An efficient treatment method for low-grade mixed tungsten ore containing high flotation agent

Through one deflotation agent, two calcium dephosphorization and three decomposition steps, strong alkaline resin and recycled acid solution are used to treat low-grade mixed tungsten ore containing high flotation agent, which solves the problem of difficult decomposition and high cost, and achieves Efficient WO3 leaching and resource utilization.

CN114657368BActive Publication Date: 2024-10-22WANGJIANG JINHUI OIL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210192385.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-03-01
Publication Date
2024-10-22
Estimated Expiration
2042-03-01

AI Technical Summary

Technical Problem

The low-grade mixed tungsten ore containing high flotation agent is difficult to decompose, has low utilization rate, high cost and waste of resources.

Method used

It adopts one deflotation agent, two calcium dephosphorization and three decomposition steps, uses 201×7 strong alkaline resin to absorb sodium tungstate, recovers hydrochloric acid solution and high-concentration sodium hydroxide, and uses processes such as stirring and washing, ball milling and pulping. Improve the leaching rate of WO3.

Benefits of technology

It increases the leaching rate of WO3, reduces processing costs, improves the utilization rate of tungsten resources, reduces the consumption of auxiliary materials, and improves environmental protection and economic benefits.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114657368B_ABST
    Figure CN114657368B_ABST
Patent Text Reader

Abstract

The present invention relates to an efficient treatment method for low-grade mixed tungsten ore containing high flotation agent, comprising the following steps: primary deflotation agent, secondary dephosphorization, and calcium-tertiary decomposition, wherein the low-grade mixed tungsten ore containing high flotation agent is first deflotated, sodium tungstate is adsorbed by 201×7 strong alkaline resin to obtain a post-delivery liquid, and the post-delivery liquid is washed by a washing liquid, and the washing residue is filtered and dried before entering the next link, and the washing residue is washed and filtered by a recovered hydrochloric acid solution, and the washed dephosphorization and calcium residues are decomposed by alkali, followed by filter pressing, and the filtrate enters the 201×7 resin adsorption WO3 process after batching, and the filter residue is first subjected to ball milling pulping, decomposition is completed, filtration, washing, filtrate collection and recovery of WO3, filter residue drying, and sample preparation to measure WO3 content. The present invention completes the efficient leaching of WO3 in low-grade mixed tungsten ore containing high flotation agent through the steps of primary deflotation agent, secondary dephosphorization, and calcium-tertiary decomposition.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of tungsten and molybdenum smelting, and in particular to a high-efficiency processing method for low-grade mixed tungsten ore containing high flotation agent. Background Art

[0002] Tungsten has excellent physical and chemical properties and is widely used in the fields of national defense industry, fine chemicals, etc. In recent years, with the application of new tungsten materials in high-tech fields, the global market demand for tungsten has increased, resulting in tight supply of high-quality tungsten and molybdenum mineral resources. Low-grade mixed tungsten ore containing high flotation reagents is a type of tungsten mineral that is difficult to smelt. Due to the high content of flotation reagents, low grade, and high impurity elements such as phosphorus and calcium, it is difficult to decompose, has low utilization, high cost, and wastes resources.

[0003] The invention aims at the problems of difficulty in decomposition, low utilization rate, high cost and waste of resources of low-grade mixed tungsten ore containing high flotation agent, and develops a high-efficiency treatment method for low-grade mixed tungsten ore containing high flotation agent. The method is processed by the steps of primary removal of flotation agent-secondary dephosphorization, calcium-tertiary decomposition, etc., so as to achieve efficient utilization of low-grade mixed tungsten ore containing high flotation agent, improve the leaching rate of WO3, reduce costs and improve the utilization rate of tungsten resources. The method is a method for efficiently treating low-grade mixed tungsten ore containing high flotation agent. Summary of the invention

[0004] The purpose of the present invention is to provide a high-efficiency treatment method for low-grade mixed tungsten ore containing high flotation agent.

