A high nickel positive electrode material and preparation method thereof
Through lithium-position doping of potassium/sodium ion and doping of other metal elements, the interlayer structure of high-nickel positive electrode materials is improved, and combined with particle surface coating technology, the problem of low lithium ion utilization is solved and battery performance and production efficiency is improved , reduces costs.
Patent Information
- Application Number
- CN202210328306.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-03-31
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2042-03-31
AI Technical Summary
The existing high-nickel positive electrode materials have low lithium ion utilization during charging and discharging, resulting in waste of lithium resources and high production costs.
Through lithium doping of potassium/sodium ion and combined with other metal elements and transition metal doping, the interlayer structure and cyclic performance of high-nickel positive electrode materials are improved, and particle surface coating technology is used to improve lithium ion utilization and electrochemical performance. .
It significantly improves lithium ion utilization and battery rate performance, reduces production costs, is suitable for industrial production, and meets market demand.
Smart Images

Figure CN114678524B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of battery materials and battery technology, and in particular to a high-nickel positive electrode material and a preparation method thereof. Background Art
[0002] With the rapid development of the new energy market, the market demand for secondary batteries, especially power batteries, has increased exponentially; high-nickel positive electrode materials have become one of the most widely used positive electrode materials in EV batteries on the current market due to their high capacity, long cycle life and high operating voltage; lithium compounds are one of the necessary raw materials for the preparation of lithium-ion battery positive electrode materials. In recent years, the market phenomenon of supply and demand has caused their prices to soar, increasing the production cost of positive electrode materials; in order to ensure sufficient lithium ion embedding when preparing positive electrode materials, excessive lithium salts are added during the preparation process, and the low lithium ion utilization rate during the charge and discharge process of the current high-nickel positive electrode materials (the first charge and discharge efficiency is only about 90% under room temperature and 0.2C test conditions) has further caused a waste of lithium resources.
[0003] Therefore, rational use of lithium resources and maximizing the utilization rate of lithium ions in batteries have become an effective way to reduce costs and increase efficiency in EV batteries. Summary of the invention
[0004] In view of the low lithium utilization rate of the prior art, the present invention aims to provide a high nickel positive electrode material and a preparation method thereof, and reduce the Li utilization rate of the high nickel positive electrode material during the first charge and discharge process by potassium / sodium ion lithium doping. + The loss is reduced, and the first discharge specific capacity and the first coulombic efficiency are improved; at the same time, the combination of lithium doping with other metal elements, transition metal doping and particle surface coating effectively improves the cycle performance of high-nickel positive electrode materials, which has the characteristics of simple preparation process, low cost, low pollution, good electrochemical performance and is conducive to industrial production.
[0005] To achieve the above object, the present invention adopts the following technical solutions:
[0006] A high nickel cathode material with the chemical formula Li a Na b K c Ni x Co y Mn z Al (1-x-y-z) T d O 2 ,
[0007] Where 0.8≤a<1, 0≤b≤0.2, 0≤c≤0.2, 0<d≤0.02, 0.8≤x≤1, 0≤y≤0.2, 0≤z≤0.2, and a+b+c=1, x+y+z≤1;
[0008] T is one or two of Mg, Al, Ti, Zr, W, Sb, Y, Nb, Sr, Sc, Mo, Ta, and Cr.
[0009] A method for preparing the above-mentioned high-nickel positive electrode material comprises the following steps:
[0010] 1) fully mixing a high nickel precursor material with lithium salt, potassium salt, sodium salt and other doped metal salts to obtain a mixture A;
[0011] 2) roasting, cooling, crushing and screening the mixture A to obtain a high nickel positive electrode material B doped with potassium / sodium ions and lithium sites;
[0012] 3) washing the high nickel cathode material B, centrifuging / filtering, drying, and cooling to obtain the high nickel cathode material C;
[0013] 4) The high-nickel positive electrode material C is fully mixed with the particle surface coating salt, and then subjected to secondary calcination, cooling, crushing, and screening to obtain the high-nickel positive electrode material.
[0014] Furthermore, the high nickel precursor material in step 1) is Ni x Co y Mn z Al (1-x-y-z) (OH) 2 ; The lithium salt is selected from any one or more of lithium hydroxide, lithium carbonate, lithium fluoride or lithium chloride; the potassium salt is selected from any one or more of potassium hydroxide, potassium carbonate, potassium acetate, potassium oxalate or potassium sulfate; the sodium salt is selected from any one or more of sodium carbonate, sodium acetate, sodium chloride, sodium acetate, sodium oxalate, sodium sulfate or sodium bicarbonate; the elements contained in the other doped metal salts are one or two of Mg, Al, Ti, Zr, W, Sb, Y, Nb, Sr, Sc, Mo, Ta, Cr.
