High-temperature resistant polyamide electronic packaging composition and its preparation method
By adding polyphenylene ether and aromatic polyhydric anhydride compatibilizers to dimer acid polyamides, the high temperature resistance and adhesion are improved, the stability problem of dimer acid polyamides in high temperature environments is solved, and the service life and production efficiency of encapsulation materials are increased.
Patent Information
- Application Number
- CN202011489427.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-12-16
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2040-12-16
AI Technical Summary
Existing dimer acid polyamides have insufficient high-temperature resistance and dimensional stability, making it difficult to meet the high-temperature environment requirements of 5G electronic products. Furthermore, the production efficiency of the packaging materials is low, and they are difficult to recycle.
Adding polyphenylene ether and aromatic polyhydric anhydride compatibilizers to dimer acid polyamide improves its high temperature resistance and adhesion to PCBs, while reducing water absorption. Low-pressure injection molding is then used for encapsulation.
It improves the high-temperature resistance and dimensional stability of polyamide electronic encapsulation adhesive, enhances its adhesion to PCBs, reduces water absorption, and improves production efficiency and the lifespan of encapsulation materials.
Smart Images

Figure BDA0002840305660000031 
Figure BDA0002840305660000032 
Figure BDA0002840305660000041
Abstract
Description
Technical Field
[0001] This application relates to electronic packaging compositions and methods for preparing the same, and particularly to high-temperature resistant polyamide electronic packaging compositions and methods for preparing the same. Background Technology
[0002] With the increasing prevalence of electronic products, corresponding technologies are also changing rapidly. Without special protection, electronic products are easily damaged during use, and electronic encapsulation adhesives primarily function to protect them. Especially now, as electronic products become more feature-rich and integrated circuit boards move towards high-density mounting and high-heat generation, the requirements for encapsulation adhesives are becoming increasingly stringent. These adhesives must not only be resistant to high temperatures, chemical corrosion, and moisture absorption, but also possess high dimensional stability, resistance to deformation, and good heat dissipation, capable of withstanding the high-power environments of 5G electronic circuits. Currently, silicone and epoxy resins are commonly used encapsulation adhesives, employing potting processes, which have long curing times, low production efficiency, and the encapsulation materials are not recyclable.
[0003] Due to their excellent physical and chemical properties, dimer acid polyamides, combined with low-pressure injection molding processes, are widely used in precision electronic packaging. They offer short curing times, high production efficiency, and excellent flame retardant and insulating properties, leading to their increasing application in electronic packaging in recent years. However, due to the limitations of the molecular chain structure of dimer acid polyamides, their high-temperature resistance is limited to around 200-210℃. For example, Henkel's Macromelt 2035 product is currently one of the best high-temperature resistant dimer acid polyamide adhesives. Improving the temperature resistance and dimensional stability of dimer acid polyamides to meet the requirements of the rapid development of 5G electronics is a pressing issue in this field. Summary of the Invention
[0004] The purpose of this invention is to improve the high-temperature resistance and high-temperature adhesion to PCBs of dimeric acid polyamide products containing aromatic and polyether groups by adding polyphenylene ether and compatibilizers. Simultaneously, it reduces the water absorption rate of the polyamide electronic encapsulation adhesive and improves its dimensional stability. This comprehensively enhances the safe use of polyamide electronic encapsulation adhesives in electronic packaging applications.
[0005] One aspect of the present invention provides a novel high-temperature resistant polyamide electronic packaging composition comprising the following components:
[0006] 1) 70-92% by weight dimer acid type polyamide hot melt adhesive,
[0007] 2) 3-25% by weight of polyphenylene ether, and
[0008] 3) 0.1-5% by weight of aromatic polyacid anhydride compatibilizer, based on the total weight of dimer acid type polyamide hot melt adhesive, polyphenylene ether and aromatic polyacid anhydride compatibilizer.
[0009] Another aspect of the present invention provides a method for preparing the above-described high-temperature resistant polyamide electronic packaging composition, comprising the following steps:
[0010] a) Mix dimer acid type polyamide hot melt adhesive, polyphenylene ether and aromatic polyacid anhydride compatibilizer evenly.
