially in terms of thermal deformation temperature and toughness, which are difficult to meet high performance requirements.

Method used

Using a non-flowable functionalized photocuring composition, the polymerization conditions of the photoplastic material with excellent mechanical properties are adjusted by controlling the temperature and electromagnetic spectrum radiation. The method includes placing the photocuring composition in a flowable state and exposing it to suitable electromagnetic spectrum radiation in an indicated mode to vary the polymerization conditions to form a three-dimensional component with high thermal deformation temperature and mechanical properties.

Benefits of technology

It achieves significant improvements in the high thermal deformation temperature, ultimate strength and ultimate stiffness of three-dimensional components, ensuring that the physical properties of the components reach or exceed the levels of traditional thermoplastic materials, and is suitable for a variety of additive manufacturing technologies.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

This article provides an additive manufacturing method for achieving three-dimensional components with excellent properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to additive manufacturing methods for achieving three-dimensional parts with excellent properties. Background Art

[0002] Single reaction mechanism energy polymerizable resins typically have inferior mechanical properties when hardened compared to conventional thermoplastics. The toughness of many engineering thermoplastics, including impact strength, elongation, and tensile strength, is much higher than that of single reaction mechanism energy polymerizable materials. In addition, conventional energy polymerizable resins exhibit even lower toughness when formulated to achieve higher heat distortion temperatures (HDT).

[0003] An attempt to improve the mechanical properties of energy-polymerizable materials with a single reaction mechanism is to use high molecular weight, multifunctional energy-polymerizable oligomers. These oligomers provide lower crosslink density when polymerized despite their higher overall chain molecular weight. However, high molecular weight oligomers bring high viscosity, which limits their ability to be used in viscosity-restricted applications, such as inkjet printing, stereolithography (SLA), digital light processing (DLP), or three-dimensional printing (3DP).

[0004] In conventional additive manufacturing techniques, the construction of three-dimensional parts is performed in a step-by-step or layer-by-layer manner. In particular, layer formation is usually performed by curing a photocurable resin under exposure to visible or ultraviolet light.

[0005] If a new layer is formed on the upper surface of the growing part, then after each irradiation step the part being built is lowered into a resin "pool", covered with a new layer of resin on top, and then a new irradiation step is performed. The disadvantage of this "top-down" technique is the need to immerse the growing object in a (potentially deep) pool of liquid resin and re-build the exact coverage of liquid resin.

[0006] If new layers are formed at the bottom of the growing object, the object being built is removed from the floor in the fabrication well after each irradiation step. This "bottom-up" technique has the potential to eliminate the need to immerse the object in a deep well by pulling it out of a relatively shallow well or pool. A limitation of both additive technologies is also viscosity, as maintaining consistent layers at the top or bottom interface typically requires fluids with viscosities below 2000 cPs. In addition, the bottom-up approach prefers more rigid materials to ensure consistent layer placement and surface finish of the final part. Pot life stability is also an important consideration for all technologies, as polymerization that may occur without energy initiation can lead to part defects or entire vat curing. Examples of such polymerization reactions can occur in many of the dual reaction mechanism materials offered by Carbon Inc., such as CE 220, CE221, EPU 40, EPX 81, FPU 50, RPU 60, RPU 61, and RPU 70.

[0007] U.S. Patent No. 10,239,255 describes single reaction mechanism energy polymerizable resins that improve the mechanical properties of such resins through formulation strategies. The '255 patent relates to and claims a free radical polymerizable liquid comprising a reactive oligomer, the reactive oligomer being at least one of (i) a multifunctional methacrylate oligomer, and (ii) a multifunctional acrylate oligomer; and a reactive monofunctional monomer, the reactive monofunctional monomer being at least one of: (i) a monofunctional N-vinyl monomer, (ii) a monofunctional vinyl ether monomer, (iii) a monofunctional vinyl ester monomer, (iv) a monofunctional vinyl amide monomer, (v) a styrene monomer, (vi) a monofunctional acrylamide monomer, (vii) a monofunctional (meth)acrylate monomer, (viii) a cyanoacrylate monomer, and (iv) a monofunctional vinyl ester monomer. acrylate monomers, (ix) monofunctional vinyl carbonate monomers, (x) monofunctional acryl monomers, and (xi) monofunctional vinyl carbamate monomers, wherein the molar bond ratio of the reactive ethylenically unsaturated groups of the reactive monofunctional species to the reactive ethylenically unsaturated groups of the reactive multifunctional species is at least 10:1, wherein the total weight percentage % of the reactive monofunctional species in the calculated molar bond ratio is at least 25% of the polymerizable liquid, wherein the total weight percentage % of the reactive multifunctional species in the calculated molar bond ratio is at least 25% of the polymerizable liquid, and the free radical polymerizable liquid is an energy polymerizable liquid that can be hardened to form a photoplastic material through a single reaction mechanism.

[0008] Nevertheless, in many three-dimensional parts manufactured, for example, by inkjet printing, SLA, DLP or 3DP, there is still a need for further improvements in physical properties (e.g. toughness with high heat distortion temperature). To date, these improvements have not been achieved. Therefore, there is still a need for a method to achieve the desired properties in these parts. Summary of the invention

[0009] This need is met here.

[0010] To a large extent, this need has been met by process technologies involving the use of functionalized materials that are non-flowable at room temperature.

[0011] A method for additive manufacturing using a photocurable composition to form a three-dimensional component is provided herein. Typically, the additive manufacturing is performed on a build substrate. And the three-dimensional component is made according to data indicating a predetermined pattern. The method comprises the following steps:

[0012] A. providing the photocurable composition in a non-flowable state to a reservoir, such as a hopper, a container or a vessel;

[0013] B. subjecting the photocurable composition to conditions conducive to placing the photocurable composition in a flowable state; and

[0014] C. Exposing the flowable photocurable composition to radiation in the electromagnetic spectrum suitable for initiating polymerization thereof when producing a three-dimensionally printed part according to data indicative of a predetermined pattern.

