Preparation method of nitrogen-doped graphene coated ternary positive electrode material
Through nitrogen-doped graphene coating technology, the rate performance and cycle performance problems of the ternary positive electrode material are solved, the conductivity and capacity of the material are improved, the cycle life of the battery is extended, and the residual alkali on the surface of the material in the existing technology is solved. Problems caused.
Patent Information
- Application Number
- CN202410998051.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-11-12
AI Technical Summary
The current ternary positive electrode materials have poor performance in rate performance, poor conductivity, low capacity and poor circulation performance. The formation of lithium hydroxide or lithium carbonate caused by residual surface alkali reduces the specific capacity and cycle life of the battery.
The preparation method of ternary positive electrode material coated with nitrogen-doped graphene is adopted. By adding dopamine monomer and mixing with ternary positive electrode material under stirring, an alkaline environment is formed to promote the self-polymerization and adhesion of polydopamine, and then sintered with the catalyst. Form a nitrogen-doped graphene coating to improve the conductivity and cyclic properties of the material.
It significantly improves the conductivity of the ternary positive electrode material, increases the battery capacity and circulation performance, effectively isolates the erosion of the electrolyte on the surface of the material, and extends the cycle life of the battery.
Smart Images

Figure CN118943328A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of ternary positive electrode materials, and in particular to a method for preparing a nitrogen-doped graphene-coated ternary positive electrode material. Background Art
[0002] With the rapid growth of the global economy and the continuous increase in population, energy demand continues to grow. Traditional fossil energy can no longer meet this demand. New energy transformation has become an effective way to deal with these problems. Among them, lithium batteries, as an energy carrier, have their performance and technological advantages. After decades of development, various technologies have become increasingly mature and have now been successfully commercialized on a large scale. According to the usage scenarios and energy size, they are specifically divided into lithium power batteries, lithium consumer batteries and lithium energy storage batteries. In 2023, the global new energy industry has achieved rapid development, and the installed capacity of power batteries will exceed 390GWh. Lithium power batteries, as the main application end of lithium batteries, have begun to use high energy density on a large scale due to the need for endurance. The cycle and safety performance are slightly poor, but the comprehensive indicators are balanced. The ternary materials. The power battery industry stipulates that when the cycle life of the power battery is less than 80% of the initial capacity, it needs to be retired. How to improve the cycle performance of the positive electrode material is a problem that the retired lithium battery industry is currently committed to solving. Ternary positive electrode materials have high energy density and good cycle performance. They are typical representatives of lithium battery positive electrode materials currently used on a large scale. However, since the surface of ternary positive electrode materials contains residual alkali, some lithium ions form lithium hydroxide or lithium carbonate when they are freed to the surface of the material, reducing the specific capacity of the battery.
[0003] The prior art discloses a water washing method and system for high-nickel ternary positive electrode materials, which uses water washing to remove residual alkali on the surface of the ternary positive electrode material, and electrolyzes the electrolyte solution to remove the residual alkali on the surface of the high-nickel ternary positive electrode material matrix. It can be seen that in the water washing method, the key step is to completely remove the residual alkali by water washing and electrolysis, which is also the consensus in the art in the process of preparing ternary positive electrode materials. However, it is precisely because of the method of removing the residual alkali of the ternary positive electrode material by water washing that the battery rate performance using the ternary positive electrode material is poor. Summary of the invention
[0004] Therefore, the technical problem to be solved by the present invention is to overcome the defect of poor rate performance of the ternary positive electrode material in the prior art, thereby providing a method for preparing a nitrogen-doped graphene-coated ternary positive electrode material.
[0005] Another technical problem to be solved by the present invention is to overcome the defects of poor conductivity, low capacity and poor cycle performance of the ternary positive electrode materials in the prior art, thereby providing a method for preparing a nitrogen-doped graphene-coated ternary positive electrode material. The prepared ternary positive electrode material has good conductivity, and the formed battery has high capacity and good cycle performance.
[0006] The present invention provides a method for preparing a nitrogen-doped graphene-coated ternary positive electrode material, comprising the following steps: S1, adding a dopamine monomer to a mixed solution of a ternary positive electrode material and water under stirring, and performing solid-liquid separation to obtain an intermediate; S2, mixing the intermediate with a catalyst to obtain a mixture, and sintering the mixture in an inert atmosphere to obtain the nitrogen-doped graphene-coated ternary positive electrode material.
