Adhesive composition for tire cord, tire cord and tire

The adhesive composition composed of the reaction product of epoxy resin and glycol compound forms a three-dimensional network structure, which solves the problem of strength reduction caused by the increase in rigidity of fiber reinforced materials in the existing technology, and because it does not contain harmful resin, Environmentally friendly high bonding strength and strength improvement are achieved.

CN114651051BActive Publication Date: 2024-10-15KOLON INDUSTRIES INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202180006346.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2021-04-08
Filing Date
2021-04-09
Publication Date
2024-10-15
Estimated Expiration
2041-04-09

AI Technical Summary

Technical Problem

While the adhesive composition of existing tire cords improves the bonding strength between fibers and rubber, it may increase the rigidity of fiber reinforcements, thereby reducing strength, affecting tire performance, and contains harmful resorcinol -Formaldehyde resin (RF resin), harmful to the environment and human body.

Method used

Adopt an adhesive composition composed of the reaction product of epoxy resin and glycol compound, isocyanate compound, water-dispersed polyurethane, amine compound and solvent to form a three-dimensional network structure, improve bonding strength and stability, and avoid the use of RF resin , ensuring environmental friendliness.

Benefits of technology

It improves the bonding strength between tire cord and tire rubber and the strength of tire cord, avoids strength deterioration caused by excessive rigidity of epoxy resin, and improves the environment and human health because it does not contain harmful resin.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003633901970000131
    Figure BDA0003633901970000131
  • Figure BDA0003633901970000141
    Figure BDA0003633901970000141
  • Figure BDA0003633901970000142
    Figure BDA0003633901970000142
Patent Text Reader

Abstract

The present invention relates to an adhesive composition for tire cords, a tire cord comprising an adhesive layer formed by the adhesive composition, and a tire comprising the tire cords. According to the present disclosure, an environmentally friendly adhesive composition for tire cords is provided, which can not only improve the bonding strength between tire rubber and tire cords, but also improve the strength of tire cords.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to an adhesive composition for a tire cord, a tire cord including an adhesive layer formed of the adhesive composition, and a tire including the tire cord. Background Art

[0002] To increase the strength of the rubber structure, fiber reinforcement is used.

[0003] For example, in rubber tires, polyester fibers, polyamide fibers, aromatic polyamide fibers, polyvinyl alcohol fibers, etc. can be used as reinforcing materials.

[0004] In some cases, depending on the fiber, the adhesion between the fiber and the rubber is not good, and therefore, an adhesive is applied on the surface of the fiber to supplement the adhesion between the fiber and the rubber.

[0005] For example, in order to improve the bonding strength between raw cords used for tire cords and tire rubber, an adhesive is coated on polyester fibers.

[0006] Generally, in the adhesive composition used for the above purpose, a rubber (or latex) containing resorcinol-formaldehyde (hereinafter referred to as "RF") or a component derived therefrom is included.

[0007] However, since RF resins are harmful to humans and the environment, their use is strictly regulated. Therefore, research on adhesive compositions that do not contain RF resins is ongoing.

[0008] The adhesive composition may be disposed on the fiber reinforcement material by dipping or spraying. The adhesive composition should not only have appropriate fluidity but also have a uniformly dispersed solid content so that the performance improvement effect according to the adhesive composition can be fully and uniformly exhibited.

[0009] Meanwhile, although the adhesive composition improves the bonding strength between the fiber reinforcement and the tire rubber, the rigidity of the fiber reinforcement may be changed by the adhesive composition. In the case where the rigidity of the fiber reinforcement increases more than required, the strength of the fiber reinforcement will decrease, thereby, the performance of the tire including the fiber reinforcement will deteriorate. Summary of the invention

[0010] Technical issues

[0011] An object of the present invention is to provide an environmentally friendly adhesive composition for a tire cord, which can not only improve the adhesive strength between the tire rubber and the tire cord, but also improve the strength of the tire cord.

[0012] Another object of the present invention is to provide a tire cord having high adhesive strength and improved strength.

[0013] Still another object of the present invention is to provide a tire including the tire cord.

[0014] Technical Solution

[0015] Hereinafter, an adhesive composition for a tire cord, a tire cord, and a tire according to an embodiment of the present invention will be described in detail.

[0016] The technical terms in the present specification are used only to refer to specific embodiments, and unless they are particularly mentioned, they are not intended to limit the present invention.

[0017] Unless explicitly stated or it is obvious from the context that it is not intended to be so, a singular expression includes its plural expression.

[0018] As used herein, the terms "including" or "having" and the like are intended to indicate the presence of actual characteristics, numbers, steps, constituent elements or combinations thereof, and they are not intended to exclude the possibility of the presence or addition of one or more other characteristics, numbers, steps, constituent elements or combinations thereof.

[0019] According to the results of continuous research by the present inventors, the reaction product between the epoxy resin and the diol compound has a large molecular size and a relatively high soft segment ratio in the molecule compared to the initial epoxy resin. Therefore, the adhesive composition for tire cords containing the reaction product can be applied to any fiber substrate to provide excellent adhesive strength and appropriate rigidity, and can achieve improved strength.

[0020] According to one embodiment of the present invention, there is provided an adhesive composition for a tire cord, comprising:

[0021] Reaction products of epoxy resins and diol compounds;

[0022] Isocyanate compounds;

[0023] latex;

[0024] Water-dispersible polyurethane;

[0025] Amine compounds; and

[0026] Solvent.

