Thermoformable polymer sheets based on pseudo-amorphous polyaryletherketone
By adjusting the viscosity and thermoforming process of polyaryl ether ketone, the problem of difficult production of PEKK sheets in the prior art is solved, and a false amorphous sheet with high heat resistance and chemical resistance is realized The production of materials and semi-crystalline products improves the quality and consistency of thermoforming.
Patent Information
- Application Number
- CN202080072267.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-10-15
- Filing Date
- 2020-10-14
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2040-10-14
AI Technical Summary
The existing thermoforming methods are difficult to produce pseudo-amorphous PEKK sheets with high thickness and high T:I ratios, resulting in insufficient deformation resistance and chemical resistance of thermoformed PEKK sheets at high temperatures.
By adjusting the viscosity of polyaryl etherketone (PAEK) to a state of at least 400 Pa·s at 100 s-1, a mold thermoforming method, including a softening and crystallization step, forms a polymer sheet with pseudo-amorphic properties, And placed on the mold during the crystallization process to form a semi-crystalline molded article.
Achieved production of pseudo-amorphous PAEK sheets with thicknesses ranging from 1000 microns to 10,000 microns, with higher heat and chemical resistance, and the semi-crystalline products after thermoforming exhibit less than 5% dimensional variations, enhancing heat Quality and consistency of molding.
Smart Images

Figure BDA0003595939430000061 
Figure BDA0003595939430000072 
Figure BDA0003595939430000073
Abstract
Description
Technical Field
[0001] The present invention relates to polymer sheets suitable for use in thermoforming applications, wherein the polymer sheets are based on pseudo-amorphous polyaryletherketone (PAEK) polymers having certain melt viscosity properties. Background Art
[0002] High temperature thermoplastic polymers, such as polyaryletherketone (PAEK), are being evaluated as a choice for a variety of applications, including those in the aerospace and integrated circuit industries. In general, PAEK has excellent properties, including high temperature and chemical resistance, very good mechanical properties, excellent wear resistance, and natural flame retardancy. PAEK parts can be produced by a variety of methods, including thermoforming methods. However, PAEK parts formed by conventional thermoforming methods may not exhibit the desired deformation resistance and other properties at elevated temperatures.
[0003] Thermoforming is a conventional manufacturing method. In conventional thermoforming, a plastic sheet is heated to a high temperature and contacted with a cold (or room temperature) mold to form a desired shape. When a pseudo-amorphous sheet is thermoformed by such conventional thermoforming methods, the thermoformed part is rapidly cooled and is therefore also amorphous, and retains the properties of the amorphous sheet undergoing thermoforming. However, in certain applications, it is desirable to form a semi-crystalline part having the shape of the desired mold. There is still a need for such a thermoforming method: it can produce semi-crystalline parts from pseudo-amorphous sheets, thereby producing molded parts that exhibit increased heat resistance, improved chemical resistance, and improved mechanical properties compared to pseudo-amorphous parts formed by conventional thermoforming methods.
[0004] WO 2018 / 232119 (the entire disclosure of which is incorporated herein by reference for all purposes) describes such a method. The method comprises the following steps:
[0005] as a softening step, heating a sheet comprising at least one pseudo-amorphous polymer to a temperature above the glass transition temperature of the pseudo-amorphous polymer to soften the pseudo-amorphous polymer;
[0006] as a crystallization step, heating the sheet comprising the pseudo-amorphous polymer to a temperature above the glass transition temperature of the pseudo-amorphous polymer and below the melting temperature of the pseudo-amorphous polymer for a time sufficient to allow the pseudo-amorphous polymer to crystallize;
[0007] placing the sheet comprising the pseudo-amorphous polymer on a mold before crystallization occurs, during a softening step or a crystallization step; and
[0008] Forming semi-crystalline molded products,
[0009] The pseudo-amorphous polymer is a polyaryletherketone (PAEK) selected from the group consisting of polyetherketoneketone (PEKK), polyetherketone (PEK), polyetherketoneetherketoneketone (PEKEKK) and mixtures thereof.
[0010] Thermoformable polyaryletherketone sheets in which the polyaryletherketone is amorphous or only slightly crystalline (no more than 5 wt% crystallinity) are known in the art, as exemplified by the disclosure of U.S. Pat. No. 4,996,287. However, the procedure for preparing such PAEK sheets described in U.S. Pat. No. 4,996,287 has significant limitations. In particular, the patent teaches that when the T:I ratio of the PEKK used to prepare such sheets is relatively high (e.g., 70:30 or 80:20), the maximum sheet thickness that can be achieved is only 625 microns (see Table 1). Therefore, prior to the present invention, neither pseudo-amorphous PEKK sheets having high thickness (e.g., at least 1000 microns) and high T:I ratios nor methods for obtaining such sheets were known. However, since the properties of thermoformed PEKK sheets are significantly affected by both sheet thickness and T:I ratio, it is highly desirable to develop methods and compositions capable of producing relatively thick thermoformable pseudo-amorphous sheets comprising PEKK having a high T:I ratio (e.g., 70:30). Summary of the invention
[0011] One aspect of the present invention provides a sheet comprising a polymer, wherein the sheet has a thickness of about 1000 microns to about 10,000 microns (e.g., 1000 microns to 10,000 microns) and the polymer is a polyaryletherketone (PAEK) in a pseudo-amorphous state having a flow rate of 100 s at 100 s as measured by a parallel plate rheometer. -1 At least about 400 Pa·s (e.g., at least 400 Pa·s) at 360°C. It has been found that using a material that meets such a viscosity requirement (i.e., a viscosity at 100 s measured by a parallel plate rheometer) -1 PAEK having a viscosity at 360° C. of at least about 400 Pa·s (at least about 400 Pa·s) is key to being able to extrude relatively thick polymer sheets comprising PAEK having pseudo-amorphous properties and thus suitable for use in mold-involving thermoforming processes to produce semi-crystalline molded articles. Having polyaryletherketone in a pseudo-amorphous state in a sheet intended for thermoforming is desirable because higher crystallinity PAEK sheets tend to be too stiff to be easily used in the molding step of a thermoforming process.
