Method for regenerating hydrogenation catalyst

Through the stepwise controlled purging method of inert gas and air, the problem of poor catalyst activity recovery is solved, the rapid and efficient regeneration of the catalyst and the improvement of the efficiency of the ring hydrogenation reaction are achieved, and the risk of excessive temperature rise during the oxidation process is avoided.

CN114643082BActive Publication Date: 2024-10-11EVONIK OXENO GMBH & CO KG
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111549489.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-12-18
Filing Date
2021-12-17
Publication Date
2024-10-11
Estimated Expiration
2041-12-17

AI Technical Summary

Technical Problem

During the catalyst activity recovery process in the prior art, especially during the hydrogenation of aromatic substances, there are problems such as reduced activity and poor sediment removal. Especially when water and other substances that reduce hydrogenation activity are present, the catalyst regeneration effect is insufficient.

Method used

Use inert gas (such as nitrogen) to purge the catalyst, then gradually add air, control the gas flow ratio and temperature, and reduce the amount of inert gas until only air flows through. Through this step, the catalyst is regenerated in the range of 50-100°C to avoid The temperature rises excessively during the oxidation process to protect the catalyst.

Benefits of technology

It achieves rapid and effective activity recovery of the catalyst, improves the conversion rate of the ring hydrogenation reaction, reduces the oxygen concentration, avoids over-oxidation of the catalyst and increase in reactor temperature, and extends the service life of the catalyst.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to a method for regenerating a hydrogenation catalyst. The subject of the invention is a method for regenerating a catalyst for the hydrogenation of aromatic substances, which comprises a plurality of steps. First, a nitrogen purge is performed, then air is metered in stepwise, and then the nitrogen addition is stopped until only air is present.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for regenerating a catalyst for the hydrogenation of aromatic substances, which comprises a plurality of steps: firstly purging with nitrogen, then gradually metering in air, and then stopping the nitrogen addition until only air is present. Background Art

[0002] The hydrogenation of aromatic substances, in particular aromatic esters, in which the aromatic rings are hydrogenated, is known and is also referred to as ring hydrogenation. In this hydrogenation, for example, transition metal-containing catalysts are used. Suitable catalysts are known to those skilled in the art. Corresponding hydrogenation processes are also used on a large scale in industry.

[0003] As the duration of the hydrogenation increases, the catalyst used loses activity, whether due to clogging, loss or poisoning of the catalyst's active sites. If the loss of activity is too great and / or the hydrogenation process can no longer be operated sufficiently economically, the activity of the catalyst must be increased. This is achieved by a regeneration process in which the catalyst is freed from deposits and adhesions. The catalyst can be calcined in which deposits are removed at high temperatures (> 200° C.) in an air or inert gas atmosphere, but this can be problematic for certain catalysts or even purely from an energy perspective due to the high temperatures.

[0004] However, it is also possible to regenerate the catalyst by passing a gas stream through the catalyst, whereby the deposits are entrained and thus removed. Such a regeneration method for ruthenium catalysts is described, for example, in WO 2008 / 015103 A1. The regeneration disclosed there is characterized in that the catalyst is purged with an inert gas until the catalyst partially or even completely regains its activity. The reason given for the regeneration described there with reference to the hydrogenation of benzene is the removal of water, i.e. the drying of the catalyst.

[0005] However, the known method has the problem that the regeneration effect may be too small, especially when not only water has to be removed from the catalyst, or not only water but also other substances which reduce the hydrogenation activity are present on the catalyst. Summary of the invention

[0006] It was therefore an object of the present invention to provide a process for regenerating catalysts for the ring hydrogenation of aromatic substances, in particular aromatic esters, with which process an acceptable activity can be achieved more quickly and better.

[0007] This object is achieved by the process as claimed in claim 1. Preferred embodiments are given in the dependent claims. The process according to the invention is a process for regenerating a catalyst for the ring hydrogenation of aromatic substances, preferably for the ring hydrogenation of aromatic esters, in at least one reactor, wherein the process comprises the following steps:

[0008] ■ purging the at least one reactor in which the catalyst used is present with an inert gas, wherein the purging with the inert gas, preferably with nitrogen, is started at a temperature of 50 to 100° C.;

[0009] ■ During the reactor purge, air is gradually added to the inert gas until the proportion of air in the total volume is between 10% and 90% by volume; then

[0010] ■ Reduce the amount of inert gas, preferably nitrogen, during the reactor purge until only air is flowing through the reactor.