[0027] The adhesive composition for a tire cord does not include an RF resin, and therefore, it does not cause environmental pollution and can improve a working environment.

[0028] In the adhesive composition for tire cords, a reaction product of an epoxy resin and a diol compound is included.

[0029] The reaction product of the epoxy resin and the diol compound has an epoxy functional group, thereby improving the reactivity and adhesion of the adhesive composition. The reaction product, together with the isocyanate compound described below, forms a three-dimensional network structure in the adhesive layer (or coating) formed by the adhesive composition, thereby improving the bonding strength and stability.

[0030] Specifically, the reaction product of the epoxy resin and the diol compound has a large molecular size compared to the initial epoxy resin, but has a relatively high soft segment ratio in the molecule. Therefore, the reaction product enables the adhesive composition to be applied to any fiber substrate to exhibit excellent bonding strength and appropriate rigidity.

[0031] Here, the soft segment refers to a segment including a carbon-carbon chain introduced from the diol compound into the molecule of the reaction product. The hard segment refers to a segment formed of an epoxy functional group and an isocyanate compound described below.

[0032] A fiber reinforcement material to which an epoxy resin having a relatively high hard segment ratio in a molecule is applied may show excessive rigidity, thereby causing deterioration in the strength of a tire cord.

[0033] According to one example, the reaction product may be obtained by reacting an epoxy resin with a diol compound at a weight ratio of 1:0.1 to 1:5.

[0034] Preferably, the reaction product can be obtained by reacting the epoxy resin with the diol compound in a weight ratio of 1:0.1 or greater than 0.1, or 1:0.5 or greater than 0.5, and 1:5.0 or less than 5.0, or 1:4.5 or less than 4.5, or 1:4.0 or less than 4.0, or 1:3.5 or less than 3.5, or 1:3.0 or less than 3.0.

[0035] Specifically, the reaction product can be obtained by reacting an epoxy resin with a diol compound in a weight ratio of 1:0.1 to 1:5.0, or 1:0.1 to 1:4.5, or 1:0.1 to 1:4.0, or 1:0.1 to 1:3.5, or 1:0.1 to 1:3.0, or 1:0.5 to 1:5.0, or 1:0.5 to 1:4.5, or 1:0.5 to 1:4.0, or 1:0.5 to 1:3.5, or 1:0.5 to 1:3.0.

[0036] In order to make the reaction product have a high soft segment ratio in the molecule, the diol compound is preferably used in a weight ratio of 1:0.1 or more based on the epoxy resin.

[0037] However, if the diol compound is used in excess, the epoxy equivalent of the reaction product will decrease, and therefore, the adhesion of the adhesive composition will deteriorate. Also, if the diol compound is used in excess, the molecular weight of the reaction product will increase excessively, and therefore, the adhesion of the adhesive composition will deteriorate. Therefore, preferably, the diol compound is used in a weight ratio of 1:5.0 or less based on the epoxy resin.

[0038] Preferably, the weight average molecular weight (Mw) of the reaction product of the epoxy resin and the diol compound is 700 g / mol to 1200 g / mol, or 700 g / mol to 1150 g / mol, or 730 g / mol to 1150 g / mol.

[0039] As used herein, weight average molecular weight refers to the weight average molecular weight of polystyrene conversion measured by GPC method. In the process of measuring the weight average molecular weight of polystyrene conversion by GPC, known analytical equipment, detectors such as refractive index detectors and analytical columns can be used, and commonly used temperature conditions, solvents and flow rates can be applied.

[0040] As a specific example of the measurement conditions, a polymer resin such as a polyurethane resin is dissolved in tetrahydrofuran (THF) to a concentration of 1.0 (w / w)% (about 0.5 (w / w)%, based on the solid content), and filtered using a syringe filter with a pore size of 0.45 μm, and then 20 μl of the solution is introduced into the GPC. Also, as the mobile phase of the GPC, tetrahydrofuran (THF) is used and introduced at a flow rate of 1.0 mL / min, as a chromatographic column, 1 Agilent PLgel 5 μm Guard (7.5×50 mm) and 2 Agilent PLgel 5 μm Mixed D (7.5×300 mm) are connected in series, as a detector, an Agilent 1260 Infinity II System RI Detector is used, and the measurement temperature is 40°C.

[0041] Polystyrene standard samples (STD A, STD B, STD C, STD D) prepared by dissolving polystyrene of various molecular weights in tetrahydrofuran at a concentration of 0.1 (w / w)% were filtered with a syringe filter having a pore size of 0.45 μm and introduced into GPC to form a calibration curve, which can be used to calculate the weight average molecular weight (Mw) of the polymer.

[0042] STD A(Mp):791,000 / 27,810 / 945

[0043] STD B(Mp):282,000 / 10,700 / 580

[0044] STD C(Mp):126,000 / 4430 / 370

[0045] STD D(Mp):51,200 / 1920 / 162

[0046] According to an example, the reaction product of the epoxy resin and the diol compound may be included in an amount of 0.5 wt % to 10.0 wt % in the adhesive composition for a tire cord.

[0047] Preferably, based on the total weight of the adhesive composition, the content of the reaction product may be 0.5 wt % or more, or 1.0 wt % or more; and 10.0 wt % or less, 5.0 wt % or less, or 4.5 wt % or less, or 4.0 wt % or less, or 3.5 wt % or less, or 3.0 wt % or less.