[0012] A further aspect of the present invention provides a method for manufacturing a semi-crystalline article by thermoforming a sheet according to the above description using a mold. Such a method may comprise the following steps:
[0013] a) as a softening step, heating the sheet according to the above description to a temperature above the glass transition temperature of the polymer to soften the polymer;
[0014] b) as a crystallization step, heating the sheet to a temperature above the glass transition temperature of the polymer and below the melting temperature of the polymer for a time sufficient to allow the polymer to crystallize;
[0015] c) placing the sheet on a mold before crystallization occurs, during a softening step or a crystallization step; and
[0016] d) forming a semi-crystalline molded article.
[0017] The semi-crystalline article thus obtained may exhibit a dimensional change of less than about 5%, less than about 4%, less than about 3%, less than about 2%, or less than about 1% compared to the mold.
[0018] The present invention also provides a method for making a sheet comprising a polymer, wherein the sheet has a thickness of about 1000 microns to about 10,000 microns (e.g., 1000 microns to 10,000 microns) and the polymer is a polyaryletherketone (PAEK) in a pseudo-amorphous state having a flow rate of 100 s at 100 s as measured by a parallel plate rheometer. -1 A viscosity at 360° C. of at least about 400 Pa·s (or at least 400 Pa·s) wherein the method comprises:
[0019] a) heating a resin composition comprising a polymer to a suitable processing temperature above the melting point of the polymer to provide a molten resin composition;
[0020] b) forming the molten resin composition into a sheet (e.g., by melt extrusion through a suitably sized die); and
[0021] c) quenching the sheet at a rate effective to obtain the polymer in a pseudo-amorphous state. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 A WAXD diffraction pattern of a PEKK sheet according to the invention after extrusion is shown.
[0023] Figure 2 A WAXD diffraction pattern of a PEKK sheet after thermoforming according to one aspect of the present invention is shown. The peaks with an asterisk "*" on the top represent PEKK Form II, while the peaks without an asterisk represent PEKK Form I.
[0024] Figure 3 is a photograph of a sheet of PEKK according to the present invention (T:I=70:30, 3 mm thickness) after thermoforming. DETAILED DESCRIPTION
[0025] As used herein, the term "article" may be used interchangeably with "component" or "object." Exemplary articles of the invention may include (or may include portions thereof), for example, speaker cones, speaker stands, back-end / burn-in integrated circuit (IC) test sockets, IC wafer carriers, IC wafer handling tools, IC handling trays, electronic packaging, blister packaging, 3D electronic circuits, bearings, backplanes, bushings, sensors, switches, electronic product housings, tubes, cylinders, cups, containers, container lids, satellite panels, mirrors, pump components {e.g., impellers, stators, housings), aerospace components {e.g., cabinets, cabinet doors, tanks, control panels, toilets, passenger seat components, including backrests and chassis), compressed natural gas (CNG) or compressed liquefied petroleum gas (CLPG) composite tank forms, composite tool forms, laminated protective cover films {e.g., for FFF / FDM / RFF tools) and chemical storage containers. Exemplary articles of the present invention may include specialized parts with complex geometries for potential applications including, but not limited to, aerospace, aircraft, oil and gas, electronics, building and construction, piping, and high temperature vessels, among others.
[0026] As used herein and in the art, "thermoforming" (covering "vacuum forming") includes heating a sheet of material to a pliable temperature (e.g., in an oven) and forming the heated sheet onto a mold. Depending on the thermoforming method selected, as will be explained in more detail later), the mold may be relatively cold or relatively warm. For example, the mold may be at about room temperature, but in other embodiments, it may be at a temperature above room temperature, such as a temperature up to the glass transition temperature of the polymer contained in the sheet to be thermoformed. A vacuum may be used to stretch the heated sheet onto or over the mold, and it may be cooled thereon to produce a molded article. Conventional thermoforming methods include heating a sheet of material (e.g., a plastic sheet) to a high temperature (e.g., in an oven), such as a temperature above the glass transition temperature of the material, and contacting the heated sheet with a cold (e.g., room temperature) mold to form a desired shape. A vacuum may be used, for example, to stretch the sheet into or onto the mold. When a sheet of pseudo-amorphous material is subjected to such a conventional thermoforming method, the thermoformed part cools rapidly on the mold, thereby taking the form of the mold. The rapidly cooled thermoformed part retains the properties of the pseudo-amorphous sheet that underwent the thermoforming.
[0027] As used herein, the term "sheet" refers to a three-dimensional article (unlike a pill, sheet, or cylinder) that is typically flat or substantially planar and has a thickness that is significantly less than the length and width of the article. For example, a sheet may have a thickness that is less than 10% of both its length and width, or less than 5% of it. Sheets differ from films in having a greater thickness; sheets have a thickness of 500 microns or more, while films have a thickness of less than 500 microns. Sheets may be adhered to a substrate or completely separate from the substrate. Depending on the application and use, a sheet may be non-porous, porous, microporous, etc. For example, the thickness of a sheet may be measured using a standard micrometer.
