A low-dielectric mobile phone middle frame substrate and preparation method thereof

By combining polycarbonate and other materials with modified hollow glass beads, a low-dielectric mobile phone middle frame substrate is prepared, which solves the problems of metal middle frames that hinder signals and is high cost and weight, and achieves an improvement in dielectric properties and mechanical properties. Improved, low cost and easy to process.

CN114716802BActive Publication Date: 2024-10-18ZHENGZHOU HOLLOWLITE MATERIALS CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202210334506.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-03-30
Publication Date
2024-10-18
Estimated Expiration
2042-03-30

AI Technical Summary

Technical Problem

The existing metal middle frame hinders 5G signal transmission, is high in cost and weight, and the polymer material has low thermal conductivity and low mechanical properties, and the addition of thermosetting resin and glass fiber leads to poor dielectric properties.

Method used

A combination of polycarbonate, polyethylene terephthalate, modified hollow glass beads, toughening agent, dispersant, antioxidant and lubricant is used to prepare the low-dielectric mobile phone middle frame substrate through injection molding , modified hollow glass microspheres are treated with epoxy resin and coupling agent to improve compatibility and interface bonding properties.

Benefits of technology

A mobile phone mid-frame substrate with excellent dielectric and mechanical properties, light weight, low cost and easy processing has been realized. The dielectric constant is 2.601-2.723, the dielectric loss is 0.00257-0.0036, and the notched impact strength is 20.22-24.40KJ/m2. The tensile strength is 36-45MPa and the bending strength is 58-70MPa.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003574038850000081
    Figure BDA0003574038850000081
Patent Text Reader

Abstract

The present invention belongs to the field of material technology, and specifically relates to a low-dielectric mobile phone middle frame substrate and a preparation method thereof. According to weight percentage, the mobile phone middle frame substrate includes the following components: 55-70 parts of polycarbonate, 10-25 parts of polyethylene terephthalate, 10-18 parts of modified hollow glass microspheres, 5-15 parts of toughening agent, 3-8 parts of dispersant, 0.4-1 parts of antioxidant and 0.5-1.5 parts of lubricant. The dielectric properties of the mobile phone middle frame substrate of the present invention are better, the mechanical properties are excellent, the weight is light, the cost is low, and the processing is easy.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of material technology, and in particular relates to a low-dielectric mobile phone middle frame substrate and a preparation method thereof. Background Art

[0002] With the development of society, the frequency of use of electronic products is getting higher and higher. As an important electronic product, mobile phones have become an indispensable part of our lives. As the functions of mobile phones become more and more abundant, consumers' demand for mobile phones is also getting higher and higher. Not only do they require high software configuration of mobile phones, but they also require higher and higher hardware configuration functions of mobile phones. The middle frame of the mobile phone is located at the junction between the front panel and the back cover. It is an important part of the mobile phone. The common mobile phone middle frame is made of metal. However, we are gradually entering the 5G era. 5G transmits millimeter waves and transmits a lot of data content, but its penetration is weak. The metal middle frame has already had a certain hindering effect on the mobile phone receiving base station signals, and the metal middle frame is relatively heavy and has a high production cost. Therefore, it is of great significance to develop a low-dielectric mobile phone middle frame with a resin substrate.

[0003] The Chinese patent application with publication number CN112409789A discloses a polyamide composition for a 5G mobile phone middle frame and its preparation method, which belongs to the field of polymers. The method puts a uniformly mixed polyamide, epoxy resin and toughening agent into the main feed port of a twin-screw extruder, adds glass fiber to the feed port on the first side of the extruder, and adds a uniformly mixed thermal conductive filler and additive to the feed port on the second side of the extruder. The melt is vacuumed in the penultimate section of the die, and the composition after shearing and mixing is extruded, and the pulling strip is cooled, granulated, dried and homogenized before packaging. The composition of the invention is a high-strength and high-thermal-conductivity polyamide material, which solves the problems of low thermal conductivity and low mechanical properties of thermal conductive materials in the prior art, has excellent thermal conductivity, mechanical strength, and is dimensionally stable, and can be used in 5G mobile phone middle frame materials. However, the addition of thermosetting resin and glass fiber in the patent will cause the dielectric properties of the substrate to deteriorate. Summary of the invention

[0004] In order to overcome the above defects, the purpose of the present invention is to provide a low-dielectric mobile phone middle frame substrate and a preparation method thereof. The obtained mobile phone middle frame substrate has excellent dielectric properties and mechanical properties, is light in weight, low in cost, and easy to process.

[0005] To achieve the above object, the present invention adopts the following technical solution:

[0006] A low-dielectric mobile phone middle frame substrate comprises the following components in parts by weight:

[0007] 55-70 parts of polycarbonate, 10-25 parts of polyethylene terephthalate, 10-18 parts of modified hollow glass microspheres, 5-15 parts of toughening agent, 3-8 parts of dispersant, 0.4-1 parts of antioxidant and 0.5-1.5 parts of lubricant.

[0008] Preferably, the toughening agent is one or more of EM-500, EM-500A, and M521.

[0009] Preferably, the dispersant is one or more of zinc stearate, calcium stearate and magnesium stearate.

[0010] Preferably, the antioxidant is one or more of antioxidant 1010, antioxidant 1076 and antioxidant B225.

[0011] Preferably, the lubricant is one or more of pentaerythritol stearate, vinyl bisstearamide and polysiloxane.