[0011] The high-temperature resistant polyamide electronic packaging composition of the present invention has a softening point of at least 220°C, a tensile strength of at least 20 MPa, low water absorption, and high shear strength. The high-temperature resistant polyamide electronic packaging composition of the present invention is suitable for electronic packaging, and particularly suitable for 5G electronic packaging. Detailed Implementation
[0012] In a preferred embodiment, the high-temperature resistant polyamide electronic packaging composition of the present invention comprises the following components:
[0013] 1) 75-90% by weight dimer acid type polyamide hot melt adhesive,
[0014] 2) 7-22% by weight of polyphenylene ether, and
[0015] 3) 0.5-3% by weight of aromatic polyacid anhydride compatibilizer, based on the total weight of dimer acid type polyamide hot melt adhesive, polyphenylene ether and aromatic polyacid anhydride compatibilizer.
[0016] In a more preferred embodiment, the dimer acid type polyamide hot melt adhesive used in the high-temperature resistant polyamide electronic packaging composition of the present invention comprises dimer acid copolymer units, aliphatic diacid copolymer units, aromatic diacid copolymer units, aliphatic and / or aromatic diamine copolymer units, and polyetheramine copolymer units.
[0017] In a more preferred embodiment, the softening point of the dimer acid type polyamide hot melt adhesive is generally in the range of 180 to 220°C, the melt viscosity range (260°C) is 800 mPa·s to 3000 mPa·s, preferably 800 to 2000 mPa·s; and the number average molecular weight Mn is generally 5000 to 30000, preferably 5000 to 15000.
[0018] In a more preferred embodiment, the dimer acid type polyamide hot melt adhesive contains C 16-20 Unsaturated aliphatic dimer acid polymerization units and polyamine polymerization units, wherein the polyamine polymerization units contain 50–95 mol% C 2-8 Aliphatic diamine polymerization units and 5–50 mol% polyether polyamine polymerization units, based on the total molar number of polyamine polymerization units, the polyamine polymerization units and C16-20 The molar ratio of unsaturated aliphatic dimer acid polymer units is (0.95–1.1):1, and the polyether polyamine is represented by the following molecular formula:
[0019]
[0020] Where x ≈ 2.5, 6.1, or 34,
[0021] Alternatively, the polyether polyamine can be represented by the following molecular formula:
[0022]
[0023] For example, see CN101372610A.
[0024] In another, more preferred embodiment, the dimer acid type polyamide hot melt adhesive comprises:
[0025] (1) Dicarboxylic acid copolymer unit, which includes:
[0026] (a) 50–90 mol% dimer acid copolymer units, and
[0027] (b) 10–50 mol% C6-C 14 Aliphatic dicarboxylic acid copolymer units, and
[0028] (c) 0–10 mol% aromatic dicarboxylic acids, based on the total molar number of dicarboxylic acid copolymer units; and
[0029] (2) Diamine copolymer unit, which includes:
[0030] (c) 70–95 mol% C2-C8 aliphatic diamine copolymer units; and
[0031] (d) 5-30 mol% aromatic diamine copolymer units, based on the total number of moles of diamine copolymer units; the number average molecular weight Mn of this polyamide hot melt adhesive is 5000-15000;
[0032] The aromatic diamine is represented by the following structural formula:
[0033]
[0034] For example, see CN102559129A.
[0035] In a more preferred embodiment, the polyphenylene ether used in the high-temperature resistant polyamide electronic packaging composition of the present invention is a non-toxic, transparent engineering plastic with low relative density, excellent mechanical strength, stress relaxation resistance, creep resistance, heat resistance, water resistance, water vapor resistance, and dimensional stability. It also has good dielectric properties, which can improve the water absorption rate, dimensional stability, and temperature resistance of polyamide adhesives, thereby enhancing the safety of polyamide adhesives in electronic applications.
[0036] In a more preferred embodiment, the polyphenylene ether used in the high-temperature resistant polyamide electronic packaging composition of the present invention has a weight-average molecular weight of 1500 to 15000 and a melting point of 235 to 265°C.
[0037] In a more preferred embodiment, the aromatic polyacid anhydride compatibilizer used in the high-temperature polyamide electronic packaging composition of the present invention includes, for example, benzoic anhydride, naphthic anhydride, or mixtures thereof, with benzoic anhydride being preferred.