[0028] As used herein, the term "pseudo-amorphous" polymer refers to a polymer having 0 wt% to 5 wt% crystallinity as determined by X-ray diffraction. Thus, the term "pseudo-amorphous" includes both completely non-crystalline polymers (0 wt% crystallinity, which may also be referred to as amorphous polymers) as well as polymers containing a limited degree of crystallinity (up to 5 wt%). For example, a pseudo-amorphous polymer as discussed herein may be 5 wt% or less crystallinity, preferably 3 wt% or less crystallinity, or 2 wt% or less crystallinity. As used herein, the term "semi-crystalline" polymer refers to a polymer having greater than 5 wt% crystallinity as determined by X-ray diffraction. A semi-crystalline polymer as discussed herein may have at least 6 wt% crystallinity or at least 7 wt% crystallinity as determined by X-ray diffraction.
[0029] As used herein, the term "about" also includes the exact value specified. For example, the range "about X to about Y" is understood to also include the range "X to Y". In addition, any stated range is understood to also include its endpoints (e.g., "X to Y" includes both X and Y values).
[0030] As used herein, each compound may be discussed interchangeably in terms of its chemical formula, chemical name, abbreviation, etc. For example, PAEK may be used interchangeably with polyaryletherketone, and PEKK may be used interchangeably with polyetherketoneketone. In addition, unless otherwise specified, each compound described herein includes homopolymers and copolymers. The term "copolymer" is intended to include polymers containing two or more different monomers and may include, for example, polymers containing two, three or four different repeating monomer units.
[0031] As used herein and in the claims, the terms "comprising" and "including" are inclusive or open-ended and do not exclude additional, unrecited elements, components, or method steps. Accordingly, the terms "comprising" and "including" encompass the more restrictive terms "consisting essentially of" and "consisting of."
[0032] The term polyaryletherketone ("PAEK") is intended to encompass all homopolymers and copolymers (including, for example, terpolymers), etc. In one embodiment, the polyaryletherketone is selected from polyetherketoneketone (PEKK), polyetheretherketone (PEEK), polyetherketone (PEK), polyetherketoneetherketoneketone (PEKEKK), and mixtures thereof. The at least one polyaryletherketone may optionally include more than one polyaryletherketone. In an embodiment, the "at least one polymer" may comprise, consist essentially of, or consist of at least one PAEK, in particular at least one PEKK.
[0033] As previously mentioned, the present inventors have discovered that the melt viscosity of the polymer or polymer combination used to make the thermoformable sheet is an important variable in being able to successfully obtain a sheet that is thick (at least about 1000 microns thick) and contains a polymer in a pseudo-amorphous state (i.e., not semi-crystalline). In particular, it has been discovered that polyaryletherketone (PAEK) or a combination of polymers comprising at least one PAEK should have a melt viscosity of 100 s as measured by a parallel plate rheometer. -1 The viscosity at 360°C is at least about 600 Pa·s. The viscosity can be measured using ASTM D4440-15. If the viscosity at 360°C measured by a parallel plate rheometer is less than 100 s -1 If the melt strength of the polymer is less than about 600 Pa·s at 100 s, the melt strength of the polymer may not be sufficient to allow extrusion of thick sheets (>1000 microns) having the desired substantially uniform thickness (i.e., the thickness of the extruded sheet will likely not be consistent). Preferably, the polyaryletherketone (PAEK) or a combination of polymers comprising at least one PAEK has a melt strength of less than about 600 Pa·s at 100 s as measured by a parallel plate rheometer. -1 More preferably, the polyaryletherketone (PAEK) or a combination of polymers comprising at least one PAEK has a viscosity at 100 s measured by a parallel plate rheometer. -1 According to certain embodiments, the viscosity of PAEK or a combination of polymers comprising at least one PAEK at 360° C. is at least about 800 Pa·s at 360° C. -1 The pressure does not exceed about 5000 Pa·s, as measured by a parallel plate rheometer.
[0034] In an exemplary embodiment, the polyaryl ketone comprises, consists essentially of, or consists of polyetherketoneketone (PEKK). Polyetherketoneketone suitable for use in the present invention may comprise, consist essentially of, or consist of repeating units represented by the following formulas I and II:
[0035] -AC(=0)-BC(=0)-I
[0036] -AC(=0)-DC(=0)-II
[0037] Wherein A is a ρ,ρ'-Ph-O-Ph-group, Ph is a phenylene group, B is a p-phenylene group, and D is a m-phenylene group. The isomer ratio of Formula I: Formula II (T:I) in the polyetherketoneketone may range from 100:0 to 0:100, but in various embodiments of the invention, may be from 50:50 to 90:10, or from 65:35 to 75:25, or from 68:32 to 72:28, or about 70:30, or 70:30. The isomer ratio may be readily varied as desired to obtain a particular set of properties, for example by varying the relative amounts of different monomers used to prepare the polyetherketoneketone. In general, a polyetherketoneketone having a relatively high ratio of Formula I: Formula II will have a faster crystallization rate than a polyetherketoneketone having a lower ratio of Formula I: Formula II. As is known in the art, samples can be prepared comprising PEKK having a high T:I ratio that is pseudo-amorphous (i.e., the PEKK is in a pseudo-amorphous state exhibiting no more than 5 wt% crystallinity), but which can be converted to a sample having semi-crystalline properties by subjecting the sample to certain heat treatments or processing.