[0048] Specifically, based on the total weight of the adhesive composition, the content of the reaction product can be 0.5 wt % to 10.0 wt %, or 0.5 wt % to 5.0 wt %, or 0.5 wt % to 4.5 wt %, or 0.5 wt % to 4.0 wt %, or 0.5 wt % to 3.5 wt %, or 0.5 wt % to 3.0 wt %, or 1.0 wt % to 10.0 wt %, or 1.0 wt % to 5.0 wt %, or 1.0 wt % to 4.5 wt %, or 1.0 wt % to 4.0 wt %, or 1.0 wt % to 3.5 wt %, or 1.0 wt % to 3.0 wt %.

[0049] In order to prevent the reactivity and crosslinking degree of the adhesive composition from being reduced, preferably, the content of the reaction product is 0.5 wt % or more based on the total weight of the adhesive composition.

[0050] However, if the reaction product is used in excess, the curing degree of the adhesive composition will increase due to excessive reactivity, thereby deteriorating the adhesive strength of the adhesive layer formed by the adhesive composition. Therefore, preferably, based on the total weight of the adhesive composition, the content of the reaction product is 10.0 wt % or less.

[0051] There is no particular limitation on the kind of the epoxy resin, and those commonly used in the technical field to which the present invention pertains may be used.

[0052] As a non-limiting example, the epoxy resin may include one or more selected from bisphenol epoxy resins, novolac epoxy resins and oxazolidinone epoxy resins. The bisphenol epoxy resin may be a bisphenol A epoxy resin, a bisphenol F epoxy resin, etc. The novolac epoxy resin may be a novolac epoxy resin, a cresol novolac epoxy resin, etc. In addition, as the epoxy resin, commercially available epoxy resins may be used, such as EX614B from NAGASE, KETL6000 from Kolon, CL16 from Ipox Chemical, GE500 from Raschig, etc.

[0053] The epoxy equivalent of the epoxy resin may be 120 to 600 in consideration of reactivity and adhesive properties of the adhesive composition, and the like.

[0054] As the diol compound, a linear or branched aliphatic diol compound having 3 to 8 carbon atoms can be preferably used.

[0055] As non-limiting examples, the diol compound may include one or more selected from 1,3-propylene glycol, 1,4-butanediol, 1,3-butanediol, 2,3-butanediol, and 1,6-hexanediol.

[0056] Meanwhile, in the adhesive composition for a tire cord, an isocyanate compound is included.

[0057] The isocyanate compound serves as a cross-linking agent.

[0058] The isocyanate compound reacts with the reaction product to form a three-dimensional network structure in an adhesive layer (coating layer) formed of the adhesive composition, thereby improving adhesive strength and stability of the adhesive layer (or coating layer).

[0059] The isocyanate compound may be an isocyanate compound having a phenyl group. Specifically, the isocyanate compound may include one or more selected from methylene diphenyl diisocyanate (MDI), toluene diisocyanate (TDI), and hexamethylene diisocyanate (HDI).

[0060] In addition, as the isocyanate compound, a blocked isocyanate may be used. The blocked isocyanate compound may be prepared by a reaction in which a known blocking agent is added to a polyisocyanate compound.

[0061] As such end-capping agents, phenols such as phenol, thiophenol, chlorophenol, cresol, resorcinol, p-sec-butylphenol, p-tert-butylphenol, p-sec-amylphenol, p-octylphenol and p-nonylphenol can be used; secondary or tertiary alcohols such as isopropyl alcohol, tert-butyl alcohol, etc.; aromatic secondary amines such as diphenylamine, dimethylaniline, etc.; imides such as phthalic acid; lactams such as δ-valerolactam, etc.; caprolactams such as ε-caprolactam; active methylene compounds such as dialkyl malonates, acetylacetone, alkyl acetoacetates, etc.; oximes such as acetone oxime, methyl ethyl ketone oxime, cyclohexanone oxime, etc.; and basic nitrogen compounds such as 3-hydroxypyridine, acidic sodium sulfite, etc. can be used.

[0062] More specifically, commercially available water-dispersible blocked products such as IL-6 from EMS, DM-6500 from MEISEIChemical, etc. can be used as isocyanate.

[0063] According to one example, the isocyanate compound may be included in an amount of 1.0 wt % to 20.0 wt % in the adhesive composition for a tire cord.

[0064] Preferably, based on the total weight of the adhesive composition, the content of the isocyanate compound may be 1.0 wt % or more, or 2.0 wt % or more, or 3.0 wt % or more; and 20.0 wt % or less, or 18.0 wt % or less, or 16.0 wt % or less, or 15.0 wt % or less, or 14.0 wt % or less, or 12.0 wt % or less, or 10.0 wt % or less.

[0065] Specifically, based on the total weight of the adhesive composition, the content of the isocyanate compound may be 1.0 wt % to 20.0 wt %, or 1.0 wt % to 18.0 wt %, or 1.0 wt % to 16.0 wt %, or 1.0 wt % to 14.0 wt %, or 1.0 wt % to 12.0 wt %, or 1.0 wt % to 10.0 wt %, or 2.0 wt % to 20.0 wt %, or 2.0 wt % to 18.0 wt %, or % to 16.0 wt %, or 2.0 wt % to 14.0 wt %, or 2.0 wt % to 12.0 wt %, or 2.0 wt % to 10.0 wt %, or 3.0 wt % to 20.0 wt %, or 3.0 wt % to 18.0 wt %, or 3.0 wt % to 16.0 wt %, or 3.0 wt % to 14.0 wt %, or 3.0 wt % to 12.0 wt %, or 3.0 wt % to 10.0 wt %.