[0011] wherein the temperature in the reactor during the regeneration is at most 10° C. higher than the temperature at the reactor inlet of said aromatic substance, preferably aromatic ester, in the hydrogenation of said aromatic substance, preferably aromatic ester,

[0012] The catalyst comprises at least one transition metal on a support material, the transition metal being selected from iron, ruthenium, nickel, rhodium, platinum, palladium or a mixture thereof, and the support material being selected from activated carbon, silicon carbide, alumina, silicon dioxide, aluminosilicate, titanium dioxide, zirconium dioxide, magnesium oxide, zinc oxide or a mixture thereof.

[0013] By means of the process according to the invention, an advantageous regeneration of the hydrogenation catalyst can be achieved, whereby the catalyst activity can be increased very easily and quickly. The regeneration described herein thus enables the ring hydrogenation for producing the actual product of value to be subsequently put back into operation at an increased conversion and thus to be carried out more efficiently. At the same time, the more likely low oxygen concentration or a correspondingly controlled process sequence prevents the occurrence of excessive (optionally even only local) elevated temperatures in the reactor due to the oxidation process, which could damage the catalyst or, in the worst case, lead to damage to the reactor.

[0014] The ring hydrogenation of aromatic substances, especially aromatic esters, described herein is usually carried out in at least one reactor, that is, the ring hydrogenation can be carried out in one or more reactors each containing a suitable catalyst. The regeneration of the catalyst used in the present invention can be carried out in each of the reactors present. In the case of multiple reactors, each reactor can be regenerated in a staggered manner or simultaneously, wherein preferably all catalysts are regenerated simultaneously in all reactors present. Therefore, the advantage of the present invention is that the regenerated catalyst does not need to be removed from the reactor, but can be retained in the reactor in which the ring hydrogenation also occurs.

[0015] According to the invention, the method is applicable to all catalysts used in the ring hydrogenation of aromatic substances, in particular aromatic esters. The catalyst comprises at least one transition metal on a support material or consists of at least one transition metal on a support material. Suitable catalysts are also familiar to those skilled in the art and can be obtained, for example, from WO 03 / 103830 A1.

[0016] The transition metal of the catalyst to be regenerated is a metal selected from iron, ruthenium, nickel, rhodium, platinum, palladium or a mixture thereof. Ruthenium is a particularly preferred transition metal of the catalyst used in the present invention. The content of transition metal in the catalyst to be regenerated is generally 0.1% to 30% by mass. The ruthenium content calculated as metal is preferably 0.1% to 10% by mass, especially 0.3% to 5% by mass, and very especially 0.4% to 2.5% by mass.

[0017] The support material on which the transition metal is present is selected from activated carbon, silicon carbide, aluminum oxide, silicon dioxide, aluminosilicates, titanium dioxide, zirconium dioxide, magnesium oxide, zinc oxide or mixtures thereof. Preferred support materials are aluminum oxide, silicon dioxide, titanium dioxide and mixtures thereof. In addition, these support materials may contain alkali metals, alkaline earth metals and / or sulfur. In a particularly preferred embodiment of the present invention, the catalyst to be regenerated is an eggshell catalyst.

[0018] The method according to the invention for regenerating a catalyst for the ring hydrogenation of aromatic substances, preferably for the ring hydrogenation of aromatic esters, comprises three steps. These steps are carried out in the at least one reactor and they are therefore carried out without unloading the catalyst. In the three steps, a gas stream having a different composition according to the current step is led through the reactor in which the catalyst is present. This frees the catalyst from possible deposits and adhesions.

[0019] In a first step, an inert gas is passed through the reactor or reactors and thus purged. The inert gas may be selected from nitrogen, helium, neon, argon, carbon dioxide and mixtures thereof. Preferably nitrogen or carbon dioxide is used, because they are most easily and cheaply available. More preferably, nitrogen is the inert gas used for the process according to the invention.

