Additives for protecting polymers from UV light
By covalently combining UV absorbers with inorganic oxide particles to form modified particles, the problem of surface migration of UV absorbers in polymers is solved, and the photostability and UV blocking properties of the polymers are improved.
Patent Information
- Application Number
- CN202210324098.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2016-02-28
- Filing Date
- 2017-02-27
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2037-02-27
AI Technical Summary
UV absorbers added to existing polymers tend to separate from the polymer and migrate to the surface, causing surface migration problems in food packaging materials and affecting light stability and product performance.
By covalently combining UV-absorbing compounds with inorganic oxide particles (such as silica, zinc oxide) to form particles with spacer chemical bonds, the modified particles are blended with polymers to reduce the surface migration of UV-absorbing agents.
It significantly reduces the surface migration of the UV absorber, maintains the photostability and UV blocking properties of the polymer film, and avoids the adverse effects of UV radiation on the material.
Smart Images

Figure BDA0003571171400000021 
Figure BDA0003571171400000041 
Figure BDA0003571171400000051
Abstract
Description
[0001] This invention application is a divisional application based on a patent application with an application date of February 27, 2017, application number 201780013323.6, and invention name “Additives for protecting polymers against ultraviolet light”.
[0002] Various additives are introduced into polymers in commercial use to facilitate processing and improve the properties of the final product. For example, compounds that absorb UV light are often added to protect plastic materials from UV radiation, thereby protecting products packaged in the plastic materials, such as food, from the adverse effects of UV radiation.
[0003] Some additives tend to separate from the bulk polymer and migrate to the polymer surface. For this reason, polymer compositions must be tested under stringent storage conditions to measure the occurrence of this surface migration.
[0004] Surface migration of additives is particularly unacceptable in food packaging materials. Therefore, it has been proposed to chemically modify ultraviolet light absorbers (UVA) intended for use as additives in food packaging materials to increase their size in an effort to reduce their migration to the surface. Another approach involves structurally modifying the packaging material (as shown in JP 2013075453 and CN202784136), for example, by using a laminated packaging material consisting of multiple layers with a UVA-free layer applied on top of a UVA-containing layer.
[0005] It has now been discovered that UV absorbing compounds can be covalently bonded to the surface of inorganic oxide particles (e.g., silicon dioxide, zinc oxide); optionally with the aid of a suitable spacer group, and the particles so formed can be compounded with various polymers to form particles, particularly polymer films, which exhibit very low surface migration of the UV absorber. For example, experimental work conducted in support of the present invention has shown that polypropylene and linear low density polyethylene (LLDPE) films incorporating the additive are able to maintain substantially constant UV blocking levels over time, with no detectable surface migration of the UV absorbing compound during testing.
[0006] Covalent binding of active molecules, including light absorbing organic compounds, to the surface of silica particles has been reported (US 6,685,924 to Merck) for the purpose of forming conjugates for use in dermatological and cosmetic preparations. An exemplary conjugate has the following structure:
[0007]
[0008] US 2008 / 0260664 describes inorganic particles (eg silica) functionalized with organic compounds (including light absorbing compounds). The organic compound is primarily present in the core of the particle.
[0009] It has now been discovered that UV-absorbing compounds (e.g., benzotriazoles and benzophenones) can be covalently attached to the surface of inorganic oxide particles by either sequentially surface modifying the particles and then reacting the modified surface with the UV-absorbing compound (referred to herein as the "sequential surface modification variant" or "first variant") or by directly reacting the UV-absorbing compound with unmodified inorganic oxide particles (referred to herein as the "one-step variant" or "second variant"). In any case, the resulting particles having UV-absorbing compounds on their surfaces can be used as additives to modify the properties of polymers in commercial applications, i.e., to improve photostability.
[0010] Thus, the present invention is generally directed to an ultraviolet light absorber suitable for use as an additive in a polymer, comprising inorganic oxide particles having an ultraviolet light absorbing compound on its surface, wherein the ultraviolet light absorbing compound is either chemically (covalently) bonded to a spacer provided on the surface of the particle or directly bonded to the particle surface. The inorganic oxide is preferably selected from silicon dioxide and zinc oxide.
[0011] With regard to the first variant, the silica particles have surface reactivity due to the presence of hydroxyl groups (or more precisely, silanol groups (SiOH) on their surfaces) and can be used for chemical bond formation. Preferably, an organosilicon spacer is constructed on the silica surface to enable connection between the surface and the ultraviolet light absorbing compound. The spacer can be constructed on the silica surface by a series of chemical reactions to provide a functional group, which in turn can react with the ultraviolet light absorbing compound. For example, the surface of the silica particles is modified by introducing SiH groups. The high chemical reactivity of the hydride silicon bond with a variety of chemical functional groups (olefins, alcohols, aldehydes, ketones) allows the appropriately functionalized ultraviolet light absorbing compound to be connected to the silica particles. For example, the hydride silicon group formed on the silica surface can be added to the carbon-carbon double bond of the olefinic compound with the ultraviolet light absorbing part.
[0012] The silica suitable for use in the first variant of the present invention is preferably fumed silica. Important properties for selecting fumed silica for use in the first variant of the present invention include particle size, specific surface area and concentration of silanol groups on the silica. Thus, the silica useful in this variant of the present invention is fumed silica, the average size of the particles of which is less than 40 nm, for example, from 5 nm to 35 nm, more specifically from 5 nm to 20 nm, even more specifically from 5 nm to 15 nm, wherein the specific surface area is not less than 150 m 2 / g, for example, not less than 200m 2 / g, for example 200 to 500 m 2 / g. The concentration of SiOH groups on the surface of the silica is preferably not less than 0.7 mmol / g, for example not less than 0.8 mmol / g, for example 0.8 mmol / g to 3.0 mmol / g (measured by thermogravimetric analysis). Commercially available fumed silica grades such as those from Cabot Corporation can be used. M5 and EH5, and from Evonik Industries 200 and 300 / 30.
[0013] As for the second variant, silica or zinc oxide particles may be used, that is, this variant of the invention involves reacting inorganic oxide particles directly with a UV-absorbing compound having suitable reactive groups, such as Si-O-alkyl groups. Silica used in this 'one-step variant' includes fumed silica having the properties described above, for example, M5 and EH5. Another type of silica tested in the experimental work reported below is colloidal silica, i.e. silica suspended in a solvent. Monodisperse colloidal silica consisting of a population of discrete, spherical particles of uniform size can show advantages in the final polymer product due to its ability to produce a uniform distribution of additives in the polymer product. As shown in the experimental work reported below, we were able to find reaction conditions that allowed this type of colloidal silica to react rapidly with the ultraviolet light absorbing compound in the same solvents used to suspend the colloidal silica in commercial products available on the market.
[0014] The 'sequential surface modification variant' and the 'one-step variant' are now described.
[0015] The sequential surface modification of silica particles includes introducing a first functional group on the silica surface and then reacting with an ultraviolet light absorbing compound; or introducing a first functional group on the silica surface and then converting the first functional group into a plurality of second functional groups, which in turn react with an ultraviolet light absorbing compound.
[0016] The second approach is generally preferred because each individual first functional group reacts with a molecule bearing multiple second functional groups, resulting in an increased concentration of reactive sites ultimately available for forming chemical bonds with the ultraviolet light absorbing compound.
[0017] Therefore, the present invention generally relates to a method for preparing an ultraviolet light absorber additive for protecting a polymer from ultraviolet radiation, which comprises introducing a first functional group on the surface of an inorganic oxide particle, reacting the inorganic particle thus formed modified by the first group with a spacer having a plurality of second functional groups; and reacting the inorganic particle thus formed modified by the second functional group with an ultraviolet light absorbing compound.