[0038] Thus, the T:I ratio can be adjusted to control parameters such as the crystallization rate in PEKK. Generally speaking, a lower T:I ratio will provide a slower crystallization rate in an extruded sheet comprising PEKK, thereby providing a longer processing window. Conversely, a higher T:I ratio will provide a faster crystallization rate, thus providing a shorter processing window. In one embodiment, a polyetherketoneketone having a T:I isomer ratio of about 50:50 to about 90:10 can be used.
[0039] For example, the chemical structure of a polyetherketoneketone repeating unit [PEKK(T)] having all p-phenylene linkages can be represented by the following Formula III:
[0040]
[0041]
[0042] The chemical structure of the polyetherketoneketone repeating unit [PEKK(I)] having one meta-phenylene linking group in the main chain can be represented by the following formula IV:
[0043]
[0044] The chemical structure of a polyetherketoneketone repeating unit having perfectly alternating T and I isomers, such as a homopolymer having 50% of both T and I isomers [PEKK(T / I), i.e., PEKK having a 50:50 T:I ratio], can be represented by the following formula V:
[0045]
[0046] Polyaryletherketone can be prepared by any suitable method, many of which exist and are well known in the art. For example, polyaryletherketone can be formed by heating a substantially equimolar mixture of at least one bisphenol and at least one dihalobenzoid compound or at least one halogenated phenol compound. As another example, polyaryletherketone can be formed by contacting at least one aromatic acid chloride and at least one aromatic ether in the presence of a Lewis acid. Polymer can be pseudo-amorphous (including amorphous) or semi-crystalline, which can be controlled by the synthesis and processing of polymer. Polymers implemented in the embodiments disclosed herein are preferably pseudo-amorphous (including amorphous). In addition, polymers can also have any suitable molecular weight (as long as the minimum melt viscosity requirement is met) and can be functionalized or sulfonated if necessary. In one embodiment, polymers undergo sulfonation or any surface modification examples known to those skilled in the art.
[0047] Suitable polyetherketoneketone (PEKK) is available from a variety of commercial sources under various trade names. For example, polyetherketoneketone is available from Arkema Inc. under the trade name Many different polyetherketoneketone polymers are manufactured and supplied by Arkema Inc.
[0048] In addition to one or more polyaryletherketones, the pseudo-amorphous polymer used in the embodiments disclosed herein may also include other polymers. In one embodiment, the other polymers share similar melting points, melt stability, etc., and are compatible by showing complete or partial miscibility with each other. In particular, other polymers that show mechanical compatibility with polyaryletherketones may be added to the composition. However, it is also contemplated that the polymers do not have to be compatible with the polyaryletherketones. Other polymers may include, for example, polyamides (e.g., available from Arkema under the name Commercially available polyamide 11 and polyamide 12, poly (hexamethylene adipamide) or poly (8-hexamethylene amide)); fluorinated polymers such as PVDF, PTFE and FEP; polyimides such as polyetherimide (PEI), thermoplastic polyimide (TPI) and polybenzimidazole (PBI); polysulfone / sulfide such as polyphenylene sulfide (PPS), polyphenylene sulfone (PPSO2), polyethersulfone (PES) and polyphenylene sulfone (PPSU); poly (arylether); and polyacrylonitrile (PAN). In one embodiment, other polymers include polyamide polymers and copolymers, polyimide polymers and copolymers, and the like. Polyamide polymers may be particularly suitable for use in high temperature applications. Additional polymers may be blended with polyaryletherketone by conventional methods.
[0049] The pseudo-amorphous polymers used in the embodiments disclosed herein may also include additional components, such as fillers or additives, to achieve specific properties desired in specific applications, such as core-shell impact modifiers; fillers or reinforcing agents, such as glass fibers, carbon fibers, etc.; plasticizers; pigments or dyes; heat stabilizers; ultraviolet light stabilizers or absorbers; antioxidants; processing aids or lubricants; flame retardant synergists, such as Sb2O3, zinc borate, etc.; or mixtures thereof. These components may optionally be present, for example, in an amount of about 0.05 wt. % to about 70 wt. %, based on the total weight of the composition forming the polymer sheet or article (for forming the semi-crystalline article of the disclosed embodiments, wherein the article comprises a polymer in a semi-crystalline state, particularly PAEK). Preferably, any such filler or additive is non-nucleating.
[0050] Suitable fillers may include fibers, powders, flakes, etc. Reinforced fillers may be used. For example, suitable fillers may include at least one of carbon nanotubes, carbon fibers, glass fibers, polyamide fibers, hydroxyapatite, aluminum oxide, titanium oxide, aluminum nitride, silicon dioxide, aluminum oxide, barium sulfate, graphene, graphite, etc. The size and shape of the filler are also not particularly limited. Such fillers may optionally be present in an amount of about 0.1% by weight to about 70% by weight, or about 10% by weight to about 70% by weight (based on the total weight of the composition of the polymer sheet or article used in the disclosed embodiment).
[0051] Resin compositions comprising one or more polyaryletherketones, possibly in combination with one or more other polymers, fillers and / or other additives as described above, can be formed into sheets using the following general procedures, which can be adjusted or modified to best suit the particular resin composition being processed and the properties (e.g., thickness, degree of crystallinity) desired in the resulting thermoformable sheet.
[0052] The sheets of the present invention are relatively thick (i.e., the sheets have a thickness of at least about 500 microns, such as about 1000 microns to about 10,000 microns, preferably about 1000 to about 3500 microns) and contain at least one polyaryletherketone, such as polyetherketoneketone, in a pseudoamorphous state. Generally, the thickness of such sheets is substantially uniform. The length and width of the sheets can vary as desired for a particular end-use application, depending on the size of the molded article (including semi-crystalline molded article) to be prepared by thermoforming the pseudoamorphous sheet.
