A three-dimensional macroporous tungsten disulfide / carbon composite material and its preparation method and application

By co-precipitating tungsten salt and carbon source on the SiO2 surface and conducting high-temperature kettle reactions, removing the template, and preparing a three-dimensional macroporous structure of tungsten disulfide/carbon composite material, the problem of insufficient stability and conductivity of tungsten disulfide is solved. Improves the electrochemical performance and material stability of sodium ion batteries.

CN114628673BActive Publication Date: 2024-11-12DALIAN INSTITUTE OF CHEMICAL PHYSICS CHINESE ACADEMY OF SCIENCES
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202011463856.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-12-11
Publication Date
2024-11-12
Estimated Expiration
2040-12-11

AI Technical Summary

Technical Problem

The stability and conductivity of tungsten disulfide as an anode material of sodium ion batteries are insufficient, resulting in structural collapse and low reversible specific capacity during charging and discharging. The active site exposure of tungsten disulfide in the existing composite material preparation methods is limited, making it difficult to Build a three-dimensional multi-channel structure.

Method used

The tungsten salt and carbon source were deposited on the SiO2 surface by co-precipitation method, and high-temperature kettle reaction was carried out and treated with strong alkali and acid. The SiO2 template was removed to prepare a tungsten disulfide/carbon composite material with a three-dimensional macroporous structure.

Benefits of technology

The reversible specific capacity and stability of the tungsten disulfide/carbon composite material are improved, and the negative electrode material of sodium ion battery shows excellent electrochemical performance, and the preparation process is simple and the application range is wide.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114628673B_ABST
    Figure CN114628673B_ABST
Patent Text Reader

Abstract

The present invention discloses a three-dimensional macroporous tungsten disulfide / carbon composite material, a preparation method thereof, and an application thereof as a negative electrode active material in a sodium ion battery system. Based on a method of coprecipitation and high-temperature autoclave reaction, a tungsten salt and a carbon source are simultaneously deposited on the surface of SiO2, and after high-temperature sulfurization treatment, a strong alkaline solution is used to treat the SiO2 template, and a hydrofluoric acid solution is used to remove the SiO2 template to obtain the target product. The method has the characteristics of simple operation and large-scale preparation. The tungsten disulfide / carbon composite material prepared by the method has a three-dimensional macroporous structure, and exhibits excellent performance and broad application prospects as a negative electrode material for sodium ion batteries.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of electrochemical materials, and in particular to a three-dimensional macroporous tungsten disulfide / carbon composite material and a preparation method and application thereof. Background Art

[0002] As one of the most promising negative electrode materials for sodium-ion batteries, tungsten disulfide has attracted extensive attention from researchers due to its unique layered structure and high theoretical specific capacity (533 mAh g-1) (Advanced Functional Materials.30.1907677 (2020)). However, the layered tungsten disulfide nanosheets are connected by weak van der Waals forces, and the nanosheets are prone to folding and stacking during the continuous charging and discharging process, resulting in structural collapse, which in turn affects the performance of the battery. At the same time, the poor conductivity of tungsten disulfide is also one of the main factors restricting its performance.

[0003] In order to improve the stability of tungsten disulfide as a negative electrode material for batteries, a common method is to compound tungsten disulfide with carbon, and use the introduction of carbon to improve the stability of tungsten disulfide and increase its conductivity (Journal of Materials Chemistry A.5.10406(2017)). For example, after tungsten disulfide is compounded with reduced graphene oxide, the performance of the material is significantly improved, indicating that the introduction of carbon has a certain enhancing effect on the stability and conductivity of tungsten disulfide (Nanoscale.7.3965(2015)); or construct a tungsten disulfide and carbon composite with a three-dimensional structure, such as directly growing tungsten disulfide on a three-dimensional carbon foam (Journal of Materials Chemistry A.6.10813(2018)). However, these reported preparation methods often directly grow tungsten disulfide on a carbon skeleton or simply carbon-coat tungsten disulfide, and the active sites of tungsten disulfide are limitedly exposed, resulting in a low reversible specific capacity. Therefore, how to construct three-dimensional multi-porous tungsten disulfide to expose more active sites and improve the reversible specific capacity of the material is still a difficult point in the research; whether carbon can be directly introduced in situ to generate a complex of tungsten disulfide and carbon in the process of constructing three-dimensional tungsten disulfide is another difficulty in the research. Summary of the invention

[0004] The present invention deposits tungsten salt and carbon source on the surface of SiO2 at the same time, treats with strong alkali solution after high temperature autoclave reaction sulfurization, and removes SiO2 template with hydrofluoric acid solution to obtain tungsten disulfide / carbon composite material. The method has the characteristics of simple operation and large-scale preparation. The prepared tungsten disulfide / carbon composite material has a three-dimensional macroporous structure and exhibits excellent electrochemical performance as a negative electrode material for sodium ion batteries.