[0066] Preferably, the content of the isocyanate compound is 1.0 wt % or more based on the total weight of the adhesive composition so that sufficient crosslinking is performed in the adhesive layer formed from the adhesive composition.

[0067] However, if the isocyanate compound is used in excess, the curing degree of the adhesive layer will increase due to excessive crosslinking reaction, and the fatigue of the tire cord will increase. Therefore, preferably, the content of the isocyanate compound is 20.0 wt % or less based on the total weight of the adhesive composition.

[0068] Meanwhile, in the adhesive composition for a tire cord, latex is included.

[0069] The latex is an adhesive component and provides adhesive strength to the adhesive layer formed by the adhesive composition. Specifically, the latex improves the affinity and adhesive strength between the adhesive layer and the rubber composition.

[0070] The latex may include one or more selected from vinylpyridine-styrene-butadiene copolymer latex and modified latex thereof, styrene-butadiene latex and modified latex thereof, natural rubber latex, acrylate copolymer latex, butyl rubber latex and chloroprene rubber latex.

[0071] Preferably, as the latex, there may be used a latex prepared by dispersing the same kind of rubber component as that used in the rubber composition for a tire in water or an organic solvent.

[0072] As the latex, commercially available products such as LM-60 from Denaka, VP-150 from APCOTEX, VB-1099 from Nippon A&L, 5218 and 0653 from Closlen, etc. may be used as non-limiting examples.

[0073] According to an example, the latex may be included in an amount of 1.0 wt % to 30.0 wt % in the adhesive composition for a tire cord.

[0074] Preferably, based on the total weight of the adhesive composition, the content of latex may be 1.0 wt % or more, or 5.0 wt % or more, or 10.0 wt % or more; and 30.0 wt % or less, or 25.0 wt % or less, or 20.0 wt % or less, or 16.0 wt % or less.

[0075] Specifically, based on the total weight of the adhesive composition, the latex content can be 1.0 wt % to 30.0 wt %, or 1.0 wt % to 25.0 wt %, or 1.0 wt % to 20.0 wt %, or 1.0 wt % to 16.0 wt %, or 5.0 wt % to 30.0 wt %, or 5.0 wt % to 25.0 wt %, or 5.0 wt % to 20.0 wt %, or 5.0 wt % to 16.0 wt %, or 10.0 wt % to 30.0 wt %, or 10.0 wt % to 25.0 wt %, or 10.0 wt % to 20.0 wt %, or 10.0 wt % to 16.0 wt %.

[0076] Preferably, the content of the latex is 1.0 wt % or more based on the total weight of the adhesive composition so that sufficient adhesive strength and rubber affinity may be exhibited in an adhesive layer formed of the adhesive composition.

[0077] However, if the latex is used in excessive amounts, the adhesive layer formed by the adhesive composition cannot be cured and becomes very sticky, thereby reducing the manufacturing efficiency of the tire cord. Therefore, based on the total weight of the adhesive composition, it is preferred that the content of the latex is 30.0 wt % or less.

[0078] Meanwhile, in the adhesive composition for a tire cord, water-dispersed polyurethane is included.

[0079] Typically, polyurethane is prepared and dispersed while being dissolved in an organic solvent. However, organic solvents are harmful to the human body and the environment and are a fire hazard. Therefore, it may be preferred to use a water-dispersible polyurethane (which is a water-based polyurethane) instead of an organic solvent-based polyurethane.

[0080] Specifically, the water-dispersed polyurethane protects or captures the amine compound as a curing agent, so that the adhesive layer formed by the adhesive composition can be stably cured. In addition, the water-dispersed polyurethane has excellent affinity with rubber, so that the rubber composition for tire can be stably adhered to the adhesive layer. In addition, the water-dispersed polyurethane can provide excellent wear resistance and elasticity for the adhesive layer.

[0081] The water-dispersed polyurethane may contain, for example, 20 to 60 wt % of polyurethane and 40 to 80 wt % of water.

[0082] Polyurethane is a polymer compound having a urethane bond in a molecule, and generally, it can be formed by a reaction of a diisocyanate compound and a polyol.

[0083] The water-dispersible polyurethane may include one or more selected from polycarbonate-based urethane, polyester-based urethane, polyacryl-based urethane, polytetramethylene-based urethane, polycaprolactone-based urethane, polypropylene-based urethane, and polyethylene-based urethane.

[0084] According to an example, the weight average molecular weight (Mw) of the polyurethane included in the water-dispersed polyurethane may be 250,000 g / mol to 350,000 g / mol.

[0085] Specifically, the weight average molecular weight (Mw) of the polyurethane may be 250,000 g / mol or more, or 255,000 g / mol or more, or 260,000 g / mol or more, or 265,000 g / mol or more, or 270,000 g / mol or more, or 275,000 g / mol or more, or 280,000 g / mol or more, or 285,000 g / mol or more, or 290,000 g / mol or more, or 295,000 g / mol or more, or 300,000 g / mol or more, or 305,000 g / mol or more.

[0086] In addition, the weight average molecular weight (Mw) of the polyurethane can be, for example, 350,000 g / mol or less, or 345,000 g / mol or less, or 340,000 g / mol or less, or 335,000 g / mol or less, or 330,000 g / mol or less, or 325,000 g / mol or less, or 320,000 g / mol or less, or 315,000 g / mol or less, or 310,000 g / mol or less, or 305,000 g / mol or less, or 300,000 g / mol or less.