[0007] The water washing liquid of the ternary material is alkaline with a pH value of 8-12. Dopamine monomer spontaneously polymerizes in the alkaline solution to form polydopamine. Polydopamine has strong viscosity and is adsorbed on the surface of the ternary material to form a stable polydopamine coating layer. The solid and liquid are separated to obtain the polydopamine-coated ternary material.
[0008] In some of the embodiments, in the mixed solution of the ternary cathode material and water in step S1, the concentration of the ternary cathode material is 18-25 mol / L.
[0009] In some of the embodiments, the molar ratio of the dopamine monomer to the ternary cathode material is (0.01-1):10.
[0010] In some of the embodiments, the molar ratio of the intermediate to the catalyst is 10:(0.01-0.03).
[0011] In some embodiments, the stirring speed in step S1 is 400-600 rpm, and the stirring time is 20-40 min.
[0012] In some embodiments, the solid-liquid separation step in step S1 is centrifugation, drying,
[0013] Optionally, the centrifugal speed is 2000-2500 rpm, and the centrifugal time is 6 min-60 min.
[0014] Optionally, the drying temperature is 100-110° C., and the drying time is 4-6 hours.
[0015] In some embodiments, the catalyst is at least one of nano nickel powder and nano iron powder.
[0016] In some embodiments, the inert atmosphere is at least one of argon and nitrogen.
[0017] In some of the embodiments, in step S2, the sintering temperature is 600-700° C., and the sintering time is 10-14 h.
[0018] In some of the embodiments, the preparation method of the ternary positive electrode material is to mix the lithium source and nickel cobalt manganese hydroxide, and then sinter at 700-1000° C. for 8-12 hours.
[0019] Optionally, the lithium source is at least one of lithium hydroxide and lithium carbonate.
[0020] In some embodiments, the chemical formula of the ternary cathode material is Li x Ni a Co b Mn 1-a-b O 2 , where x is 1-1.2, a is 0.4-0.99, and b is 0.01-0.5.
[0021] Preferably, the chemical formula of the ternary cathode material is Li 1.05 Ni 0.7 Co 0.1 Mn 0.2 O 2 、LiNi 0.8 Co 0.1 Mn 0.1 O 2 , Li 1.2 Ni 0.9 Co 0.05 Mn 0.05 O 2 , Li 1.05 Ni 0.5 Co 0.2 Mn 0.3 O 2 .
[0022] The technical solution of the present invention has the following advantages:
[0023] The present invention provides a method for preparing a nitrogen-doped graphene-coated ternary positive electrode material, comprising the following steps: S1, adding a dopamine monomer to a mixed solution of a ternary positive electrode material and water under stirring, wherein the ternary material water washing solution is alkaline, and the dopamine monomer spontaneously polymerizes in the alkaline solution to form polydopamine, which has strong viscosity and is adsorbed on the surface of the ternary material to form a stable polydopamine coating layer, and solid-liquid separation is performed to obtain a polydopamine-coated ternary material, i.e., an intermediate; S2, mixing the intermediate with a catalyst to obtain a mixture, and sintering the mixture in an inert atmosphere to obtain the nitrogen-doped graphene-coated ternary positive electrode material. The present invention utilizes the alkaline environment formed by the residual alkali generated during the water washing process of the ternary positive electrode material to oxidize the monomer dopamine to form o-phenolic anhydride, and the o-phenolic anhydride and dopamine undergo a condensation reaction to form polydopamine, which has strong adhesion and self-polymerization reaction, so the formed polydopamine can be evenly and densely coated on the surface of the ternary positive electrode material. Subsequently, the polydopamine evenly and densely coated on the surface of the ternary positive electrode material is carbonized using a catalyst to form a uniformly distributed nitrogen-doped graphene coating layer on the surface of the ternary positive electrode material, thereby improving the conductivity of the ternary positive electrode material, increasing the capacity, cycle performance and rate performance of the material, and effectively isolating the electrolyte from eroding the surface of the ternary positive electrode material. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0025] Figure 1 Schematic diagram of the reaction process of the nitrogen-doped graphene-coated ternary positive electrode material in Example 1 of the present invention;
[0026] Figure 2 This is a SEM image of the nitrogen-doped graphene-coated ternary positive electrode material prepared in Example 1 of the present invention;
[0027] Figure 3 This is a SEM image of the nitrogen-doped graphene-coated ternary positive electrode material prepared in Comparative Example 1 of the present invention;
[0028] Figure 4 It is a result diagram of battery cycle capacity retention rate in the experimental example of the present invention;
[0029] Reference numerals:
[0030] 1-Dopamine monomer. DETAILED DESCRIPTION
[0031] The following examples are provided for a better understanding of the present invention, but are not intended to limit the best mode of implementation, nor to limit the content and protection scope of the present invention. Any product identical or similar to the present invention obtained by anyone under the inspiration of the present invention or by combining the features of the present invention with other prior arts shall fall within the protection scope of the present invention.