[0018] For this purpose, the first functional groups (preferably carbon-carbon double bonds) are introduced on the silica surface by reacting the silica particles with a vinyl compound, for example of the formula (H2C=CH) i Si(OC j H 2j+1 ) 4-i A vinyl compound, for example, vinyl trimethoxysilane (i=1, j=1) or trivinyl ethoxysilane (i=3, j=2). These two vinyl compounds are high boiling point liquids, and the reaction can be carried out as follows: in a reaction medium without a solvent, use an excess of (H2C=CH i Si(OC j H 2j+1 ) 4-i To provide a stirrable reaction mixture. Therefore, the silica particles and the vinyl compound are added to a reaction vessel and reacted under heating (e.g., above 100° C., preferably at reflux temperature) with stirring to obtain silica particles with vinyl groups. The reaction is allowed to complete after several hours. The reaction mixture is cooled, the surface-modified particles are separated by filtration, washed to remove excess reactants, and dried.
[0019] Next, a spacer with multiple functional groups is chemically linked to the first functional group present on the surface of the silica particles. The number of functional groups in the spacer is represented by n, where n is an integer equal to or greater than 3. It should be noted that one of the n functional groups participates in the bond-forming reaction with the first functional group present on the surface of the silica particles, thus leaving at most n-1 reaction sites available for the bond-forming reaction with the corresponding n-1 ultraviolet light absorbing compounds. The number of functional groups in the spacer is preferably not less than four (n≥4).
[0020] Preferably, the spacer has a plurality of mutually identical functional groups, such as a plurality of silicon hydride groups. The silicon hydride functional group has two useful features. First, in the presence of a suitable catalyst, the addition reaction (hydrosilylation) of silicon hydride with a carbon-carbon double bond proceeds rapidly. In addition, as described above, the high chemical reactivity of the silicon hydride groups to be placed on the silicon dioxide surface with various chemical functional groups makes it possible to connect many different ultraviolet light absorbing compounds in the final step of additive formation. Some exemplary organosilicon spacers containing a plurality of silicon hydride groups are shown below:
[0021]
[0022]
[0023] It should be remembered that silica with UV absorbing compounds is intended to be used as an additive in polymers. Therefore, the higher the concentration of UV absorbing compounds that can be loaded onto the surface of silica particles, the lower the amount of silica additive that is ultimately required in the final polymer formulation. Therefore, a major factor affecting the concentration of UV absorbing compounds that can be achieved on the silica surface is the number of functional groups in the spacer used. Another important property for screening suitable spacers is the compatibility of silica-spacer-UVA additive with the relevant polymer formulation. Preferably, the number of functional groups in the spacer molecule is 4 to 80 (4≤n≤80).
[0024] A class of spacer molecules operable in the present invention is characterized in that the number of functional groups in the spacer molecule is 4 to 10 (inclusive) (4≤n≤10). For 4≤n≤10, bulky spacers are preferred over 'linear' spacers, that is, compounds in which the silicon hydride group is a pendant group and the immediate surroundings of the silicon atom in the silicon hydride group are occupied by two hydrocarbon groups such as alkyl (e.g. methyl, ethyl) or phenyl groups, over compounds in which the silicon hydride is part of the backbone. The experimental results reported below show that the concentration of the UV absorbing compound in the silica additive was almost doubled (0.3 mmol / g to 0.5 mmol / g) when the linear A6 spacer was replaced by a 'bulky' A6y spacer.
[0025] Another class of spacer molecules operable in the present invention is characterized in that the number of functional groups in the spacer molecule is greater than 20 (n ≥ 20). These spacer molecules have a long (n ≥ 20) main chain in which a silicon hydride group is part of a repeating unit; in particular, poly(methylhydrogensiloxane) consisting of 10 to 80 repeating units is found to be an excellent spacer from the studies reported below. For example, poly(methylhydrogensiloxane) consisting of about 50-80 (e.g., about 75) silicon hydride groups and preferably terminated with trimethylsiloxy groups has been shown to increase the concentration of ultraviolet light absorbing compounds on the surface of silica to about 2 mmol / g. Poly(methylhydrogensiloxane) suitable for use as spacers in the present invention are commercially available, for example, MH30 (hereinafter referred to as MH30; from AB Specialty Silicones) The experimental results also show that the chemical bonding of the ultraviolet light absorbing compound to MH30 leads to enhanced thermal stability of siloxane.
[0026] The addition of the spacer to the vinyl functional group provided on the silica surface is carried out in a solvent. The solvent is preferably an aromatic hydrocarbon, such as an alkyl-substituted aromatic hydrocarbon such as toluene. The reaction is carried out under heating, for example at a temperature of 40°C to 90°C.
[0027] The addition reaction is promoted with the aid of a catalyst, preferably from a metal of Group VIII, in particular platinum. The catalyst is selected so that the reaction can be carried out smoothly at a temperature low enough to minimize side reactions. For example, when the spacer with a hydride silicon group is a methylhydrogenpolysiloxane, the reaction temperature should not exceed 60° C., for example about 50° C. Other addition reactions with the above-mentioned spacers are allowed to be carried out at higher temperatures (for example about 70-80° C.) at shorter reaction times (for example less than 10 hours).
[0028] Exemplary Pt catalysts include [(C2H5)2S]2PtCl2, which has proven to be very useful in the addition of hydride-containing spacers to vinyl-modified silicas. Pt2[(Me2SiCH=CH2)2O]3, designated as Karstedt's catalyst, or commercially available catalysts from Umicore: Umicore HS 425 or Umicore HS432, may also be used. Other transition metal-containing catalysts, such as those based on rhodium or ruthenium, for example [Cp*Ru(MeCN)3]PF6, may also be used.
[0029] The reaction mixture is maintained at the selected elevated temperature with stirring.After completion of the addition reaction, the particles (ie, silicon hydride-modified silica) are separated from the reaction mixture by filtration and optionally washed and dried.
[0030] Next, the silicon dioxide modified with silicon hydride is reacted with a UV absorbing compound. For example, organic compounds of the benzotriazole class are known to absorb UV light in the range of 300 nm to 400 nm and can be used in the present invention. Preferred benzotriazoles are those in which the nitrogen atom at position 2 of the benzotriazole fused system is bonded to a substituted benzene ring. The substituents on the phenyl moiety preferably include hydroxyl groups. Hydroxyphenyl-benzotriazole derivatives have shown effective UV protection in a wide variety of polymers. Therefore, more specifically, the preferred UV absorbing compound for use in the present invention is a 2-(2'-hydroxyphenyl)benzotriazole derivative:
[0031]
[0032] The benzene ring is further substituted by reactive functional groups.
[0033] Particularly preferred are 2-(2'-hydroxyphenyl)benzotriazole derivatives in which the 2'-hydroxyphenyl ring is substituted with a functional group that exhibits high reactivity with silicon hydride, such as a vinyl or allyl group. For example, 2-(3-allyl-2-hydroxy-5-methyl-phenyl)-2H-benzotriazole [also known as 2-(2H-benzotriazol-2-yl)-4-methyl-6-(2-propenyl)phenol] has the following structure:
[0034]
[0035] The silicon hydride group of the spacer is added to the carbon-carbon double bond of the allyl group so as to be chemically bonded to the silicon dioxide particles. Therefore, in the presence of a suitable catalyst (for example, Pt catalyst as mentioned above), the silicon dioxide particles and 2-(2'-hydroxyphenyl) benzotriazole ultraviolet light absorbing compounds of the silicon hydride surface modification are combined in an organic solvent. For example, the catalyst is added to the reaction vessel of the silicon dioxide and 2-(2'-hydroxyphenyl) benzotriazole derivatives pre-added in the aromatic hydrocarbons, and the reaction mixture is kept heated under agitation to complete the addition reaction. The product composed of the silicon dioxide particles chemically connected to the ultraviolet light absorbing compounds is separated by filtration, washed and dried. The filtrate is collected to reclaim the unreacted ultraviolet light absorbing compounds therefrom.
[0036] The "sequential surface modification variant" in its most preferred embodiment produces a light stabilizer suitable for use as an additive in a polymer. This light stabilizer forms a specific embodiment of the present invention; it includes silica particles having a UV light absorbing compound on the surface of the particles, wherein the carbon atom of the UV light absorbing compound is covalently bonded to the silicon atom of the organosilicon spacer, characterized in that in addition to the carbon atom, the nearest environment of the silicon atom also includes an oxygen atom and two hydrocarbon groups or includes two oxygen atoms and one hydrocarbon group. The hydrocarbon group includes, but is not limited to, an alkyl group (such as methyl or ethyl) and a phenyl group. More specifically, the UVA light absorbing compound is a 2-(2'-hydroxyphenyl)benzotriazole compound, which is connected by an alkylene chain (-CH2-) n (n=2-5, for example, n=3) covalently bonded to the silicon atom of the organosilicon spacer, the alkylene chain is connected to the benzene ring of the hydroxyphenyl-benzotriazole compound.
