A low-cost biodegradable composite film that can contact food, and its preparation method and use

By adopting a sandwich structure composite membrane design, using polybutylene terephthalate-co-succinate (PBST) as the core layer and polybutylene succinate (PBS) as the outer layer, the PBS problem is solved The problems of high manufacturing costs and complex PBST production have led to the realization of low-cost, high mechanical properties, and completely biodegradable food-grade composite films to meet the needs of the food packaging field.

CN114654852BActive Publication Date: 2024-10-22CHINESE TEXTILE ACAD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210287574.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-03-22
Publication Date
2024-10-22
Estimated Expiration
2042-03-22

AI Technical Summary

Technical Problem

In the existing technology, polybutylene succinate (PBS) has limited its wide application in the field of food packaging due to its high manufacturing cost, and polybutylene terephthalate-co-succinate (PBST) ) Although it has good biodegradability, the production process is complicated and it is difficult to prepare food-grade slices, resulting in its limited application in the field of food packaging.

Method used

Composite membrane design with sandwich structure, the core layer is made of polybutylene terephthalate-co-succinate (PBST), and the outer layers on both sides are made of polybutylene succinate (PBS) , prepared through a composite stretched film process, controlling the cross-sectional area ratio between the core layer and the outer layer at 1.0-2.0:1 to ensure the mechanical properties and biodegradability of the composite film.

Benefits of technology

A low-cost, high-mechanical, and completely biodegradable composite film is achieved that meets food-grade requirements, reduces production costs, and expands the application scope in the food packaging field.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114654852B_ABST
    Figure CN114654852B_ABST
Patent Text Reader

Abstract

The present invention discloses a low-cost biodegradable composite film that can contact food, as well as a preparation method and use. The composite film includes a core layer and an outer layer located on both sides of the core layer, wherein the outer layer sandwiches the core layer, and the material of the core layer is polybutylene terephthalate-co-succinate (PBST), and the material of the outer layer is polybutylene succinate (PBS). In the cross section of the composite film, the ratio of the cross-sectional area of ​​the core layer to the cross-sectional area of ​​the outer layer is (1-2):1. The preparation method includes: composite film drawing of polybutylene terephthalate-co-succinate slices and polybutylene succinate slices, so that polybutylene terephthalate-co-succinate forms the core layer, and polybutylene succinate forms the outer layers on both sides to obtain a composite film. The composite film of the present invention has low cost, high mechanical properties, is completely biodegradable, meets food grade requirements, and can better meet the requirements of the field of food packaging.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of composite films, and in particular relates to a low-cost biodegradable composite film that can contact food, a preparation method and a use thereof. Background Art

[0002] Polybutylene succinate (PBS) is a polymer compound with the structural formula H-[O(CH2)4OOC(CH2)2CO] n -OH is a white semi-crystalline polymer. Its structural unit contains an ester group that is easily hydrolyzed. Under conditions such as composting and contact with specific microorganisms, it is easily decomposed and metabolized by a variety of microorganisms in nature or enzymes in animals and plants, and finally forms CO2 and H2O. It can be biodegraded and circulated in nature, so it is an ideal green polymer material.

[0003] The synthetic raw material source of polybutylene succinate (PBS) can be either petroleum resources or obtained by fermentation of biological resources, and large-scale production has been achieved at present. PBS has a wide range of uses, such as can be used for the preparation of biodegradable fibers, biodegradable films and plastic products. In addition, PBS can also be used as food packaging materials and other fields, but due to its high manufacturing cost, it is subject to certain restrictions in some wider food packaging fields. Therefore, how to prepare a biodegradable, low-cost film that can contact with food is a problem that needs to be solved.

[0004] In view of this, the present invention is proposed. Summary of the invention

[0005] The technical problem to be solved by the present invention is to overcome the deficiencies of the prior art and provide a low-cost biodegradable composite film that can contact food, as well as a preparation method and use thereof. The composite film of the present invention has low cost, high mechanical properties, is completely biodegradable, meets food grade requirements, and can better meet the requirements of the food packaging field.