[0087] In the case where the above-mentioned weight average molecular weight (Mw) range of the polyurethane is satisfied, adhesive strength, abrasion resistance, and elasticity according to the use of the water-dispersed polyurethane may be ensured.

[0088] The preparation method of the water-dispersible polyurethane is not particularly limited as long as the above weight average molecular weight is satisfied. For example, the water-dispersible polyurethane can be obtained by neutralizing a prepolymer having units from polyester polyol, diol and diisocyanate with a neutralizing agent and then stirring with distilled water.

[0089] According to an example, the water-dispersed polyurethane may be included in an amount of 0.5 wt % to 10.0 wt % in the adhesive composition for a tire cord.

[0090] Preferably, based on the total weight of the adhesive composition for tire cord, the content of the water-dispersed polyurethane may be 0.5 wt % or more, or 1.0 wt % or more, or 1.5 wt % or more; and 10.0 wt % or less, or 8.0 wt % or less, or 5.0 wt % or less.

[0091] Specifically, based on the total weight of the adhesive composition for tire cord, the content of the water-dispersed polyurethane can be 0.5 wt % to 10.0 wt %, or 0.5 wt % to 8.0 wt %, or 0.5 wt % to 8.0 wt %, or 0.5 wt % to 5.0 wt %, or 1.0 wt % to 10.0 wt %, or 1.0 wt % to 8.0 wt %, or 1.0 wt % to 8.0 wt %, or 1.0 wt % to 5.0 wt %, or 1.5 wt % to 10.0 wt %, or 1.5 wt % to 8.0 wt %, or 1.5 wt % to 8.0 wt %, or 1.5 wt % to 5.0 wt %.

[0092] Preferably, the content of the water-dispersed polyurethane is 0.5 wt % or more based on the total weight of the adhesive composition for a tire cord, so that an adhesive strength improving effect may be exhibited.

[0093] However, if the water-dispersible polyurethane is used in an excessive amount, the adhesive layer formed by the adhesive composition cannot be cured and becomes very sticky, thereby deteriorating the adhesive strength and durability of the adhesive layer. Therefore, preferably, the content of the water-dispersible polyurethane is 10.0 wt % or less based on the total weight of the adhesive composition for tire cord.

[0094] Meanwhile, in the adhesive composition for a tire cord, an amine compound is included.

[0095] The amine compound serves as a curing agent. The amine compound can achieve or accelerate the curing of the adhesive composition, thereby forming a stable adhesive layer from the adhesive composition.

[0096] The type of the amine compound is not particularly limited, and an amine compound known to be useful as a curing agent may be used. For example, the amine compound may include one or more selected from aliphatic amines and alicyclic amines.

[0097] As a non-limiting example, as the amine compound, commercially available products such as Piperazine from DAEJUNG, G640 from Kukdo Chemical, HK511 from Huntsman, and the like may be used.

[0098] According to one example, the amine compound may be included in an amount of 0.1 wt % to 10.0 wt % in the adhesive composition for a tire cord.

[0099] Preferably, based on the total weight of the adhesive composition for tire cord, the content of the amine compound may be 0.1 wt % or more, or 0.2 wt % or more, or 0.3 wt % or more; and 10.0 wt % or less, or 5.0 wt % or less, or 3.0 wt % or less, or 2.5 wt % or less, or 2.0 wt % or less, or 1.5 wt % or less, or 1.0 wt % or less.

[0100] Specifically, the content of the amine compound may be 0.1 wt % to 10.0 wt %, or 0.1 wt % to 5.0 wt %, or 0.1 wt % to 3.0 wt %, or 0.1 wt % to 2.5 wt %, or 0.1 wt % to 2.0 wt %, or 0.1 wt % to 1.5 wt %, or 0.1 wt % to 1.0 wt %, or 0.2 wt % to 10.0 wt %, or 0.2 wt % to 5.0 wt %, or 0.2 ...%. % to 3.0 wt %, or 0.2 wt % to 2.5 wt %, or 0.2 wt % to 2.0 wt %, or 0.2 wt % to 1.5 wt %, or 0.2 wt % to 1.0 wt %, or 0.3 wt % to 10.0 wt %, or 0.3 wt % to 5.0 wt %, or 0.3 wt % to 3.0 wt %, or 0.3 wt % to 2.5 wt %, or 0.3 wt % to 2.0 wt %, or 0.3 wt % to 1.5 wt %, or 0.3 wt % to 1.0 wt %.

[0101] Preferably, the content of the amine compound is 0.1 wt % or more based on the total weight of the adhesive composition for a tire cord so that curing of the adhesive composition can be sufficiently achieved.

[0102] However, if the amine compound is used in excess, the adhesive strength of the adhesive layer formed by the adhesive composition may deteriorate due to overcuring. Therefore, preferably, the content of the amine compound is preferably 10.0 wt % or less based on the total weight of the adhesive composition for tire cord.

[0103] Meanwhile, in the adhesive composition for a tire cord, a solvent is included.

[0104] Preferably, water (H2O) may be used as the solvent.

[0105] More preferably, demineralized water, distilled water or the like can be used as the solvent.

[0106] According to an example, the content of the solvent in the adhesive composition for a tire cord is 60.0 wt % to 85.0 wt %.

[0107] Preferably, the content of the solvent may be 60.0 wt % or more, or 65.0 wt % or more, or 70.0 wt % or more; and 85.0 wt % or less, or 80.0 wt % or less, based on the total weight of the adhesive composition for a tire cord.

