A method for preparing a high manganese steel spectral standard sample
The production of high manganese steel spectral standards through vacuum smelting and forging processes solves the problems of high price and easy error in the existing technology, achieves cost reduction, improves composition uniformity and analysis accuracy, and forms an efficient spectral standard.
Patent Information
- Application Number
- CN202210278115.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-03-21
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2042-03-21
AI Technical Summary
Existing high manganese steel spectral samples are expensive, have low yields, and can easily lead to uneven composition and non-dense structure, leading to analysis errors.
High manganese steel spectrum standards are produced using vacuum smelting and forging processes, including material preparation, smelting, heat treatment, forging, sawing and grinding. The forging process eliminates casting defects, improves composition uniformity and accuracy, and ensures it through multi-point spectral analysis. Ingredient Accuracy.
It reduces procurement and testing costs, improves yield and component uniformity, enhances the accuracy and reliability of analysis, and forms an efficient component detection tool.
Smart Images

Figure CN114689402B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of standard sample preparation, and specifically relates to a method for preparing a high manganese steel spectrum standard sample. Background Art
[0002] Most of the high manganese steel spectral samples currently sold on the market are directly cast after smelting in a vacuum smelting furnace or an electric furnace. They are relatively expensive and have a low yield. In addition, during use, they may have uneven composition or loose structure (internal gas, debris, etc.), which can easily lead to analytical errors. Summary of the invention
[0003] The purpose of the present invention is to overcome the shortcomings of the prior art, solve the technical problems of high manganese steel spectral standard sample high price, low product rate and easy analysis error, and provide a method for preparing high manganese steel spectral standard sample.
[0004] The technical solution adopted by the present invention to solve the technical problems existing in the background technology is:
[0005] A method for preparing a high manganese steel spectral standard sample comprises the following steps:
[0006] S1. Material preparation and smelting: prepare materials according to the medium limit of high manganese steel composition, use vacuum smelting test furnace for smelting, cast and mold to obtain rods with a diameter of 100mm, and the casting temperature is 1420-1430℃;
[0007] S2, heat treatment: heat the bar obtained in step S1 to 1080±10°C, keep it at this temperature for 2h, and then perform quenching treatment;
[0008] S3, Forging:
[0009] S3-1, removing the casting defect areas at both ends of the bar after the heat treatment in step S2;
[0010] S3-2, preheating before forging: heat the bar obtained in step S3-1 to 1200±10°C and keep it warm for 3h;
[0011] S3-3, roughening: roughening the bar material after preheating before forging in step S3-2, with roughening process parameters as follows: height-to-diameter ratio of 2, pressing amount during roughening not more than 50 mm, and roughening to a diameter of 150 mm;
[0012] S3-4, drawing: the bar material after being upset in step S3-3 is re-drawn to a diameter of 100 mm, and the drawing process parameters are: the feed amount is not more than 20 mm, and the pressing amount is not more than 10 mm;
[0013] S3-5, secondary roughening: the bar material stretched in step S3-4 is subjected to secondary roughening to a diameter of 150 mm, and the roughening process parameters are the same as those in step S3-3;
[0014] S3-6, secondary drawing: the bar material after secondary roughening in step S3-5 is secondary drawn to a diameter of 80 mm, and the drawing process parameters are the same as those in step S3-4;
[0015] S3-7, post-forging treatment: cooling the bar obtained after the secondary drawing in step S3-6 to room temperature in the furnace;
[0016] S4, sawing and grinding: sawing the bar material forged in step S3 into small sections of bar material with a length of 80 mm, grinding and polishing both end surfaces of the small sections of bar material to obtain a high manganese steel spectrum standard sample.
[0017] Furthermore, in step S2, the quenching medium of the quenching treatment is water, and the water temperature is 20-25°C.
[0018] Furthermore, in the step S3-2, the heating rate in the preheating stage before forging is the maximum heating rate of the chamber furnace.