[0006] In order to solve the above technical problems, the basic concept of the technical solution adopted by the present invention is:

[0007] The first object of the present invention is to provide a low-cost biodegradable composite film that can contact food. The composite film includes a core layer and outer layers located on both sides of the core layer, and the outer layers sandwich the core layer in the middle. The material of the core layer is polybutylene terephthalate-co-succinate, and the material of the outer layers is polybutylene succinate.

[0008] Polybutylene terephthalate-co-succinate (PBST) has excellent biodegradability and its current market price is much lower than PBS. It is easy to process into films. However, due to its complex production process, it is difficult to prepare food-grade PBST slices, which makes it difficult to be widely used in the field of food packaging.

[0009] The composite film of the present invention is a sandwich structure, the core layer is made of polybutylene terephthalate-co-succinate (PBST), and the outer layers on both sides are made of polybutylene succinate (PBS). PBST has good biodegradability, and is much cheaper than PBS. The core layer is made of PBST, which can greatly reduce costs, and will not directly contact with food, so that the composite film can be applied to some scenes, and can be completely biodegraded, environmentally friendly, and can be sustainable. The outer layer of the core layer is made of PBS, so that the composite film can retain the characteristics of the PBS film, has good toughness, and can contact with food. In this way, the composite film of the present invention has high mechanical properties, good toughness, can be completely biodegraded, has low cost, meets food grade requirements, and can better meet the requirements of the field of food packaging.

[0010] In a further embodiment, in a cross section of the composite film, a ratio of a cross-sectional area of ​​the core layer to a cross-sectional area of ​​the outer layer is (1.0-2.0):1;

[0011] Preferably, the ratio of the cross-sectional area of ​​the core layer to the cross-sectional area of ​​the outer layer is (1.6-2.0):1;

[0012] Preferably, in the cross section of the composite membrane, the core layer and the outer layers on the upper and lower sides are arranged in parallel.

[0013] In the present invention, when the ratio of the cross-sectional area of ​​the core layer to the cross-sectional area of ​​the outer layer is (1.0-2.0):1, the composite film can have better mechanical properties and good toughness, and can also achieve the purpose of reducing production costs. Compared with pure PBS film, the cost of the composite film of the present invention can be greatly reduced. The price of PBS raw material is 45,000 yuan / ton, and the price of PBST is 17,000 yuan / ton. The core layer is PBST, which can effectively reduce the price of the composite film product.

[0014] According to a further solution, the tensile strength of the composite film is 35-45 MPa, the elongation at break is 200%-300%, the tear strength is 130-200 / KN.m-1, and the degradation rate is 70-80% in 120 days under composting conditions.

[0015] The composite film of the invention has good toughness and comprehensive mechanical properties, is basically completely biodegradable, is environmentally friendly, and complies with the policy of sustainable development.

[0016] The second object of the present invention is to provide a method for preparing a low-cost biodegradable composite film that can contact food as described above, comprising:

[0017] Polybutylene terephthalate-co-succinate slices and polybutylene succinate resin slices are composited and drawn into a film, so that polybutylene terephthalate-co-succinate forms a core layer and polybutylene succinate resin forms outer layers on both sides, thereby obtaining a low-cost biodegradable composite film that can contact food.

[0018] The polybutylene succinate slices are food grade, have a melting index of 2.0-5.0 g / 10 min, preferably a melting index of 4.0-5.0 g / 10 min, and have an ash content of less than 0.1%, preferably less than 0.05%.

[0019] Before use, the polybutylene succinate slices are vacuum dried, and the vacuum drying conditions include: vacuum drying temperature of 90-100° C., drying time of 12 h to 16 h; vacuum degree of 30-100 Pa, preferably 30-50 Pa.