[0015] Furthermore, the calcination process in step 2) is calcination at a temperature of 450-550° C. for 1-5 hours, and then calcination at a temperature of 600-850° C. for 4-20 hours.
[0016] Furthermore, in the step 3), the solid content during water washing is 40% to 70% (mass ratio), and the water washing time is 1 to 20 minutes.
[0017] Furthermore, in step 3), the drying temperature is 110-200° C., and the drying time is 1-8 hours.
[0018] Furthermore, the elements contained in the salt coating the particle surface in step 4) are selected from any one or more of Co, F, B, W, and Al.
[0019] Furthermore, in step 4), the calcination temperature is 250-350° C., and the calcination time is 4-12 hours.
[0020] Compared with the prior art, the present invention has the following beneficial effects:
[0021] (1) Potassium or sodium salts are added during the preparation of high-nickel positive electrode materials, and potassium and sodium ion lithium doping is achieved through high-temperature calcination; according to the principle of ion solvation, during the first charge and discharge process, potassium and sodium ions that migrate faster reach the counter electrode earlier than lithium ions, and preferentially form SEI and CEI films, thereby reducing Li + Irreversible consumption improves lithium ion utilization;
[0022] (2) During the first discharge lithium insertion process, Li + It can occupy potassium and sodium vacancies, thus significantly improving the initial capacity and initial coulombic efficiency of the battery;
[0023] (3) Sodium and potassium ions have larger diameters than lithium ions, and can play a role in supporting the interlayer structure, preventing structural collapse during the process of lithium ion extraction / insertion, thereby stabilizing the layered structure of high-nickel positive electrode materials; combined with lithium doping of other metal elements and transition metal doping, while stabilizing the layered structure of high-nickel positive electrode materials, the interlayer spacing is widened, making the ions extract / insert more rapidly during the charge and discharge process, thereby effectively improving the rate performance of the battery; finally, combined with particle surface coating, the cycle performance of high-nickel positive electrode materials is effectively improved;
[0024] (4) The earth's reserves of sodium salts and potassium salts are higher than those of lithium salts. They are widely available and have low market prices, which can reduce the production cost of positive electrode materials.
[0025] (5) The preparation process is simple, does not require the addition of new steps, is green and pollution-free, has low cost, is suitable for large-scale industrial production, and greatly improves the electrochemical properties of high-nickel positive electrode materials, which well meets the needs of current social market development. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 This is a SEM photograph of the high-nickel positive electrode material prepared in Example 1 of the present invention at 5000 times magnification;
[0027] Figure 2 This is a SEM photograph of the high-nickel positive electrode material prepared in Example 1 of the present invention at 1000 times magnification;
[0028] Figure 3 This is the XRD pattern of the high nickel positive electrode material prepared in Example 1 of the present invention;
[0029] Figure 4 The electrochemical cycle performance diagrams of the high nickel positive electrode materials prepared in Example 1 of the present invention and Comparative Examples 1 and 2 at 0.3C are shown. Specific implementation plan
[0030] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0031] The present invention provides a high nickel positive electrode material, the chemical formula of which is Li a Na b K c Ni x Co y Mn z Al (1-x-y-z) T d O 2 ,
[0032] Where 0.8≤a<1, 0≤b≤0.2, 0≤c≤0.2, 0<d≤0.02, 0.8≤x≤1, 0≤y≤0.2, 0≤z≤0.2, and a+b+c=1, x+y+z≤1;
[0033] T is one or two of Mg, Al, Ti, Zr, W, Sb, Y, Nb, Sr, Sc, Mo, Ta, and Cr.
[0034] The present invention also provides a method for preparing the above-mentioned high-nickel positive electrode material, comprising the following steps:
[0035] 1) fully mixing a high nickel precursor material with lithium salt, potassium salt, sodium salt and other doped metal salts to obtain a mixture A;
[0036] 2) roasting, cooling, crushing and screening the mixture A to obtain a high nickel positive electrode material B doped with potassium / sodium ions and lithium sites;
[0037] 3) washing the high nickel cathode material B, centrifuging / filtering, drying, and cooling to obtain the high nickel cathode material C;
[0038] 4) The high-nickel positive electrode material C is fully mixed with the particle surface coating salt, and then subjected to secondary calcination, cooling, crushing, and screening to obtain the high-nickel positive electrode material.