[0020] Temperature is an important feature of the present invention. For example, the temperature in the reactor during the regeneration process should be at most 10°C higher than the temperature at the reactor inlet of the aromatic esters in the aromatic ester hydrogenation. Therefore, the teaching of the present invention should prevent the burning of the catalyst or the calcination of the catalyst, which may be caused by the optional extreme temperature increase caused by the addition of oxygen in the air. According to the present invention, the temperature in the reactor can be measured at various arbitrary positions in the reactor. The first step, i.e., purging with an inert gas, preferably with nitrogen, starts at a temperature of 50-100°C. Since the temperature in the cyclic hydrogenation occurring before regeneration may be higher than 100°C, it may be necessary to cool the reactor before regeneration, for example by simply leaving it to stand or by actively cooling the hydrogenated product through a cooler.

[0021] It is preferred that the temperature decreases over time during the regeneration process. However, subsequent steps may result in a temporary, short-term increase in temperature. Nevertheless, a decrease in temperature over time should be detectable, since the reactor or the gas flow is not heated in a targeted manner.

[0022] Before the first step, purging the reactor with an inert gas, preferably nitrogen, and after the hydrogenation has stopped, further steps may be carried out. Preferably the following steps are carried out:

[0023] depressurizing the at least one reactor to a pressure of less than 10 bar, preferably less than 7.5 bar, more preferably less than 5 bar;

[0024] Removing the remaining hydrogen from the at least one reactor by pressing in an inert gas, preferably nitrogen, to a pressure of more than 10 bar, preferably more than 12.5 bar, more preferably more than 15 bar and subsequently depressurizing the at least one reactor to a pressure of less than 10 bar, preferably less than 7.5 bar, more preferably less than 5 bar.

[0025] In a preferred embodiment, the process of pressurizing with an inert gas, preferably nitrogen, and subsequently depressurizing is carried out at least twice. This is followed by the first step of the regeneration method according to the invention, namely purging with an inert gas.

[0026] In the second step of the regeneration method according to the present invention, air is gradually added to the inert gas during the purge process of the reactor or reactors until the proportion of air in the total volume is 10% to 90% by volume, preferably 20% to 80% by volume, more preferably 20% to 60% by volume. The gradual addition of air is preferably carried out in at least 3 steps, wherein the air in the above proportion is present only by the last step. Oxygen is guided into the system by the addition of air, which can lead to oxidation reactions and thus local temperature rise. It is therefore recommended to monitor the temperature in the at least one reactor, for example using a suitable measuring sensor. It may be advantageous to have a plurality of measuring sensors in the at least one reactor so that the temperature rise that occurs locally can also be determined.

[0027] In a preferred embodiment, in the second step, more preferably also temporarily, the temperature during the step of gradually adding air is at most 20° C., more preferably at most 15° C. higher than at the beginning of the same corresponding step of gradually adding air. The air is added in a controlled manner here, which prevents burning of the catalyst and / or excessive oxidation of the catalyst. If higher temperatures still occur, even locally, it is advisable to take measures for reverse control. Preferably, according to the invention, when the temperature during the step of gradually adding air is 20° C., preferably 15° C. or more higher than at the beginning of the same corresponding step of gradually adding air, the (further) addition of air is at least temporarily stopped. It is also possible to additionally meter in an inert gas, preferably nitrogen, during the cessation of further addition of air.

[0028] The third step of the regeneration method according to the invention is characterized in that the amount of inert gas, preferably nitrogen, is gradually reduced during the reactor purge until the reactor is only still flowed through by air. This step can be carried out either only after the end of the second step or partly or completely during the execution of the second step. If a (local) increase in temperature occurs here, the reduction in the amount of inert gas can be temporarily stopped or even further inert gas, preferably nitrogen, can be metered in. When the addition of inert gas has completely ended, the third step, i.e. the flow of air, is preferably carried out at a temperature of up to 70° C. The temperature is preferably further reduced over time, preferably to ambient temperature, i.e. to a temperature of 20-35° C.