[0015] In one embodiment, when polymerized, the photocurable composition has adjustable mechanical properties by additional exposure to radiation in the electromagnetic spectrum to modify subsequent energy polymerization conditions. DETAILED DESCRIPTION

[0016] As described above, a method for additive manufacturing using a photocurable composition to form a three-dimensional component is provided herein. Typically, the additive manufacturing is performed on a build substrate. And the three-dimensional component is made according to data indicating a predetermined pattern. The method comprises the following steps:

[0017] A. providing a photocurable composition in a non-flowable state to a reservoir;

[0018] B. subjecting the photocurable composition to conditions conducive to placing the photocurable composition in a flowable state; and

[0019] C. Exposing the flowable photocurable composition to radiation in the electromagnetic spectrum suitable for initiating polymerization thereof when producing a three-dimensionally printed part according to data indicative of a predetermined pattern.

[0020] The photocurable composition comprises a functionalized component that is solid or non-flowable at room temperature. The solid functionalized component should have at least one, preferably at least two, functional groups selected from the following: (meth)acrylates, α-olefins, N-vinyl, vinylamides, cyanoacrylates, (meth)acrylamides, acrylamides, styrenes, epoxides, thiols, 1,3-dienes, vinyl halides, acrylonitriles, vinyl esters, maleimides, nadimides, itaconimides, vinyl ethers, vinyl carbonates and vinyl carbamates. Preferably, the functional group is (meth)acrylate. And preferably there are at least two (meth)acrylate functional groups.

[0021] In one aspect, the photocurable composition comprises a functionalized component that is solid or non-flowable at room temperature, the component having a backbone selected from the group consisting of sulfones, styrenes, isocyanurates, cyanates, maleimides, nadic imides, itaconimides, bicycloalkyls (e.g., adamantyl, fenchyl or norbornyl), biphenyls, novolacs, triazines, carbonates, amides, carbamates, ureas, polyesters, and combinations thereof. The term "backbone" refers to a chemical moiety to which or between which functional groups are attached.

[0022] Suitable choices for functionalized components that are solid or nonflowable at room temperature include those commercially available from Dymax Corporation, Torrington, CT, such as BR-571, Sartomer Inc., Exton, PA, such as CN9788, Huntsman Corporation, such as many bismaleimides, and Evonik, such as Compimide MDAB and Compimide 200.

[0023] In some embodiments, the photocurable composition comprises from about 1, 2 or 5 weight % to 20, 30, 40, 90 or 99 weight % of a functionalized material that is solid or non-flowable at room temperature. Preferably, the amount of the solid functionalized component should be from about 90 to about 99 weight % based on the photocurable composition.

[0024] The photocurable composition comprises a functionalized component that is solid or non-flowable at room temperature and has a molecular weight greater than about 400 Mn, desirably greater than about 800 Mn, and more desirably greater than about 1200 Mn, all measured in daltons.

[0025] The photocurable composition comprises a functionalized component that is solid or non-flowable at room temperature and, in one aspect, comprises a crystalline structure at a temperature at or above about 25° C., which is generally considered to be room temperature.

[0026] Suitable choices for the functionalized component that is solid or non-flowable at room temperature in a crystalline structure include sulfones, styrenes, isocyanurates, cyanates, maleimides, nadic imides, itaconimides, bicycloalkyls (e.g., adamantyl, fenchyl or norbornyl), biphenyls, novolacs, triazines, carbonates, amides, carbamates, ureas, polyesters, and combinations thereof.

[0027] The photocurable composition comprises a functionalized component that is solid or non-flowable at room temperature, which component in another aspect exhibits a phase transition from solid to liquid within a temperature increase of 1°C to 10°C, such as 5°C, as measured by DSC over a 20 minute period.

[0028] In many cases, the photocurable composition should also contain a photoinitiator. Suitable photoinitiators include triazines, ketones, peroxides, diketones, azides, azo derivatives, disulfide derivatives, disilane derivatives, thiol derivatives, diselenide derivatives, diphenylditelluride derivatives, digermane derivatives, distannane derivatives, carbon-germanium compounds, carbon-silicon derivatives, sulfur-carbon derivatives, sulfur-silicon derivatives, peresters, Barton's ester derivatives, hydroxamic acids and thiohydroxamic acids and esters, organic borate esters, organometallic compounds, titanocene, chromium complexes, aluminate complexes, carbon-sulfur or sulfur-sulfur initiator-transfer-terminator compounds, oxygen amines, aldehydes, acetals, silanes, phosphorus-containing compounds, borane complexes, thioxanthone derivatives, coumarins, anthraquinones, fluorenones and ferrocenium salts. Particularly desirable photoinitiators include benzophenones, anthraquinones and fluorenones.

[0029] When used, the photoinitiator should be present in an amount from about 0.01 wt % to about 15 wt %.

[0030] The photocurable composition may include a thermal initiator, but a thermal initiator is not required.

[0031] In step B of the method of the present invention, the photocurable composition should be exposed to a temperature of about 45°C to about 160°C, preferably about 60°C to about 120°C.

[0032] In step B of the method of the present invention, the vapor pressure of the photocurable composition should be less than about 1 mm Hg, preferably less than about 0.1 mm Hg, and more preferably less than about 0.01 mm Hg.

[0033] And in step C of the method of the present invention, the vapor pressure of the photocurable composition should be less than about 1 mm Hg, preferably less than about 0.1 mm Hg, and more preferably less than about 0.01 mm Hg.

[0034] In step B of the method of the present invention, the photocurable composition is maintained in a reservoir which is heated to a temperature of about 45°C to about 160°C, preferably about 60°C to about 120°C.

[0035] And in step C of the method of the present invention, the photocurable composition is maintained in a reservoir, which is heated to a temperature of about 45°C to about 160°C, preferably about 60°C to about 120°C.

[0036] In step C of the method of the present invention, the photocurable composition should be maintained at a temperature that allows the photocurable composition to flow. The temperature can be about 30°C to about 120°C higher than room temperature, at which dispensing or printing can be performed. Room temperature is generally considered to be about 25°C.

[0037] In step C of the method of the present invention, the photocurable composition is exposed to radiation in the electromagnetic spectrum ranging from 355 nm to 405 nm. The radiation can be emitted from an LED source, which can be selected from a laser, a plurality of lasers, a projector or a plurality of projectors. The LED source can be applied from below or above the reservoir containing the photocurable composition.