[0020] In a further embodiment, the method for preparing the poly(butylene terephthalate-co-succinate) slice comprises:

[0021] (1) mixing terephthalic acid, succinic acid, butanediol and a catalyst, and performing an esterification reaction at 160-180° C., and then continuing to heat to 200-205° C. after the esterification rate reaches 49.3-49.9%, and continuing the esterification reaction, and the esterification reaction is completed when the esterification rate reaches 99.5-99.9%;

[0022] (2) heating to 240° C. and performing a pre-polycondensation reaction for 20-40 minutes; then slowly evacuating the vacuum, controlling the high vacuum degree at 10-20 Pa, and performing a polycondensation reaction at a temperature of 250-260° C. When the intrinsic viscosity reaches 1.30-1.35 dL / g, the material is discharged, pelletized, and vacuum dried to obtain a dried film-grade PBST copolymer slice;

[0023] Preferably, the vacuum drying conditions include: temperature of 100°C to 105°C, drying time of 25h to 36h; vacuum degree of 30-100Pa, preferably 30-50Pa.

[0024] The molar ratio of terephthalic acid to succinic acid is 1:1.39;

[0025] Preferably, the ratio of the total moles of terephthalic acid and succinic acid to the moles of butanediol is 1.00:(1.32-1.42), preferably, the ratio is 1.00:(1.38-1.40).

[0026] Preferably, the molar amount of the catalyst added is 0.06 to 0.08% of the total molar amount of terephthalic acid and succinic acid, preferably 0.06 to 0.07%;

[0027] Preferably, the catalyst is titanium butanediol, and the purity of the titanium butanediol is 99.8-99.9%.

[0028] In the present invention, PBST is used as the core layer and will not directly contact food, so the requirements are relatively low. In addition, the preparation method provided by the present invention is simple and easy to operate.

[0029] The method for measuring the intrinsic viscosity of the PBST copolymer comprises the following steps:

[0030] Phenol and tetrachloroethane in a mass ratio of 1:1 are prepared as a solvent;

[0031] Adding the PBST copolymer into the solvent to prepare a solution with a content of 0.1 g / dL;

[0032] At 25°C, the intrinsic viscosity was determined using the Ubbelohde viscometer.

[0033] In a further solution, the composite film drawing process adopts a controlled film blowing device for blow molding;

[0034] The process conditions of composite film blowing include: the temperature of the upper and lower outer layers is 130°C; the temperature of the core layer is 160°C; the screw speed of the main machine of the film blowing device is 300rpm; the traction speed is 5-8m / min, preferably 5-7m / min; the blowing ratio is 4.0-5.0, preferably 4.0-4.5;

[0035] Three-layer coextrusion blow molding was used to prepare low-cost biodegradable composite films that can come into contact with food.

[0036] The third object of the present invention is to provide a use of the above-mentioned low-cost biodegradable composite film that can contact food in the preparation of food packaging. The composite film of the present invention can contact food, is completely biodegradable, and can be widely used in the field of food packaging, such as packaging occasions for bread, cakes, etc. It will not produce white pollution and is in line with the contemporary development trend of green and environmental protection.

[0037] After adopting the above technical solution, the present invention has the following beneficial effects compared with the prior art:

[0038] The composite film of the present invention is a sandwich structure, the core layer is made of polybutylene terephthalate-co-succinate (PBST), and the outer layers on both sides are made of polybutylene succinate (PBS). PBST has good biodegradability, and is much cheaper than PBS. The core layer is made of PBST, which can greatly reduce the cost, so that the composite film can be applied to some scenes, and can be completely biodegraded, environmentally friendly, and can be sustainable. The outer layer of the core layer is made of PBS, so that the composite film can retain the characteristics of the PBS film, has good toughness, and can be in contact with food. In this way, the composite film of the present invention has improved tear strength, good elongation, can be completely biodegraded, low cost, meets food grade requirements, and can better meet the requirements of the field of food packaging.

[0039] The specific implementation modes of the present invention are further described in detail below in conjunction with the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0040] The accompanying drawings are part of the present invention and are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention, but do not constitute an improper limitation of the present invention. Obviously, the drawings described below are only some embodiments. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work. In the accompanying drawings:

[0041] Figure 1 It is a schematic diagram of the cross-sectional structure of the low-cost biodegradable composite film that can contact food of the present invention;

[0042] Among them, 1 is an outer layer (upper layer) made of PBS, 2 is a core layer made of PBST, and 3 is an outer layer (lower layer) made of PBS.