[0053] The thermoformable sheet according to the present invention is preferably manufactured by melt extrusion. Conventional single-screw or twin-screw extruders, tableting dies and winding devices designed for extruding thermoplastic resins into sheets can be used. The extrusion temperature will depend on the polymer melt temperature (which is affected by the T:I ratio in the case of PEKK) and the molecular weight or melt viscosity. For example, when the T:I isomer ratio in PEKK is 70:30 or 50:50, the preferred extrusion temperature is between about 360°C and about 380°C. As a further example, when the T:I isomer ratio is 60:40, the preferred extrusion temperature is between about 325°C and about 360°C. Generally, an extrusion temperature of about 5°C to about 70°C or about 10°C to about 50°C above the melting point of the polyaryletherketone is satisfactory. Extrusion temperatures close to the lower limit of the above range are preferred, and preferably should be lower than 400°C. Lower extrusion temperatures may be preferred so that the extruded resin composition has a viscosity that is conducive to extruding a sheet with uniform thickness and acceptable structural integrity and reducing the crystallization window time. In addition, as the sheet thickness increases, it is generally preferred to operate at the lower end of the usable temperature range. Higher extrusion temperatures are possible, but may result in an undesirably long time for the crystallization phase of the thermoforming process.
[0054] The extruded sheet containing polyaryletherketone is directly transferred from the die to a polished metal or textured roller (commonly referred to as a "chill roller") because the surface temperature of these rollers is maintained at a level below the melting temperature of the polymer. Air or other gas streams can also be directed to the extruded sheet to promote cooling. The rate at which the sheet cools and solidifies (called the quench rate) is an important aspect of achieving a pseudo-amorphous sheet structure. The quench rate is primarily determined by the temperature of the chill roller, the sheet thickness, and the line speed, and must be fast enough to achieve the desired pseudo-amorphous properties in the sheet without causing the sheet to warp, wrinkle, or curl too quickly. Typically, the extruded sheet is expected to cool to about room temperature as quickly as possible while avoiding any warping, wrinkling, or curling of the sheet. It is believed that the dependence of physical properties and thermoformability on the quench rate is related to inherent polymer properties (e.g., the solidification rate and crystallization rate of the polymer when it is cooled through its glass transition temperature). After extrusion and quenching, the extruded sheet may be cut or segmented to provide individual sheets having a size suitable for use in a particular desired thermoforming operation.
[0055] According to certain embodiments, a sheet according to the present invention may be reheated to a state where the sheet has softened (without significant crystallization) and then formed into an article, wherein the polymer (e.g., PAEK) present in the formed article then crystallizes (e.g., by heating to a higher temperature at which crystallization occurs).
[0056] The sheet according to the invention can be used in any type of molding process to produce a final molded article, but is particularly suitable for use in thermoforming. As will be described in more detail later, such a sheet is particularly useful for producing semi-crystalline molded articles in which the polymer component of the sheet has been transformed from a pseudo-amorphous state to a semi-crystalline state.
[0057] The shaped articles can be prepared from the sheet using a thermoforming process according to the present invention. Thermoforming is a process in which a thermoplastic sheet is heated to its processing temperature and, using mechanical means or a pressure differential created by vacuum and / or pressure, it is brought into contact with the mold surface and cooled while being held to the contours of the mold until it retains the shape of the mold. The sheet of the present invention is particularly useful in such a process because the thermoformed semi-crystalline molded article thus obtained can have dimensions very similar to the dimensions of the mold used to form such an article. For example, the semi-crystalline molded article can exhibit a dimensional change of less than about 5%, less than about 4%, less than about 3%, less than about 2%, or even less than about 1% compared to the mold. Thus, the sheet of the present invention makes it possible to produce thermoformed articles that exhibit less deformation, less shrinkage, and / or better dimensional tolerances compared to other PAEK-based sheets known in the art. The sheet before thermoforming can be transparent. As a result of the sheet being thermoformed and the increased crystallinity of the polyaryletherketone, the molded article obtained from the initially transparent sheet can be opaque.
[0058] The sheets of the present invention can be readily thermoformed by standard methods using standard equipment, such as by vacuum, pressure, mechanical or dual sheet thermoforming. The optimal thermoforming conditions will vary depending on the specific type of thermoforming machine and mold used, but such conditions can be easily established by techniques commonly and conventionally used in the art. For example, when the polyaryletherketone is polyetherketoneketone (PEKK), the thermoforming temperature range of the sheet (i.e., the temperature of the sheet during thermoforming) is typically in the range of 160°C to 300°C. However, sheet temperatures of about 160°C to about 220°C are generally preferred, because sheet temperatures greater than 220°C can result in excessively rapid crystallization rates.
[0059] The time required to heat the sheet to the thermoforming temperature range prior to the forming event can be an important variable in the process of thermoforming the sheet of the present invention. Generally speaking, in certain types of thermoforming procedures, it is desirable to minimize the preheating time while still maintaining a uniform heat distribution in the sheet so as to achieve uniform stretching during the forming step. Since the residence time will depend on process variables, such as sheet size (especially sheet thickness), thermal characteristics of a particular oven, and the desired forming temperature range, the ideal forming conditions must be determined experimentally, but can be easily determined by those skilled in the art of plastic thermoforming. For PEKK-based sheets, the residence time will typically be short, such as 1 to 5 minutes.