[0038] Energy polymerization with a single reaction mechanism involves the use of energy to initiate and drive polymerization through a reaction mechanism. Irradiation is performed by exposure to actinic radiation, ultraviolet light, and visible light. Such examples include ultraviolet light (100nm-405nm), visible light (405nm-700nm), or electron beams. Examples of suitable light sources include LEDs, laser diodes, laser beams, lamps (halogen lamps, Xe lamps, Xe-Hg lamps, etc.), LED lasers or LED projectors used in additive manufacturing, LCDs, LED or plasma screens that irradiate visible light, mobile or flat-panel devices. This polymerization is then carried out through a single reaction mechanism, such as free radicals, cations, Michael additions, step-growth, click chemistry, and the like.

[0039] After the method of the present invention is implemented, a photoplastic material is formed through a single reaction mechanism of the photocurable composition. Compared with existing photosensitive polymers, the photoplastic material has mechanical properties comparable to those of thermoplastic materials.

[0040] As with US Pat. No. 10,239,255 (Talken), polymerization of the photocurable composition occurs via a single reaction mechanism. See the '255 patent for further discussion.

[0041] In step C of the method of the present invention, in addition to exposure to radiation in the electromagnetic spectrum, the photocurable composition may be exposed to elevated temperature conditions above those used in step B to render the photocurable composition flowable.

[0042] The three-dimensional component formed in step C of the method of the present invention may have a heat deformation temperature (@ 0.455 MPa) at least as high as the elevated temperature of step B or step C.

[0043] The three-dimensional component formed in step C of the method of the present invention should achieve at least about 50% of at least one of its ultimate strength, ultimate stiffness, and ultimate heat deformation temperature.

[0044] In some embodiments, the methods of the present invention utilize photocurable compositions in the form of a substrate, pellets, powder, wire, spool, or some other particulate solid form factor.

[0045] In some embodiments, the photocurable composition is exposed to an elevated temperature of about 45° C. to about 160° C. in a hopper system to render it flowable.

[0046] In some embodiments, the photocurable composition is exposed to elevated temperatures in a continuous manner through a nozzle, heated core, hot end, heated extruder, or the like.

[0047] In some embodiments, the photocurable composition is provided in a physical form factor having a high surface area to volume ratio, such as 0.5:1, to enable rapid heat transfer during step B.

[0048] In some embodiments, the method of the present invention adds a step D, which comprises contacting the three-dimensional component with a solvent or a washing liquid. The solvent or washing liquid can be selected from lower alkyl alcohols, such as isopropyl alcohol, or mild surfactants.

[0049] When used herein, the solvent or wash fluid may be heated to an elevated temperature. In this manner, unreacted material on the surface of the component may become mobile, making it easier to remove the unreacted material by solvation or mechanical agitation such as sonication.

[0050] In some embodiments, the method of the present invention adds step E, which includes exposing the three-dimensional component formed in step C to elevated temperature conditions. The elevated temperature conditions here can be at least 160° C. Step E can be after one or both of steps C and D.

[0051] In step E of the method of the present invention, the elevated temperature condition is a temperature condition higher than the elevated temperature condition to which the photocurable composition is exposed in step C. The elevated temperature condition should be achieved by ramping from the temperature condition of step C to at least one higher temperature condition at a predetermined rate. The higher temperature condition should be about 45°C to about 160°C higher than step C.

[0052] In some embodiments, the method of the present invention adds a step F, which includes exposing the three-dimensional component formed in step C to radiation in the electromagnetic spectrum of a wavelength different from the radiation in the electromagnetic spectrum used in step C. The radiation in step F can be emitted from a light source selected from an LED light source, which can be selected from a laser, multiple lasers, a projector or multiple projectors, or a broadband light source. The radiation in step F can be a second radiation form in the electromagnetic spectrum, such as gamma radiation, electron beam, or microwave radiation.

[0053] After step E of the method of the present invention, the formed three-dimensional component should achieve about 100% of at least one of its ultimate strength, ultimate stiffness, and ultimate heat deformation temperature.

[0054] Indeed, in some embodiments, the three-dimensional part formed after step E exhibits substantially uniform strength, stiffness, and heat deformation temperature throughout its volume, regardless of the size, geometry, internal complexity, or surface of the part, wherever measurements are taken.

[0055] The three-dimensional component formed after step E can show that the tensile elongation of the three-dimensional component is ≥ yield strength, the tensile elongation is at least about 6%, preferably at least about 10%, and the heat deformation temperature (@0.455MPa) is higher than 100°C, preferably higher than 120°C, and more preferably higher than 160°C.

[0056] The photocurable composition can achieve specified physical or mechanical properties with or without exposure to elevated temperature conditions. Such thermal exposure can be achieved by active heating (e.g., in an oven, such as an electric oven, a gas oven, or a solar oven) or passive heating (e.g., at ambient temperature). Active heating is generally more rapid than passive heating and is preferred in some embodiments, but passive heating is preferred in some embodiments, such as simply keeping the intermediate at ambient temperature for a sufficient time to achieve further polymerization.

[0057] The method of the present invention allows the formation of a three-dimensional part with dimensional stability after implementation of some or all of the post-processing steps (i.e., steps D, E and / or F). This means that 90% of the final part structure is within a certain tolerance or error, such as less than about 500 μm, such as 200 μm, preferably 100 μm dimensional error, when compared to the original design / CAD model or to the part after step C.

[0058] Any suitable filler may be used in the various embodiments described herein, depending on the desired properties of the component or object to be manufactured. Thus, the filler may be solid or liquid, organic or inorganic, and may be reactive and non-reactive rubbers, examples of all of which include siloxanes, organophosphinates, acrylonitrile-butadiene rubbers; reactive and non-reactive thermoplastics (e.g., poly(etherimides), maleimide-styrene terpolymers, polyarylates, polysulfones, and polyethersulfones), inorganic fillers such as silicates (e.g., talc, clay, silica, or mica), glass, carbon nanotubes, graphene, carbon fibers, metal and cellulose nanocrystals, and combinations thereof.