[0038] In a more preferred embodiment, the phthalic anhydride includes phthalic anhydride, biphenyltetracarboxylic dianhydride, or mixtures thereof. Phthalic anhydrides, especially phthalic anhydrides, are highly reactive and can promote interpenetration and compatibility at the interface between dimer-type polyamides and polyphenylene ether systems. They also provide good wetting of the PCB substrate surface, improving the adhesion of the system to the PCB.
[0039] In a more preferred embodiment, the dimer acid type polyamide hot melt adhesive, polyphenylene ether and aromatic polyacid anhydride compatibilizer are mixed at a temperature of 230-250°C for 15-60 minutes, preferably 20-40 minutes, until homogeneous, thereby obtaining the high-temperature resistant polyamide electronic packaging composition of the present invention.
[0040] This invention presents a high-temperature resistant polyamide electronic packaging composition with advantages such as excellent high-temperature resistance, high toughness, low water absorption, good flowability, low injection pressure, and easy demolding. Compared with traditional dimer acid-based polyamides, it has advantages such as high softening point, high strength, impact resistance, heat resistance, water resistance, and moisture resistance. This polyamide electronic packaging material can be injection molded under low pressure, effectively encapsulating injection molded parts such as engineering plastics PA, ABS, and PC, and also has excellent adhesion to PCB printed circuit boards. After encapsulation, it does not damage electronic components and has high adhesion to the outer casing material of electronic components. At the same time, its service life is significantly improved compared with traditional dimer acid-based encapsulating adhesives.
[0041] In addition to the dimer acid type polyamide hot melt adhesive, polyphenylene ether and aromatic polyacid anhydride compatibilizer components mentioned above, the high temperature resistant polyamide electronic packaging composition of the present invention may also contain some conventional additives in the art, such as antioxidants, rheology modifiers, release agents, ultraviolet agents, etc., not exceeding 3% of the total mass.
[0042] The polyamide electronic packaging composition of the present invention has a softening point range of 220℃ to 255℃, preferably 230-250℃; it has high tensile strength, generally 20-30MPa; elongation of more than 200%; good toughness; low water absorption; and excellent adhesion performance to PCB boards at high and low temperatures. It can be used as a packaging material and molded using low-pressure injection molding process.
[0043] Example
[0044] The following embodiments are used to further illustrate the present invention, but it should be understood that these embodiments are not intended to limit the scope of protection of the present invention.
[0045] The polyamide electronic packaging compositions prepared in the following examples were tested for performance using the following methods:
[0046] Softening point test: The test shall be conducted in accordance with the standard GB / T 15332—94.
[0047] Melt viscosity test: The melt viscosity of the sample at 260℃ was tested according to the standard HG / T 3660-1999B method using a Brookfield DV-E rotational viscometer.
[0048] Tensile strength and elongation tests: conducted in accordance with GB / T 528-2009.
[0049] Water absorption test: Refer to GB / T 1034-2008. Sample size: 50mm*50mm*4mm. Soak for 24 hours at the specified water temperature. Test the weight gain before and after soaking.
[0050] Shear strength test: conducted according to GB / T 2790-1995. The substrate is semi-rigid PVC and rigid PCB circuit board. The semi-rigid PVC contains approximately 20% plasticizer; the PCB circuit board is 4C or 5C board.
[0051] Preparation Example 1:
[0052] 0.4 mol of dimer acid (brand name P1013, purchased from Croda, USA), 0.07 mol of sebacic acid, 0.03 mol of phthalic anhydride, 0.45 mol of ethylenediamine, 0.05 mol of polyetheramine D-2000 and other comonomers, as well as a small amount of antioxidant, were placed into a 1000 ml three-necked flask. Nitrogen gas was introduced to purge the mixture three times. After purging, the reactants in the flask were slowly heated to 180 °C, and the pressure was maintained at 0.2–0.5 MPa for 30 min. Then, the reaction temperature was slowly increased at a rate of 10 °C / h until it reached 240–260 °C, and this temperature range was maintained for at least 1 h, while the pressure was continued to be maintained. Afterward, nitrogen gas was introduced into the reaction flask to depressurize it, and the temperature was maintained for 1 h. When the distilled water reached 80% of the theoretical amount, the pressure was gradually reduced. Finally, the entire reaction was completed under high vacuum, with a vacuum reaction time of approximately 2–10 hours. Then, pressurize the mixture with nitrogen to atmospheric pressure, pour the polyamide onto the PTFE plate while it is still hot, and cut it into particles after it cools and solidifies.