[0032] If no specific experimental steps or conditions are specified in the examples, the conventional experimental steps or conditions described in the literature in the field can be used. If no manufacturer is specified for the reagents or instruments used, they are all conventional reagent products that can be obtained commercially.
[0033] Example 1
[0034] This embodiment provides a method for preparing a nitrogen-doped graphene-coated ternary positive electrode material, and the specific steps and parameters are as follows:
[0035] (1) 10.5 mol LiOH, 10 mol Ni 0.7 Co 0.1 Mn 0.2 (OH) 2 , mixed evenly in a high-speed mixer, and sintered at 750℃ for 10h to obtain Li 1.05 Ni 0.7 Co 0.1 Mn 0.2 O 2 Positive electrode material.
[0036] (2) 10 mol of Li 1.05 Ni 0.7 Co 0.1 Mn 0.2 O 2 The positive electrode material was dispersed in 500 g of water, 1 mol of dopamine monomer was added, and stirring was continued for 30 min at a speed of 500 rpm to obtain a dispersion.
[0037] (3) The dispersion was centrifuged at 2000 rpm for 30 min, and the obtained precipitate was dried in a vacuum oven at 105° C. (−0.1 MPa) for 5 h to obtain a polydopamine-coated positive electrode material as an intermediate.
[0038] (4) 10 mol of the intermediate and 0.02 mol of nano-nickel were mixed evenly, and sintered at 650° C. for 12 h in an argon atmosphere to obtain a nitrogen-doped graphene-coated ternary positive electrode material.
[0039] In step (2), the water washing liquid of the ternary material is alkaline. Dopamine monomer 1 reacts spontaneously in the alkaline solution to form polydopamine. Polydopamine has strong viscosity and is adsorbed on the surface of the ternary material to form a stable polydopamine coating layer. The solid and liquid are separated to obtain the polydopamine-coated ternary material.
[0040] Step (4) reaction diagram Figure 1 It can be seen that polydopamine is evenly and densely distributed on the surface of the ternary positive electrode material, that is, the intermediate is obtained. In the presence of a catalyst, after high-temperature sintering treatment, a uniformly distributed coating layer can be formed on the surface of the ternary positive electrode material. The nitrogen-doped graphene-coated ternary positive electrode material obtained in this embodiment is scanned by an electron microscope. Figure 2 .
[0041] Example 2
[0042] This embodiment provides a method for preparing a nitrogen-doped graphene-coated ternary positive electrode material, and the specific steps and parameters are as follows:
[0043] (1) 10.5 mol LiOH, 10 mol Ni 0.7 Co 0.1 Mn 0.2 (OH) 2 , mixed evenly in a high-speed mixer, sintered at 700℃ for 12h, and Li 1.05 Ni 0.7 Co 0.1 Mn 0.2 O 2 Positive electrode material.
[0044] (2) 10 mol of Li 1.05 Ni 0.7 Co 0.1 Mn 0.2 O 2 The positive electrode material was dispersed in 554 g of water, 0.1 mol of dopamine monomer was added, and stirring was continued at 600 rpm for 20 min to obtain a dispersion.
[0045] (3) The dispersion was centrifuged at 2500 rpm for 6 min, and the obtained precipitate was dried in a vacuum oven at 110° C. (−0.1 MPa) for 4 h to obtain a polydopamine-coated positive electrode material as an intermediate.
[0046] (4) 10 mol of the intermediate and 0.03 mol of nano-nickel were mixed evenly, and sintered at 700° C. for 10 h in an argon atmosphere to obtain a nitrogen-doped graphene-coated ternary positive electrode material.