[0029] How long the regeneration as described herein must be carried out in order to increase the catalyst activity to a sufficient degree depends on various factors. Examples of these factors are the type and amount of impurities, or the characteristics of the reactor (size, diameter). The duration of the entire regeneration, i.e. the execution of all steps, is preferably at least 24 hours, more preferably at least 3 days. In the case of a shorter time, the equipment can be put back into operation more quickly. However, the regeneration is not so extensive at this time, and it may be necessary to regenerate as soon as possible.

[0030] The gas flow in each step of the method according to the invention is preferably in the range of m / h. 3 Catalyst at least 2 m 3 A volume flow of 100 mol / l is conducted through the reactor or through the catalyst. Such a volume flow enables a relatively fast regeneration. The gas streams in the individual steps of the regeneration can be conducted through the catalyst in the same or opposite flow direction, based on the flow direction in the hydrogenation; this is preferably carried out in the same flow direction.

[0031] The regeneration according to the invention is carried out when the catalyst is used for the ring hydrogenation of aromatic substances. In a preferred embodiment, the regeneration according to the invention is carried out when the catalyst is used for the ring hydrogenation of aromatic esters. The aromatic esters are preferably benzoates, phthalates, trimellitic esters or pyrolytic esters, preferably phthalates or trimellitic esters. These include phthalates, isophthalates, terephthalates and trimellitic esters. Phthalate esters are preferred, i.e. phthalates, isophthalates and terephthalates. Among them, C8- to C10-alkyl esters are particularly preferred, especially C8- to C10-alkyl esters of phthalic acid (e.g. dioctyl phthalate, diethylhexyl phthalate, diisononyl phthalate, dipropylheptyl phthalate) or C8- to C10-alkyl esters of terephthalic acid (e.g. dioctyl terephthalate, diethylhexyl terephthalate, diisononyl terephthalate, dipropylheptyl terephthalate).

[0032] The cyclohydrogenation is preferably carried out in the liquid phase. The cyclohydrogenation can be carried out continuously or discontinuously over a suspended catalyst or over a catalyst arranged in a fixed bed in block form. In the process according to the invention, preference is given to continuous cyclohydrogenation over a catalyst arranged in a fixed bed, wherein the product / reactant phase is predominantly in the liquid state under the reaction conditions. The reactor(s) is / are preferably operated as a trickle bed reactor which can be fully or partially overflowed.

[0033] If the cyclohydrogenation is carried out continuously over a catalyst arranged in a fixed bed, it is expedient to convert the catalyst into an active form before the first cyclohydrogenation. After regeneration, this activation is not absolutely necessary. Activation can be achieved by reducing the catalyst using a hydrogen-containing gas according to a temperature program. The reduction here can optionally be carried out in the presence of a liquid phase dripping through the catalyst. The liquid phase used here can be a solvent or a hydrogenation product. Under corresponding hydrogenation conditions, this activation can also be omitted, since this is also carried out under the reaction conditions.

[0034] Various process variants can be selected for the ring hydrogenation. It can be carried out adiabatically, polytropically or almost isothermally, i.e., in one or more stages, with a temperature rise of usually less than 10° C. In the latter case, all reactors (suitably tubular reactors) can be operated adiabatically or almost isothermally, and one or more adiabatically and others almost isothermally. In addition, the aromatic polycarboxylic acid esters can be hydrogenated in a straight-through manner or in the case of product circulation. There can also be two reactors, wherein the first reactor is operated in the case of product circulation and the second reactor is operated in a straight-through manner. The ring hydrogenation can also be carried out in the form of a trickle bed. The reactor here can also be partially or completely overflowed. In addition, more than two reactors can also be used. It will also be particularly preferred that all reactors except the last one are operated in the case of product circulation ("loop reactor") and only the last one is operated in a straight-through manner.