[0005] The technical means adopted by the present invention are as follows:

[0006] A tungsten disulfide / carbon composite material with a three-dimensional macroporous structure.

[0007] A method for preparing a tungsten disulfide / carbon composite material comprises the following steps:

[0008] (1) using a co-precipitation method to co-deposit a tungsten salt and a carbon source on the surface of SiO2 to obtain a precursor mixture;

[0009] (2) transferring the precursor mixture obtained in step (1) and the sulfur source into a high-temperature reaction kettle under an inert atmosphere; the inert atmosphere is sealed in the kettle to form a non-flowing system;

[0010] (3) placing the high temperature reaction kettle in a muffle furnace, heating the temperature to the end point temperature and then maintaining the temperature;

[0011] (4) treating the product obtained in step (3) with alkali, washing and drying to obtain a SiO2 / tungsten disulfide / carbon composite material;

[0012] (5) treating the product obtained in step (4) with acid, washing and drying to obtain a tungsten disulfide / carbon composite material.

[0013] Furthermore, in step (1), the tungsten salt is one of ammonium tungstate, ammonium metatungstate, ammonium tetrathiotungstate, sodium metatungstate or sodium tungstate; the carbon source is one of soluble starch, sucrose, anhydrous glucose, dopamine hydrochloride, melamine or dicyandiamide; and the mass ratio of the tungsten salt to the carbon source is 1:0.1-1.

[0014] Furthermore, in step (1), the co-deposition temperature is 60 to 100° C. and the time is 12 to 24 hours.

[0015] Furthermore, in step (2), the inert atmosphere is one of argon, nitrogen or helium; the sulfur source is one of carbon disulfide, sodium sulfide, potassium sulfide, ammonium sulfide or thioacetamide; and the mass ratio of tungsten salt to sulfur source is 1:0.5-2.

[0016] Furthermore, in step (3), the programmed temperature treatment is carried out by heating the temperature at a rate of 5 to 15°C / min to a final temperature of 400 to 600°C, and then maintaining the temperature for 3 to 5 hours.

[0017] Furthermore, in step (4), the alkali in the alkali treatment is a sodium hydroxide solution with a concentration of 4 to 6 mol / L or a potassium hydroxide solution with a concentration of 4 to 6 mol / L, the alkali treatment time is 2 to 5 hours, and the alkali treatment temperature is 60 to 100° C.; the drying temperature is 60 to 80° C., and the drying time is 12 to 24 hours.

[0018] Furthermore, in step (5), the acid in the acid treatment is a hydrofluoric acid solution with a concentration of 10 to 15%, and the acid treatment time is 12 to 24 hours; the drying temperature is 60 to 80° C., and the drying time is 12 to 24 hours.

[0019] The present invention also provides a tungsten disulfide / carbon composite material obtained according to the above preparation method.

[0020] Furthermore, the tungsten disulfide / carbon composite material has a three-dimensional macroporous structure.

[0021] The present invention also provides an application of a tungsten disulfide / carbon composite material with a three-dimensional macroporous structure as a negative electrode material in a sodium ion battery system.

[0022] Compared with the prior art, the present invention has the following advantages:

[0023] 1. The tungsten disulfide / carbon composite material prepared by the present invention has a three-dimensional macroporous structural feature. When used as a negative electrode material for sodium ion batteries, it not only exposes more active sites and increases the battery capacity, but also improves the stability of the material and ensures the stability of the battery in long-term cycle testing.

[0024] 2. The present invention directly obtains the composite of tungsten disulfide and carbon through a high-temperature autoclave reaction without the need for an additional calcination and carbonization process, and the preparation process is simple.

[0025] 3. The method of the present invention can be prepared in large quantities and has a wide range of applications. The obtained tungsten disulfide / carbon composite material has potential application prospects in the field of energy storage. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.

[0027] Figure 1 This is a transmission electron microscope (TEM) image of the tungsten disulfide / carbon composite material in Example 1.

[0028] Figure 2 This is the transmission electron microscope (TEM) image of the tungsten disulfide material in Comparative Example 1.

[0029] Figure 3 The tungsten disulfide material in Comparative Example 1 was tested in a voltage range of 0.01 to 3 V and a current density of 100 mA·g -1 Performance graph when .