[0060] Although either radiant or convection ovens are suitable for preheating, radiant heaters are generally preferred because of their efficiency. Radiant heater surface temperatures are generally maintained between 500° C. and 1100° C., preferably between 600° C. and 900° C. Excessively high sheet temperatures or oven residence times can result in poor forming properties of the pseudo-amorphous polyaryletherketone-containing sheet, such as insufficient stretching or lack of mold definition and brittleness of the formed article.
[0061] Thermoforming of the sheet can be achieved by vacuum forming, with or without pressure or plug assistance. The vacuum level is typically at least 68 kPa. The forming pressure may range from atmospheric pressure to 690 kPa. For example, the mold temperature may range from ambient temperature to 290° C. According to certain embodiments of the present invention, a mold temperature of about 160° C. to about 280° C. may be employed. Elevated mold temperatures and / or additional pressures generally minimize internal stresses and provide better detail and material distribution, resulting in more uniform parts.
[0062] The sheet according to the present invention is particularly suitable for use in the thermoforming procedure described in WO 2018 / 232119 (the entire disclosure of which is incorporated herein by reference for all purposes). The procedure described in the aforementioned published patent application allows the production of semi-crystalline thermoformed parts from pseudo-amorphous polymer sheets (such as sheets according to the present invention). According to an embodiment of the present invention, a method for producing a molded part includes thermoforming a sheet according to the present invention under conditions effective to produce a semi-crystalline molded article.
[0063] According to one embodiment, a method of making a semi-crystalline article from a sheet comprising at least one pseudo-amorphous polymer comprises: a softening step, wherein the sheet is heated to a temperature above the glass transition temperature of the pseudo-amorphous polymer to soften the pseudo-amorphous polymer without substantial crystallization of the pseudo-amorphous polymer; and a crystallization step, wherein the at least one pseudo-amorphous polymer is heated to a temperature above the glass transition temperature of the pseudo-amorphous polymer and below the melting temperature of the pseudo-amorphous polymer for a time sufficient to allow the pseudo-amorphous polymer to crystallize (thereby forming a semi-crystalline polymer). During the softening step, it is contemplated that some crystallization may occur; however, preferably, if crystallization occurs during the softening step, such crystallization is less than about 10 wt%, less than about 5 wt%, less than about 2 wt%, less than about 0.5 wt%, less than about 0.1 wt%, or less than about 0.01 wt%. In some embodiments, the sheet comprising the pseudo-amorphous polymer may be placed on a mold during the softening step. In some embodiments, the sheet comprising the pseudo-amorphous polymer may be placed on a mold during the crystallization step before at least some crystallization occurs. A semi-crystalline molded article may be formed on the mold.The semi-crystalline molded article may be opaque; however, in certain embodiments, the semi-crystalline article may be nearly translucent or translucent.
[0064] During the crystallization step, the sheet can remain on the mold for a period of time ranging from a few seconds to several minutes, depending on factors such as the thickness of the sheet. For example, if the sheet is about 1000 microns to about 2000 microns thick, the sheet can remain on the mold for a period of time ranging from about 30 seconds to about 1 minute. As another example, if the sheet is about 3000 microns thick, the sheet can remain on the mold for 4 minutes or longer (e.g., up to about 6 to 7 minutes).
[0065] In some embodiments, the mold may be heated on at least one side. In some embodiments, the sheet containing the pseudo-amorphous polymer may be heated to a temperature above the glass transition temperature (Tg) of the pseudo-amorphous polymer during the softening step, for example, a temperature in the range of about 160°C to about 220°C or about 190°C to about 215°C during the softening step. During the softening step, in some embodiments, the temperature of the sheet can be measured using a non-contact method, such as by using a non-contact infrared gun. In some embodiments, the mold and the sheet containing the pseudo-amorphous polymer can be heated to a temperature in the range of about 210°C to about 280°C, about 230°C to about 260°C, or about 250°C during the crystallization step. In some embodiments, the temperature of the sheet containing the pseudo-amorphous polymer can be measured by using a probe in the mold.
[0066] In some embodiments, the sheet comprising a pseudo-amorphous polymer is placed on the mold during or immediately prior to the crystallization step. In some embodiments, the sheet comprising a pseudo-amorphous polymer may be placed on the mold using a vacuum after the softening step. In other embodiments, the sheet comprising a pseudo-amorphous polymer is held on the mold during both the softening step and the crystallization step.
[0067] In some embodiments, the molded article produced can exhibit at least 1 wt% higher crystallinity (in absolute terms), at least 5 wt% higher crystallinity, at least 10 wt% higher crystallinity, at least 15 wt% higher crystallinity, at least 20 wt% higher crystallinity, or at least 25 wt% higher crystallinity, or a crystallinity that is about 10 to about 30 wt% higher or about 10 to about 25 wt% higher than the crystallinity of the sheet comprising the pseudoamorphous polymer. For example, a molded article having 25 wt% crystallinity can be produced from a sheet comprising PEKK in pseudoamorphous form having 2 wt% crystallinity (an increase in crystallinity of 23 wt%, i.e., the molded article has a 23 wt% higher crystallinity than the starting pseudoamorphous PEKK-based sheet.
[0068] Illustrative aspects of the invention can be summarized as follows:
[0069] Aspect 1: A sheet comprising a polymer, wherein the sheet has a thickness of about 1000 microns to about 10,000 microns (or 1000 microns to 10,000 microns) and the polymer is a polyaryletherketone (PAEK) in a pseudo-amorphous state having a flow rate of 100 s at 100 s as measured by a parallel plate rheometer. -1 The viscosity at 360° C. is at least about 400 Pa·s (or at least 400 Pa·s).