[0035] The cyclohydrogenation can be carried out in a three-phase reactor in a liquid / gas mixed phase or in the liquid phase in cocurrent, with the hydrogenation gas being distributed in a manner known per se in the liquid reactant / product stream. For uniform liquid distribution, improved heat output of the reaction and high space-time yields, the reactor is preferably heated to 100 % by volume with a flow rate of 20 % by volume per hour. 2 Empty reactor cross section 15-120, especially 25-80 m 3 When the reactor is operated in a straight-through mode, the specific catalyst loading (liquid hourly space velocity, LHSV) can be 0.1-10 h -1 The value of .

[0036] The ring hydrogenation can be carried out in the absence of a solvent or preferably in the presence of a solvent. The solvent used can be any liquid which forms a homogeneous solution with the reactants and products, is inert under the hydrogenation conditions and can be easily separated from the product. The solvent can also be a mixture of various substances and optionally contains water.

[0037] For example, the following can be used as solvents: linear or cyclic ethers, such as tetrahydrofuran or dioxane, and aliphatic alcohols in which the alkyl group has 1 to 13 carbon atoms. Preferred alcohols are, for example, isopropanol, n-butanol, isobutanol, n-pentanol, 2-ethylhexanol, nonanol, technical nonanol mixtures, decanol, technical decanol mixtures, tridecanol.

[0038] When an alcohol is used as solvent, it may be appropriate to use such an alcohol or such an alcohol mixture which is formed during the saponification of the product. This excludes the formation of by-products by transesterification. A further preferred solvent is the hydrogenation product itself.

[0039] By using a solvent, the concentration of aromatic substances in the reactor inlet can be limited, whereby better temperature control in the reactor can be achieved. This can minimize side reactions and thus lead to an increase in product yield. The aromatic substance content in the reactor inlet is preferably 1% to 35%, in particular 5% to 25%. In the case of a reactor operated in loop mode, the desired concentration range can be adjusted via the circulation rate (ratio of circulating hydrogenation effluent to reactants).

[0040] The ring hydrogenation can be carried out in the pressure range of 20-300 bar, preferably 40-200 bar. The hydrogenation temperature is preferably 60°C to 200°C, especially 80°C to 180°C.

[0041] The hydrogenation gas used can be any hydrogen-containing gas mixture which does not contain harmful amounts of catalyst poisons such as carbon monoxide or hydrogen sulfide. The inert gas component can be, for example, nitrogen or methane. Preferably, hydrogen with a purity of greater than 95%, in particular greater than 98%, is used. DETAILED DESCRIPTION

[0042] The invention is illustrated hereinafter by means of examples. These examples show exemplary embodiments and should not be construed as limiting.

[0043] Embodiment 1:

[0044] The process according to the invention was tested in an industrial large-scale plant. A ring hydrogenation of diisononyl phthalate (DINP) was carried out beforehand. The hydrogen required for the hydrogenation was taken from the existing plant network and compressed to the required reaction pressure by a compressor. The hydrogenation was carried out in a first reactor at a reaction pressure of about 100 bar and a reaction temperature of about 110° C. over a catalyst arranged as a fixed bed (1% Ru on TiO2 as support material). DINP was converted in the reactor to a residual concentration of about 10%. The process was carried out with two reactors: a main reactor and a post-reactor. The main reactor was operated as an adiabatic circulation reactor. The heat of reaction formed by the exothermic hydrogenation was discharged by circulating a large circulation flow back from the bottom of the main reactor via an air cooler to the top of the main reactor with a pump. Downstream of the air cooler, the reactant stream was metered into the circulation flow and regulated to the required temperature before entering the main reactor by regulating the circulation flow temperature. The discharge from the circulation flow of the main reactor was directed to the post-reactor. The remaining approximately 10% DINP in the discharge stream of the main reactor was hydrogenated to <100 ppm in the postreactor under similar reaction conditions as in the main reactor.

[0045] Subsequently, the reactor was first rendered inert. To this end, the reactor was depressurized to about 3 bar, then nitrogen was introduced to about 20 bar and depressurized again three times in order to remove residual hydrogen from the reactor.