[0039] Potassium or sodium salts are added during the preparation of high-nickel positive electrode materials, and potassium and sodium ion lithium doping is achieved through high-temperature calcination; according to the principle of ion solvation, during the first charge and discharge process, potassium and sodium ions that migrate faster reach the counter electrode earlier than lithium ions, and preferentially form SEI and CEI films, thereby reducing Li +Irreversible consumption improves lithium ion utilization; during the first discharge lithium insertion process, Li + It can occupy potassium and sodium vacancies, thereby significantly improving the first capacity and first coulomb efficiency of the battery; potassium and sodium ion lithium doping combined with other metal elements lithium doping and transition metal doping, while stabilizing the layered structure of the high-nickel positive electrode material, widens the interlayer spacing, making the ions more rapidly de-embedded during the charge and discharge process, thereby effectively improving the rate performance of the battery; finally, combined with particle surface coating, the cycle performance of the high-nickel positive electrode material is effectively improved. The present invention has the characteristics of simple preparation process, low cost, low pollution, good electrochemical performance and is conducive to industrial production.
[0040] The ion solvation principle means that it is generally believed that potassium and sodium ions have larger volume and atomic mass than lithium ions, and their kinetic performance is not as good as that of lithium ions. However, for ion diffusion in solvents, ions always exist in a solvated form. Due to their weak Lewis acidity, the solvated ions of potassium and sodium ions are smaller than those of lithium solvated ions. The mobility of the electrolyte is high, the migration number is large, and the desolvation energy is low. Therefore, the diffusion kinetics of potassium and sodium ions are faster than those of lithium ions.
[0041] Preferably, the high nickel precursor material in step 1) is Ni x Co y Mn z Al (1-x-y-z) (OH) 2 ; Lithium salt is selected from any one or more of lithium hydroxide, lithium carbonate, lithium fluoride or lithium chloride; Potassium salt is selected from any one or more of potassium hydroxide, potassium carbonate, potassium acetate, potassium oxalate or potassium sulfate; Sodium salt is selected from any one or more of sodium carbonate, sodium acetate, sodium chloride, sodium acetate, sodium oxalate, sodium sulfate or sodium bicarbonate; The elements contained in other doped metal salts are one or two of Mg, Al, Ti, Zr, W, Sb, Y, Nb, Sr, Sc, Mo, Ta, Cr.
[0042] Preferably, the calcination process in step 2) is calcination at a temperature of 450-550° C. for 1-5 hours, and then calcination at a temperature of 600-850° C. for 4-20 hours.
[0043] Preferably, in step 3), the solid content during water washing is 40% to 70% (mass ratio), and the water washing time is 1 to 20 minutes.
[0044] Preferably, in step 3), the drying temperature is 110-200° C. and the drying time is 1-8 hours.
[0045] Preferably, in step 4), the elements contained in the salt coating the particle surface are selected from any one or more of Co, F, B, W, and Al.
[0046] Preferably, in step 4), the calcination temperature is 250-350° C. and the calcination time is 4-12 hours.
[0047] Example 1
[0048] A method for preparing a high-nickel positive electrode material comprises the following steps:
[0049] 1) Mix high nickel precursor material, lithium hydroxide, potassium hydroxide and sodium hydroxide in a molar ratio of 1:1.01:0.015:0.005. The high nickel precursor material is Ni 0.90 Co 0.05 Mn 0.04 Al 0.01 (OH) 2 , then add 3000ppm ZrO 2 and 3000ppm Sb 2 O 3 (based on the mass of the high nickel precursor material) and fully mixed to obtain a mixture A;
[0050] 2) The mixture A is calcined at 500° C. for 4 h in an oxygen atmosphere, and then calcined at 810° C. for 12 h, and after cooling, crushing and screening, a high nickel cathode material B doped with potassium / sodium ions and lithium sites is obtained;
[0051] 3) Mix the high-nickel cathode material B with an equal mass of pure water (solid content 50%) and wash with water for 3 minutes, then centrifuge / filter, dry under vacuum at 160° C. for 2 hours, and then cool to obtain the high-nickel cathode material C;
[0052] 4) Combine high nickel cathode materials C and H 3 BO 3 After being fully mixed at a molar ratio of 1:0.01, the mixture was calcined twice at a temperature of 300°C for 8 hours. After cooling, crushing and screening, a high-nickel positive electrode material was obtained, whose chemical formula is Li 0.98 Na 0.005 K 0.015 Ni 0.90 Co 0.05 Mn 0.037 Al 0.007 Zr 0.003 Sb 0.003 O 2 .