[0043] It should be noted that these drawings and textual descriptions are not intended to limit the conceptual scope of the present invention in any way, but are intended to illustrate the concept of the present invention for those skilled in the art by referring to specific embodiments. DETAILED DESCRIPTION

[0044] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. The following embodiments are used to illustrate the present invention but are not used to limit the scope of the present invention.

[0045] The test standards for tensile strength and elongation at break are: ISO11566-1996;

[0046] Tear strength test standard: GB / T16578.2-2009

[0047] Degradation rate test standard: ISO14855-1:2005,

[0048] Food grade test standard: Regulation (EU) No10 / 2011.

[0049] The method for measuring the intrinsic viscosity of the PBST copolymer comprises the following steps:

[0050] Phenol and tetrachloroethane in a mass ratio of 1:1 are configured into a solvent; the PBST copolymer is added into the solvent to configure a solution with a content of 0.1 g / dL; and the intrinsic viscosity is measured using an Ubbelohde viscometer at 25°C.

[0051] Example 1

[0052] 1.1 Choose food-grade PBS slices

[0053] Food grade PBS, white granules, melt index 2.0g / 10min, ash content 0.05%.

[0054] The food-grade PBS slices were vacuum dried to obtain dried food-grade PBS slices, wherein the vacuum drying temperature was 90° C., the drying time was 16 h, and the vacuum degree was 30 Pa.

[0055] 1.2 Preparation of PBST slices

[0056] (1) Terephthalic acid, succinic acid, butanediol and a catalyst are mixed and added to a polymerization reactor; the molar ratio of terephthalic acid to succinic acid is 1:1.39, and the molar ratio of the total molar amount of terephthalic acid and succinic acid to butanediol is 1.00:1.34. The catalyst is titanium butanediol (purity is 99.9%), and the molar amount of titanium butanediol added is 0.06% of the total molar amount of succinic acid and terephthalic acid; the esterification reaction is carried out at 160°C, and the esterification rate reaches 49.5%; the temperature is continued to rise to 200°C to continue the esterification reaction, and the esterification rate reaches 99.5%, and the esterification reaction is completed.

[0057] (2) The temperature is raised to 240°C and a pre-polycondensation reaction is carried out for 20 minutes; then the temperature is slowly evacuated, the temperature is raised to 250°C, and the high vacuum degree is controlled at 20Pa for polycondensation reaction. When the characteristic viscosity is 1.30dL / g, the material is discharged and pelletized to obtain the membrane-grade PBST copolymer. The obtained membrane-grade PBST copolymer slices are vacuum dried to obtain dried membrane-grade PBST copolymer slices. The vacuum drying conditions include: temperature of 100°C, drying time of 25h, and vacuum degree of 30Pa.

[0058] 1.3 Composite blown film

[0059] The process conditions of composite blown film include:

[0060] The temperatures of the three zones of outer layer (upper layer), core layer, and outer layer (lower layer) are 130°C, 160°C, and 130°C respectively;

[0061] The main screw speed of the film blowing device is 300rpm, the traction speed is 6m / min, the blowing ratio is 4.0, the thickness of the three-layer co-extrusion blown composite film is 30 microns, and the ratio of the cross-sectional area of ​​the core layer to the cross-sectional area of ​​the outer layer is 1:1.

[0062] The performance parameters of the composite membrane prepared in this example are shown in Table 1.

[0063] Example 2

[0064] 2.1 Choose food-grade PBS slices

[0065] Food grade PBS, white granules, melt index 3.0g / 10min, ash content 0.05%.

[0066] The food-grade PBS slices were vacuum dried to obtain dried food-grade PBS slices, wherein the vacuum drying temperature was 90° C., the drying time was 16 h, and the vacuum degree was 30 Pa.