[0108] Specifically, based on the total weight of the adhesive composition for tire cord, the content of the solvent can be 60.0 wt % to 85.0 wt %, or 60.0 wt % to 80.0 wt %, or 65.0 wt % to 85.0 wt %, or 65.0 wt % to 80.0 wt %, or 70.0 wt % to 85.0 wt %, or 70.0 wt % to 80.0 wt %, or 70.0 wt % to 75.0 wt %, or 65.0 wt % to 70.0 wt %.

[0109] Preferably, the content of the solvent is 60.0 wt % or more based on the total weight of the adhesive composition for a tire cord in order to ensure mixing and dispersibility of the solid component.

[0110] However, if the solvent is used in an excessive amount, it may be difficult to form an adhesive layer by the adhesive composition, and it may take a long time to dry.Therefore, preferably, the content of the solvent is 85.0 wt % or less based on the total weight of the adhesive composition for a tire cord.

[0111] As an example, the content of water in the total composition may refer to the content of water mixed as a solvent.

[0112] As another example, the content of water in the total composition may refer not only to the content of water mixed as a solvent but also to the content of water mixed in other components such as water-dispersible polyurethane.

[0113] In addition, the adhesive composition for tire cords may further include conventional additives such as a chain extender, a dispersant, and a heat stabilizer.

[0114] The relative viscosity of the adhesive composition for tire cord measured using an Ubbelohde viscometer at 25° C. may be 2.0 to 3.0. Preferably, the relative viscosity of the adhesive composition for tire cord measured using an Ubbelohde viscometer at 25° C. may be 2.00 or more, or 2.20 or more; and 3.00 or less, or 2.85 or less, or 2.80 or less, or 2.77 or less, or 2.75 or less, or 2.70 or less.

[0115] Specifically, the relative viscosity of the adhesive composition for tire cord measured at 25° C. using an Ubbelohde viscometer may be 2.00 to 3.00, or 2.00 to 2.85, or 2.00 to 2.80, or 2.00 to 2.77, or 2.00 to 2.75, or 2.00 to 2.70, or 2.20 to 3.00, or 2.20 to 2.85, or 2.20 to 2.80, or 2.20 to 2.77, or 2.20 to 2.75, or 2.20 to 2.70.

[0116] By satisfying the above-mentioned viscosity range of the adhesive composition for a tire cord, when manufacturing the tire cord, an appropriate pick rate can be ensured, processability and productivity can be improved, and excellent adhesive strength can be provided.

[0117] Meanwhile, according to another embodiment of the present invention, there is provided a tire cord, comprising:

[0118] fibrous substrate; and

[0119] An adhesive layer is formed on the fiber base, and the adhesive layer is formed of the above-mentioned adhesive composition for tire cord.

[0120] With regard to the detailed description of the adhesive composition for tire cords, the above description applies.

[0121] The adhesive composition for tire cord does not contain RF resin or components derived therefrom, and is therefore environmentally friendly. In particular, the adhesive composition for tire cord can not only improve the bonding strength between tire rubber and tire cord, but also improve the strength of tire cord.

[0122] As the fiber base, those generally used as tire cords in the technical field to which the present invention pertains may be used without particular limitation.

[0123] For example, the fiber base may be raw cords including polyester fibers.

[0124] The adhesive layer may be formed by dipping the fiber base in the adhesive composition for a tire cord, or spraying the adhesive composition for a tire cord onto the fiber base.

[0125] The adhesive layer may be formed to have an appropriate thickness so that the adhesive strength between the tire rubber and the tire cord may be improved without hindering the performance of the fiber base.

[0126] When manufacturing a tire cord, the method of providing the adhesive composition for a tire cord on the fiber base, the drying and curing conditions, and the like can be changed within a general range as required.

[0127] According to one example, a method for preparing a tire cord may include: a first coating step, in which a fiber substrate is immersed in a first coating solution and dried to form a first coating layer on the fiber substrate; and a second coating step, in which the first coated fiber substrate is immersed in a second coating solution and dried to form a second coating layer on the first coating layer.

[0128] The first coating solution comprises a reaction product between an epoxy resin and a diol compound and an isocyanate. The first coating formed by the first coating solution provides an adhesive functional group for the fiber substrate.

[0129] The fiber substrate treated with the first coating solution is heat-treated at a temperature of 100° C. to 160° C. for 30 seconds to 150 seconds, thereby being dried. Thus, a first coating layer is formed on the fiber substrate. Subsequently, the fiber substrate is heat-treated at a temperature of 200° C. to 260° C. for 30 seconds to 150 seconds, thereby being cured. Through the heat treatment, the first coating layer can be stably formed on the fiber substrate.

[0130] The second coating solution is the above-described adhesive composition for tire cords.

[0131] The fiber substrate after the first coating is immersed in the second coating solution and heat-treated at a temperature of 100° C. to 160° C. for 30 seconds to 150 seconds, thereby being dried. Thus, the second coating layer is formed on the first coating layer. Subsequently, the fiber substrate is heat-treated at a temperature of 200° C. to 260° C. for 30 seconds to 150 seconds, thereby being cured. Through the heat treatment, the second coating layer can be stably formed on the first coating layer.

[0132] Meanwhile, according to still another embodiment of the present invention, a tire including the above tire cord is provided.

[0133] The tire may have conventional construction except for including the tire cords described above.