[0059] One or more polymeric toughening agents and / or inorganic toughening agents may be included in the photocurable composition. The toughening agent may be substantially uniformly distributed in the polymer product in the form of particles. The diameter of the particles may be less than 5 μm. Such toughening agents include those toughening agents formed by elastomers, branched polymers, hyperbranched polymers, dendritic polymers, rubbery polymers, rubbery copolymers, block copolymers, core-shell particles, oxides or inorganic materials such as clay, polyhedral oligomeric silsesquioxanes (POSS), carbonaceous materials (e.g., carbon black, carbon nanotubes, carbon nanofibers and fullerenes), ceramics and silicon carbide, etc., with or without surface modification or functionalization. Examples of block copolymers include, for example, the copolymers described in U.S. Patent No. 6,894,113, the entire contents of which are incorporated herein by reference, including NANOSTRENGTH SBM (polystyrene-polybutadiene-polymethacrylate) and AMA (polymethacrylate-polybutylacrylate-polymethacrylate) produced by Arkema. Other suitable block copolymers include the amphiphilic block copolymers described in FORTEGRA and U.S. Patent No. 7,820,760, the entire contents of which are incorporated herein by reference. Examples of known core-shell particles include core-shell (dendritic polymer) particles whose composition is described in U.S. Patent Application Publication No. 2010 / 0280151. For amine branched polymers as shells grafted to core polymers polymerized by polymerizable monomers containing unsaturated carbon-carbon bonds, such as core-shell rubber particles described in EP 1632533A1 and EP 2123711A1, the entire contents of which are incorporated herein by reference, and the Kane Ace MX product line of such particles / epoxy resins with mixtures of the following particles: the particles have a polymer core polymerized by polymerizable monomers such as butadiene, styrene, other unsaturated carbon-carbon bond monomers or combinations thereof, and a polymer shell compatible with epoxy resins, typically polymethyl methacrylate, polyglycidyl methacrylate, polyacrylonitrile or similar polymers, as further discussed below. Also suitable as block copolymers in the present invention are the JSR SX series carboxylated polystyrene / polydivinylbenzene produced by JSR Corporation; KUREHA PARALOID EXL-2655 (produced by Kureha Chemical Industry Co., Ltd.), which is a butadiene alkyl methacrylate styrene copolymer; STAFILOID AC-3355 and TR-2122 (both produced by Takeda Chemical Industries, Ltd.), both of which are acrylate methacrylate copolymers; and PARALOID EXL-2611 and EXL-3387 (both produced by Dow Chemical), both of which are butyl acrylate methyl methacrylate copolymers.Examples of suitable oxide particles include NANOPOX produced by Nanoresins AG. This is a primary mixture of functionalized nanosilica particles and epoxy resin.

[0060] Core-shell rubbers are particulate materials (particles) having a rubber core. Such materials are known and described, for example, in U.S. Patent Application Publication Nos. 2015 / 0184039 and 2015 / 0240113 and U.S. Patent Nos. 6,861,475, 7,625,977, 7,642,316 and 8,088,245, all of which are incorporated herein and elsewhere by reference in their entirety.

[0061] In some embodiments, the core-shell rubber particles are nanoparticles [i.e., have an average particle size of less than 1000 nanometers (nm)]. Typically, the core-shell rubber nanoparticles have an average particle size of less than 500 nm, such as less than 300 nm, less than 200 nm, less than 100 nm, or even less than 50 nm. Typically, such particles are spherical, and thus the particle size is the diameter; however, if the particle is not spherical, the particle size is defined by the longest dimension of the particle.

[0062] In some embodiments, the rubber core may have a Tg of less than -25°C, more preferably less than -50°C, and even more preferably less than -70°C. The Tg of the rubber core may be much lower than -100°C. The core-shell rubber also has at least one shell portion preferably having a Tg of at least 50°C. "Core" refers to the inner portion of the core-shell rubber. The core may form the center of the core-shell particle, or the inner shell or functional domain of the core-shell rubber. The shell is a portion of the core-shell rubber located outside the rubber core. The shell portion (or portions) typically forms the outermost portion of the core-shell rubber particle. The shell material may be grafted onto the core or crosslinked. The rubber core may constitute 50-95% by weight of the total amount of the core-shell rubber particles, for example 60-90% by weight.

[0063] The core of the core-shell rubber can be a polymer or copolymer of a conjugated diene such as butadiene or a lower alkyl acrylate such as n-butyl acrylate, ethyl acrylate, isobutyl acrylate or 2-ethylhexyl acrylate. The core polymer may additionally contain up to 20% by weight of other copolymerized monounsaturated monomers, such as styrene, vinyl acetate, vinyl chloride, methyl methacrylate, etc. The core polymer is optionally crosslinked. The core polymer optionally contains up to 5% of copolymerized graft-linked monomers having two or more unsaturated sites of unequal reactivity, such as diallyl maleate, monoallyl fumarate, allyl methacrylate, etc., wherein at least one reactive site is non-conjugated.

[0064] The core polymer may also be a silicone rubber. The glass transition temperature of these materials is generally below -100°C. Core-shell rubbers having a silicone rubber core include those commercially available from Wacker Chemie, Munich, Germany under the trade name Genioperl.

[0065] The shell polymer, which is optionally chemically grafted or crosslinked to the rubber core, may be polymerized from at least one lower alkyl methacrylate such as methyl methacrylate, ethyl methacrylate, or tert-butyl methacrylate. Homopolymers of such methacrylate monomers may be used. In addition, up to 40% by weight of the shell polymer may be formed from other monovinylidene monomers such as styrene, vinyl acetate, vinyl chloride, methyl acrylate, ethyl acrylate, butyl acrylate, and the like. The molecular weight of the grafted shell polymer may be from 20,000 to 500,000.

[0066] One suitable type of core-shell rubber has reactive groups in the shell polymer that can react with epoxy resins or epoxy resin hardeners. Glycidyl groups are suitable. These can be provided by monomers such as glycidyl methacrylate.