[0047] Example 3
[0048] This embodiment provides a method for preparing a nitrogen-doped graphene-coated ternary positive electrode material, and the specific steps and parameters are as follows:
[0049] (1) 10.5 mol LiOH, 10 mol Ni 0.7 Co 0.1 Mn 0.2 (OH) 2 , mixed evenly in a high-speed mixer, sintered at 1000℃ for 8h, and obtained Li 1.05 Ni 0.7 Co 0.1 Mn 0.2 O 2 Positive electrode material.
[0050] (2) 10 mol of Li 1.05 Ni 0.7 Co 0.1 Mn 0.2 O 2 The positive electrode material was dispersed in 400 g of water, 1 mol of dopamine monomer was added, and stirring was continued for 40 min at a rotation speed of 400 rpm to obtain a dispersion.
[0051] (3) The dispersion was centrifuged at 2000 rpm for 60 min, and the obtained precipitate was dried in a 100° C. vacuum oven (−0.1 MPa) for 6 h to obtain a polydopamine-coated positive electrode material as an intermediate.
[0052] (4) 10 mol of the intermediate and 0.01 mol of nano-nickel were mixed evenly, and sintered at 600° C. for 14 h in an argon atmosphere to obtain a nitrogen-doped graphene-coated ternary positive electrode material.
[0053] Example 4
[0054] This embodiment provides a method for preparing a nitrogen-doped graphene-coated ternary positive electrode material, and the specific steps and parameters are as follows:
[0055] (1) 10.5 mol LiOH, 10 mol Ni 0.8 Co 0.1 Mn 0.1 (OH) 2 , mixed evenly in a high-speed mixer, sintered at 700℃ for 10h, and Li 1.05 Ni 0.8 Co 0.1 Mn 0.1 O 2 Positive electrode material.
[0056] (2) 10 mol of Li 1.05 Ni 0.8 Co0.1 Mn 0.1 O 2 The positive electrode material was dispersed in 500 g of water, 0.01 mol of dopamine monomer was added, and stirring was continued for 30 min at a speed of 500 rpm to obtain a dispersion.
[0057] (3) The dispersion was centrifuged at 2000 rpm for 30 min, and the obtained precipitate was dried in a vacuum oven at 105° C. (−0.1 MPa) for 5 h to obtain a polydopamine-coated positive electrode material as an intermediate.
[0058] (4) 10 mol of the intermediate and 0.02 mol of nano-iron were mixed evenly, and sintered at 650° C. for 12 h in a nitrogen atmosphere to obtain a nitrogen-doped graphene-coated ternary positive electrode material.
[0059] Example 5
[0060] This embodiment provides a method for preparing a nitrogen-doped graphene-coated ternary positive electrode material. The specific steps and parameters are the same as those in Example 1, except that the ternary material in step (1) is Ni 0.5 Co 0.2 Mn 0.3 (OH )2 .
[0061] Example 6
[0062] This embodiment provides a method for preparing a nitrogen-doped graphene-coated ternary positive electrode material. The specific steps and parameters are the same as those in Example 1, except that the ternary material in step (1) is Ni 0.9 Co 0.05 Mn 0.05 (OH) 2 .
[0063] Example 7
[0064] This embodiment provides a method for preparing a nitrogen-doped graphene-coated ternary positive electrode material. The specific steps and parameters are the same as those in Example 1, except that the lithium source in step (1) is lithium carbonate (0.5 mol).
[0065] Comparative Example 1
[0066] This comparative example provides a method for preparing a ternary positive electrode material, and the specific steps and parameters are as follows:
[0067] (1) 10.5 mol LiOH, 10 mol Ni 0.7 Co 0.1 Mn 0.2 (OH) 2, mixed evenly in a high-speed mixer, and sintered at 750℃ for 10h to obtain Li 1.05 Ni 0.7 Co 0.1 Mn 0.2 O 2 Positive electrode material.
[0068] (2) 10 mol of Li 1.05 Ni 0.7 Co 0.1 Mn 0.2 O 2 The positive electrode material was dispersed in 500 g of water and stirred at 500 rpm for 30 min to obtain a dispersion.