[0070] Aspect 2: The sheet of Aspect 1, wherein the polymer has a flow rate of 100 s as measured by a parallel plate rheometer.-1 The viscosity at 360° C. is at least about 600 Pa·s (or at least 600 Pa·s).
[0071] Aspect 3: The sheet of Aspect 1, wherein the polymer has a flow rate of 100 s as measured by a parallel plate rheometer. -1 The viscosity at 360° C. is at least about 800 Pa·s (or at least 800 Pa·s).
[0072] Aspect 4: The sheet of Aspect 1, wherein the polymer has a flow rate of 100 s as measured by a parallel plate rheometer. -1 A viscosity at 360° C. of no greater than about 5000 Pa·s (or no greater than 5000 Pa·s).
[0073] Aspect 5: The sheet of any of Aspects 1 to 4, wherein the polyaryletherketone (PAEK) is selected from the group consisting of polyetherketoneketone (PEKK), polyetherketone (PEK), polyetherketoneetherketoneketone (PEKEKK), and combinations thereof.
[0074] Aspect 6: The sheet of any of Aspects 1 to 5, wherein the polyaryletherketone (PAEK) is polyetherketoneketone (PEKK).
[0075] Aspect 7: The sheet of Aspect 6, wherein the polyetherketoneketone (PEKK) has a T:I isomer ratio of about 50:50 to about 90:10 (or 50:50 to 90:10).
[0076] Aspect 8: The sheet of Aspect 6, wherein the polyetherketoneketone (PEKK) has a T:I isomer ratio of about 65:35 to about 75:25 (or 65:35 to 75:25).
[0077] Aspect 9: The sheet of Aspect 6, wherein the polyetherketoneketone (PEKK) has a T:I isomer ratio of about 68:32 to about 72:28 (or 68:32 to 72:28).
[0078] Aspect 10: The sheet of Aspect 6, wherein the polyetherketoneketone (PEKK) has a T:I isomer ratio of about 70:30 (or 70:30).
[0079] Aspect 11: The sheet material of any of Aspects 1 to 10, wherein the sheet material further comprises one or more non-nucleating fillers.
[0080] Aspect 12: The sheet of any of Aspects 1 to 11, wherein the sheet further comprises one or more non-nucleating fillers selected from reinforcing fibers, pigments, heat stabilizers, antioxidants, glass spheres, silica, and talc.
[0081] Aspect 13: The sheet material of any of Aspects 1 to 12, wherein the sheet material is transparent.
[0082] Aspect 14: A method of making a semi-crystalline article, wherein the method comprises thermoforming the sheet according to any of aspects 1 to 13 using a mold.
[0083] Aspect 15: A method of making a semi-crystalline article, comprising:
[0084] a) as a softening step, heating the sheet according to any of aspects 1 to 13 to a temperature above the glass transition temperature of the polymer to soften the polymer;
[0085] b) as a crystallization step, heating the sheet to a temperature above the glass transition temperature of the polymer and below the melting temperature of the polymer for a time sufficient to allow the polymer to crystallize;
[0086] c) placing the sheet on a mold before crystallization occurs, during a softening step or a crystallization step; and
[0087] d) forming a semi-crystalline molded article.
[0088] Aspect 16: The semi-crystalline article obtained according to Aspect 14 or Aspect 15, wherein the semi-crystalline article exhibits a dimensional change of less than about 3% (or less than 3%) compared to the mold.
[0089] Aspect 17: A method of making a sheet according to any of aspects 1 to 13, wherein the method comprises:
[0090] a) heating a resin composition comprising a polymer to a suitable processing temperature above the melting point of the polymer to provide a molten resin composition;
[0091] b) forming the molten resin composition into a sheet; and
[0092] c) quenching the sheet at a rate effective to obtain the polymer in a pseudo-amorphous state.
[0093] In this specification, embodiments have been described in a manner that enables a clear and concise description to be written, but it is intended and will be understood that the embodiments may be combined or separated in various ways without departing from the present invention. For example, it will be understood that all preferred features described herein are applicable to all aspects of the present invention described herein.
[0094] In some embodiments, the invention herein can be interpreted as excluding any element or method step that does not substantially affect the basic and novel characteristics of the composition or method. In addition, in some embodiments, the invention can be interpreted as excluding any element or method step not specified herein.
[0095] Although the present invention is illustrated and described herein with reference to specific embodiments, the present invention is not intended to be limited to the details shown. On the contrary, various modifications may be made to the details within the scope and range of the equivalents of the claims and without departing from the present invention.
[0096] Example
[0097] Example 1
[0098] Using a single screw extruder and two chill roll systems, the extruder was prepared with a T:I ratio of 70:30 and the flow rate was measured by parallel plate rheometer at 100 s. -1 A 3 mm thick pseudo-amorphous sheet was produced from a PEKK copolymer having a viscosity of 850 Pa·s at 360° C. The extrusion temperature was set at 375° C. and the line speed was 0.5 m / min; cooling was provided only by chill rolls and ambient air.
[0099] The sheet was thermoformed using a shuttle-type thermoforming machine equipped with a vacuum forming female mold. The sheet was placed in a heated oven and taken out when the surface temperature of the sheet reached 210°C. The sheet was then quickly placed on the mold, and the mold was heated to 250°C with a torch heater. After vacuum forming, the part was allowed to contact the mold for 4 minutes before demolding so that crystallization could occur. The resulting object was opaque and crystalline in the area where it contacted the mold, and transparent in the area where it did not contact the mold. Wide-angle X-ray diffraction of the sheet before and after thermoforming showed that the crystallinity had increased from <1wt% before thermoforming to about 29wt% after thermoforming.