[0067] An example of suitable core-shell rubber is the type described in U.S. Patent Application Publication No. 2007 / 0027233, the entire contents of which are incorporated herein by reference. The core-shell rubber particles wherein said include a crosslinked rubber core, the crosslinked rubber core being a crosslinked copolymer of butadiene in most cases, and a shell, the shell being preferably a copolymer of styrene, methyl methacrylate, glycidyl methacrylate and optionally present acrylonitrile. The core-shell rubber is preferably dispersed in a polymer or epoxy resin, also as described in the document. Suitable core-shell rubber includes but is not limited to those products sold by Kaneka Corporation under the name Kane Ace, including Kane Ace 15 and 120 series products, including Kane Ace MX 120, Kane Ace MX 153, Kane Ace MX 154, Kane Ace MX 156, Kane Ace MX170 and Kane Ace MX 257 and Kane Ace MX120 core-shell rubber dispersions and combinations thereof.

[0068] Suitable resins for the photocurable composition include photocurable silicones. UV polymerizable silicone rubbers, such as SILIOPREN UV polymerizable silicone rubber and LOCTITE polymerizable silicone adhesive sealants. Applications include optical instruments, medical and surgical equipment, external lighting and accessories, electrical connectors / sensors, optical fibers, gaskets and molds.

[0069] Biodegradable resins for use in the photocurable compositions are particularly important for implantable devices to deliver drugs or for temporary performance applications, such as biodegradable screws and stents (U.S. Pat. Nos. 7,919,162 and 6,932,930, the entire contents of which are incorporated herein by reference). Biodegradable copolymers of lactic acid and glycolic acid (PLGA) can be dissolved in PEG di(meth)acrylate to produce a transparent resin suitable for use, and polycaprolactone and PLGA oligomers can be functionalized with acrylic or methacrylic groups to make them effective resins for use.

[0070] Another suitable resin for the photocurable composition includes photocurable polyurethanes (including polyureas, and copolymers of polyurethanes and polyureas [e.g., poly(urethane-ureas)]. Photocurable polyurethane / polyurea compositions comprise (1) a polyurethane based on an aliphatic diisocyanate, poly(ethylene hexamethylene isophthalate), and optionally 1,4-butanediol; (2) a multifunctional acrylate; (3) a photoinitiator; and (4) an antioxidant, and can be formulated to provide a hard, abrasion-resistant, and stain-resistant material (U.S. Pat. No. 4,337,130, the entire contents of which are incorporated herein by reference). Photocurable thermoplastic polyurethane elastomers may contain photoreactive diacetylenic diols as chain extenders.

[0071] The photocurable composition may have other ingredients dissolved or dispersed therein, including pigments, dyes, detectable compounds (eg, fluorescent, phosphorescent and radioactive compounds), fillers, light absorbers or polymerization inhibitors, again depending on the particular use of the product being manufactured.

[0072] In some embodiments, organic peroxides may be included in energy polymerizable liquids or resins of a single reaction mechanism, for example to promote the reaction of potentially unreacted double bonds during heating and / or microwave irradiation. Such organic peroxides may be included in resins or polymerizable liquids in any suitable amount, for example 0.001 wt % or 0.01 wt % or 0.1 wt %, up to 1 wt %, 2 wt % or 3 wt %. Examples of suitable organic peroxides include, but are not limited to, 2,5-bis(tert-butylperoxy)-2,5-dimethylhexane (e.g., LUPEROX 101), dilauroyl peroxide (e.g., LUPEROX LP), benzoyl peroxide (e.g., LUPEROX A98) and bis(tert-butyldioxyisopropyl)benzene (e.g., VulCUP R). Such organic peroxides are commercially available from a variety of sources, including but not limited to Arkema Inc.

[0073] It will be clear to those skilled in the art that the method of the present invention will be applicable to a wide range of additive manufacturing techniques, including jet melting and inkjet methods.

[0074] The photocurable compositions may be used in bottom-up additive manufacturing techniques, such as the continuous liquid interface printing technique described in the '255 patent, or in other additive manufacturing techniques as described herein.

[0075] The three-dimensional printed parts produced by the methods and procedures of the present invention may be final, finished or substantially finished products, or may be intermediate products that are subject to further manufacturing steps such as surface treatment, laser cutting or electrospark machining. Intermediate products include products that may be further additively manufactured in the same or different equipment. For example, a fault or cleavage line may be intentionally introduced into an ongoing "build" by disrupting and then restoring the gradient of a polymerized region, to terminate one area of ​​the finished product, or simply because a particular area of ​​the finished product or "build" is less susceptible to damage than other areas.

[0076] Many different products can be manufactured by the methods and apparatus of the present invention, including large models or prototypes, small customized products, miniature or microminiature products or devices. Examples include medical devices and implantable medical devices, such as hearing aids, stents, drug delivery stations, functional structures, microneedle arrays, fibers and rods, such as waveguides, micromechanical devices, and microfluidic devices.

[0077] In some embodiments, the product has at least one or more pores or channels formed therein, as discussed further below.

[0078] The methods described herein can produce products with a variety of different properties. Therefore, in some embodiments, the product is rigid; in other embodiments, the product is flexible or elastic. In some embodiments, the product is solid; in other embodiments, the product is a gel, such as a hydrogel. In some embodiments, the product has shape memory (i.e., substantially returns to a previous shape after deformation, as long as it is not deformed to a structural failure point). In some embodiments, the product is single (i.e., formed by a single, single reaction mechanism energy polymerizable liquid); in some embodiments, the product is composite (i.e., formed by two or more different single reaction mechanism energy polymerizable liquids). Specific properties will be determined by factors such as the selection of the energy polymerizable liquid of the single reaction mechanism used.

[0079] In some embodiments, the manufactured product or article has at least one overhanging feature (or "overhang"), such as a bridging element between two supports, or a cantilevered element protruding from a substantially vertical support. Due to the unidirectional, continuous nature of some embodiments of the methods of the present invention, as each layer is polymerized to substantial completion and a substantial time interval occurs before proceeding to the next pattern, the problem of fault or cleavage lines forming between layers is significantly reduced. Thus, in some embodiments, the methods are particularly advantageous for reducing or eliminating the number of such overhanging support structures that are manufactured simultaneously with the article.

[0080] In some embodiments, the method of the present invention for additive manufacturing using a photocurable composition to form a three-dimensional part with improved physical properties, wherein the three-dimensional printed part is made according to data indicating a predetermined pattern, comprises the following steps: providing a photocurable composition in a non-flowable state to a reservoir; subjecting the photocurable composition to conditions that are conducive to placing the photocurable composition in a flowable state; when the three-dimensional printed part is made according to the data indicating the predetermined pattern, exposing the flowable photocurable composition to radiation in the electromagnetic spectrum suitable for initiating its polymerization; exposing the three-dimensional part formed in step C to elevated temperature conditions.