[0037] Preferably, the concentration of the ultraviolet light absorbing compound in the silica is not less than 0.07 mmol / g, such as not less than 0.15 mmol / g, more preferably not less than 0.2 mmol / g, such as 0.2 to 3.0 mmol / g, such as 0.3 to 0.7 mmol / g or 2.0 mmol / g to 2.5 mmol / g (measured by TGA as exemplified below). The additive may also contain some silicon hydride groups.
[0038] Now, we will discuss the 'one-step variant', which is based on the direct reaction of a UV-absorbing compound with unmodified silica particles or zinc oxide particles. Any UV-absorbing compound having a functional group capable of undergoing a bond-forming reaction with a surface -OH group can be used in the 'one-step variant', such as a UV-absorbing compound substituted with -Si(-O-alkyl)3, such as -Si(-O-C2H5)3. Two UV-absorbing compounds with -Si(-O-C2H5)3 functional groups are described below, one being a 2-hydroxybenzophenone and the other being a 2-(2'-hydroxyphenyl)benzotriazole:
[0039]
[0040] [The 2'-hydroxyphenyl)benzotriazole described above is described by Farkas et al. in Molecules (15), p. 6205-6216 (2010)]
[0041] Thus, an inorganic oxide such as silicon dioxide or zinc oxide is mixed with a UV absorbing compound in a suitable organic solvent (e.g. in an aromatic hydrocarbon such as toluene) with stirring and heating, preferably at the boiling point of the solvent under reflux. Upon completion, the reaction mixture is cooled and the product is separated from the liquid phase, washed and dried.
[0042] Alternatively, a 'one-step variant' is performed using commercially available colloidal silica as a starting material, wherein the reaction between the silica and the UV-absorbing compound is carried out in a solvent, wherein the colloidal silica is suspended in a commercially available product (typically at a concentration of 25-40 wt%). In this way, the UV-absorbing compound can be loaded onto the silica particles at not less than 0.10 mmol of UV-absorbing compound per gram of silica. For example, isopropanol has been shown to be a useful solvent for the reaction. A mixture of ethylene glycol and isopropanol is also feasible. Other solvents, such as alkanols and aromatic hydrocarbons such as toluene, may also be used. The molar ratio of the OH surface groups of the silica to the UV-absorbing compound (e.g., 2-hydroxy-4-(3-triethoxysilylpropoxy)-diphenyl ketone) is preferably 8:1 to 2:1, for example 3.5:1 to 2.5:1. The reaction is allowed to proceed under heating (e.g., under reflux) for about 24 hours.
[0043] The present invention also provides a method for improving the photostability of a polymer, which comprises adding to the polymer inorganic oxide particles having an ultraviolet light absorbing compound on their surface, such as silica and zinc oxide particles functionalized with the above-mentioned ultraviolet light absorbing compound.
[0044] Thermoplastic polymers containing UV stabilizer additives form another aspect of the present invention. The surface-modified inorganic particles of the present invention can be added to a wide range of polymers, including polypropylene (homopolymers and copolymers), polyethylene such as high-density polyethylene (HDPE), medium-density polyethylene (MDPE), low-density polyethylene (LDPE) and linear low-density polyethylene (LLDPE), polyethylene terephthalate (PET), and PDMS. The concentration of the additive of the present invention is not more than 15wt%, such as 1.0wt% to 12.0wt%, preferably 1.0wt% to 8.0wt%, based on the weight of the polymer formulation. The additive is introduced into the polymer by conventional methods to complete the compounding, for example, by using an extruder such as a twin-screw extruder. The formed pellets are then processed and formed into desired articles such as films using conventional film / sheet extrusion (e.g., blown extrusion and cast extrusion). Illustrative steps for preparing polypropylene and LLDPE films into which additives are introduced are as follows.
[0045] The polymers incorporating additives were tested to measure the migration of UV absorbing compounds to the surface by periodically washing and rinsing the membrane surface with clean hexane and measuring the UV transmittance of the wash solution to detect trace amounts of UV absorbing material and measuring the UV transmittance of the membrane (kept under different conditions as described below) to record any degradation in the UV absorbing properties of the membrane. The results reported below indicate that the UV absorbing compounds did not migrate out of the membrane even after extended storage periods.
[0046] The present invention comprises:
[0047] 1. An ultraviolet light absorber suitable for use as an additive in a polymer, comprising inorganic oxide particles having an ultraviolet light absorbing compound on the surface thereof, wherein the ultraviolet light absorbing compound is either chemically bonded to a spacer provided on the surface of the particle or chemically bonded directly to the surface of the particle.
[0048] 2. The ultraviolet light absorber according to item 1, wherein the inorganic oxide is selected from silicon dioxide and zinc oxide.
[0049] 3. The ultraviolet light absorber according to item 2, wherein the inorganic oxide is silicon dioxide and the spacer is an organic silicon spacer.
[0050] 4. An ultraviolet light absorber according to item 3, wherein the carbon atom of the ultraviolet light absorbing compound is covalently bonded to the silicon atom of the organic silicon spacer, characterized in that the nearest environment of the silicon atom consists of the carbon atom, one oxygen atom and two hydrocarbon groups or consists of the carbon atom, two oxygen atoms and one hydrocarbon group.
[0051] 5. The ultraviolet light absorber according to item 3 or 4, wherein the ultraviolet light absorbing compound is a hydroxyphenyl-benzotriazole compound, which is connected to the benzene ring of the hydroxyphenyl-benzotriazole compound through an alkylene chain (-CH2-) n Covalently bonded to the silicon atom of the organosilicon spacer.
[0052] 6. The ultraviolet light absorber according to item 5, wherein the hydroxyphenyl-benzotriazole compound is a 2-(2'-hydroxyphenyl)benzotriazole compound:
[0053]
[0054] wherein the benzene ring is substituted with a -CH2-CH2-CH2- chain and optionally with one or more further groups.
[0055] 7. The ultraviolet light absorber according to item 2, wherein the ultraviolet light absorbing compound is a 2-hydroxybenzophenone compound.
[0056] 8. The ultraviolet light absorber additive according to any one of the preceding items, wherein the concentration of the ultraviolet light absorbing compound in the additive is not less than 0.07 mmol / g.
[0057] 9. A method for improving the photostability of a polymer, comprising adding the inorganic oxide particles having an ultraviolet light absorbing compound on the surface thereof as described in any one of items 1 to 8 to the polymer.
[0058] 10. A thermoplastic polymer comprising the additive according to any one of items 1 to 8.
[0059] 11. A film comprising the thermoplastic polymer according to item 10.
[0060] 12. A method for preparing an ultraviolet light absorber additive for protecting a polymer from ultraviolet radiation, comprising introducing a first functional group onto the surface of an inorganic oxide particle, reacting the inorganic oxide particle thus formed modified by the first group with a spacer having a plurality of second functional groups; reacting the inorganic particle thus formed modified by the second functional group with an ultraviolet light absorbing compound, and separating the ultraviolet light absorber additive from the reaction mixture.
[0061] 13. A method according to item 12, wherein the inorganic oxide is silicon dioxide.
[0062] 14. A method according to claim 13, wherein the first functional group is a carbon-carbon double bond.
[0063] 15. A method according to item 14, wherein carbon-carbon double bonds are introduced onto the surface of the silica by reacting the silica particles with a vinyl compound of the formula: (H2C=CH) i Si(OC j H 2j+1 ) 4-i [1≤i≤3, 1≤j≤3].
[0064] 16. The method according to item 14, wherein silicon dioxide modified by a carbon-carbon double bond is reacted with an organic silicon compound having a silicon hydride (SiH) functional group, wherein the number of SH groups in the organic silicon compound is not less than 4.
[0065] 17. The method according to item 16, wherein the organosilicon compound comprises four to ten silicon hydride groups in which the nearest environment of the silicon atom is occupied by two hydrocarbon groups and one oxygen atom.