[0053] Example 2
[0054] A method for preparing a high-nickel positive electrode material comprises the following steps:
[0055] 1) Mix high nickel precursor material, lithium hydroxide, potassium hydroxide and sodium hydroxide in a molar ratio of 1:1.01:0.015:0.005. The high nickel precursor material is Ni 0.90 Co 0.05 Mn 0.04 Al 0.01 (OH) 2 , then add 3000ppm TiO 2 and 3000ppm Sb 2 O 3 (based on the mass of the high nickel precursor material) and fully mixed to obtain a mixture A;
[0056] 2) The mixture A is calcined at 500° C. for 4 h in an oxygen atmosphere, and then calcined at 810° C. for 12 h, and after cooling, crushing and screening, a high nickel cathode material B doped with potassium / sodium ions and lithium sites is obtained;
[0057] 3) Mix the high-nickel cathode material B with an equal mass of pure water (solid content 50%) and wash with water for 3 minutes, then centrifuge / filter, dry under vacuum at 160° C. for 2 hours, and then cool to obtain the high-nickel cathode material C;
[0058] 4) Combine high nickel cathode materials C and H 3 BO 3 After being fully mixed at a molar ratio of 1:0.01, the mixture was calcined twice at a temperature of 300°C for 8 hours. After cooling, crushing and screening, a high-nickel positive electrode material was obtained, whose chemical formula is Li 0.98 Na 0.005 K 0.015 Ni 0.90 Co 0.05 Mn 0.037 Al 0.007 Ti 0.003 Sb 0.003 O 2 .
[0059] Example 3
[0060] A method for preparing a high-nickel positive electrode material comprises the following steps:
[0061] 1) Mix high nickel precursor material, lithium hydroxide, potassium hydroxide and sodium hydroxide in a molar ratio of 1:1.01:0.005:0.015. The high nickel precursor material is Ni 0.90 Co 0.05 Mn 0.04 Al 0.01 (OH) 2 , then add 3000ppm ZrO 2and 3000ppm Sb 2 O 3 (based on the mass of the high nickel precursor material) and fully mixed to obtain a mixture A;
[0062] 2) The mixture A is calcined at 450° C. for 5 h in an oxygen atmosphere, and then calcined at 690° C. for 12 h, and after cooling, crushing and screening, a high nickel cathode material B doped with potassium / sodium ions and lithium sites is obtained;
[0063] 3) Mix the high nickel cathode material B with pure water (solid content 40%) and wash with water for 1 min, then centrifuge / filter, dry under vacuum at 200° C. for 2 h, and then cool to obtain the high nickel cathode material C;
[0064] 4) Combine high nickel cathode materials C and H 3 BO 3 After being fully mixed at a molar ratio of 1:0.01, the mixture was calcined twice at a temperature of 300°C for 12 hours. After cooling, crushing and screening, a high-nickel positive electrode material was obtained, whose chemical formula is Li 0.98 Na 0.015 K 0.005 Ni 0.90 Co 0.05 Mn 0.037 Al 0.007 Zr 0.003 Sb 0.003 O 2 .
[0065] Example 4
[0066] 1) Mix high nickel precursor material, lithium hydroxide, potassium hydroxide and sodium hydroxide in a molar ratio of 1:1.01:0.02:0.02. The high nickel precursor material is Ni 0.90 Co 0.05 Mn 0.04 Al 0.01 (OH) 2 , then add 3000ppm ZrO 2 and 3000ppm Sb 2 O 3 (based on the mass of the high nickel precursor material) and fully mixed to obtain a mixture A;
[0067] 2) The mixture A is calcined at 550° C. for 1 h in an oxygen atmosphere, and then calcined at 650° C. for 12 h, and after cooling, crushing and screening, a high nickel cathode material B doped with potassium / sodium ions and lithium sites is obtained;
[0068] 3) Mix the high nickel cathode material B with pure water (solid content 70%) and wash with water for 20 min, then centrifuge / filter, dry under vacuum at 200° C. for 2 h, and then cool to obtain the high nickel cathode material C;
[0069] 4) Combine high nickel cathode materials C and H 3 BO 3 After being fully mixed at a molar ratio of 1:0.01, the mixture was calcined twice at a temperature of 250°C for 12 hours. After cooling, crushing and screening, a high-nickel positive electrode material was obtained, whose chemical formula is Li 0.96 Na 0.02 K 0.02 Ni 0.90 Co 0.05 Mn 0.037 Al 0.007 Zr 0.003 Sb 0.003 O 2 .