[0081] The physical or structural properties of the three-dimensional part can be selected along with the properties of the photocurable composition forming the three-dimensional printed part to provide a wide range of properties for the three-dimensional printed part. The method of the present invention can be used to form complex shapes with desired material properties to form a wide range of three-dimensional parts.

[0082] In some embodiments, the three-dimensional printed parts can be rigid and have, for example, a Young's modulus (MPa) of about 800 to 4500 or any range included therein, a tensile strength (MPa) of about 30 to 250 or any range included therein, an elongation at break of about 1 to 100 or any range included therein, and / or a notched IZOD impact strength of about 10 to 200 J / m or any range included therein. Examples of such rigid three-dimensional parts can include fasteners; electronic equipment housings; gears, propellers, and impellers; wheels, mechanical device housings; tools, and other rigid three-dimensional printed parts.

[0083] In some embodiments, the three-dimensional printed parts can be semi-rigid and have, for example, a Young's modulus (MPa) of about 300 to 3500 or any range subsumed therein, a tensile strength (MPa) of about 20 to 90 or any range subsumed therein, an elongation at break of about 20 to 300 or 600 or any range subsumed therein, and / or a notched IZOD impact strength of about 30 to 400 J / m or any range subsumed therein. Examples of such semi-rigid three-dimensional printed parts can include structural elements; hinges, including living hinges; hulls and decks of boats and ships; wheels; bottles, cans and other containers; pipes, liquid pipes and connectors, and other semi-rigid three-dimensional printed parts.

[0084] In some embodiments, the three-dimensionally printed component can be an elastomer and have, for example, a Young's modulus (MPa) of about 0.25 to 300 or any range included therein, a tensile strength (MPa) of about 0.5 to 30 or any range included therein, an elongation at break of about 50 to 1500 or any range included therein, and / or a tear strength of about 10 to 200 kN / m or any range included therein. Examples of such elastomeric three-dimensionally printed components can include soles, heels, insoles, and midsoles.

[0085] The manufacture of the component can be paused or interrupted one or more times to change the photocurable composition. The three-dimensional component manufactured by the method of the present invention can include a variety of photocurable compositions, which have the ability to achieve different tensile strengths once cured. Although fault lines or sections may be formed in the intermediate by interruption, if the photocurable composition reacts with the photocurable composition of the first version in its second version, the two different fragments of the intermediate will cross-react and covalently couple to each other (for example, by heating or microwave radiation) during the second polymerization. Therefore, a component having a plurality of different fragments with different tensile properties can be formed by the method of the present invention, while still being a single product with different fragments covalently coupled to each other. In some embodiments, the three-dimensional component can be formed to have a plurality of regions with different materials and properties. For example, the three-dimensional component may have one or more regions with a tensile strength (MPa) of about 30 to 100 or any range contained therein formed by the first material or the first group of one or more materials, and / or one or more regions with a tensile strength (MPa) of about 20 to 70 or any range contained therein formed by the second material or the second group of one or more materials, and / or one or more regions with a tensile strength (MPa) of about 0.5 to 30 or any range contained therein formed by the third material or the third group of one or more materials, or any combination of the foregoing. For example, the three-dimensional component may have 1 to 10 or more different regions (or any range contained therein) having different tensile strengths selected from any of the above materials and tensile strengths. For example, a hinge may be formed by successively changing an energy polymerizable liquid of a single reaction mechanism during the formation of a three-dimensional intermediate, the hinge comprising a rigid segment connected to a second elastic segment and connected to a third rigid segment. A shock absorber or vibration damper may be formed in a similar manner, the second segment being elastic or semi-rigid. A single rigid funnel and flexible hose assembly may be formed in a similar manner.

[0086] In some embodiments, photocurable compositions comprising energy-polymerizable resins of one or more single reaction mechanisms can be used to achieve adjustable mechanical properties within the same photoplastic material (or part made thereof). This can be achieved by changing the energy polymerization of the photoplastic material, which changes the reaction kinetics of the system. For example, by changing the light irradiance, light energy, light wavelength, or using an electron beam, the polymerization reaction mechanism and polymerization reaction rate can be changed. This is partly due to the different polymerizable functional groups contained in the resin, and its ability to react or not react with the same functional group or different functional groups, which can change the molecular weight or network of the final polymer. This is also partly due to the fact that the same type of initiation can polymerize all functional groups in the photoplastic material.

[0087] In some embodiments, the three-dimensional parts formed by the methods of the present invention meet the UL94 rating of V-1 or V-0. And in some embodiments, the three-dimensional parts formed by the methods of the present invention meet the Airbus standard for published FST (AITM2).

[0088] In addition, different polymer networks, molecular weights, liquid-solid, solid-solid solubility or phase separation can be adjusted and controlled by the above-mentioned method parameters. Therefore, the mechanical properties of a single resin can be greatly changed, whether it is changed pixel by pixel in the film or voxel by voxel in the component. Specifically, in additive manufacturing, VAT polymerization is usually carried out using laser, projector or screen light sources. Each of these and future light sources can be controlled to emit lower wattage or lower energy on a pixel by pixel basis. Therefore, three-dimensional control of voxel polymerization is possible, which can allow objects with different mechanical properties to be created in three-dimensional space.

[0089] Although the present invention is preferably implemented by stereolithography, material jetting or inkjet printing, in some embodiments, alternative methods and apparatus for bottom-up or top-down three-dimensional manufacturing, including layer-by-layer manufacturing, may be used. Examples of such methods and apparatus include, but are not limited to, U.S. Patent Nos. 5,236,637, 5,391,072, 5,529,473, 7,438,846, 7,892,474, and 8,110,135; U.S. Patent Application Publication Nos. 2013 / 0292862 and 2013 / 029521; and those described in PCT Application Publication No. WO 2015 / 164234, which are incorporated herein by reference in their entirety.