[0030] Figure 4 The tungsten disulfide material in Comparative Example 2 was tested in a voltage range of 0.01 to 3 V and a current density of 100 mA·g -1 Performance graph when .

[0031] Figure 5 The tungsten disulfide / carbon composite material in Example 1 is tested in the voltage range of 0.01 to 3 V and the current density of 200 mA·g -1 Performance graph when .

[0032] Figure 6 The tungsten disulfide / carbon composite material in Example 2 is tested in the voltage range of 0.01 to 3 V and the current density of 100 mA·g -1 Performance graph when .

[0033] Figure 7 The tungsten disulfide / carbon composite material in Example 2 is tested in the voltage range of 0.01-3V and the current density of 2A·g -1 Performance graph when . DETAILED DESCRIPTION

[0034] The whole material preparation process is described in detail below through examples.

[0035] (1) Add tungsten salt and carbon source to deionized water in sequence and stir until completely dissolved. Then add SiO2 and perform ultrasonic dispersion to form a uniform dispersion.

[0036] (2) The dispersion prepared in (1) was placed on a magnetic stirrer and stirred at room temperature until the solvent was fully evaporated, and then the obtained sample was placed in a forced air drying oven for further drying.

[0037] (3) Under the protection of argon atmosphere, the dried sample in (2) and a sulfur source are transferred to a high-temperature reaction kettle and sealed.

[0038] (4) Place the reactor in (3) in a muffle furnace, raise the temperature to 400-600°C, and maintain the temperature for 3-5 hours.

[0039] (5) Treat the sample obtained in (4) with an alkaline solution for 2 to 5 hours to remove excess CS2, then filter it and wash it with water and ethanol several times until the filtrate is neutral.

[0040] (6) Treat the sample obtained in (5) with an acid solution for 12 to 24 hours to remove SiO2, then filter it, wash it with water and ethanol several times until the filtrate is neutral, and then dry it to obtain a three-dimensional macroporous tungsten disulfide / carbon composite material.

[0041] The ultrasonic dispersion time after adding SiO2 in step (1) is preferably 45 to 90 minutes.

[0042] The drying temperature in step (2) is preferably 60-80°C.

[0043] The programmed heating rate in step (4) is preferably 10-15°C / min; the preferred end temperature is 500°C, and the preferred constant temperature time is 4h.

[0044] In step (5), the preferred alkaline solution is a 4-6 mol / L NaOH solution; the preferred treatment temperature is 60° C. and the treatment time is 3 h.

[0045] The preferred concentration of the hydrofluoric acid solution used in step (6) is 10%.

[0046] Example 1

[0047] 1. Dissolve 370 mg sodium tungstate and 100 mg anhydrous glucose in 20 mL deionized water, add 800 mg SiO2, and disperse evenly by ultrasonic.

[0048] 2. Place the ultrasonic dispersion in (1) on a magnetic stirrer and stir. After the solvent evaporates completely, transfer it to a forced air drying oven and dry it at 60°C for 24 hours.

[0049] 3. Under the protection of argon atmosphere, transfer the completely dried sample in (2) and 10 mL CS2 into a high temperature reactor.

[0050] 4. Place the high temperature reactor in a muffle furnace, heat it to 500°C at a heating rate of 10°C / min and keep it at this temperature for 4 hours.

[0051] 5. Treat the sample obtained in (4) with 6 mol / L sodium hydroxide solution for 3 h at 60° C. After treatment, filter and wash with water and ethanol several times until the filtrate is neutral.

[0052] 6. Treat the sample obtained in (5) with a 10% hydrofluoric acid solution for 12 h. After treatment, filter and wash with water and ethanol several times until the filtrate is neutral.

[0053] 7. Place the sample washed in (6) in a forced air drying oven and dry for 12 hours to obtain a tungsten disulfide / carbon composite material.

[0054] Transmission electron microscopy (see Figure 1 ) showed that the obtained sample had a very regular three-dimensional macroporous structure, the sample surface was rough and there were amorphous substances present.

[0055] Example 2

[0056] 1. Dissolve 370 mg sodium tungstate and 300 mg anhydrous glucose in 20 mL deionized water, add 800 mg SiO2, and disperse evenly by ultrasonic.

[0057] 2. Place the ultrasonic dispersion in (1) on a magnetic stirrer and stir. After the solvent evaporates completely, transfer it to a forced air drying oven and dry it at 60°C for 24 hours.

[0058] 3. Under the protection of argon atmosphere, transfer the completely dried sample in (2) and 10 mL CS2 into a high temperature reactor.

[0059] 4. Place the high temperature reactor in a muffle furnace, heat it to 500°C at a heating rate of 10°C / min and keep it at this temperature for 4 hours.