[0066] 18. The method according to item 17, wherein the organosilicon spacer comprises not less than twenty silicon hydride groups, the spacer having a main chain having the silicon hydride in a repeating unit.
[0067] 19. The method of item 18, wherein the spacer is a poly(methylhydrogensiloxane) consisting of 50-80 repeating units.
[0068] 20. The method according to any one of items 12 to 19, wherein the ultraviolet light absorbing compound belongs to the class of hydroxyphenyl-benzotriazoles.
[0069] 21. The method of item 20, wherein the ultraviolet light absorbing compound is 2-(3-allyl-2-hydroxy-5-methyl-phenyl)-2H-benzotriazole:
[0070] Example
[0071] method:
[0072] Thermogravimetric analysis (TGA) : TGA analysis was performed using a Mettler-Toledo instrument model TGA / SDTA851. 10 mg of sample was heated from room temperature to about 1000°C at a heating rate of 10°C / min in a standard 70 μL TGA alumina crucible in a nitrogen atmosphere. The concentration of UVA molecules on the silica surface was calculated according to the following equation:
[0073]
[0074] Wherein dc1 is the decomposition content (%) of silica-spacer at 150-1000°C, dc2 is the decomposition content of silica-spacer-UVA, and MW is the molecular weight of UVA (for example, 265.31 g / mol in the case of 2-(2H-benzotriazole-2-yl)-4-methyl-6-(2-propenyl)phenol).
[0075] Fourier transform infrared spectroscopy (FTIR ): The FTIR instrument used was Scientific, Nicolet iS10.
[0076] Nuclear Magnetic Resonance (NMR) Spectroscopy : NMR spectra were acquired on a Bruker Avance II instrument, 500 MHz, CP-MAS 4 mm.
[0077] X-ray Photoelectron Spectroscopy (XPS) : The X-ray photoelectron spectrometer used was from Kratos Analytical Ltd. (Kratos Axis Ultra).
[0078] Elemental analysis : The elemental analyzer used was a 2400 Series II analyzer from PerkinElmer.
[0079] The following set of examples (1-3) illustrate the covalent attachment of UV light absorbing compounds (benzotriazole family) on the surface of silica particles via small spacer molecules with four (or six) SiH functional groups, as shown by the synthetic route described below.
[0080]
[0081] Preparation 1
[0082] Preparation of Silica-Vinyl
[0083] Formulation 1A
[0084] 10 g of silica (Cab-O-sil M5, Cabot Corporation) and 40 g of vinyltrimethoxysilane (VTMS; from Sigma-Aldrich, catalog number 440221-97%) were mixed in a three-necked flask equipped with a reflux condenser and a CaCl2 trap. The mixture was heated to the boiling point of VTMS (bp 123°C) using an oil bath (150°C) and stirred at this temperature with a mechanical stirrer (225 rpm) for 11 hours. After cooling to room temperature, the silica was washed with hexane (3×250 ml) in a filter funnel (P4) with sintered glass and dried in an oven at 165°C in a petri dish for half an hour to obtain 9.56 g of silica-vinyl (1, Scheme 1).
[0085] Formulation 1B
[0086] Silica (Cab-O-sil M5, Cabot Corporation) was pressed under 0.5 tons of pressure to a volume reduction of about 1.5. Then 10 grams of silica and 40 grams of vinyl trimethoxysilane (from Sigma-Aldrich, catalog number 440221-97%) were mixed in a 250 ml three-necked flask equipped with a reflux condenser and a CaCl2 trap. The mixture was heated to the boiling point of VTMS (boiling point 123°C) using an oil bath (150°C) and stirred at this temperature with a mechanical stirrer (278 rpm) for 11 hours. After cooling to room temperature, the silica was washed with hexane (4×250 ml) on a filter funnel (P4) with sintered glass, dried in an oven at 165°C for half an hour, and silica-vinyl (1, Scheme 1) was collected.
[0087] Preparation 1C :
[0088] Silica (Cab-O-sil M5, Cabot Corporation) was pressed at 1 ton of pressure for 10 minutes. Then 100 grams of pressed silica and 400 grams of vinyl trimethoxysilane (from Sigma-Aldrich, catalog number 440221-97%) were mixed in a 1L cylindrical reactor equipped with a reflux condenser and a mechanical stirrer (half-moon, 90mm PTFE blade). The mixture was heated to the boiling point of VTMS (boiling point 123°C) using a heating jacket and stirred at this temperature under nitrogen for 19 hours with a mechanical stirrer (300rpm). After cooling to room temperature, about 400ml of hexane was added to the reaction mixture, and after mixing, the resulting suspension was filtered on a 1L filter funnel (P4) with sintered glass. The reactor was washed with another 40ml of hexane and the suspension was also filtered. The silica remaining on the filter was washed with additional hexane (3 x 800 ml), which was dried in an oven at 160°C for 3 hours using a chemical beaker (14 cm diameter and 7.5 cm height) to collect the silica-vinyl (1, Scheme 1).
[0089] Silica-vinyl (1, Scheme 1) was characterized by NMR, FTIR and XPS analysis.
[0090] NMR spectroscopy Figure 1As shown; the two peaks at 134ppm and 128ppm are attributed to the carbon atoms of the vinyl groups added to the silica surface. The peak at about 48ppm is attributed to the unreacted methoxy groups (due to steric considerations, an average of about two of the three -OCH3 groups in vinyltrimethylsilane participate in the bond formation reaction with the silica surface).
[0091] Figure 2 Shown are the FTIR spectra of original unmodified commercial silica (lower) and the FTIR spectrum of silica-vinyl (upper).
[0092] The characteristic peaks of unmodified silica are:
[0093] At about 3433cm - The large band at , which is attributed to the presence of OH stretching frequency of silanol groups and adsorbed water;
[0094] At 1631cm -1 The sharp band at is attributed to the bending vibration of molecular water;
[0095] At 1254-1026cm -1 The broad strong peak at about 980 cm-1 is attributed to the stretching vibration of the Si-O-Si asymmetric bond. -1 There are some "shoulders" at the center, which correspond to the asymmetric vibration of Si-OH.
[0096] At 806cm -1 The band at , which is attributed to the stretching vibration of the network Si-O-Si symmetric bond; and
[0097] At 460cm -1 The band at , which is related to the bending vibration of the network Si-O-Si bonds.
[0098] The spectrum of vinyl-modified silica is at 3060 cm -1 and 3020cm -1 A new weak peak appears at 1600 cm-1, which is attributed to the CH band of Si-CH=CH2 group. -1 The peak at 1410 cm is a typical C=C vibration. -1 The peak at 2986cm is attributed to the CH deformation vibration of the =CH2 group. -1 、2958cm -1 and 2987cm -1 The peak at is attributed to the CH band of the residual methoxy group (characteristic Si-OCH3 band, expected at about 1000-1100 cm -1 It is found in the presence of Si-O-Si, which is masked by strong Si-O-Si absorption).
[0099] Finally, it should be noted that in the modified silica, the -1 The broad band at about 980 cm -1 The disappearance of the “shoulder” at 4° clearly indicates that the surface silanol groups are involved in the chemical reaction, i.e., vinyltrimethoxysilane is covalently linked to the silica surface via the surface silanol groups.
[0100] The successful attachment of vinyltrimethoxysilane to the surface of the silica particles is also confirmed by the XPS analysis in the table below. Modification of the silica surface is expected to result in a decrease in the oxygen / carbon and silicon / carbon ratios measured on the silica surface. This is indeed shown by the results listed in Table 1 below:
[0101] Table 1
[0102]
[0103] Example 1
[0104] Preparation of silica-spacer A4-UVA
[0105] [UVA molecule is a 2-(2'-hydroxyphenyl)benzotriazole derivative]
[0106] Preparation of Silica-Spacer A4
[0107] Then 10.00 g of the silica-vinyl of preparation 1A (which was dried at 160° C. for 1 h), 4.70 g of tetrakis(dimethylsiloxy)silane (A4; from ABCR, catalog number AB111396-97%) and 54 g of toluene were mixed in a 500 ml single-necked flask with a mechanical stirrer, and then a Pt catalyst {cis-dichlorobis(diethylsulfide)platinum(II), from Sigma-Aldrich, catalog number 432849} was added. The catalyst was added in the form of a 2% toluene solution (425 μl).