[0019] Furthermore, the prepared high manganese steel spectrum standard sample was subjected to component detection and data analysis:
[0020] Composition detection: Each polished section of the bar is subjected to chemical analysis and spectral analysis, and at least two spectrometers are used for the spectral analysis process, and each end face is tested at 6 points using a spectrometer;
[0021] Data analysis: All components detected by the spectrometer are compared with the component data obtained by chemical analysis. A small section of bar material with a composition deviation that meets the standard requirements is selected. Then the average of all components detected by the spectrometer and the components obtained by chemical analysis is used as the composition of the high manganese steel spectral standard.
[0022] Compared with the prior art, the present invention has the following beneficial effects:
[0023] 1. The high manganese steel spectral standard prepared by the present invention has a greatly reduced procurement cost, reduced detection and analysis costs, has wide applicability, is easy to prepare, and is highly economical.
[0024] 2. The process flow adds a forging step, which reduces the deviation of the standard sample composition, improves its yield rate, and has high accuracy.
[0025] 3. Optimize the smelting method and change it to vacuum method to improve the uniformity of standard sample composition and high reliability.
[0026] In conclusion, the high manganese steel spectral standard sample prepared by the present invention can efficiently complete the component detection work. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1It is a conventional high manganese steel spectral standard sample in the prior art; since no standard sample has gone through the forging process, shrinkage occurs inside the standard sample;
[0028] Figure 2 This is the metallographic diagram of the conventional high manganese steel spectral standard sample in the prior art; since no standard sample has undergone a forging process, the grain size grade is level 1;
[0029] Figure 3 It is a schematic diagram of the process of the present invention;
[0030] Figure 4 It is the high manganese steel spectrum standard sample in the present invention; because it has gone through the forging process, the standard sample has no casting defects;
[0031] Figure 5 This is the metallographic diagram of the spectrum standard sample of the high manganese steel in the present invention; due to the forging process, the grain size grade is level 5. DETAILED DESCRIPTION
[0032] The present invention is further described in detail below in conjunction with the accompanying drawings and embodiments.
[0033] A method for preparing a high manganese steel spectral standard sample comprises the following steps:
[0034] S1. Material preparation and smelting: Material preparation is performed according to the medium limit of high manganese steel composition. The high manganese steel used in this specific implementation is ZGMn13Mo, and its chemical composition is shown in Table 1 below:
[0035]
[0036] A vacuum smelting test furnace (50 kg) was used for smelting and casting to obtain a rod with a diameter of 100 mm. The casting temperature was 1420°C.
[0037] S2, heat treatment: heat the bar obtained in step S1 to 1080°C, keep it at that temperature for 2 hours, and then perform quenching treatment, the quenching medium is water, and the water temperature is 20°C;
[0038] S3, Forging:
[0039] S3-1, removing the casting defect areas at both ends of the bar after the heat treatment in step S2;
[0040] S3-2, preheating before forging: heat the bar obtained in step S3-1 to 1200°C, the heating rate is the maximum heating rate of the chamber furnace, and keep warm for 3 hours;
[0041] S3-3, roughening: roughening the bar material after preheating before forging in step S3-2, with roughening process parameters as follows: height-to-diameter ratio of 2 (i.e., bar material height not exceeding 200 mm), pressing amount during roughening not exceeding 50 mm, and roughening to a diameter of 150 mm;
[0042] S3-4, drawing: the bar material after being upset in step S3-3 is re-drawn to a diameter of 100 mm, and the drawing process parameters are: the feed amount is not more than 20 mm, and the pressing amount is not more than 10 mm, so as to ensure that the casting defects (such as shrinkage) of the internal structure of the bar material are eliminated;
[0043] S3-5, secondary roughening: the bar material stretched in step S3-4 is subjected to secondary roughening to a diameter of 150 mm, and the roughening process parameters are the same as those in step S3-3;
[0044] S3-6, secondary drawing: the bar material after secondary roughening in step S3-5 is secondary drawn to a diameter of 80 mm, and the drawing process parameters are the same as those in step S3-4;
[0045] S3-7, post-forging treatment: cooling the bar obtained after the secondary drawing in step S3-6 to room temperature in the furnace;
[0046] S4, sawing and grinding: sawing the bar material forged in step S3 into small sections of bar material with a length of 80 mm, grinding and polishing both end surfaces of the small sections of bar material to obtain a high manganese steel spectrum standard sample.