[0053] The test results show that its softening point is 212℃, its molecular weight is 8100, and its melt viscosity at 260℃ is 1010 mPa·s. Other indicators are shown in Table 1.
[0054] Comparative Example 1:
[0055] The high softening point dimer acid type copolyamide prepared in Preparation Example 1 and Asahi Kasei high-flowability polyphenylene ether PPO1950J (glass transition temperature 210℃, melting point 260℃, molecular weight 7800) were accurately weighed in a mass ratio of 90:10. Then, antioxidants and polyamide wax were added as flow modifiers according to the amounts shown in Table 1. The mixture was then kneaded for 30 minutes at 240℃ in a YT-ML15D mixer (purchased from Dongguan Yitong Equipment Factory) and discharged.
[0056] The performance data of the product obtained by the above method are shown in Table 1.
[0057] Examples 1-6
[0058] The high softening point dimer acid type copolyamide prepared in Preparation Example 1, Asahi Kasei high flowability polyphenylene ether PPO (purchased from Asahi Kasei Corporation, Japan, molecular weight 5000-8000, melting point 235-265℃), and compatibilizer acid anhydride substances were accurately weighed in a certain amount according to the mass ratio shown in Table 1. Then, antioxidants and polyamide wax flow modifiers were added in the amounts shown in Table 1. The mixture was then kneaded together in a mixer (as above) at 240℃ for 30 minutes and discharged.
[0059] The performance data of the products obtained by the above method are detailed in Table 1.
[0060]
Claims
1. A high-temperature resistant polyamide electronic packaging composition, comprising the following components: 1) 70-92% by weight dimer acid type polyamide hot melt adhesive, 2) 3-25% by weight of polyphenylene ether, and 3) 0.1-5% by weight of aromatic polyacid anhydride compatibilizer, based on the total weight of dimer acid type polyamide hot melt adhesive, polyphenylene ether, and aromatic polyacid anhydride compatibilizer. The softening point of the dimer acid type polyamide hot melt adhesive is in the range of 180-220℃, and the number average molecular weight Mn is 5000-30000. The dimer acid type polyamide hot melt adhesive comprises dimer acid copolymer units, aliphatic diacid copolymer units, aromatic diacid copolymer units, aliphatic and / or aromatic diamine copolymer units, and polyetheramine copolymer units.
2. The high temperature resistant polyamide electronic encapsulation composition of claim 1, wherein, It includes the following components: 1) 75-90% by weight dimer acid type polyamide hot melt adhesive, 2) 7-22% by weight of polyphenylene ether, and 3) 0.5-3% by weight of aromatic polyacid anhydride compatibilizer, based on the total weight of dimer acid type polyamide hot melt adhesive, polyphenylene ether and aromatic polyacid anhydride compatibilizer.
3. The high temperature resistant polyamide electronic encapsulation composition according to claim 1 or 2, wherein, The polyphenylene ether used has a weight-average molecular weight of 1500–15000 and a melting point of 235–265℃.
4. The high temperature resistant polyamide electronic encapsulant composition of claim 1 or 2, wherein, The aromatic polyacid anhydride compatibilizers include benzoic anhydride, naphthic anhydride, or mixtures thereof.
5. The high temperature resistant polyamide electronic encapsulant composition of claim 1 or 2, wherein, It also contains no more than 3% by weight of antioxidants, rheology modifiers, release agents, UV agents, or mixtures thereof.
6. A method for preparing a high-temperature resistant polyamide electronic packaging composition according to any one of claims 1-5, comprising uniformly mixing dimer acid type polyamide hot melt adhesive, polyphenylene ether and aromatic polyacid anhydride compatibilizer.
7. The production method according to claim 6, wherein The mixing process is carried out at a temperature of 230-250°C.
Citation Information
Patent Citations
Low temperature resistant polyamide thermosol adhesive and use thereof
CN101372610A
Packaging bag (Dongguan sausage)
CN3188332D
Polyamide hot melt adhesive and application thereof
CN102559129A
Packaging material for LED filament