[0069] (3) The dispersion was centrifuged at 2000 rpm for 30 min, and the obtained precipitate was dried in a vacuum oven at 105° C. (−0.1 MPa) for 5 h to obtain an intermediate.
[0070] (4) 10 mol of the intermediate was sintered at 650°C for 12 h in an argon atmosphere to obtain a ternary positive electrode material.
[0071] The nitrogen-doped graphene-coated ternary positive electrode material obtained in this comparative example was scanned by an electron microscope and obtained Figure 3 .
[0072] Comparative Example 2
[0073] This comparative example provides a method for preparing a polydopamine-coated ternary positive electrode material, and the specific steps and parameters are as follows:
[0074] (1) 10.5 mol LiOH, 10 mol Ni 0.7 Co 0.1 Mn 0.2 (OH) 2 , mixed evenly in a high-speed mixer, and sintered at 750℃ for 10h to obtain Li 1.05 Ni 0.7 Co 0.1 Mn 0.2 O 2 Positive electrode material.
[0075] (2) 10 mol of Li 1.05 Ni 0.7 Co 0.1 Mn 0.2 O 2 The positive electrode material was dispersed in 500 g of water, 1 mol of dopamine monomer was added, and stirring was continued for 30 min at a speed of 500 rpm to obtain a dispersion.
[0076] (3) The dispersion was centrifuged at 2000 rpm for 30 min, and the precipitate was dried in a vacuum oven at 105 °C (-0.1 MPa) for 5 h to obtain polydopamine-coated Li 1.05 Ni 0.7 Co 0.1 Mn 0.2 O 2 Positive electrode material, to obtain a polydopamine-coated ternary positive electrode material.
[0077] Comparative Example 3
[0078] This comparative example provides a method for preparing a nitrogen-doped carbon-coated ternary positive electrode material, and the specific steps and parameters are as follows:
[0079] (1) 10.5 mol LiOH, 10 mol Ni 0.7 Co 0.1 Mn 0.2 (OH) 2 , mixed evenly in a high-speed mixer, and sintered at 750℃ for 10h to obtain Li 1.05 Ni 0.7 Co 0.1 Mn 0.2 O 2 Positive electrode material.
[0080] (2) 10 mol of Li 1.05 Ni 0.7 Co 0.1 Mn 0.2 O 2 The positive electrode material was dispersed in 500 g of water and stirred at 500 rpm for 30 min to obtain a dispersion.
[0081] (3) The dispersion was centrifuged at 2000 rpm for 30 min, and the obtained precipitate was dried in a vacuum oven at 105° C. (−0.1 MPa) for 5 h to obtain an intermediate.
[0082] (4) 10 mol of the intermediate, 1 mol of glucose and 1 mol of dicyandiamide were mixed evenly, and sintered at 650° C. for 12 h in an argon atmosphere to obtain a ternary positive electrode material.
[0083] Experimental example
[0084] The electrical conductivity of the ternary positive electrode materials prepared in Examples 1-4 and Comparative Examples 1-3 was tested by a powder resistance test. The specific steps were as follows: the final products prepared in Examples 1-4 and Comparative Examples 1-3 were ground through a 325-mesh sieve, about 1.00 g of the sample was weighed with weighing paper, the sample surface was smoothly placed into a sample holder, and the powder resistance of the material was tested under three 10 MPa pressures. The powder resistance model was FT-7200A automatic four-probe powder resistivity tester.
[0085] The final product prepared in Examples 1-4 and Comparative Examples 1-3 is a positive electrode material for a button battery. A button battery is assembled in the order of a negative electrode shell, a gasket, a gasket, a negative electrode material, a separator, a positive electrode material and a positive electrode shell. The battery is charged and discharged once at 0.2C, once at 0.5C and once at 1.0C to measure the discharge capacity, and then charged and discharged 200 times at 1C to test the cycle retention rate.
[0086] The test results are shown in Table 1.
[0087] Table 1 Positive electrode materials and button cell performance parameters
[0088]
[0089] In the embodiment of the present invention, dopamine monomer is added during the washing process of the positive electrode material, and the dopamine monomer self-polymerizes to form polydopamine. Under the catalysis of nano Ni particles, the polydopamine is thermally decomposed to catalyze the formation of nitrogen-doped graphene, thereby increasing the electronic conductivity of the material. After the battery is manufactured, the capacity and cycle performance are significantly improved, as shown in Table 1 and Figure 4 It can be seen that in Examples 1 to 4, the 0.2C first discharge is greater than 195.8 mAh / g, the 0.5C first discharge is greater than 189.5 mAh / g, and the 1C first discharge is greater than 184.6 mAh / g. The capacity retention rate after 200 cycles remains above about 94% of the initial discharge capacity.