[0067] 2.2 Preparation of PBST slices

[0068] (1) Terephthalic acid, succinic acid, butanediol and a catalyst are mixed and added to a polymerization reactor; the molar ratio of terephthalic acid to succinic acid is 1:1.39, and the molar ratio of the total molar amount of terephthalic acid and succinic acid to butanediol is 1.00:1.34. The catalyst is titanium butanediol (purity is 99.9%), and the molar amount of titanium butanediol added is 0.06% of the total molar amount of succinic acid and terephthalic acid; the esterification reaction is carried out at 160°C, and the esterification rate reaches 49.5%; the temperature is continued to rise to 200°C to continue the esterification reaction, and the esterification rate reaches 99.5%, and the esterification reaction is completed.

[0069] (2) The temperature is raised to 240°C and a pre-polycondensation reaction is carried out for 20 minutes; then, the temperature is slowly evacuated, the temperature is raised to 250°C, and the high vacuum degree is controlled at 15Pa for polycondensation reaction. When the characteristic viscosity is 1.33dL / g, the material is discharged and pelletized to obtain the membrane-grade PBST copolymer. The obtained membrane-grade PBST copolymer slices are vacuum dried to obtain dried membrane-grade PBST copolymer slices. The vacuum drying conditions include: temperature of 100°C, drying time of 25h, and vacuum degree of 30Pa.

[0070] 2.3 Composite blown film

[0071] The process conditions of composite blown film include:

[0072] The temperatures of the three zones of outer layer (upper layer), core layer, and outer layer (lower layer) are 130°C, 160°C, and 130°C respectively;

[0073] The main screw speed of the film blowing device is 300rpm, the traction speed is 6m / min, the blowing ratio is 4.0, the thickness of the three-layer co-extrusion blown composite film is 30 microns, and the ratio of the cross-sectional area of ​​the core layer to the cross-sectional area of ​​the outer layer is 1.4:1.

[0074] The performance parameters of the composite membrane prepared in this example are shown in Table 1.

[0075] Example 3

[0076] 3.1 Choose food-grade PBS slices

[0077] Food grade PBS, white granules, melt index 4.0g / 10min, ash content 0.05%.

[0078] The food-grade PBS slices were vacuum dried to obtain dried food-grade PBS slices, wherein the vacuum drying temperature was 90° C., the drying time was 16 h, and the vacuum degree was 30 Pa.

[0079] 3.2 Preparation of PBST slices

[0080] (1) Terephthalic acid, succinic acid, butanediol and a catalyst are mixed and added to a polymerization reactor; the molar ratio of terephthalic acid to succinic acid is 1:1.39, and the molar ratio of the total molar amount of terephthalic acid and succinic acid to butanediol is 1.00:1.34. The catalyst is titanium butanediol (purity is 99.9%), and the molar amount of titanium butanediol added is 0.06% of the total molar amount of succinic acid and terephthalic acid; the esterification reaction is carried out at 160°C, and the esterification rate reaches 49.5%; the temperature is continued to rise to 200°C to continue the esterification reaction, and the esterification rate reaches 99.5%, and the esterification reaction is completed.

[0081] (2) The temperature is raised to 240°C and a pre-polycondensation reaction is carried out for 20 minutes; then, the temperature is slowly evacuated, the temperature is raised to 250°C, and the high vacuum degree is controlled at 10Pa for polycondensation reaction. When the characteristic viscosity is 1.35 dL / g, the material is discharged and pelletized to obtain the membrane-grade PBST copolymer. The obtained membrane-grade PBST copolymer slices are vacuum dried to obtain dried membrane-grade PBST copolymer slices. The vacuum drying conditions include: temperature of 100°C, drying time of 25h, and vacuum degree of 30Pa.