[0108] The resulting suspension was stirred at 80°C with a mechanical stirrer (300 rpm) for 5 hours. After cooling to room temperature, the product was washed with toluene (2×500 ml) and hexane (3×500 ml) on a filter funnel with sintered glass (P4). The product was placed in a petri dish and dried in an oven at 70°C for 1 hour to obtain 9.95 g of silica-A4 (2, Scheme 1).
[0109] Preparation of silica-spacer A4-UVA
[0110] 9.45 g of silica-spacer A4, 5.33 g of 2-(2H-benzotriazol-2-yl)-4-methyl-6-(2-propenyl)phenol {UVA; from Sigma-Aldrich, catalog number 559857-99%} and 60 g of toluene were mixed in a 250 ml single-necked flask with a mechanical stirrer, and then a Pt catalyst {cis-dichlorobis(diethylsulfide)platinum(II), from Sigma-Aldrich, catalog number 432849} was added. The catalyst was added in the form of a 2% toluene solution (445 μl).
[0111] The resulting suspension was stirred at 80°C for 16 hours. After cooling to room temperature, the product was washed with toluene (3×400 ml) and hexane (4×500 ml) on a filter funnel with sintered glass (P4). The UV absorbance (250 nm-450 nm) of the last portion of hexane was measured to ensure that all UVA was washed off. The product was placed in a petri dish and dried in an oven at 70°C for 1 hour to obtain 9.29 grams of silica-spacer A4-UVA (3, Scheme 1).
[0112] The additive so formed was characterized by FTIR, TGA and elemental analysis. Figure 3 The FTIR spectrum shown in -1 A peak is shown at 2135 cm, which is attributed to the UVA molecules that have been successfully attached to the particles. -1 and 910cm -1 The peak at is due to the presence of unreacted SiH groups that have not formed chemical bonds with UVA molecules. According to the above method, the concentration of UVA molecules applied to the silica particles was calculated on the basis of TGA analysis and was found to be 0.26 mmol / g (measured dc1 and dc2 values of 4.87% and 11.40%, respectively). The concentration determined by TGA showed fairly good agreement with the results obtained by elemental analysis [measured %C: 9.62; calculated concentration: 0.28 mmol / g (C ea)]
[0113] Example 2
[0114] Preparation of silica-spacer A6-UVA
[0115] [UVA compound is a 2-(2'-hydroxyphenyl)benzotriazole derivative]
[0116] Preparation of Silica-Spacer A6
[0117] Then 1 gram of silica-vinyl of Formulation 1A, 1.32 grams of poly(dimethylsiloxane-co-methylhydrogensiloxane), end-capped trimethylsilyl {A6; from Sigma-Aldrich, catalog number 482196 - average Mn about 950} and 5.22 grams of toluene were mixed in a 40 ml vial, and then a Pt catalyst {cis-dichlorobis(diethylsulfide)platinum(II), from Sigma-Aldrich, catalog number 432849} was added. The catalyst was added as a 2% toluene solution (50 μl).
[0118] The resulting suspension was stirred at 80°C for 5 hours. After cooling to room temperature, the product was washed with toluene (3×50 ml) and hexane (4×50 ml) on a filter funnel with sintered glass (P4). The product was placed in a petri dish and dried in an oven at 70°C for 1 hour to obtain 0.982 g of silica-spacer A6.
[0119] Preparation of silica-spacer A6-UVA
[0120] 750.8 mg of silica-spacer A6, 424.8 mg of 2-(2H-benzotriazol-2-yl)-4-methyl-6-(2-propenyl)phenol {UVA; from Sigma-Aldrich, catalog number 559857-99%} and 4.78 grams of toluene were mixed in a 20 ml vial, and then a Pt catalyst {cis-dichlorobis(diethylsulfide)platinum(II), from Sigma-Aldrich, catalog number 432849} was added. The catalyst was added as a 2% toluene solution (36 μl).
[0121] The resulting suspension was stirred at 80°C for 8 hours. After cooling to room temperature, the product was washed with toluene (4×40 ml) and hexane (3×40 ml) on a filter funnel (P4) with sintered glass. The UV absorbance (250 nm-450 nm) of the last portion of hexane was measured to ensure that all UVA was washed off. The product was placed in a petri dish and dried in an oven at 70°C for 1 hour to obtain 0.625 g of silica-spacer A6-UVA.
[0122] The additive so formed was characterized by FTIR and TGA. Figure 4 The FTIR spectrum shown in -1 The characteristic peaks are shown at , indicating the presence of UVA molecules on the silica surface. According to the above method, the concentration of UVA molecules loaded on the silica particles was calculated based on TGA analysis and was found to be 0.31 mmol / g (the measured dc1 and dc2 values were 6.08% and 13.73%, respectively).
[0123] Example 3
[0124] Preparation of silica-spacer A6y–UVA
[0125] [UVA molecule 2-(2'-hydroxyphenyl)benzotriazole derivative]
[0126] Preparation of silica-spacer A6y
[0127] 1 gram of silica-vinyl of preparation 1A, 780 mg of A6y (prepared according to the procedure described in US 5,691,435) and 3.6 grams of toluene were mixed in a 40 ml vial, and then a Pt catalyst {cis-dichlorobis(diethylsulfide)platinum(II), from Sigma-Aldrich, catalog number 432849} was added. The catalyst was added as a 2% toluene solution (36 μl).
[0128] The resulting suspension was stirred at 80°C for 5 hours. After cooling to room temperature, the product was washed with toluene (4×40 ml) and hexane (4×40 ml) on a filter funnel (P4) with sintered glass. The product was placed in a petri dish and dried in an oven at 70°C for 1 hour to obtain 0.984 g of silica-spacer A6y.
[0129] Preparation of silica-spacer A6y-UVA
[0130] 627.8 mg of silica-spacer A6y, 354.8 mg of 2-(2H-benzotriazol-2-yl)-4-methyl-6-(2-propenyl)phenol {UVA; from Sigma-Aldrich, catalog number 559857-99%} and 2.26 grams of toluene were mixed in a 20 ml vial, and then a Pt catalyst {cis-dichlorobis(diethylsulfide)platinum(II) from Sigma-Aldrich, catalog number 432849} was added. The catalyst was added as a 2% toluene solution (28 μl).
[0131] The resulting suspension was stirred at 80°C for 8 hours. After cooling to room temperature, the product was washed with toluene (4×40 ml) and hexane (3×40 ml) on a filter funnel (P4) with sintered glass. The UV absorbance (250nm-450nm) of the last portion of hexane was measured to ensure that all UVA was washed off. The product was placed in a petri dish and dried in an oven at 70°C for 1 hour to obtain 0.518 grams of silica-spacer A6y-UVA.
[0132] The additive so formed was characterized by FTIR and TGA. Figure 5 The FTIR spectrum shown in -1The characteristic peaks are shown at , indicating the presence of UVA molecules on the silica surface. According to the above method, the concentration of UVA molecules present on the silica particles was calculated based on TGA analysis and found to be 0.51 mmol / g (the measured dc1 and dc2 values were 6.13% and 19.04%, respectively).
[0133] The following set of examples (4-8) illustrate the covalent bonding of UV light absorbing compounds (benzotriazole family) to the surface of silica particles via long spacers such as poly(methylhydrogensiloxane) consisting of approximately 75 repeating units (ie, Si-H functional groups).
[0134] Example 4
[0135] Preparation of silica-spacer MH30-UVA
[0136] [UVA compound is a 2-(2'-hydroxyphenyl)benzotriazole derivative]
[0137] Preparation of silica-spacer MH30
[0138] The silica-vinyl (1 g) of Formulation 1A was dried at 160° C. for 1 h. The silica-vinyl, 3.29 g Andisil MH30 (from AB Specialty Silicones) and 2.6 g toluene were mixed in a 20 ml flask with a magnetic stirrer, and then the Pt catalyst {cis-dichlorobis(diethylsulfide)platinum(II), from Sigma-Aldrich, catalog number 432849} was added. The catalyst was added as a 2% toluene solution (45 μl).