Claims

1. A method for additive manufacturing using a photocurable composition to form a three-dimensional component, wherein the three-dimensional component is made according to data indicating a predetermined pattern, the method comprising the following steps: A. providing a photocurable composition in a non-flowable state to a reservoir, the photocurable composition comprising a functionalized component that is solid or non-flowable at room temperature, the functionalized component having at least one functional group selected from the group consisting of (meth)acrylates, α-olefins, N-vinyls, vinylamides, cyanoacrylates, (meth)acrylamides, acryls, styrenes, epoxides, thiols, 1,3-dienes, vinyl halides, acrylonitriles, vinyl esters, maleimides, nadic imides, itaconimides, vinyl ethers, vinyl carbonates, and vinyl carbamates, or having a backbone selected from the group consisting of sulfones, styrenes, isocyanurates, cyanates, maleimides, nadic imides, itaconimides, adamantyl, biphenyl, novolac, norbornyl, triazines, carbonates, amides, carbamates, ureas, polyesters, and combinations thereof; B. subjecting the photocurable composition to conditions conducive to placing the photocurable composition in a flowable state; as well as C. exposing the flowable photocurable composition to radiation in the electromagnetic spectrum suitable for initiating polymerization thereof when producing a three-dimensionally printed part according to data indicating a predetermined pattern, In step B, the photocurable composition is exposed to a temperature of about 45°C to about 160°C.

2. The method according to claim 1, wherein in step B, the photocurable composition is exposed to a temperature of about 60°C to about 120°C.

3. The method of claim 1, wherein in step B, the photocurable composition has a vapor pressure of less than about 1 mm Hg.

4. The method of claim 1, wherein in step B, the photocurable composition has a vapor pressure of less than about 0.1 mm Hg.

5. The method of claim 1, wherein in step B, the photocurable composition has a vapor pressure of less than about 0.01 mm Hg.

6. The method of claim 1, wherein in step C, the photocurable composition has a vapor pressure of less than about 1 mm Hg.

7. The method of claim 1, wherein in step C, the photocurable composition has a vapor pressure of less than about 0.1 mm Hg.

8. The method of claim 1, wherein in step C, the photocurable composition has a vapor pressure of less than about 0.01 mm Hg.

9. The method according to claim 1, wherein in step B, the photocurable composition is maintained in a reservoir, and the reservoir is heated to a temperature of about 45°C to about 160°C.

10. The method according to claim 1, wherein in step B, the photocurable composition is maintained in a reservoir, and the reservoir is heated to a temperature of about 60°C to about 120°C.

11. The method according to claim 1, wherein in step C, the photocurable composition is exposed to a temperature of about 45°C to about 160°C.

12. The method according to claim 1, wherein in step C, the photocurable composition is exposed to a temperature of about 60°C to about 120°C.

13. The method according to claim 1, wherein in step C, the photocurable composition is maintained at a temperature that allows the photocurable composition to flow.

14. The method according to claim 1, wherein in step B, the photocurable composition is dispensed at a temperature of about 30°C to about 120°C higher than room temperature.

15. The method according to claim 1, wherein in step C, the photocurable composition is printed at a temperature of about 30°C to about 120°C higher than room temperature.

16. The method according to claim 1, wherein in step C, the photocurable composition is exposed to radiation in the electromagnetic spectrum in the range of 355 nm to 405 nm.

17. The method according to claim 1, wherein in step C, the photocurable composition is exposed to radiation in the electromagnetic spectrum emitted from an LED source.

18. The method of claim 1, wherein in step C, the photocurable composition is exposed to radiation in the electromagnetic spectrum emitted from an LED source selected from a laser, a plurality of lasers, a projector, or a plurality of projectors.

19. The method of claim 1, wherein in step C, the photocurable composition is exposed to radiation in the electromagnetic spectrum emitted from an LED source, the LED source being applied from below a reservoir in which the photocurable composition is contained.

20. The method of claim 1, wherein in step C, the photocurable composition is exposed to radiation in the electromagnetic spectrum emitted from an LED source applied from above a reservoir containing the photocurable composition.

21. The method according to claim 1, wherein in step C, polymerization of the photocurable composition occurs via a single reaction mechanism.

22. The method according to claim 1, wherein in step A, the photocurable composition comprises a solid functionalized material.

23. The method of claim 1, wherein in step A, the photocurable composition comprises a solid functionalized component having a molecular weight greater than about 400 Daltons.

24. The method of claim 1, wherein in step A, the photocurable composition comprises a solid functionalized component having a molecular weight greater than about 800 Daltons.

25. The method of claim 1, wherein in step A, the photocurable composition comprises a solid functionalized component having a molecular weight greater than about 1200 Daltons.

26. The method of claim 1, wherein in step A, the photocurable composition comprises a solid functional component comprising a crystalline structure at a temperature at or above about 25°C.

27. The method according to claim 1, wherein in step A, the photocurable composition comprising a solid functionalized component exhibits a phase transition from solid to liquid within a temperature increase of 5°C as measured by DSC over a period of 20 minutes.

28. The method according to claim 1, wherein in step A, the photocurable composition comprises a solid functional component and a photoinitiator.

29. The method according to claim 1, wherein in step A, the photocurable composition comprises a solid functional component, wherein no thermal initiator is added.

30. The method of claim 1, wherein in step C, in addition to exposure to radiation in the electromagnetic spectrum, the photocurable composition is exposed to temperature conditions above the elevated temperature conditions used in step B that made the photocurable composition flowable.

31. The method of claim 1, wherein the three-dimensional component formed in step C has a heat distortion temperature (@0.455 MPa) at least as high as the elevated temperature of step B.

32. The method of claim 1, wherein the three-dimensional component formed in step C has a heat distortion temperature (@ 0.455 MPa) at least as high as the elevated temperature of step C.

33. The method according to claim 1, further comprising step D: D. contacting the three-dimensional component with a solvent or a cleaning solution.

34. The method according to claim 1, further comprising step E: E. Exposing the three-dimensional component formed in step C to elevated temperature conditions.

35. The method according to claim 33, further comprising step E: E. Exposing the three-dimensional component formed in step C to elevated temperature conditions.

36. The method according to claim 2, further comprising step E: E. Exposing the three-dimensional component formed in step C to elevated temperature conditions.