[0046] Then comes regeneration. Regeneration begins at a reactor temperature of about 60-90°C in the inlet. For this purpose, the main reactor and the post-reactor are purged with nitrogen respectively. The amount of nitrogen is adjusted so that the pressure drop on each reactor is < 0.1 bar, which corresponds to about 5 Nm³ per hour and per m³ of catalyst material for the main reactor and about 15 Nm³ per hour and per m³ of catalyst material for the post-reactor. After 3-6 hours, air is gradually added in 4 steps over the course of 21 hours until the air ratio in the gas flow is about 50% of the volume flow. Subsequently, at a reactor temperature of 15-70°C, the addition of nitrogen is correspondingly reduced in 2 steps over the course of 7 hours until the reactor is only flowed through by air. In all steps, it should be noted that the temperature in the reactor does not increase by 10°C relative to the inlet temperature to avoid burning of the catalyst due to oxygen in the air. The flow of air continues for several days.

[0047] The hydrogenation rate constants were determined before and after the reaction and used to calculate the catalyst activity before and after. The rate constants were determined using the Aspen Plus® simulation software from Aspen Tech from various measurements of the equipment, with specific feed amounts ensuring data comparability.

[0048] In the context of this application, the catalyst activity is determined as a rate constant (k 当前 ) and the theoretical rate constant (k 理论 ) is determined by the relationship between the catalyst activity and the catalyst activity.

[0049]

[0050] The experimental results are shown in Table 1.

[0051] Table 1: Catalyst activity determined after regeneration

[0052] .

[0053] This shows that the regeneration according to the invention leads to a significantly higher catalyst activity.

Claims

1. A process for regenerating a catalyst for the ring hydrogenation of aromatic esters in at least one reactor, wherein the process The following steps are involved: ■ purging the at least one reactor in which the catalyst used is present with an inert atmosphere, wherein the purging is started with an inert atmosphere at a temperature of 50 to 100° C.; followed by ■ gradually adding air to the inert atmosphere during the reactor purge until the proportion of air in the total volume is 10% to 90% by volume; then ■ reducing the amount of inert atmosphere during the reactor purge until only air still flows through the reactor, wherein the temperature in the reactor during the regeneration is at most 10° C. higher than the temperature at the reactor inlet of the aromatic ester in the hydrogenation of the aromatic ester, The catalyst comprises at least one transition metal on a support material, the transition metal being selected from iron, ruthenium, nickel, rhodium, platinum, palladium or a mixture thereof, and the support material being selected from activated carbon, silicon carbide, alumina, silicon dioxide, aluminosilicate, titanium dioxide, zirconium dioxide, magnesium oxide, zinc oxide or a mixture thereof.

2. The method according to claim 1, wherein the temperature in the at least one reactor is monitored during the gradual addition of air and / or during the reduction of the amount of inert atmosphere.

3. The method according to claim 2, wherein the temperature during the gradual addition of air is at most 20°C higher than at the beginning of the corresponding step of gradual addition of air.

4. A method according to claim 2 or 3, wherein further addition of air is at least temporarily stopped when the temperature during the gradual addition of air is 20°C or more higher than the temperature at the start of the respective step of gradual addition of air.

5. The process according to claim 4, wherein an inert atmosphere is metered in during the shut down.

6. The process according to any one of claims 1 to 3, wherein the following steps are performed before purging the reactor with nitrogen: - depressurizing the at least one reactor to a pressure of less than 10 bar; • Removing the remaining hydrogen from the at least one reactor by pressing in an inert atmosphere to a pressure greater than 10 bar and subsequently depressurizing the at least one reactor to a pressure less than 10 bar.

7. The method according to claim 6, wherein the pressure into the inert atmosphere and the subsequent pressure reduction are performed at least twice.

8. The method according to any one of claims 1 to 3, wherein the duration of the entire regeneration, ie the performance of all steps, is at least 24 hours.

9. The method according to any one of claims 1 to 3, wherein the inert atmosphere is selected from nitrogen, helium, neon, argon, carbon dioxide and mixtures thereof.

10. The method of claim 1, wherein the aromatic ester is a benzoate, a phthalate, a trimellitic acid ester, or a pyromellitic acid ester.

11. The method according to claim 1, wherein the aromatic ester is a C8- to C10-alkyl ester of phthalic acid or a C8- to C10-alkyl ester of terephthalic acid.