[0082] 3.3 Composite blown film

[0083] The process conditions of composite blown film include:

[0084] The temperatures of the three zones of outer layer (upper layer), core layer, and outer layer (lower layer) are 130°C, 160°C, and 130°C respectively;

[0085] The main screw speed of the film blowing device is 300rpm, the traction speed is 6m / min, the blowing ratio is 4.0, the thickness of the three-layer co-extrusion blown composite film is 30 microns, and the ratio of the cross-sectional area of ​​the core layer to the cross-sectional area of ​​the outer layer is 1.8:1.

[0086] The performance parameters of the composite membrane prepared in this example are shown in Table 1.

[0087] Comparative Example 1

[0088] 1.1 Selection of food-grade PBS slices

[0089] Food grade PBS, white granules, melt index 2.0g / 10min, ash content 0.05%.

[0090] The food-grade PBS slices were vacuum dried to obtain dried food-grade PBS slices, wherein the vacuum drying temperature was 90° C., the drying time was 16 h, and the vacuum degree was 30 Pa.

[0091] 1.2 Film blowing

[0092] The process conditions of composite blown film include:

[0093] The temperatures of the three zones of outer layer (upper layer), core layer and outer layer (lower layer) are 130℃, 160℃ and 130℃ respectively.

[0094] The main screw speed of the film blowing device is 300rpm, the traction speed is 6m / min, and the blowing ratio is 4.0;

[0095] The thickness of the three-layer co-extruded blown composite film is 30 μm.

[0096] Among them, the raw materials of the outer layer (upper layer), the core layer, and the outer layer (lower layer) are all dried food-grade PBS slices.

[0097] The performance parameters of the composite membrane prepared in this comparative example are shown in Table 1.

[0098] Comparative Example 2

[0099] 3.1 Choose food-grade PBS slices

[0100] Food grade PBS, white granules, melt index 4.0g / 10min, ash content 0.05%.

[0101] The food-grade PBS slices were vacuum dried to obtain dried food-grade PBS slices, wherein the vacuum drying temperature was 90° C., the drying time was 16 h, and the vacuum degree was 30 Pa.

[0102] 3.2 Preparation of PBST slices

[0103] (1) Terephthalic acid, succinic acid, butanediol and a catalyst are mixed and added to a polymerization reactor; the molar ratio of terephthalic acid to succinic acid is 1:1.39, and the molar ratio of the total molar amount of terephthalic acid and succinic acid to butanediol is 1.00:1.34. The catalyst is titanium butanediol (purity is 99.9%), and the molar amount of titanium butanediol added is 0.06% of the total molar amount of succinic acid and terephthalic acid; the esterification reaction is carried out at 160°C, and the esterification rate reaches 49.5%; the temperature is continued to rise to 200°C to continue the esterification reaction, and the esterification rate reaches 99.5%, and the esterification reaction is completed.

[0104] (2) The temperature is raised to 240°C and a pre-polycondensation reaction is carried out for 20 minutes; then, the temperature is slowly evacuated, the temperature is raised to 250°C, and the high vacuum degree is controlled at 10Pa for polycondensation reaction. When the characteristic viscosity is 1.35 dL / g, the material is discharged and pelletized to obtain the membrane-grade PBST copolymer. The obtained membrane-grade PBST copolymer slices are vacuum dried to obtain dried membrane-grade PBST copolymer slices. The vacuum drying conditions include: temperature of 100°C, drying time of 25h, and vacuum degree of 30Pa.

[0105] 3.3 Composite blown film

[0106] The process conditions of composite blown film include:

[0107] The temperatures of the three zones of outer layer (upper layer), core layer, and outer layer (lower layer) are 130°C, 160°C, and 130°C respectively;

[0108] The main screw speed of the film blowing device is 300rpm, the traction speed is 6m / min, the blowing ratio is 4.0, the thickness of the three-layer co-extrusion blown composite film is 30 microns, and the ratio of the cross-sectional area of ​​the core layer to the cross-sectional area of ​​the outer layer is 0.5:1.

[0109] The performance parameters of the composite membrane prepared in this example are shown in Table 1.