[0090] In Comparative Example 1, the ternary material is washed to remove residual alkali, but dopamine monomer is not added during the washing process, and no nitrogen-doped graphene is formed on the surface of the final material. The material has poor conductivity, high resistivity, poor capacity and cycle performance, and the 0.1C first discharge and 0.5C first discharge decrease. The capacity retention rate after 200 cycles also decreases significantly, indicating that water washing alone cannot improve the surface conductivity of the material; in Comparative Example 2, the ternary material is washed to remove residual alkali, and dopamine monomer is added during the washing process to form a polydopamine-coated ternary material, but nitrogen-doped graphene is not formed under the catalysis of nano-Ni particles. Because the polyaniline polymer has poor conductivity, the final material has poor conductivity, high resistivity, poor capacity and cycle performance. In the comparative example 3, the residual alkali is removed during the washing process, but glucose is used as a long-chain carbon source, and a nitrogen source is additionally added. Under the catalysis of nano-Ni, nitrogen-doped graphene cannot be formed. This is because the long-chain carbon source is difficult to self-assemble to form a ring-shaped graphene structure of 6 C atoms, and finally a nitrogen-doped carbon material is formed, which is not as conductive as nitrogen-doped graphene. The data further proves that the electronic resistivity of the material obtained in comparative example 3 is higher than that of the material obtained in embodiments 1 to 4, indicating that the conductivity of the surface coating layer is not significantly improved, which further leads to poor capacity and cycle performance.
[0091] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the scope of protection of the invention.
Claims
1. A method for preparing a nitrogen-doped graphene-coated ternary cathode material, It is characterized in that The following steps are included: S1, adding dopamine monomer to a mixture of ternary cathode material and water under stirring, and performing solid-liquid separation to obtain an intermediate; S2, mixing the intermediate with the catalyst to obtain a mixture, and sintering the mixture in an inert atmosphere to obtain a nitrogen-doped graphene-coated ternary positive electrode material.
2. The preparation method according to claim 1, It is characterized in that In the mixed solution of the ternary positive electrode material and water in step S1, the concentration of the ternary positive electrode material is 18-25 mol / L.
3. The preparation method according to claim 2, It is characterized in that The molar ratio of the dopamine monomer to the ternary positive electrode material is (0.01-1):
10.
4. The preparation method according to claim 3, It is characterized in that The molar ratio of the intermediate to the catalyst is 10:(0.01-0.03).
5. The method for preparing the ternary cathode material according to claim 1, It is characterized in that The stirring speed in step S1 is 400-600 rpm, and the stirring time is 20-40 min.
6. The preparation method according to claim 5, It is characterized in that The solid-liquid separation steps in step S1 are centrifugation, drying, The centrifugal speed is 2000-2500rpm, and the centrifugal time is 6min-60min. The drying temperature is 100-110° C., and the drying time is 4-6 hours.
7. The preparation method according to claim 1, It is characterized in that The catalyst is at least one of nano nickel powder and nano iron powder; and / or, Therefore, the inert atmosphere is at least one of argon and nitrogen.
8. The preparation method according to claim 7, It is characterized in that In step S2, the sintering temperature is 600-700°C and the sintering time is 10-14h.
9. The preparation method according to claim 1, It is characterized in that The preparation method of the ternary positive electrode material is to mix the lithium source and nickel-cobalt-manganese hydroxide, and then sinter at 700-1000° C. for 8-12 hours.
10. The preparation method according to claim 9, It is characterized in that The lithium source is at least one of lithium hydroxide and lithium carbonate; and / or, The chemical formula of the ternary cathode material is Li x Ni a Co b Mn 1-a-b O 2 , where x is 1-1.2, a is 0.5-0.99, and b is 0.01-0.5.
Citation Information
Cited By
Preparation method of in-situ interface residual alkali conversion stable secondary battery positive electrode material
CN119430315A
Positive electrode material and preparation method thereof, positive electrode plate and battery