[0139] The resulting suspension was stirred at 50°C with a magnetic stirrer for 8 hours. After cooling to room temperature, the product was washed with toluene (50 ml) and hexane (4×50 mL) on a filter funnel (P4) with sintered glass. The product was placed in a petri dish and dried in an oven at 45°C for 1 hour to obtain 1.2 grams of silica-MH30.
[0140] Preparation of silica-spacer MH30-UVA
[0141] 0.5 g of silica-spacer MH30, 1.5 g of 2-(2H-benzotriazol-2-yl)-4-methyl-6-(2-propenyl)phenol (Sigma-Aldrich, catalog number 559857-99%) and 3 g of toluene were mixed in a 20 ml flask with a magnetic stirrer, and then Pt-catalyst {cis-dichlorobis(diethylsulfide)platinum(II), from Sigma-Aldrich, catalog number 432849} was added. The catalyst was added in the form of a 2% toluene solution (80 μl).
[0142] The resulting suspension was stirred at 80°C for 8 hours. After cooling to room temperature, the product was washed with toluene (3×100 ml) and hexane (3×100 ml) on a filter funnel (P4) with sintered glass. The UV absorbance (250nm-450nm) of the last portion of hexane was measured to ensure that all UVA was washed off. The product was placed in a petri dish and dried in an oven at 70°C for 1 hour to obtain 0.45 grams of silica-spacer MH30-UVA.
[0143] The additive thus formed was characterized by FTIR and TGA. The FTIR spectrum was as follows Figure 6 As shown; note that at 745cm -1 、1217cm -1 and 1264cm -1 There is a strong characteristic peak at , which is attributed to UVA molecules. According to the above method, the concentration of UVA molecules present on the silica particles was calculated based on TGA analysis and found to be 2.35 mmol / g (the measured dc1 and dc2 values were 5.19% and 41.63%, respectively).
[0144] Example 5
[0145] Preparation of silica-spacer MH30-UVA
[0146] [UVA molecule is a 2-(2'-hydroxyphenyl)benzotriazole derivative]
[0147] Preparation of silica-spacer MH30
[0148] 50 g of silica-vinyl of Formulation 1C (dried at 160° C. for 1 h), 106.4 g of Andisil MH30 and 124.7 g of toluene were mixed in a 1 L cylindrical reactor equipped with a mechanical stirrer (half-moon shape, 90 mm PTFE blades) and then a Pt catalyst {cis-dichlorobis(diethylsulfide)platinum(II), from Sigma-Aldrich, catalog number 432849} was added. The catalyst was added as a 2% toluene solution (1.9 ml).
[0149] The obtained suspension was stirred for 16 hours at 50 ° C with a mechanical stirrer (340rpm). After cooling to room temperature, 300ml of toluene was added to vigorously mix the reaction mixture. The suspension was then allowed to stand for half an hour, and after sedimentation, the solid was separated by decanting the solvent. The product was washed twice with hexane (240ml, centrifugal-decantation, 3000rpm, 10 minutes each time). After the final decantation, the solid was introduced into a 1L filter funnel (P4) with sintered glass and washed with hexane (4×500ml). The last part of hexane was evaporated and the residue was weighed to ensure that all unreacted polymers were washed away. The product was placed in a petri dish and dried in an oven at 50 ° C for 1 hour to obtain 45 grams of silica-MH30.
[0150] Preparation of silica-spacer MH30-UVA
[0151] 43.3 g of silica-spacer MH30, 129 g of 2-(2H-benzotriazol-2-yl)-4-methyl-6-(2-propenyl)phenol (composed of equal amounts of material purchased from Sigma-Aldrich, catalog number 559857-99% and recycled material recovered from a previous batch as described below) and 258 g of toluene were mixed in a 1 L cylindrical reactor equipped with a mechanical stirrer (half-moon, 90 mm PTFE blade) and then Pt-catalyst {cis-dichlorobis(diethylsulfide)platinum(II), from Sigma-Aldrich, catalog number 432849} was added. The catalyst was added as a 2% toluene solution (7 ml).
[0152] The resulting suspension was stirred at 80°C with a mechanical stirrer (340 rpm) for 16 hours. After cooling to room temperature, the product was washed with toluene (5×800 ml) and hexane (3×800 ml) on a 1 L filter funnel (P4) with sintered glass. The UV absorbance (250 nm-450 nm) of the last portion of hexane was measured to ensure that all UVA was washed off. The filtrates were combined, evaporated and concentrated, and the unreacted 2-(2H-benzotriazol-2-yl)-4-methyl-6-(2-propenyl)phenol was collected and reused. The product was placed in a Petri dish and dried in an oven at 70°C for 1.5 hours to obtain 55 grams of silica-spacer MH30-UVA.
[0153] Example 6
[0154] Preparation of silica-spacer MH30-UVA
[0155] [UVA molecule is a 2-(2'-hydroxyphenyl)benzotriazole derivative]
[0156] Preparation of silica-spacer MH30
[0157] 14.39 g of silica-vinyl of Preparation 1C (dried at 160° C. for 1 h), 31.58 g of Andisil MH30 and 36.75 g of toluene were mixed in a 500 ml three-necked flask equipped with a mechanical stirrer, and then a Pt catalyst {cis-dichlorobis(diethylsulfide)platinum(II), from Sigma-Aldrich, catalog number 432849; the catalyst was added as a 2% toluene solution (0.55 ml)} was added.
[0158] The resulting suspension was stirred at 50°C with a mechanical stirrer (340 rpm) for 16 hours. After cooling to room temperature, 90 ml of toluene was added and the reaction mixture was thoroughly mixed. The suspension was then allowed to stand for half an hour, and after settling, the solid was separated by decanting the solvent. The silica was washed four times with hexane (4×250 ml, centrifugation-decantation, 3000 rpm, 10 minutes each). The last portion of hexane was evaporated and the residue was weighed to ensure that all unreacted Andisil MH30 was washed away. The product was placed in a Petri dish and dried in an oven at 50°C to obtain 14.82 grams of silica-spacer MH30.
[0159] Preparation of silica-spacer MH30-UVA
[0160] 0.787 g of silica-spacer MH30, 0.787 g of 2-(2H-benzotriazol-2-yl)-4-methyl-6-(2-propenyl)phenol (Sigma-Aldrich, catalog number 559857-99%) and 4.92 g of toluene were mixed in a 20 ml flask with a mechanical stirrer, and then a Pt catalyst {cis-dichlorobis(diethylsulfide)platinum(II), from Sigma-Aldrich, catalog number 432849; the catalyst was added in the form of a 2% toluene solution (105 μl)}.
[0161] The resulting suspension was stirred at 80°C for 16 hours. After cooling to room temperature, the product was washed with toluene (2×50 ml), hexane (3×50 ml) on a filter funnel with sintered glass (P4). The UV absorbance (250 nm-450 nm) of the last portion of hexane was measured to ensure that all unreacted benzotriazole was washed out. The product was placed in a petri dish and dried in an oven at 70°C for 1 hour.
[0162] Example 7
[0163] Study of the properties of poly(methylhydrogensiloxane) as a spacer for attaching UV-absorbing compounds to the surface of silica particles
[0164] In the set of measurements reported in this example, poly(methylhydrogensiloxane) (MH30, available from Andisil) was used as a spacer. 2-(3-allyl-2-hydroxy-5-methylphenyl)-2H-benzotriazole was used as the UV absorbing compound.
[0165] Optical properties : Figure 7 Shows the transmission spectra of 2-(3-allyl-2-hydroxy-5-methylphenyl)-2H-benzotriazole and the product of the reaction between MH30 and 2-(3-allyl-2-hydroxy-5-methylphenyl)-2H-benzotriazole in the UV-visible range:
[0166]
[0167] The addition reaction was carried out in toluene at 50° C. under the same conditions as detailed in the previous examples to give poly(methylhydrogensiloxane) with pendant 2-(3-propyl-2-hydroxy-5-methylphenyl)-2H-benzotriazole. To obtain the spectra, 50 ppm of 2-(3-allyl-2-hydroxy-5-methylphenyl)-2H-benzotriazole in toluene was used, and similarly 50 ppm of the reaction product in toluene was used. Figure 7 The spectra shown show that the absorbance of 2-(3-allyl-2-hydroxy-5-methylphenyl)-2H-benzotriazole and its reaction product with MH30 is comparable (at Figure 7 The spectra of represent TinB and MH30-TinB or MH30-TinB, respectively).