[0070] Example 5
[0071] A method for preparing a high-nickel positive electrode material comprises the following steps:
[0072] 1) Mix high nickel precursor material, lithium hydroxide, potassium hydroxide and sodium hydroxide in a molar ratio of 1:1.01:0.01:0.01. The high nickel precursor material is Ni 0.90 Co 0.05 Mn 0.04 Al 0.01 (OH) 2 , then add 3000ppm ZrO 2 and 3000ppm Sb 2 O 3 (based on the mass of the high nickel precursor material) and fully mixed to obtain a mixture A;
[0073] 2) The mixture A is calcined at 500° C. for 4 h in an oxygen atmosphere, and then calcined at 850° C. for 4 h, and after cooling, crushing and screening, a high nickel cathode material B doped with potassium / sodium ions and lithium sites is obtained;
[0074] 3) Mix the high nickel cathode material B with the same mass of pure water (solid content 50%) and wash with water for 3 min, then centrifuge / filter, dry under vacuum at 110° C. for 8 h, and cool to obtain the high nickel cathode material C;
[0075] 4) Combine high nickel cathode materials C and H 3 BO 3After being fully mixed at a molar ratio of 1:0.01, the mixture was calcined twice at a temperature of 300°C for 8 hours. After cooling, crushing and screening, a high-nickel positive electrode material was obtained, whose chemical formula is Li 0.98 Na 0.01 K 0.01 Ni 0.90 Co 0.05 Mn 0.037 Al 0.007 Zr 0.003 Sb 0.003 O 2 .
[0076] Example 6
[0077] A method for preparing a high-nickel positive electrode material comprises the following steps:
[0078] 1) Mix high nickel precursor material, lithium hydroxide, potassium hydroxide and sodium hydroxide in a molar ratio of 1:1.01:0.005:0.005. The high nickel precursor material is Ni 0.90 Co 0.05 Mn 0.04 Al 0.01 (OH) 2 , then add 3000ppm ZrO 2 and 3000ppm Sb 2 O 3 (based on the mass of the high nickel precursor material) and fully mixed to obtain a mixture A;
[0079] 2) The mixture A is calcined at 500° C. for 4 h in an oxygen atmosphere, and then calcined at 600° C. for 20 h, and after cooling, crushing and screening, a high nickel cathode material B doped with potassium / sodium ions and lithium sites is obtained;
[0080] 3) Mix the high-nickel cathode material B with an equal mass of pure water (solid content 50%) and wash with water for 3 minutes, then centrifuge / filter, dry under vacuum at 200° C. for 1 hour, and then cool to obtain the high-nickel cathode material C;
[0081] 4) Combine high nickel cathode materials C and H 3 BO 3 After being fully mixed at a molar ratio of 1:0.01, secondary calcination is performed at a temperature of 350°C for 4 hours. After cooling, crushing and screening, a high-nickel positive electrode material is obtained, whose chemical formula is Li 0.99 Na 0.005 K 0.005 Ni 0.90 Co 0.05 Mn 0.037 Al 0.007 Zr0.003 Sb 0.003 O 2 .
[0082] Example 7
[0083] A method for preparing a high-nickel positive electrode material comprises the following steps:
[0084] 1) Mix high nickel precursor material, lithium hydroxide and sodium hydroxide in a molar ratio of 1:1.01:0.2. The high nickel precursor material is Ni 0.90 Co 0.05 Mn 0.04 Al 0.01 (OH) 2 , then add 3000ppm ZrO 2 and 3000ppm Sb 2 O 3 (based on the mass of the high nickel precursor material) and fully mixed to obtain a mixture A;
[0085] 2) The mixture A is calcined at 500° C. for 4 h in an oxygen atmosphere, and then calcined at 810° C. for 12 h, and after cooling, crushing and screening, a high nickel cathode material B doped with potassium / sodium ions and lithium sites is obtained;
[0086] 3) Mix the high-nickel cathode material B with an equal mass of pure water (solid content 50%) and wash with water for 3 minutes, then centrifuge / filter, dry under vacuum at 160° C. for 2 hours, and then cool to obtain the high-nickel cathode material C;
[0087] 4) Combine high nickel cathode materials C and H 3 BO 3 After being fully mixed at a molar ratio of 1:0.01, the mixture was calcined twice at a temperature of 300°C for 8 hours. After cooling, crushing and screening, a high-nickel positive electrode material was obtained, whose chemical formula is Li 0.80 Na 0.20 Ni 0.90 Co 0.05 Mn 0.037 Al 0.007 Zr 0.003 Sb 0.003 O 2 .
[0088] Example 8
[0089] A method for preparing a high-nickel positive electrode material comprises the following steps:
[0090] 1) Mix high nickel precursor material, lithium hydroxide and potassium hydroxide in a molar ratio of 1:1.01:0.2. The high nickel precursor material is Ni0.90 Co 0.05 Mn 0.04 Al 0.01 (OH) 2 , then add 3000ppm ZrO 2 and 3000ppm Sb 2 O 3 (based on the mass of the high nickel precursor material) and fully mixed to obtain a mixture A;
[0091] 2) The mixture A is calcined at 500° C. for 4 h in an oxygen atmosphere, and then calcined at 810° C. for 12 h, and after cooling, crushing and screening, a high nickel cathode material B doped with potassium / sodium ions and lithium sites is obtained;
[0092] 3) Mix the high-nickel cathode material B with an equal mass of pure water (solid content 50%) and wash with water for 3 minutes, then centrifuge / filter, dry under vacuum at 160° C. for 2 hours, and then cool to obtain the high-nickel cathode material C;
[0093] 4) Combine high nickel cathode materials C and H 3 BO 3 After being fully mixed at a molar ratio of 1:0.01, the mixture was calcined twice at a temperature of 300°C for 8 hours. After cooling, crushing and screening, a high-nickel positive electrode material was obtained, whose chemical formula is Li 0.80 K 0.20 Ni 0.90 Co 0.05 Mn 0.037 Al 0.007 Zr 0.003 Sb 0.003 O 2 .