[0110] Table 1 Performance index table of composite membranes of embodiments and comparative examples

[0111]

[0112]

[0113] It can be seen from Table 1 that the prepared low-cost biodegradable composite film that can contact food has improved mechanical properties, improved tear strength, and improved elongation.

[0114] Compared with the PBS film prepared in comparative example 1, the tensile strength, tear strength and elongation at break of the composite films prepared in examples 1-3 of the present invention are correspondingly improved, that is, the mechanical properties of the composite films of the present invention are improved, which are better than those of the PBS film, and have high strength and good toughness. At the same time, the composite films of the present invention are more inexpensive, biodegradable, meet food grade requirements, can better meet the requirements of the food packaging field, and expand the scope of application.

[0115] The ratio of the cross-sectional area of ​​the core layer to the cross-sectional area of ​​the outer layer in Comparative Example 2 is 0.5:1, which is not within the scope of the present invention. The tensile strength, tear strength and elongation at break of the composite film prepared in Comparative Example 2 are basically equivalent to those of Comparative Example 1, and are lower than those of Examples 1-3 of the present invention.

[0116] Therefore, in the present invention, when the ratio of the cross-sectional area of ​​the core layer to the cross-sectional area of ​​the outer layer is (1.0-2.0):1, the composite film can have better mechanical properties and good toughness, and can also achieve the purpose of reducing production costs.

[0117] The above is only a preferred embodiment of the present invention, and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment, it is not used to limit the present invention. Any technician familiar with this patent can make some changes or modify the technical contents suggested above into equivalent embodiments without departing from the scope of the technical solution of the present invention. However, any simple modification, equivalent change and modification made to the above embodiments according to the technical essence of the present invention without departing from the content of the technical solution of the present invention still fall within the scope of the solution of the present invention.

Claims

1. A low-cost biodegradable composite film that can contact food, characterized in that: The composite film comprises a core layer and outer layers located on both sides of the core layer, wherein the outer layers sandwich the core layer, the material of the core layer is polybutylene terephthalate-co-succinate, and the material of the outer layers is polybutylene succinate; In the cross section of the composite film, the ratio of the cross-sectional area of ​​the core layer to the cross-sectional area of ​​the outer layer is (1.0-2.0): 1; The preparation method of the polybutylene terephthalate-co-succinate comprises: (1) terephthalic acid, succinic acid, butanediol and a catalyst are mixed, and an esterification reaction is carried out at 160-180° C. After the esterification rate reaches 49.3-49.9%, the temperature is continuously raised to 200-205° C., and the esterification reaction is continued. When the esterification rate reaches 99.5-99.9%, the esterification reaction is terminated; the molar ratio of terephthalic acid to succinic acid is 1:1.39; the molar ratio of the total molar amount of terephthalic acid and succinic acid to butanediol is 1.00:(1.32-1.42); (2) The temperature is raised to 240°C and a pre-polycondensation reaction is carried out for 20-40 minutes; then, the temperature is slowly increased to 250-260°C and the vacuum degree is controlled at 10-20 Pa to carry out a polycondensation reaction. When the intrinsic viscosity reaches 1.30-1.35 dL / g, the material is discharged, pelletized, and vacuum dried to obtain polybutylene terephthalate-co-succinate.

2. The low-cost biodegradable composite film that can contact food according to claim 1, characterized in that: The ratio of the cross-sectional area of ​​the core layer to the cross-sectional area of ​​the outer layer is (1.6-2.0):

1.

3. The low-cost biodegradable composite film that can contact food according to claim 1 or 2, characterized in that: In the cross section of the composite film, the core layer is arranged in parallel with the outer layers on both sides.

4. The low-cost biodegradable composite film that can contact food according to claim 1 or 2, characterized in that: The tensile strength of the composite film is 35-45MPa, the elongation at break is 200%-300%, the tear strength is 130-200 / KN.m-1, and under composting degradation conditions, the degradation rate is 70-80% in 120 days.