37. The method according to claim 34, wherein in step E, the elevated temperature condition is a temperature condition that is higher than the elevated temperature condition to which the photocurable composition was exposed in step B.

38. The method of claim 34, wherein in step E, the elevated temperature conditions are achieved by ramping from the temperature conditions of step B to at least one higher temperature condition at a predetermined rate.

39. The method according to claim 34, wherein in step E, the elevated temperature conditions are at least 160°C.

40. The method of claim 34, wherein in step E, polymerization of the photocurable composition occurs via a single reaction mechanism.

41. The method according to claim 1, further comprising step F: F. Exposing the three-dimensional component formed in step C to radiation in the electromagnetic spectrum having a wavelength different from the radiation in the electromagnetic spectrum used in step C.

42. A method according to claim 41, wherein in step F, the three-dimensional component is exposed to radiation in the electromagnetic spectrum emitted from a light source selected from an LED light source or a broadband light source.

43. The method of claim 41, wherein in step F, the three-dimensional component is exposed to a second form of radiation in the electromagnetic spectrum.

44. The method of claim 41, wherein in step F, the three-dimensional component is exposed to a second form of radiation in the electromagnetic spectrum, the second form of radiation being selected from gamma radiation, electron beam or microwave radiation.

45. The method of claim 36, wherein the three-dimensional component formed after step C achieves at least about 50% of at least one of its ultimate strength, ultimate stiffness, and ultimate heat deformation temperature.

46. ​​The method of claim 45, wherein the three-dimensional component formed after step E achieves about 100% of at least one of its ultimate strength, ultimate stiffness, and ultimate heat deformation temperature.

47. A method according to claim 46, wherein the three-dimensional component formed after step E exhibits substantially uniform strength, stiffness and heat deformation temperature throughout its volume regardless of the size, geometry, internal complexity or surface of the component and wherever the measurement is made.

48. The method according to claim 46, wherein the three-dimensional component formed after step E exhibits a tensile elongation of the three-dimensional component ≥ yield strength.

49. The method of claim 46, wherein the three-dimensional component formed after step E exhibits a tensile elongation of at least about 6%.

50. The method of claim 46, wherein the three-dimensional component formed after step E exhibits a tensile elongation of at least about 10%.

51. The method of claim 46, wherein the three-dimensional component formed after step E exhibits a heat distortion temperature (@ 0.455 MPa) greater than 100°C.

52. The method of claim 46, wherein the three-dimensional component formed after step E exhibits a heat distortion temperature (@ 0.455 MPa) greater than 120°C.

53. The method of claim 46, wherein the three-dimensional component formed after step E exhibits a heat distortion temperature (@ 0.455 MPa) greater than 160°C.

54. A method of additively manufacturing using a photocurable composition to form a three-dimensional component on a build substrate, the three-dimensional component being made according to data indicating a predetermined pattern, the method comprising: A. subjecting the photocurable composition to conditions conducive to rendering the photocurable composition flowable, wherein the photocurable composition comprises a functionalized component that is solid or non-flowable at room temperature, the functionalized component having at least one functional group selected from the group consisting of (meth)acrylates, α-olefins, N-vinyls, vinylamides, cyanoacrylates, (meth)acrylamides, acryls, styrenes, epoxides, thiols, 1,3-dienes, vinyl halides, acrylonitriles, vinyl esters, maleimides, nadic imides, itaconimides, vinyl ethers, vinyl carbonates, and vinyl carbamates, or having a backbone selected from the group consisting of sulfones, styrenes, isocyanurates, cyanates, maleimides, nadic imides, itaconimides, adamantyl, biphenyl, novolacs, norbornyl, triazines, carbonates, amides, carbamates, ureas, polyesters, and combinations thereof; B. Exposing the photocurable composition to radiation in the electromagnetic spectrum suitable for initiating polymerization thereof when producing a three-dimensionally printed part according to data indicative of a predetermined pattern.

55. The method according to claim 1, wherein the photocurable composition is provided in the form of a substrate, pellets, powder, wire, spool, or some other particulate solid form factor.

56. The method according to claim 1, wherein the photocurable composition is exposed to an elevated temperature of about 45°C to about 160°C in a hopper system to render it flowable.

57. The method according to claim 1, wherein the photocurable composition is exposed to the elevated temperature in a continuous manner via a nozzle, heated core, hot end, heated extruder, or the like.

58. The method of claim 1, wherein the photocurable composition is provided in a physical form factor having a surface area to volume ratio greater than 0.5:

1.

59. A method for additive manufacturing using a photocurable composition to form a three-dimensional component having excellent physical properties, the three-dimensional component being made according to data indicating a predetermined pattern, the method comprising the steps of: providing a photocurable composition in a non-flowable state to a reservoir, wherein the photocurable composition comprises a functionalized component that is solid or non-flowable at room temperature, the functionalized component having at least one functional group selected from the group consisting of (meth)acrylates, α-olefins, N-vinyls, vinylamides, cyanoacrylates, (meth)acrylamides, acryls, styrenes, epoxides, thiols, 1,3-dienes, vinyl halides, acrylonitriles, vinyl esters, maleimides, nadic imides, itaconimides, vinyl ethers, vinyl carbonates, and vinyl carbamates, or having a backbone selected from the group consisting of sulfones, styrenes, isocyanurates, cyanates, maleimides, nadic imides, itaconimides, adamantyl, biphenyl, novolac, norbornyl, triazines, carbonates, amides, carbamates, ureas, polyesters, and combinations thereof; subjecting the photocurable composition to conditions conducive to placing the photocurable composition in a flowable state; exposing the flowable photocurable composition to radiation in the electromagnetic spectrum suitable for initiating polymerization thereof when a three-dimensionally printed part is produced according to data indicative of a predetermined pattern; as well as The three-dimensional feature formed in step C is exposed to elevated temperature conditions.

Citation Information

Patent Citations

  • Process for producing modified epoxy resin

    EP1632533A1

  • Thermosetting resin composition having rubbery polymer particle dispersed therein, and process for production thereof

    EP2123711A1

  • Fabrication of solid materials or films from a polymerizable liquid

    US10239255B2

  • Process for producing modified epoxy resin

    US20070027233A1

  • Toughened fiber reinforced polymer composite with core-shell particles

    US20100280151A1