[0094] Example 9
[0095] A method for preparing a high-nickel positive electrode material comprises the following steps:
[0096] 1) Mix high nickel precursor material, lithium hydroxide, potassium hydroxide and sodium hydroxide in a molar ratio of 1:1.01:0.01:0.01. The high nickel precursor material is Ni 0.90 Co 0.06 Mn 0.04 (OH) 2 , then add 3000ppm ZrO 2 and 3000ppmSb 2 O 3 (based on the mass of the high nickel precursor material) and fully mixed to obtain a mixture A;
[0097] 2) The mixture A is calcined at 500° C. for 4 h in an oxygen atmosphere, and then calcined at 850° C. for 4 h, and after cooling, crushing and screening, a high nickel cathode material B doped with potassium / sodium ions and lithium sites is obtained;
[0098] 3) Mix the high nickel cathode material B with the same mass of pure water (solid content 50%) and wash with water for 3 min, then centrifuge / filter, dry under vacuum at 110° C. for 8 h, and cool to obtain the high nickel cathode material C;
[0099] 4) Combine high nickel cathode materials C and H 3 BO 3 After being fully mixed at a molar ratio of 1:0.01, the mixture was calcined twice at a temperature of 300°C for 8 hours. After cooling, crushing and screening, a high-nickel positive electrode material was obtained, whose chemical formula is Li 0.98 Na 0.01 K 0.01 Ni 0.90 Co 0.06 Mn 0.034 Zr 0.003 Sb 0.003 O 2 .
[0100] Example 10
[0101] A method for preparing a high-nickel positive electrode material comprises the following steps:
[0102] 1) Mix high nickel precursor material, lithium hydroxide and sodium hydroxide in a molar ratio of 1:1.01:0.02. The high nickel precursor material is Ni 0.90 Co 0.06 Mn 0.04 (OH) 2 , then add 3000ppm ZrO 2 and 3000ppm Sb 2 O 3 (based on the mass of the high nickel precursor material) and fully mixed to obtain a mixture A;
[0103] 2) The mixture A is calcined at 500° C. for 4 h in an oxygen atmosphere, and then calcined at 810° C. for 12 h, and after cooling, crushing and screening, a high nickel cathode material B doped with potassium / sodium ions and lithium sites is obtained;
[0104] 3) Mix the high-nickel cathode material B with an equal mass of pure water (solid content 50%) and wash with water for 3 minutes, then centrifuge / filter, dry under vacuum at 160° C. for 2 hours, and then cool to obtain the high-nickel cathode material C;
[0105] 4) Combine high nickel cathode materials C and H3 BO 3 After being fully mixed at a molar ratio of 1:0.01, the mixture was calcined twice at a temperature of 300°C for 8 hours. After cooling, crushing and screening, a high-nickel positive electrode material was obtained, whose chemical formula is Li 0.98 Na 0.02 Ni 0.90 Co 0.06 Mn 0.034 Zr 0.003 Sb 0.003 O 2 .
[0106] Embodiment 11
[0107] A method for preparing a high-nickel positive electrode material comprises the following steps:
[0108] 1) Mix high nickel precursor material, lithium hydroxide and potassium hydroxide in a molar ratio of 1:1.01:0.02. The high nickel precursor material is Ni 0.90 Co 0.06 Mn 0.04 (OH) 2 , then add 3000ppm ZrO 2 and 3000ppm Sb 2 O 3 (based on the mass of the high nickel precursor material) and fully mixed to obtain a mixture A;
[0109] 2) The mixture A is calcined at 500° C. for 4 h in an oxygen atmosphere, and then calcined at 810° C. for 12 h, and after cooling, crushing and screening, a high nickel cathode material B doped with potassium / sodium ions and lithium sites is obtained;
[0110] 3) Mix the high-nickel cathode material B with an equal mass of pure water (solid content 50%) and wash with water for 3 minutes, then centrifuge / filter, dry under vacuum at 160° C. for 2 hours, and then cool to obtain the high-nickel cathode material C;
[0111] 4) Combine high nickel cathode materials C and H 3 BO 3 After being fully mixed at a molar ratio of 1:0.01, the mixture was calcined twice at a temperature of 300°C for 8 hours. After cooling, crushing and screening, a high-nickel positive electrode material was obtained, whose chemical formula is Li 0.98 K 0.02 Ni 0.90 Co 0.06 Mn 0.034 Zr 0.003 Sb 0.003 O 2 .