[0060] 5. Treat the sample obtained in (4) with 6 mol / L sodium hydroxide solution for 3 h at 60° C. After treatment, filter and wash with water and ethanol several times until the filtrate is neutral.

[0061] 6. Treat the sample obtained in (5) with a 10% hydrofluoric acid solution for 12 h. After treatment, filter and wash with water and ethanol several times until the filtrate is neutral.

[0062] 7. Place the sample washed in (6) in a forced air drying oven and dry for 12 hours to obtain a tungsten disulfide / carbon composite material.

[0063] Comparative Example 1

[0064] 1. Dissolve 370 mg sodium tungstate in 20 mL deionized water, add 800 mg SiO2, and disperse evenly by ultrasonic.

[0065] 2. Place the ultrasonic dispersion in (1) on a magnetic stirrer and stir. After the solvent evaporates completely, transfer it to a forced air drying oven and dry it at 60°C for 24 hours.

[0066] 3. Under the protection of argon atmosphere, transfer the completely dried sample in (2) and 10 mL CS2 into a high temperature reactor.

[0067] 4. Place the high temperature reactor in a muffle furnace, heat it to 500°C at a heating rate of 10°C / min and keep it at this temperature for 4 hours.

[0068] 5. Treat the sample obtained in (4) with 6 mol / L sodium hydroxide solution for 3 h at 60° C. After treatment, filter and wash with water and ethanol several times until the filtrate is neutral.

[0069] 6. Treat the sample obtained in (5) with a 10% hydrofluoric acid solution for 12 h. After treatment, filter and wash with water and ethanol several times until the filtrate is neutral.

[0070] 7. Place the sample washed in (6) in a forced air drying oven and dry for 12 hours to obtain a three-dimensional macroporous tungsten disulfide material.

[0071] Transmission electron microscopy (see Figure 2 ) shows that the obtained sample has a very regular three-dimensional macroporous structure, but because no carbon source is introduced, the sample surface is smoother than the sample surface in Example 1. Electrochemical test (see Figure 3 ) shows that the capacity of the sample in this comparative example continues to decay during long-term charge and discharge tests and fails to maintain good cycle stability, indicating the importance of carbon introduction in improving material stability.

[0072] Comparative Example 2

[0073] 1. Under argon atmosphere, transfer 370 mg sodium tungstate and 10 mL CS2 into a high temperature reactor.

[0074] 2. Place the high-temperature reactor in a muffle furnace, heat it to 500°C at a heating rate of 10°C / min and keep it at this temperature for 4 hours.

[0075] 3. Treat the sample obtained in (4) with 6 mol / L sodium hydroxide solution for 3 h at 60° C. After the treatment, filter and wash with water and ethanol several times until the filtrate is neutral.

[0076] 4. Place the sample washed in (3) in a forced air drying oven and dry for 12 hours to obtain tungsten disulfide material.

[0077] Electrochemical test (see Figure 4 ) shows that the sample in this comparative example failed to maintain good cycle stability in the long-term charge and discharge test. Compared with the sample in Example 1, the reversible capacity of the material in this comparative example is not only low but also shows a very obvious attenuation trend, indicating that the good combination of the three-dimensional macroporous structure and carbon not only exposes more sodium insertion active sites, increases the reversible capacity of the material, but also improves the stability of the material during long-term charge and discharge.

[0078] Application Example 1

[0079] The tungsten disulfide / carbon composite material obtained in Example 1 was applied to a sodium ion battery system to examine its electrochemical performance when used as a negative electrode material of the battery.

[0080] 1.Battery preparation:

[0081] Active material, acetylene black and binder (PVDF) were weighed in a mass ratio of 7:2:1 in a suitable amount of 1-methyl-2-pyrrolidone to form a uniform active material slurry, and the active material slurry was coated on a copper foil using a coating machine, and then placed in an oven at 60°C for 24 hours. In a glove box filled with argon (to ensure that the water and oxygen values ​​are all below 0.1ppm), sodium metal was used as the counter electrode, Whatman glass fiber was used as the diaphragm, 1.0M NaPF6 was dissolved in propylene carbonate and 5% fluoroethylene carbonate was added as the electrolyte to assemble the CR2016 battery.

[0082] 2.Electrochemical performance evaluation:

[0083] Test conditions: temperature: 30°C; voltage range: 0.01-3V; current density: 200mA·g -1 .

[0084] 3. Results and Discussion:

[0085] The first cycle charge and discharge capacity of the tungsten disulfide / carbon composite material is 597 mAh g -1 and 903mAh·g -1 After 100 cycles of charge and discharge tests, the material still maintained a capacity of 515 mAh g -1 The reversible specific capacity (see Figure 5 ).