[0005] The technical problem of the present invention is mainly solved by the following technical solutions:

[0006] An efficient treatment method for low-grade mixed tungsten ore containing high flotation agent comprises the following steps:

[0007] (1) Primary removal of flotation reagents: remove the flotation reagents from the low-grade mixed tungsten ore containing high flotation reagents, and use 201×7 strong alkaline resin to adsorb sodium tungstate to obtain a post-delivery liquid, wherein the NaOH concentration in the post-delivery liquid is greater than 5g / L, and the post-delivery liquid is stirred and washed once with a washing liquid, and then washed again with water twice the mass of the low-grade mixed tungsten ore containing high flotation reagents, wherein the washing water is collected and enters environmental protection treatment, and the washing residue is filtered and dried before entering the next link;

[0008] (2) Secondary dephosphorization and decalcification: The washed filter residue obtained in step (1) is subjected to secondary dephosphorization and decalcification. The washed filter residue is washed with a recovered hydrochloric acid solution, wherein the liquid-to-solid ratio is 3 / 1-4 / 1, the stirring speed is 60-90 r / min, the temperature is room temperature, the reaction time is 60-120 min, and the acid concentration at the reaction end point is controlled to be 0.5 mol / L-1.5 mol / L. After the reaction is completed, the filter is filtered, the filtrate is collected and processed, and the filter residue is washed twice with hot water. The washed dephosphorization and decalcification residue enters the next step.

[0009] (3) Three-time decomposition: The dephosphorized calcium slag obtained in step (2) is firstly dissolved with the residual alkali in the alkali decomposition concentrate, and the liquid-to-solid ratio of the solution is 3 / 1-4 / 1. After the dissolution is completed, the filter is pressed. After the filtrate is mixed, it enters the 201×7 resin adsorption process of WO3. The filter residue is firstly subjected to ball milling to prepare pulp, and the ball milling intensity is controlled to be ≥97% of -325μm. The liquid-to-solid ratio of the prepared slurry is 1 / 0.8-1 / 1, the sodium hydroxide concentration is 400-600g / L, the decomposition pressure is 0.2-0.4Mpa, the decomposition time is 2-4h, and the decomposition stirring speed is 60-90r / min. After the decomposition is completed, it is filtered, washed, and the filtrate is collected to recover WO3. The filter residue is dried, and the WO3 content is measured by sample preparation. The leaching rate of WO3 in the low-grade mixed scheelite containing high mineral processing agents is calculated.

[0010] Preferably, when the post-coital fluid is stirred and washed once with a washing liquid, the washing liquid-to-solid ratio is 3 / 1-4 / 1, the stirring and washing time is controlled to be 60-120 minutes, and the washing is performed at room temperature.

[0011] Preferably, when the filter residue is washed with hot water, the temperature of the hot water is controlled to be 60-80° C., and the amount of hot water used for washing is 2-4 times the mass of the filter residue.

[0012] The beneficial effects of the present invention are as follows: the present invention completes the efficient leaching of WO3 in low-grade mixed tungsten ore containing high flotation reagents through the steps of primary deflotation reagent-secondary dephosphorization, calcium-tertiary decomposition, etc., solves the problems of high processing cost of such minerals and low WO3 leaching rate, and at the same time utilizes 201×7 strong alkaline resin to absorb sodium hydroxide in the post-delivery liquid of sodium tungstate solution and spray to recover hydrochloric acid in dilute hydrochloric acid solution, thereby reducing auxiliary material consumption and improving environmental protection benefits and economic benefits. BRIEF DESCRIPTION OF THE DRAWINGS

[0013] Figure 1 It is a schematic diagram of the process of the present invention. DETAILED DESCRIPTION

[0014] The technical solution of the present invention is further specifically described below through embodiments and in conjunction with the accompanying drawings.

[0015] Example 1

[0016] In this embodiment, low-grade mixed tungsten ore containing high flotation reagent comes from a tungsten smelter in Ganzhou. After drying, samples are taken and the test results are WO3 23.12%, Mo 0.42%, P 1.13%, Ca 14.56%, S 0.89%, and SiO2 12.77%.

[0017] An efficient treatment method for low-grade mixed tungsten ore containing high flotation agent comprises the following steps:

[0018] (1) Primary removal of flotation reagent: Weigh 600g of the low-grade mixed tungsten ore containing high flotation reagent, and take samples from the post-delivery liquid collected by 201×7 strong alkaline resin adsorbing sodium tungstate for testing. The NaOH concentration is 8.38g / L. The washing liquid-to-solid ratio is 4 / 1, and the stirring washing time is controlled to be 120min. Wash at room temperature. After washing is completed, wash again with water twice the mass of the low-grade mixed tungsten ore containing high flotation reagent. The washing water is collected and enters environmental protection treatment. After the washing residue is filtered dry, it enters the next stage.