[0112] Comparative Example 1
[0113] A method for preparing a high-nickel positive electrode material, compared with Example 1, the difference is that sodium hydroxide and potassium hydroxide are not added in step 1), and the remaining parameters and steps are exactly the same as those in Example 1.
[0114] Comparative Example 2
[0115] A method for preparing a high nickel positive electrode material, compared with Example 1, the difference is that ZrO is not added in step 1) 2 and Sb 2 O 3 , the remaining parameters and steps are exactly the same as those in Example 1.
[0116] Comparative Example 3
[0117] A method for preparing a high-nickel positive electrode material, compared with Example 1, the difference is that in step 1), no sodium hydroxide and potassium hydroxide are added, and no ZrO is added 2 and Sb 2 O 3 , the remaining parameters and steps are exactly the same as those in Example 1.
[0118] The high nickel cathode material obtained in Example 1 was characterized by SEM and XRD, wherein: Figure 1 and Figure 2 The SEM photos are magnified 5000 times and 1000 times respectively. It can be seen that the material is a secondary particle sphere formed by the aggregation of primary particles. Figure 3 The XRD diagram shows sharp diffraction peaks, indicating that the material has high crystallinity and stable crystal structure.
[0119] Table 1 lists the first discharge specific capacity at different current densities, the first coulombic efficiency at 0.2C, and the capacity retention rate after 100 cycles of the button-type batteries assembled with the high nickel positive electrode materials prepared in Examples 1-11 and Comparative Examples 1-3; the test conditions of the button-type batteries are LR2032, 2.5-4.25V, vs. Li + / Li. The positive electrode sheet of this battery is prepared according to the mass ratio of sample: conductive agent: PVDF = 96:1.5:2.5.
[0120] From the data in Table 1, we can see that:
[0121] (1) Compared with Comparative Example 1, the discharge specific capacity at different current densities, the first coulombic efficiency at 0.2C, and the 100-cycle capacity retention rate at 0.3C of Examples 1 to 11 are significantly better than those of Comparative Example 1. According to the principle of ion solvation, during the first charge and discharge process, potassium and sodium ions that migrate faster reach the counter electrode earlier than lithium ions, and preferentially form SEI and CEI films, thereby reducing Li + Irreversible consumption; during the first discharge lithium insertion process, Li + It can occupy potassium and sodium vacancies, thus significantly improving the initial capacity and initial coulombic efficiency of the battery;
[0122] (2) Compared with Comparative Example 2, the discharge specific capacity at different current densities, the first coulombic efficiency at 0.2C, and the 100-cycle capacity retention rate at 0.3C of Examples 1 to 11 are significantly better than those of Comparative Example 2. It can be seen that the doping of interlayer inactive sites is crucial to the electrochemical performance of high-nickel positive electrode materials. The presence of doping elements in interlayer inactive sites can not only support the interlayer structure, widen the interlayer spacing, and increase the lithium ion active sites, thereby improving the capacity, but also maintain the stability of the layered structure during lithium ion extraction / insertion, thereby improving the cycle stability of high-nickel positive electrode materials.
[0123] (3) Compared with Comparative Example 3, Comparative Example 2 has significantly better discharge capacity at different current densities, first coulombic efficiency at 0.2C, and 100-cycle capacity retention rate at 0.3C than Comparative Example 3, which indicates that the introduction of sodium ions and potassium ions can help maintain the stability of the layered structure to a certain extent;
[0124] (4) The electrochemical performances of Example 1 and Example 2 at different current densities, discharge specific capacity, first coulomb efficiency at 0.2C, and 100-cycle capacity retention at 0.3C are similar, which shows that interlayer doping elements with the same effect as Zr and Ti can be freely replaced and do not affect the effects of sodium ions and potassium ions. Therefore, sodium ions and potassium ions can better play their role by doping lithium sites on the basis of doping in the interlayer inactive sites;
[0125] (5) Compared with Example 9, Example 5 has a better 100-cycle capacity retention rate than Example 9, and the discharge specific capacity of Example 9 is higher than that of Example 5 at different current densities; Compared with Example 10, Example 7 has a better 100-cycle capacity retention rate than Example 10, and the discharge specific capacity of Example 10 is higher than that of Example 7 at different current densities; Compared with Example 11, Example 8 has a better 100-cycle capacity retention rate than Example 11, and the discharge specific capacity of Example 11 is higher than that of Example 8 at different current densities; This shows that the aluminum element occupies part of the active lithium sites and the inactive lithium sites, which hinders the capacity improvement of the high-nickel positive electrode material, but can effectively improve the cycle retention rate of the layered positive electrode material; This shows that the lithium-site doping of sodium ions and potassium ions to improve the electrochemical performance of the high-nickel positive electrode material battery is not affected by the precursor element ratio and element type, and this method is applicable to the high-nickel positive electrode materials described above.