[0086] Application Example 2

[0087] The tungsten disulfide / carbon composite material obtained in Example 2 was applied to a sodium ion battery system to examine its electrochemical performance when used as a negative electrode material of the battery.

[0088] 1.Battery preparation:

[0089] Active material, acetylene black and binder (PVDF) were weighed in a mass ratio of 7:2:1 in a suitable amount of 1-methyl-2-pyrrolidone to form a uniform active material slurry, and the active material slurry was coated on a copper foil using a coating machine, and then placed in an oven at 60°C for 24 hours. In a glove box filled with argon (to ensure that the water and oxygen values ​​are all below 0.1ppm), sodium metal was used as the counter electrode, Whatman glass fiber was used as the diaphragm, 1.0M NaPF6 was dissolved in propylene carbonate and 5% fluoroethylene carbonate was added as the electrolyte to assemble the CR2016 battery.

[0090] 2.Electrochemical performance evaluation:

[0091] Test conditions: temperature: 30°C; voltage range: 0.01-3V; current density: 100mA·g -1 and 2A·g -1 .

[0092] 3. Results and Discussion:

[0093] When the current density is 100 mA g -1 When the first cycle charge and discharge capacity of tungsten disulfide / carbon composite material is 557mAh·g -1 and 842mAh·g -1 After 100 cycles of charge and discharge tests, the material still maintained a capacity of 418 mAh g -1 The reversible specific capacity (see Figure 6 ). This material can withstand high current of 2A·g -1 The cycle test showed excellent cycle stability, and after 1000 cycles of charge and discharge tests, it still maintained 270mAh g -1 The reversible specific capacity (see Figure 7 ).

[0094] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A tungsten disulfide / carbon composite material, It is characterized in that The tungsten disulfide / carbon composite material has a three-dimensional macroporous structure; The preparation method of the material comprises the following steps: (1) Tungsten salt and carbon source are co-deposited on SiO 2 to obtain a precursor mixture; (2) transferring the precursor mixture obtained in step (1) and the sulfur source into a high-temperature reaction vessel under an inert atmosphere; (3) placing the high temperature reaction kettle in a muffle furnace, heating the temperature to the end point temperature and then maintaining the temperature; (4) treating the product obtained in step (3) with alkali, washing and drying to obtain SiO 2 / tungsten disulfide / carbon composite material; (5) treating the product obtained in step (4) with acid, washing and drying to obtain a tungsten disulfide / carbon composite material; In the step (1), the mass ratio of the tungsten salt to the carbon source is 1:0.1-1, the co-deposition temperature is 60-100° C., and the time is 12-24 h; In the step (2), the mass ratio of the tungsten salt to the sulfur source is 1:0.5-2; In the step (3), the programmed temperature treatment is performed by heating the temperature at a rate of 5 to 15°C / min to a final temperature of 400 to 600°C, and then maintaining the temperature for 3 to 5 hours; In the step (4), the alkali in the alkali treatment is a sodium hydroxide solution with a concentration of 4 to 6 mol / L or a potassium hydroxide solution with a concentration of 4 to 6 mol / L, the alkali treatment time is 2 to 5 hours, and the alkali treatment temperature is 60 to 100° C.; In the step (5), the acid used in the acid treatment is a hydrofluoric acid solution with a concentration of 10 to 15%, and the acid treatment time is 12 to 24 hours.

2. The tungsten disulfide / carbon composite material according to claim 1, Features: In the step (1), the tungsten salt is one of ammonium tungstate, ammonium metatungstate, ammonium tetrathiotungstate, sodium metatungstate or sodium tungstate; and the carbon source is one of soluble starch, sucrose, anhydrous glucose, dopamine hydrochloride, melamine or dicyandiamide.

3. The tungsten disulfide / carbon composite material according to claim 1, Features: In the step (2), the inert atmosphere is one of argon, nitrogen or helium; and the sulfur source is one of carbon disulfide, sodium sulfide, potassium sulfide, ammonium sulfide or thioacetamide.

4. The tungsten disulfide / carbon composite material according to claim 1, Features: In the step (4), the drying temperature is 60 to 80° C. and the drying time is 12 to 24 hours.

5. The tungsten disulfide / carbon composite material according to claim 1, Features: The drying temperature is 60-80°C and the drying time is 12-24h.

6. Use of the tungsten disulfide / carbon composite material according to any one of claims 1 to 5 as a negative electrode material in a sodium ion battery system.