[0134] For example, the tire may include: a tread portion; a pair of shoulder portions, respectively extending to both sides surrounding the tread portion; a pair of sidewall portions, extending to respective shoulder portions; a pair of bead portions, respectively extending to respective sidewall portions; a carcass layer formed inside the tread portion, the shoulder portion, the sidewall portion and the bead portion; a cord located inside the carcass layer; a belt portion located between the inner surface of the tread portion and the carcass layer; and an inner liner bonded to the inner side of the carcass layer.

[0135] Beneficial Effects

[0136] According to the present disclosure, an environmentally friendly adhesive composition for a tire cord is provided, which can not only improve the adhesive strength between the tire rubber and the tire cord, but also improve the strength of the tire cord. DETAILED DESCRIPTION

[0137] The present invention will be described in more detail in the following examples. However, these examples are presented only to illustrate the present invention, and the scope of the present invention is not limited thereto.

[0138] Preparation Example A

[0139] (Preparation of reaction product between epoxy resin and diol compound)

[0140] An epoxy resin (EX614B from NAGASE) was mixed with a diol compound in the weight ratio described in Tables 1 to 3 below and stirred at room temperature (20° C.) for 2 hours to obtain reaction products #1 to #14. #C1 is an epoxy resin (EX614B from NAGASE) that was not reacted with a diol compound.

[0141] [Table 1]

[0142]

[0143] [Table 2]

[0144]

[0145] [Table 3]

[0146]

[0147] Preparation Example B

[0148] (Preparation of water-dispersed polyurethane)

[0149] Polyester polyol (weight average molecular weight of 2000g / mol), diol (1,6-hexanediol) and ionomer (dimethylolbutyric acid) were introduced into a reactor at a molar ratio of 1:0.2:0.8, and mixed at 75±5°C and atmospheric pressure for 4 hours to obtain a mixture. Based on polyester polyol, methylene diphenyl diisocyanate (MDI) was added to the mixture at a molar ratio of 1:2, and reacted for 2 hours to prepare a polyurethane prepolymer. The reaction temperature of the prepared polyurethane prepolymer was reduced to 60°C, and a neutralizer (triethanolamine, TEA) was introduced into a solvent (acetone) for dispersion. In the neutralized polyurethane prepolymer, distilled water was introduced so that the solid content became 60% by weight, and stirred. In addition, based on polyester polyol, a chain extender (ethylenediamine) was added at a molar ratio of 1:1, and stirred to obtain a water-dispersed polyurethane (weight average molecular weight: 308,000g / mol).

[0150] Examples 1 to 14 and Comparative Example 1

[0151] (Preparation of Adhesive Composition for Tire Cord)

[0152] The components were mixed in the contents (weight %) described in Table 4, Table 5, and Table 6 below, and stirred at room temperature (20° C.) for 24 hours to prepare respective adhesive compositions of Examples 1 to 14 and Comparative Example 1.

[0153] In the following Tables 4 to 6, the components marked with letters are as follows.

[0154] -E: the reaction product between the epoxy resin according to Preparation Example A and the diol compound, or the epoxy resin

[0155] -I: Isocyanate compound (IL-6 from EMS, caprolactam-terminated 4,4'-MDI)

[0156] -L: latex (0653 from Closlen, vinylpyridine-styrene-butadiene copolymer)

[0157] -U: water-dispersible polyurethane according to Preparation Example B

[0158] -A: Amine compound (Piperazine from DAEJUNG)

[0159] -S: solvent (softened water)

[0160] [Table 4]

[0161]

[0162] [Table 5]

[0163]

[0164] [Table 6]

[0165]

[0166] Comparative Example 2

[0167] (Preparation of Adhesive Composition for Tire Cord)

[0168] An adhesive composition was prepared by the same method as in Example 1, except that 1.2 wt % of an epoxy resin (EX614B from NAGASE) and 0.6 wt % of 1,4-butanediol were added together with the I, L, U, A and S components and stirred, instead of 1.8 wt % of the “reaction product between an epoxy resin and a diol compound” (E component) according to Preparation Example A #1 in Example 1.

[0169] Comparative Example 3

[0170] (Preparation of Adhesive Composition for Tire Cord)

[0171] An adhesive composition was prepared by the same method as in Example 1, except that 1.8 wt % of 1,6-hexanediol diglycidyl ether was added together with the I, L, U, A and S components and stirred, instead of 1.8 wt % of the "reaction product between an epoxy resin and a diol compound" (E component) according to Preparation Example A #1 in Example 1.

[0172] Manufacturing tire cord

[0173] Polyester yarn was used to prepare 2 primary twist yarns with a twist number of 360 TPM (Z direction). The two primary twist yarns were twisted together with a twist number of 360 TPM (S direction) to prepare a plied yarn (1650 dtex / 2 strands). The plied yarn thus prepared was used as the original cord.

[0174] The original cord was dipped in the adhesive composition of the example or comparative example and then heat-treated at a drying temperature of 150° C. and a curing temperature of 243° C. for 1 minute, respectively, to prepare a tire cord sample including an adhesive layer formed on the original cord.

[0175] Test example

[0176] (1) The relative viscosity of each composition of the Examples and Comparative Examples prepared above was measured using an Ubbelohde viscometer in a constant temperature water tank at 25° C. Before measuring the relative viscosity, a certain amount of demineralized water was introduced into the Ubbelohde viscometer, and then the viscosity of the demineralized water was measured.

[0177] The relative viscosity (RV) of each of the adhesive compositions of Examples and Comparative Examples was measured based on the measured viscosity of demineralized water.