5. A method for preparing a low-cost biodegradable composite film that can contact food according to any one of claims 1 to 4, characterized in that: include: Polybutylene terephthalate-co-succinate slices and polybutylene succinate resin slices are composited and drawn into a film, so that polybutylene terephthalate-co-succinate forms a core layer and polybutylene succinate resin forms outer layers on both sides, thereby obtaining a low-cost biodegradable composite film that can contact food.

6. The preparation method according to claim 5, characterized in that: The polybutylene succinate slices are food grade, have a melt index of 2.0-5.0 g / 10 min, and an ash content of less than 0.1%.

7. The preparation method according to claim 6, characterized in that: The melt index is 4.0-5.0g / 10min.

8. The preparation method according to claim 6, characterized in that: The ash content is less than 0.05%.

9. The preparation method according to claim 6, characterized in that: Before use, the polybutylene succinate resin slices are vacuum dried, and the vacuum drying conditions include: vacuum drying temperature of 90-100° C., drying time of 12 h to 16 h; vacuum degree of 30-100 Pa.

10. The preparation method according to claim 9, characterized in that: The vacuum degree is 30-50 Pa.

11. The preparation method according to any one of claims 5 to 10, characterized in that: The preparation method of the poly(butylene terephthalate-co-succinate) slice comprises: (1) terephthalic acid, succinic acid, butanediol and a catalyst are mixed and esterification reaction is carried out at 160-180°C. When the esterification rate reaches 49.3-49.9%, the temperature is further raised to 200-205°C and the esterification reaction is continued. When the esterification rate reaches 99.5-99.9%, the esterification reaction is completed; (2) The temperature is raised to 240°C and a pre-polycondensation reaction is carried out for 20-40 minutes; then, the vacuum is slowly drawn and the temperature is raised to 250-260°C. The vacuum degree is controlled at 10-20 Pa and a polycondensation reaction is carried out. When the intrinsic viscosity reaches 1.30-1.35 dL / g, the material is discharged, pelletized, and vacuum dried to obtain dried membrane-grade PBST copolymer slices.

12. The preparation method according to claim 11, characterized in that: In step (2), the vacuum drying conditions include: temperature of 100°C to 105°C, drying time of 25h to 36h; vacuum degree of 30-100Pa.

13. The preparation method according to claim 12, characterized in that: The vacuum degree is 30-50 Pa.

14. The preparation method according to claim 11, characterized in that: In step (1), the molar ratio of terephthalic acid to succinic acid is 1:1.

39.

15. The preparation method according to claim 11, characterized in that: In step (1), the molar ratio of the total molar amount of terephthalic acid and succinic acid to butanediol is 1.00:(1.32-1.42).

16. The preparation method according to claim 15, characterized in that: The molar ratio of the total molar amount of terephthalic acid and succinic acid to butanediol is 1.00:(1.38-1.40).

17. The preparation method according to claim 11, characterized in that: In step (1), the molar amount of the catalyst added is 0.06 to 0.08% of the total molar amount of terephthalic acid and succinic acid.

18. The preparation method according to claim 17, characterized in that: The molar amount of the catalyst added is 0.06-0.07% of the total molar amount of terephthalic acid and succinic acid.

19. The preparation method according to claim 11, characterized in that: The catalyst is titanium butanediol, and the purity of the titanium butanediol is 99.8-99.9%.

20. The preparation method according to any one of claims 5 to 10, characterized in that: The composite film drawing process adopts controlled film blowing device for blow molding; The process conditions of composite blown film include: the temperature of the upper and lower outer layers is 130°C; the temperature of the core layer is 160°C; the screw speed of the main machine of the film blowing device is 300rpm; the traction speed is 5-8m / min; the blowing ratio is 4.0-5.0; three-layer co-extrusion blow molding is used to prepare a low-cost biodegradable composite film that can contact food.

21. The preparation method according to claim 20, characterized in that: The pulling speed is 5-7 m / min.

22. The preparation method according to claim 20, characterized in that: The blowing ratio is 4.0-4.

5.

23. Use of the low-cost biodegradable composite film that can contact food according to any one of claims 1 to 4 in preparing food packaging.