[0168] Thermal properties Thermal stability was studied using TGA analysis (which measures the weight loss of a sample as its temperature increases). The following samples were subjected to TGA analysis and the results are shown in Figure 8 In the thermal spectrum:
[0169] Poly(methylhydrogensiloxane) (in Figure 8 is referred to as “MH30” in the thermogram of
[0170] The reaction product of poly(methylhydrogensilane) and 2-(3-allyl-2-hydroxy-5-methylphenyl)-2H-benzotriazole, as described above (in Figure 8 is referred to as “MH30-UVA” in the thermogram of
[0171] The reaction product of silica particles and MH30, as described in the previous example (in Figure 8 “Sil-MH30” in the thermogram of
[0172] The additive of the present invention, prepared as described in the previous examples, consists of silica particles having MH30 spacers attached to the silica surface and 2-(3-allyl-2-hydroxy-5-methylphenyl)-2H-benzotriazole chemically bonded to the spacers (in Figure 8 is referred to as “Sil-MH30-UVA” in the thermogram).
[0173] TGA shows that the decomposition of poly(methylhydrogensiloxane) (i.e., MH30) begins at a temperature of about 250°C. The thermal stability of MH30 decreases when MH30 is attached to the surface of silica particles because the decomposition of the "Sil-MH30" conjugate begins at 150°C. Therefore, coupling to silica particles has an adverse effect on the thermal stability of MH30. However, the chemical bonding of 2-(3-allyl-2-hydroxy-5-methylphenyl)-2H-benzotriazole to the MH30 chain has a favorable effect on thermal stability, with the reaction product MH30-UVA showing increased thermal stability because decomposition occurs at a higher temperature of about 450°C. Most importantly, in the additive Sil-MH30-UVA of the present invention, the favorable effect of 2-(3-allyl-2-hydroxy-5-methylphenyl)-2H-benzotriazole on the thermal stability of MH30 exceeds the adverse effect of coupling to silica particles.
[0174] Example 8
[0175] Preparation of silica-UVA
[0176] [UVA is a 2-hydroxybenzophenone derivative]
[0177] 1.00 g of silica (Cab-O-sil M5, Cabot Corporation), 0.96 g of 2-hydroxy-4-(3-triethoxysilylpropoxy)-benzophenone (95%, from Gelest) and 17.40 g of toluene were mixed in a 50 ml flask equipped with a reflux condenser and a CaCl2 trap using a magnetic stirrer. The mixture was heated to the boiling point of toluene (bp 111°C) using an oil bath (120°C) and stirred at this temperature with a magnetic stirrer for 5 hours.
[0178] After cooling to room temperature, the product was washed with toluene (3×250 ml) and hexane (2×250 ml) on a filter funnel with sintered glass (P4). The UV absorbance (250 nm-450 nm) of the last portion of hexane was measured to ensure that all hydroxy-4-(3-triethoxysilylpropoxy)-diphenyl ketone was washed off. The product was placed in a petri dish and dried in an oven at 70° C. for 1 hour to obtain 1.08 g of silica-UVA.
[0179] The additive thus formed was characterized by FTIR and TGA. The FTIR spectrum was as follows Fig. 9 As shown; at 1626.7cm -1 The peak at corresponds to the intense band of the carbonyl group in the UVA molecule. The concentration of UVA molecules present on the silica particles calculated based on TGA analysis was 0.315 mmol / g.
[0180] Example 9
[0181] Preparation of silica-UVA
[0182] [UVA is a 2-hydroxybenzophenone derivative]
[0183] In the experiments reported in this example, colloidal silica ( From Evonik Industries AG). The silica starting material consisted of a suspension of a monodisperse silica particle population in isopropanol (30 wt%-40 wt%). The concentration of silanol groups on the surface of the silica starting material was measured by TGA and found to be 1.81 mmol / g (TGA after solvent evaporation in the temperature range from room temperature to 1100°C).
[0184] The reaction of silica particles with the UV-absorbing compound 2-hydroxy-4-(3-triethoxysilylpropoxy)-diphenyl ketone takes place in isopropanol at reflux temperature (82°C). The molar ratio of the OH surface groups of silica to 2-hydroxy-4-(3-triethoxysilylpropoxy)-diphenyl ketone is 3:1, allowing the reaction to proceed for 24 hours at reflux. Under the chosen conditions of reactant ratios and reaction time, the suspension retains its transparency through the reaction, indicating that no aggregation is experienced. The particles are examined by cryo-transmission electron microscopy (Cryo-Tem) analysis (5% concentration in isopropanol), Fig.10 The cryo-TEM images in Figure 2 show the dispersibility of the discrete particles. The concentration of the UV absorbing compound was measured (TGA) to be 0.15 mmol / g.
[0185] Example 10
[0186] Preparation of ZnO-UVA
[0187] [UVA is a 2-hydroxybenzophenone derivative]
[0188] 36.03 g ZnO ( 20, from Umicore Zinc Chemicals), 53.60 grams of 2-hydroxy-4-(3-triethoxysilylpropoxy)-diphenyl ketone and 144.13 grams of toluene were stirred with a mechanical stirrer in a 250 ml flask equipped with a reflux condenser and a CaCl2 trap. The mixture was heated to the boiling point of toluene (boiling point 111°C) using an oil bath (120°C) and stirred at this temperature (250rpm) for 65 hours. After cooling to room temperature, the ZnO particles were washed with toluene and hexane on a filter funnel with sintered glass. The UV absorbance (250nm-450nm) of the last portion of hexane was measured to ensure that all UVA was washed off. The ZnO was dried in a Petri dish at 70°C in an oven for 1 hour to obtain 35.4 grams of ZnO-UVA.
[0189] The additive so formed was characterized by FTIR, TGA and XPS analysis.
[0190] FTIR spectrum Fig.11 As shown (the lower spectrum corresponds to ZnO, and the upper curve corresponds to UVA-modified ZnO). It can be seen that the spectrum of UVA-modified ZnO has a peak at 2967 cm -1 and 2920cm -1 A new weak peak is shown at 1628.5 cm -1 The strong peak at 1118-1023cm is attributed to the carbonyl group in the UVA molecule. The fingerprint region also shows a new characteristic peak of the UVA molecule. -1 The broad peaks are attributed to Si-O-Si and Si-OC bands; the Si-O-Zn absorption band is located at 916 cm -1 Place.
[0191] TGA analysis showed that the calculated concentration of UVA molecules on the particle surface was 0.09 mmol / g.
[0192] XPS was used to analyze the composition of the original ZnO particles and the surface-modified ZnO particles to determine the atomic percentage of elements on the particle surface. The data are listed in Table 2 and Table 3, respectively:
[0193] Table 2 (original ZnO)
[0194] name Peak BE FWHM Area (P) CPS.eV atom% Q C1s 284.75 1.20 2971.98 9.34 1 O1s 529.80 1.12 40861.81 46.81 1 Zn2p3 1020.94 1.50 193072.40 43.85 1
[0195] Table 3 (ZnO-UVA)
[0196] name Peak BE FWHM Area (P) CPS.eV atom% Q C1s 284.92 1.78 2666.74 25.81 1 O1s 530.93 2.20 13462.47 45.78 1 Zn2p3 1023.48 2.34 39986.96 24.65 1 Si2P 101.98 1.41 321.54 3.76 1
[0197] The UVA molecule 2-hydroxy-4-(3-triethoxysilylpropoxy)-diphenyl ketone is linked to the ZnO particles via the reaction shown below:
[0198]
[0199] This is indicated by a new peak located at about 102 eV, which is attributed to the binding energy (BE) of silicon (note that the UVA molecule contains Si atoms). The atomic ratio between oxygen and zinc measured in the original ZnO particles is about 1:1; this ratio increases to about 2:1 in the reaction product due to masking by the oxygen atoms of the UVA molecules and the surface zinc. The carbon content in the reaction product is higher than that measured for commercial ZnO particles. Finally, deconvolution of the XPS spectrum for the Zn2p line shows that there are three different binding energies of zinc in the reaction product (about 1022.1 eV, about 1023.3 eV, and about 1024.3 eV), as listed in Table 4. On the other hand, the spectrum of the original ZnO particles contains only one binding energy band (corresponding to a single chemical state of Zn).