[0019] (2) Secondary dephosphorization and decalcification The washed filter residue obtained in step (1) is subjected to secondary dephosphorization and decalcification by washing with a recovered hydrochloric acid solution at a liquid-to-solid ratio of 4 / 1, a stirring speed of 60 r / min, a temperature of room temperature, a reaction time of 60 min, and an acid concentration of 1.0 mol / L at the reaction end. After the reaction is completed, the filter is filtered, and the filtrate is collected and processed. The filter residue is subjected to secondary washing by washing with hot water at a temperature of 80° C. The amount of hot water used for washing is 4 times the mass of the filter residue to ensure that the residual acid is washed away. The washed dephosphorization and decalcification residue enters the next step.

[0020] (3) Three-time decomposition: The dephosphorized calcium slag obtained in (2) is first dissolved with the residual alkali in the alkali decomposition concentrate, with the liquid-to-solid ratio of 4 / 1. After the dissolution is completed, it is filtered. After the filtrate is mixed, it enters the 201×7 resin adsorption process of WO3. The filter residue is first ball milled to make pulp. The ball milling intensity is controlled to control the proportion of -325μm to ≥97%. The liquid-to-solid ratio of the slurry is 1 / 0.8, the sodium hydroxide concentration is 500g / L, the decomposition pressure is 0.3Mpa, the decomposition time is 3h, and the decomposition stirring speed is 60r / min. After the decomposition is completed, it is filtered, washed, and the filtrate is collected to recover WO3. The filter residue is dried and weighed to 353.25g. The sample is prepared to measure the WO3 content of 0.45%. The leaching rate of WO3 in the low-grade mixed scheelite containing high-grade dressing agents is calculated to be 98.85%.

[0021] Example 2

[0022] In this embodiment, low-grade mixed tungsten ore containing high flotation reagent comes from a tungsten smelter in Ganzhou. After drying, samples are taken and the test results are WO3 18.71%, Mo 0.23%, P 2.69%, Ca 24.56%, S 0.52%, and SiO2 9.08%.

[0023] An efficient treatment method for low-grade mixed tungsten ore containing high flotation agent comprises the following steps:

[0024] (1) Primary removal of flotation reagent: Weigh 600g of the low-grade mixed tungsten ore containing high flotation reagent, and take samples from the post-delivery liquid collected by 201×7 strong alkaline resin adsorbing sodium tungstate for testing. The NaOH concentration is 6.35g / L. The washing liquid-to-solid ratio is 4 / 1, and the stirring washing time is controlled to be 120min. Wash at room temperature. After washing is completed, wash again with water twice the mass of the low-grade mixed tungsten ore containing high flotation reagent. The washing water is collected and enters environmental protection treatment. After the washing residue is filtered dry, it enters the next stage.

[0025] (2) Secondary dephosphorization and decalcification The washed filter residue obtained in step (1) is subjected to secondary dephosphorization and decalcification by washing with a recovered hydrochloric acid solution at a liquid-to-solid ratio of 4 / 1, a stirring speed of 60 r / min, a temperature of room temperature, a reaction time of 120 min, and an acid concentration of 1.5 mol / L at the end of the reaction. After the reaction is completed, the filter is filtered, and the filtrate is collected and processed. The filter residue is subjected to secondary washing by washing with hot water at a temperature of 80° C. The amount of hot water used for washing is 4 times the mass of the filter residue to ensure that the residual acid is washed away. The washed dephosphorization and decalcification residue enters the next step.

[0026] (3) Three-time decomposition: The dephosphorized calcium slag obtained in (2) is first dissolved with the residual alkali in the alkali decomposition concentrate, with a liquid-to-solid ratio of 4 / 1. After the dissolution is completed, it is filtered. After the filtrate is mixed, it enters the 201×7 resin adsorption process of WO3. The filter residue is first ball milled to make pulp. The ball milling intensity is controlled to be ≥97% of -325μm. The liquid-to-solid ratio of the slurry is 1 / 1. The sodium hydroxide concentration is 500g / L, the decomposition pressure is 0.3Mpa, the decomposition time is 3h, and the decomposition stirring speed is 60r / min. After the decomposition is completed, it is filtered, washed, and the filtrate is collected to recover WO3. The filter residue is dried and weighed to be 323.16g. The sample is prepared to measure the WO3 content of 0.45%. The leaching rate of WO3 in the low-grade mixed scheelite containing high-grade dressing agents is calculated to be 98.70%.