[0178] (2) For each tire cord specimen having an adhesive layer formed of the adhesive composition of Examples and Comparative Examples, the adhesive strength per unit area was evaluated according to the ASTM D4393 standard test method.

[0179] Specifically, a rubber sheet with a thickness of 0.6 mm, a tire cord sample, a rubber sheet with a thickness of 0.6 mm, a tire cord sample, and a rubber sheet with a thickness of 0.6 mm were sequentially stacked and heated at 170° C., 60 kg / cm 2 The samples were vulcanized at a pressure of 100°C for 15 minutes to produce the samples. The samples were cut to prepare test specimens with a width of 1 inch. For reference, the rubber sheet is a sheet used in the carcass of the tire. By using a laminate using such a rubber sheet, the bonding strength between the tire cord and the carcass layer can be confirmed.

[0180] For the prepared sample, a peel strength test was performed at a speed of 125 mm / min at 25° C. using a universal testing machine (Instron) to measure the bonding strength between the tire cord and the carcass layer, and the average value of the three loads generated during the peeling process was determined as the bonding strength. The measured values ​​were normalized relative to the values ​​of the bonding layer formed by the adhesive composition of Example 1, and the results are shown in Tables 7 and 8 below.

[0181] (3) For the tire cord samples with the adhesive layer formed by each adhesive composition of the embodiment and the comparative example, the tire cord strength and rigidity were evaluated according to the ASTM D883 / D885M standard test method. The measured values ​​were normalized relative to the values ​​of the adhesive layer formed by the adhesive composition of Example 1, and the results are shown in Tables 7 and 8 below.

[0182] [Table 7]

[0183] Relative viscosity (RV) Adhesion strength (%) Stiffness(%) strength(%) Example 1 2.24 100 100 100 Example 2 2.26 98 105 94 Example 3 2.33 96 94 102 Example 4 2.21 97 102 97 Example 5 2.23 95 106 95 Example 6 2.29 99 97 103 Example 7 2.32 98 94 104 Example 8 2.41 98 92 106 Example 9 2.48 97 89 108 Example 10 2.53 96 88 108 Embodiment 11 2.55 95 84 108 Example 12 2.61 95 81 109 Example 13 2.63 95 79 109 Embodiment 14 2.77 94 78 109

[0184] [Table 8]

[0185] Relative viscosity (RV) Adhesion strength (%) Stiffness(%) strength(%) Comparative Example 1 2.14 87 124 79 Comparative Example 2 2.01 71 113 81 Comparative Example 3 2.11 59 40 98

[0186] Referring to Tables 7 and 8 above, it can be confirmed that the tire cord including the adhesive layer formed of the adhesive composition according to the Example not only has excellent adhesive strength with the tire rubber but also exhibits improved strength.

Claims

1. An adhesive composition for tire cord, comprising: 0.5 to 10.0 wt. % of a reaction product of an epoxy resin and a diol compound; 1.0 wt % to 20.0 wt % of an isocyanate compound; 1.0 to 30.0 wt. % latex; 0.5 to 10.0 wt. % of a water-dispersible polyurethane; 0.1 wt% to 10.0 wt% of an amine compound; and 60.0% to 85.0% by weight of a solvent, in, The reaction product is formed by reacting the epoxy resin with the diol compound in a weight ratio of 1:0.1 to 1:

5.

2. The adhesive composition for tire cord according to claim 1, wherein The epoxy resin includes one or more selected from bisphenol epoxy resin, novolac epoxy resin and oxazolidinone epoxy resin.

3. The adhesive composition for tire cord according to claim 1, wherein The diol compound is a linear or branched aliphatic diol compound having 3 to 8 carbon atoms.

4. The adhesive composition for tire cord according to claim 1, wherein The diol compound includes one or more selected from 1,3-propylene glycol, 1,4-butanediol, 1,3-butanediol, 2,3-butanediol and 1,6-hexanediol.

5. The adhesive composition for tire cord according to claim 1, wherein The isocyanate compound includes one or more selected from methylene diphenyl diisocyanate, toluene diisocyanate and hexamethylene diisocyanate.

6. The adhesive composition for tire cord according to claim 1, wherein The latex includes one or more selected from vinylpyridine-styrene-butadiene copolymer latex and modified latex thereof, styrene-butadiene latex and modified latex thereof, natural rubber latex, acrylate copolymer latex, butyl rubber latex and chloroprene rubber latex.

7. The adhesive composition for tire cord according to claim 1, wherein The water-dispersible polyurethane includes one or more selected from polycarbonate carbamate, polyester carbamate, polyacryl carbamate, polytetramethylene carbamate, polycaprolactone carbamate, polypropylene carbamate and polyethylene carbamate.

8. The adhesive composition for tire cord according to claim 1, wherein The amine compound includes one or more selected from aliphatic amines and alicyclic amines.

9. The adhesive composition for tire cord according to claim 1, wherein The solvent is water.

10. The adhesive composition for tire cord according to claim 1, wherein The composition has a relative viscosity of 2.0 to 3.0 measured at 25° C. using an Ubbelohde viscometer.

11. A tire cord, comprising: Fiber substrate; and An adhesive layer is formed on the fiber base, and the adhesive layer is formed of the adhesive composition for tire cord according to claim 1.

12. The tire cord according to claim 11, wherein The fiber base is raw cords including polyester fibers.

13. A tire comprising the tire cord according to claim 11.