[0200] Table 4
[0201] name Peak BE FWHM Area (P) CPS.eV atom% Q Zn2p Scan B 1022.06 1.88 6524.62 16.31 1 Zn2p Scan C 1023.29 1.54 14095.63 35.27 1 Zn2p Scan A 1024.26 1.69 19336.71 48.41 1
[0202] Embodiment 11
[0203] Polypropylene film preparation
[0204] This example illustrates the preparation of a polypropylene film using the additive of the present invention. The composition of the film consists of 95% polypropylene and 5% additive (by weight).
[0205] Polypropylene homopolymer (Repol H034SG from 'Reliance Polymers') and the additive of the invention prepared in Example 1 were compounded by melt mixing in a EUROLAB Digital 16 ('Prism') twin screw co-rotating extruder (D=16 mm, L / D=24) using a uniform temperature profile of 200-225°C and operating at a screw speed of 250 rpm to obtain a batch size of 100 g of compound. The materials were mixed in a plastic bag and added to the extruder at the same upstream feed port. The molten compound strands were continuously cooled under water at room temperature to solidify and then cut into pellets using a pelletizer. The pre-compounded pellets were dried (70°C, overnight, vacuum) before further processing.
[0206] The pellets were then fed to a MICROTRUDER ('Rand Castle') cast film single screw extruder (D=13 mm, L / D=20) using a temperature profile of 200-220° C. The machine was operated at a screw speed of 70 rpm to give films of 50 micron wall thickness and 150 mm width.
[0207] The polymers incorporating additives were tested to measure migration of UV absorbing compounds to the surface by periodically washing and rinsing the membrane surface with clean hexane and measuring the UV transmittance of the wash solution to detect trace amounts of UV absorbing material and measuring the UV transmittance of the membrane to record any degradation of the UV absorbing properties of the membrane.
[0208] Recorded immediately after film preparation and approximately two years after film preparation Fig.12 It should be noted that after the first measurement in hexane, the membranes were stored in glass vials under the following conditions (see Fig.12 Reference numerals film "1", film "2" and film "3") in FIG:
[0209] Film #1, in air @30℃
[0210] Membrane #2, in 95% ethanol @ 30°C
[0211] Film #3, in air @60℃
[0212] The results show that in all cases the UV blocking level does not decrease over time, indicating that the surface migration of UV light absorbing compounds is effectively inhibited by the additives of the present invention.
[0213] Example 12
[0214] LLDPE film preparation
[0215] This example illustrates the preparation of an oriented 15 μm thick multilayer film (three layers) by incorporating the additive of the invention into a 7 μm thick core layer. The composition of the film consists of 93% LLDPE and 7% additive (by weight).
[0216] LLDPE(NOVA Chemicals FP112-A) and the additive of the invention prepared in Example 4 were compounded as follows: they were melt mixed in a 16 mm twin screw extruder (Prism, England) with a screw L / D ratio of 25:1, using a temperature profile of 160-225°C and operating at a screw speed of 200-230 rpm to obtain a batch size of 1500 grams of compound. The materials were mixed and fed to the extruder through the same upstream feed port. The molten compound strands were continuously cooled under water at room temperature to solidify and then cut into pellets using a pelletizer. The pre-compounded pellets were dried before further processing.
[0217] The pre-compounded material samples were fed into a MICROTRUDER ('RandCastle') cast film single screw extruder (D = 13 mm, L / D = 20) to prepare a three-layer cast film. For extruder A, the process was carried out at a temperature profile of 200-220 ° C, and for extruder C, the process was carried out at a temperature profile of 200-230 ° C. For extruder A, the machine was operated at a screw speed of 64 rpm, and for extruder C, the machine was operated at a screw speed of 115 rpm, resulting in a three-layer film with a total thickness of 400 μm and a width of 150 mm. The 400 μm film was then stretched to the final size.
[0218] UV spectra were recorded a few days after the films were prepared and then again about thirteen months later (film "1", film "2" and film "3" have the same meanings as above). Fig.13 The UV spectra shown indicate that no migration of additives to the film surface occurred over this approximately one year period, indicating that the UV blocking exhibited by the film immediately after film preparation was substantially equivalent to the UV blocking exhibited by the film one year after film preparation.
Claims
1. A UV absorber suitable for use as an additive in a polymer, comprising inorganic oxide particles having a UV absorbing compound on their surface, wherein the UV absorbing compound is chemically bonded to a spacer provided on the surface of the particles, wherein the inorganic oxide is silicon dioxide, wherein the silicon dioxide particles have silanol groups SiOH on their surface; wherein vinyltrimethoxysilane is covalently attached to the silica surface via silanol groups; wherein the spacer is chemically linked to the vinyltrimethoxysilane; The spacer is an organosilicon spacer, wherein the organosilicon spacer comprises a plurality of silicon hydride groups selected from: 4≤n≤80 and trimethylsilyl-terminated poly(dimethylsiloxane-co-methylhydrogensiloxane), and The ultraviolet light absorbing compound is hydroxyphenyl-benzotriazole, and the hydroxyphenyl-benzotriazole is connected to the benzene ring of the hydroxyphenyl-benzotriazole compound through an alkylene chain (-CH2-) n Covalently bonded to the silicon atom of the organosilicon spacer, wherein n=3.
2. The ultraviolet light absorber according to claim 1, wherein the organosilicon spacer is 4≤n≤10.
3. The ultraviolet light absorber according to claim 1, wherein the organosilicon spacer is selected from MH30 and trimethylsilyl terminated poly(dimethylsiloxane-co-methylhydrogensiloxane).
4. The ultraviolet light absorber according to claim 1, wherein the hydroxyphenyl-benzotriazole compound is a 2-(2'-hydroxyphenyl)benzotriazole derivative.
5. The ultraviolet light absorber according to claim 4, wherein the organosilicon spacer is And wherein the ultraviolet light absorber comprises the structure:
6. The ultraviolet light absorber according to claim 4, wherein the organosilicon spacer is trimethylsilyl-terminated poly(dimethylsiloxane-co-methylhydrogensiloxane).
7. The ultraviolet light absorber according to claim 4, wherein the organosilicon spacer is 8. The ultraviolet light absorber according to claim 4, wherein the organosilicon spacer is MH30.
9. The ultraviolet light absorber according to claim 1, wherein the organosilicon spacer is a poly(methylhydrogensiloxane) composed of 50 to 80 silicon hydride groups and terminated with trimethylsiloxy groups.
10. The ultraviolet light absorber according to any one of the preceding claims, wherein the concentration of the ultraviolet light absorbing compound in the silicon dioxide is not less than 0.2 mmol / g. 11 . The ultraviolet light absorber according to claim 10 , wherein the concentration of the ultraviolet light absorbing compound in the silicon dioxide is 0.3 to 0.7 mmol / g. 12 . The ultraviolet light absorber according to claim 10 , wherein the concentration of the ultraviolet light absorbing compound in the silicon dioxide is 2.0 mmol / g to 2.5 mmol / g.
13. A method for improving the light stability of a polymer, comprising adding the ultraviolet light absorber according to any one of claims 1 to 12 to the polymer.
14. A thermoplastic polymer comprising the ultraviolet light absorber according to any one of claims 1 to 12.
15. The thermoplastic polymer according to claim 14, wherein the thermoplastic polymer is selected from the group consisting of polypropylene homopolymer, polypropylene copolymer, polyethylene and polyethylene terephthalate.
16. The thermoplastic polymer of claim 14, wherein the thermoplastic polymer is a polypropylene homopolymer or a polyethylene, wherein the polyethylene is a linear low density polyethylene (LLDPE).
17. A film comprising the thermoplastic polymer of any one of claims 14 to 16.