[0047] Furthermore, the prepared high manganese steel spectrum standard sample was subjected to component detection and data analysis:
[0048] Composition detection: Each polished section of the bar is subjected to chemical analysis and spectral analysis, and at least two spectrometers are used for the spectral analysis process, and each end face is tested at 6 points using a spectrometer;
[0049] Data analysis: All components detected by the spectrometer are compared with the component data obtained by chemical analysis. A small section of bar material with a composition deviation that meets the standard requirements is selected. Then the average of all components detected by the spectrometer and the components obtained by chemical analysis is used as the composition of the high manganese steel spectral standard.
[0050] The comparison of component deviations between the high manganese steel spectral standard sample prepared by this specific implementation and the conventional high manganese steel spectral standard sample is shown in Table 2 below.
[0051]
[0052] The above is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed by the present invention should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention shall be based on the protection scope of the claims.
Claims
1. A method for preparing a high manganese steel spectral standard sample, characterized in that The following steps are involved: S1. Material preparation and smelting: prepare materials according to the medium limit of high manganese steel composition, use vacuum smelting test furnace for smelting, cast and mold to obtain rods with a diameter of 100mm, and the casting temperature is 1420-1430℃; S2, heat treatment: heat the bar obtained in step S1 to 1080±10°C, keep it at this temperature for 2h, and then perform quenching treatment; S3, Forging: S3-1, removing the casting defect areas at both ends of the bar after the heat treatment in step S2; S3-2, preheating before forging: heat the bar obtained in step S3-1 to 1200±10°C and keep it warm for 3h; S3-3, roughening: roughening the bar material after preheating before forging in step S3-2, with roughening process parameters as follows: height-to-diameter ratio of 2, pressing amount during roughening not more than 50 mm, and roughening to a diameter of 150 mm; S3-4, drawing: the bar material after being upset in step S3-3 is re-drawn to a diameter of 100 mm, and the drawing process parameters are: the feed amount is not more than 20 mm, and the pressing amount is not more than 10 mm; S3-5, secondary roughening: the bar material stretched in step S3-4 is subjected to secondary roughening to a diameter of 150 mm, and the roughening process parameters are the same as those in step S3-3; S3-6, secondary drawing: the bar material after secondary roughening in step S3-5 is secondary drawn to a diameter of 80 mm, and the drawing process parameters are the same as those in step S3-4; S3-7, post-forging treatment: cooling the bar obtained after the secondary drawing in step S3-6 to room temperature in the furnace; S4, sawing and grinding: sawing the bar material forged in step S3 into small sections of bar material with a length of 80 mm, grinding and polishing both end surfaces of the small sections of bar material to obtain a high manganese steel spectrum standard sample.
2. The method for preparing a high manganese steel spectrum standard sample according to claim 1, characterized in that: In step S2, the quenching medium of the quenching treatment is water, and the water temperature is 20-25°C.
3. The method for preparing a high manganese steel spectrum standard sample according to claim 1, characterized in that: In step S3-2, the heating rate in the preheating stage before forging is the maximum heating rate of the chamber furnace.
4. The method for preparing a high manganese steel spectrum standard sample according to claim 1, characterized in that: The prepared high manganese steel spectrum standard sample was subjected to composition detection and data analysis: Composition detection: Each polished section of the bar is subjected to chemical analysis and spectral analysis, and at least two spectrometers are used for the spectral analysis process, and each end face is tested at 6 points using a spectrometer; Data analysis: All components detected by the spectrometer are compared with the component data obtained by chemical analysis. A small section of bar material with a component deviation that meets the standard requirements is selected. Then the average of all components detected by the spectrometer and the components obtained by chemical analysis is used as the composition of the high manganese steel spectral standard.
Citation Information
Patent Citations
Method for preparing low-carbon metal manganese iron by using manganese-poor powdered ore
CN101113496A
Laboratory preparation method of iron-base amorphous spectral standard sample
CN103115870A