[0100] WAXD condition
[0101] The WAXD diffraction patterns of the polymer sheets were obtained using the following procedure. X-ray diffraction experiments were performed on a Rigaku SmartLab diffractometer. All data acquisition was done in 1D mode.
[0102] Experimental collection conditions:
[0103] WAXS : 1.0°-80.0° 2θ range. Step = 0.03°. Scanning speed = 1.0° / min.
[0104] IS = 1.0 mm; RS1 = 3.0 mm; RS2 = 3.1 mm. Cross beam optics.
[0105] Example 2
[0106] In this example, a computational study was performed to measure the crystallinity of extruded PEKK sheets with T:I ratios between 68:32 and 74:26 and thicknesses between 1 mm and 10 mm using a finite element model. The model specifies the density, thermal conductivity, and heat capacity of each PEKK grade, an extruder temperature of 380°C, an extrusion rate of 10 cm / min, and an extrusion rate of 65 W / m 2 Heat transfer coefficients of 1000 W / K were used with convective cooling in ambient air at 25°C (assuming some air circulation), and sheet thicknesses between 1 mm and 10 mm. The model uses crystallization rates based on isothermal and non-isothermal crystallization equations in Choupin, "Mechanical performances of PEKK thermoplastic composites linked to their processing parameters" (2017), with parameters adjusted to match the measured crystallization half-times for each grade. Table 1 lists the estimated maximum thickness required for extruded PEKK sheets by grade (T:I ratio) to maintain 5 wt% or less crystallinity in any portion of the sheet.
[0107] Table 1. Estimated maximum thickness of extruded PEKK sheets to maintain pseudo-amorphous sheets ("pseudo-amorphous" means that the crystallinity does not exceed 5 wt%)
[0108]
[0109] Comparative Example 1
[0110] Using a single screw extruder and two chill roll systems, the extruder was prepared with a T:I ratio of 70:30 and the flow rate was measured by parallel plate rheometer at 100 s. -1 A 3 mm thick pseudo-amorphous sheet was produced from a PEKK copolymer having a viscosity of 850 Pa·s at 360° C. The extrusion temperature was set at 375° C. and the line speed was 0.5 m / min; cooling was provided only by chill rolls and ambient air.
[0111] The sheet was thermoformed using a shuttle-type thermoforming machine equipped with a vacuum forming female mold. The sheet was placed in a heated oven and removed when the surface temperature of the sheet reached 210°C. The sheet was then quickly placed on the mold, which was heated to 120°C using only a torch heater. After vacuum forming, the part was allowed to remain in contact with the mold for 4 minutes before demolding. The resulting object was transparent. Wide-angle X-ray diffraction was performed on the sheet before and after thermoforming, indicating that the crystallinity remained <1wt% before and after thermoforming.
Claims
1. A method for producing a semi-crystalline product, comprising: a) as a softening step, heating a sheet comprising a polymer to a temperature above the glass transition temperature of the polymer to soften the polymer; b) as a crystallization step, heating the sheet to a temperature above the glass transition temperature of the polymer and below the melting temperature of the polymer, in the range of 210° C. to 280° C., for a time sufficient to allow crystallization of the polymer; c) placing the sheet on a mold before crystallization occurs, during a softening step or a crystallization step; and d) forming a semi-crystalline molded article, The polymer-containing sheet has a thickness of 1000 micrometers to 10,000 micrometers and the polymer is a polyaryletherketone (PAEK) in a pseudo-amorphous state having a flow rate of 100 s at 100 s as measured by a parallel plate rheometer. -1 The viscosity at 360°C is at least 600 Pa·s.
2. The method of claim 1, wherein the polymer has a flow rate of 100 s as measured by a parallel plate rheometer. -1 The viscosity at 360°C is at least 800 Pa·s.
3. The method of claim 1, wherein the polymer has a flow rate of 100 s as measured by a parallel plate rheometer. -1 The viscosity at 360°C is not greater than 5000 Pa·s.
4. The method of claim 1, wherein the polyaryletherketone (PAEK) is selected from the group consisting of polyetherketoneketone (PEKK), polyetherketone (PEK), polyetherketoneetherketoneketone (PEKEKK), and combinations thereof.
5. The method of claim 1, wherein the polyaryletherketone (PAEK) is a polyetherketoneketone (PEKK).
6. The method of claim 5, wherein the polyetherketoneketone (PEKK) has a T:I isomer ratio of 50:50 to 90:
10.
7. The method of claim 5, wherein the polyetherketoneketone (PEKK) has a T:I isomer ratio of 65:35 to 75:
25.
8. The method of claim 5, wherein the polyetherketoneketone (PEKK) has a T:I isomer ratio of 68:32 to 72:
28.
9. The method of claim 1, wherein the sheet material additionally comprises one or more non-nucleating fillers.
10. The method of claim 1, wherein the sheet further comprises one or more non-nucleating additives selected from the group consisting of reinforcing fibers, pigments, heat stabilizers, antioxidants, glass spheres, silica, and talc.
11. The method of claim 1 wherein the sheet is transparent.
12. Semi-crystalline article obtained according to the process according to any one of claims 1 to 11, wherein the semi-crystalline article exhibits a dimensional variation of less than 3% compared to the mould.