[0027] In the present invention: 1. The primary defloating agent is to use the residual alkali in the strong alkaline ion exchange liquid for washing and defloating, which saves the use of alkali. At the same time, the calcium tungstate in the scheelite does not react with the alkali in this process. The reaction mechanism is: C 17 H 35 COOH+NaOH=C 17H 35 COONa+H2O, decomposes the flotation agent and enters the washing liquid, and the washing slag contains tungsten. Second, secondary dephosphorization and decalcification, using recycled low-concentration hydrochloric acid for washing, mainly to wash out part of the calcium and phosphorus, which not only saves the use of acid, but also completes the preliminary removal of phosphorus and calcium. Third, tertiary decomposition, dephosphorization calcium slag, using the residual alkali in the high-concentration sodium hydroxide decomposition solution to first dissolve the dephosphorization calcium slag, remove the residual acid, and then decompose it with concentrated alkali. In this method, the residual alkali is recycled in multiple dimensions, and at the same time, the mechanism of action of each link is inconsistent with the traditional decomposition process.

[0028] The present invention is described in detail above, but the contents are only preferred embodiments of the present invention and cannot be considered to limit the scope of implementation of the present invention. All equivalent changes and improvements made according to the scope of application of the present invention should still fall within the scope of the patent coverage of the present invention.

Claims

1. An efficient treatment method for low-grade mixed tungsten ore containing high flotation agent, characterized in that: The steps include: (1) Primary removal of flotation reagents: remove the flotation reagents from the low-grade mixed tungsten ore containing high flotation reagents, and use 201×7 strong alkaline resin to adsorb sodium tungstate to obtain a post-delivery liquid, wherein the NaOH concentration in the post-delivery liquid is greater than 5g / L, and the post-delivery liquid is stirred and washed once with a washing liquid, and then washed again with water twice the mass of the low-grade mixed tungsten ore containing high flotation reagents, wherein the washing water is collected and enters environmental protection treatment, and the washing residue is filtered and dried before entering the next link; (2) Secondary dephosphorization and decalcification: The washed filter residue obtained in step (1) is subjected to secondary dephosphorization and decalcification, and the washed filter residue is washed with a recovered hydrochloric acid solution, wherein the liquid-to-solid ratio is 3 / 1-4 / 1, the stirring speed is 60-90 r / min, the temperature is room temperature, the reaction time is 60-120 min, and the acid concentration at the reaction end is controlled to be 0.5 mol / L-1.5 mol / L. After the reaction is completed, the filter is filtered, the filtrate is collected and processed, and the filter residue is washed twice with hot water. The washed dephosphorization and decalcification residue enters the next step; (3) Three-time decomposition: The dephosphorized calcium slag obtained in step (2) is firstly dissolved with the residual alkali in the alkali decomposition concentrate, and the liquid-to-solid ratio of the solution is 3 / 1-4 / 1. After the dissolution is completed, the filter is pressed. After the filtrate is mixed, it enters the 201×7 resin adsorption process of WO3. The filter residue is firstly subjected to ball milling to prepare pulp, and the ball milling intensity is controlled to be ≥97% of -325μm. The liquid-to-solid ratio of the prepared slurry is 1 / 0.8-1 / 1, the sodium hydroxide concentration is 400-600g / L, the decomposition pressure is 0.2-0.4Mpa, the decomposition time is 2-4h, and the decomposition stirring speed is 60-90r / min. After the decomposition is completed, it is filtered, washed, and the filtrate is collected to recover WO3. The filter residue is dried, and the WO3 content is measured by sample preparation. The leaching rate of WO3 in the low-grade mixed scheelite containing high mineral processing agents is calculated.

2. The method for efficiently treating low-grade mixed tungsten ore containing high flotation agent according to claim 1 is characterized in that: When the post-coital fluid is stirred and washed once with washing liquid, the washing liquid-to-solid ratio is 3 / 1-4 / 1, the stirring and washing time is controlled to be 60-120 minutes, and the washing is carried out at room temperature.

3. The efficient treatment method of low-grade mixed tungsten ore containing high flotation agent according to claim 1 is characterized in that: When the filter residue is washed with hot water, the temperature of the hot water is controlled to be 60-80°C, and the amount of hot water used for washing is 2-4 times the mass of the filter residue.