[0126] Table 1
[0127]
[0128] Part of the implementation of the present invention has been specifically described above, but the present invention is not limited to the above-mentioned embodiments. Those skilled in the art may make equivalent modifications or substitutions without violating the spirit of the present invention. These equivalent modifications or substitutions are all included in the scope defined by the claims of this application.
Claims
1. A method for preparing a high-nickel positive electrode material, characterized in that: The chemical formula of the high nickel positive electrode material is Li a Na b K c Ni x Co y Mn z Al (1-x-y-z) T d O2, where 0.8≤a<1, 0<b≤0.2, 0<c≤0.2, 0<d≤0.02, 0.8≤x≤1, 0≤y≤0.2, 0≤z≤0.2, and a+b+c=1, x+y+z<1; T is one or two of Mg, Al, Ti, Zr, W, Sb, Y, Nb, Sr, Sc, Mo, Ta, and Cr; The method for preparing the high-nickel positive electrode material comprises the following steps: 1) A high nickel precursor material is fully mixed with lithium salt, potassium salt, sodium salt and other doped metal salts to obtain a mixture A; the high nickel precursor material is Ni x Co y Mn z Al (1-x-y-z) (OH)2; 2) roasting, cooling, crushing and screening the mixture A to obtain a high nickel positive electrode material B doped with potassium / sodium ions and lithium sites; 3) washing the high nickel cathode material B, centrifuging / filtering, drying, and cooling to obtain the high nickel cathode material C; 4) The high-nickel positive electrode material C is fully mixed with the particle surface coating salt, and then subjected to secondary calcination, cooling, crushing, and screening to obtain the high-nickel positive electrode material.
2. The method for preparing a high nickel positive electrode material according to claim 1, characterized in that: In step 1), the lithium salt is selected from any one or more of lithium hydroxide, lithium carbonate, lithium fluoride or lithium chloride; the potassium salt is selected from any one or more of potassium hydroxide, potassium carbonate, potassium acetate, potassium oxalate or potassium sulfate; the sodium salt is selected from any one or more of sodium carbonate, sodium acetate, sodium chloride, sodium acetate, sodium oxalate, sodium sulfate or sodium bicarbonate; the elements contained in the other doped metal salts are one or two of Mg, Al, Ti, Zr, W, Sb, Y, Nb, Sr, Sc, Mo, Ta, and Cr.
3. The method for preparing a high nickel positive electrode material according to claim 1, characterized in that: The calcination process in step 2) is to calcine at a temperature of 450-550° C. for 1-5 hours and then calcine at a temperature of 600-850° C. for 4-20 hours.
4. The method for preparing a high-nickel positive electrode material according to claim 1, characterized in that: In the step 3), the solid content during water washing is 40% to 70% (mass ratio), and the water washing time is 1 to 20 minutes.
5. The method for preparing a high-nickel positive electrode material according to claim 4, characterized in that: In the step 3), the drying temperature is 110-200° C. and the drying time is 1-8 hours.
6. The method for preparing a high nickel cathode material according to claim 1, characterized in that: In step 4), the elements contained in the salt coating the particle surface are selected from any one or more of Co, F, B, W, and Al.
7. The method for preparing a high nickel cathode material according to claim 1, characterized in that: In the step 4), the calcination temperature is 250-350° C. and the calcination time is 4-12 hours.
Citation Information
Patent Citations
Lithic natrium doping type lithium iron phosphate cathode material for lithium-ion battery and preparation method thereof
CN101540400A
Method for manufacturing cathode active material for lithium secondary battery, cathode active material for lithium secondary battery, cathode, comprising same, for lithium secondary battery, and lithium secondary battery comprising same
CN111867979A
Lithium ion battery positive electrode material, preparation method of positive electrode material and application of positive electrode material in lithium ion battery
CN112701264A
Lithium-doped modified high-nickel low-cobalt ternary positive electrode material for lithium ion battery, and preparation method thereof
CN112768687A
Method of Preparing Positive Electrode Active Material For Lithium Secondary Battery, Positive Electrode Active Material For Lithium Secondary Battery, And Positive Electrode For Lithium Secondary Battery and Lithium Secondary Battery Including The Same
US20210005874A1