[0012] Preferably, the method for preparing the modified hollow glass microspheres comprises the following steps:

[0013] (1) At room temperature, add 2-6 parts of tetraethyl silicate to 10-20 parts of anhydride curing agent and stir for 30-60 minutes, then add 0.2-1.0 parts of KH550 coupling agent and 10-20 parts of epoxy resin in sequence, and continue stirring for 30-60 minutes to obtain a mixed solution;

[0014] (2) diluting the mixed solution of step (1) by 50-80 times with deionized water, slowly adding 50-80 parts of hollow glass microspheres while stirring, stirring for 30-60 minutes, drying, and sieving to obtain modified hollow glass microspheres.

[0015] Preferably, the hollow glass microspheres have a particle size of 20-30 μm and a specific gravity of 0.4-0.5 g / cm 3 , strength 12000-18000psi.

[0016] Preferably, the drying conditions are: drying temperature 120-140° C., time 4-8 h.

[0017] A method for preparing the above-mentioned low-dielectric mobile phone middle frame substrate comprises the following steps:

[0018] The modified hollow glass microspheres, polyethylene terephthalate, polycarbonate, toughening agent, antioxidant, lubricant and dispersant are uniformly mixed according to the weight proportions, and granulated to obtain master batches containing hollow glass microspheres, and the master batches are added into an injection molding machine for injection molding.

[0019] Preferably, the injection molding temperature of the injection molding machine is 280-300° C., and the injection molding pressure is 80-120 bar.

[0020] The positive beneficial effects of the present invention are:

[0021] 1. An organic-inorganic epoxy / silicon dioxide hybrid layer is formed on the surface of the modified hollow glass microspheres of the present invention, which effectively improves the compatibility and interface bonding performance of the hollow glass microspheres with polycarbonate and polyethylene terephthalate. The addition of a toughening agent further compensates for the reduction in the mechanical properties of the material caused by the hollow glass microspheres. The various raw materials of the present invention work synergistically, and the obtained mobile phone middle frame substrate has excellent dielectric properties and mechanical properties, is light in weight, low in cost, and easy to process. DETAILED DESCRIPTION

[0022] The present invention is further described below in conjunction with some specific embodiments.

[0023] Example 1

[0024] A low-dielectric mobile phone middle frame substrate comprises the following components in parts by weight:

[0025] 55 parts of polycarbonate, 15 parts of polyethylene terephthalate, 10 parts of modified hollow glass microspheres, 5 parts of toughening agent, 3 parts of dispersant, 0.4 parts of antioxidant and 1.0 parts of lubricant.

[0026] Furthermore, the toughening agent is EM-500.

[0027] Furthermore, the dispersant is zinc stearate.

[0028] Furthermore, the antioxidant is antioxidant 1076.

[0029] Furthermore, the lubricant is vinyl bisstearamide.

[0030] Furthermore, the method for preparing the modified hollow glass microspheres comprises the following steps:

[0031] (1) At room temperature, add 2 parts of tetraethyl silicate to 20 parts of anhydride curing agent and stir for 30 minutes, then add 0.5 parts of KH550 coupling agent and 10 parts of epoxy resin in sequence, and continue stirring for 50 minutes to obtain a mixed solution;

[0032] (2) diluting the mixed solution of step (1) by 50 times with deionized water, slowly adding 60 parts of hollow glass microspheres while stirring, stirring for 60 minutes, drying at 120° C. for 4 hours, and sieving to obtain modified hollow glass microspheres.

[0033] Furthermore, the hollow glass microspheres have a particle size of 20-30 μm and a specific gravity of 0.4-0.5 g / cm 3 , strength 12000-18000psi.

[0034] The method for preparing the low-dielectric mobile phone middle frame substrate comprises the following steps:

[0035] The modified hollow glass microspheres, polyethylene terephthalate, polycarbonate, toughening agent, antioxidant, lubricant and dispersant are uniformly mixed according to the weight proportions, and granulated to obtain a master batch containing hollow glass microspheres. The master batch is added into an injection molding machine for injection molding. The injection molding temperature of the injection molding machine is 280-300° C., and the injection molding pressure is 80-120 bar.

[0036] Example 2

[0037] A low-dielectric mobile phone middle frame substrate comprises the following components in parts by weight:

[0038] 56 parts of polycarbonate, 12 parts of polyethylene terephthalate, 10 parts of modified hollow glass microspheres, 10 parts of toughening agent, 8 parts of dispersant, 0.5 parts of antioxidant and 0.5 parts of lubricant.

[0039] Furthermore, the toughening agent is EM-500A.

[0040] Furthermore, the dispersant is calcium stearate.

[0041] Furthermore, the antioxidant is antioxidant 1010.

[0042] Furthermore, the lubricant is pentaerythritol stearate.

[0043] Furthermore, the method for preparing the modified hollow glass microspheres comprises the following steps:

[0044] (1) At room temperature, 3 parts of tetraethyl silicate were added to 10 parts of anhydride curing agent and stirred for 40 minutes, followed by adding 0.2 parts of KH550 coupling agent and 15 parts of epoxy resin in sequence, and stirring was continued for 30 minutes to obtain a mixed solution;

[0045] (2) diluting the mixed solution of step (1) by 60 times with deionized water, slowly adding 70 parts of hollow glass microspheres while stirring, stirring for 30 minutes, drying at 130° C. for 5 hours, and sieving to obtain modified hollow glass microspheres.

[0046] Furthermore, the hollow glass microspheres have a particle size of 20-30 μm and a specific gravity of 0.4-0.5 g / cm 3 , strength 12000-18000psi.

[0047] The preparation method of the low-dielectric mobile phone middle frame substrate is detailed in Example 1.

[0048] Example 3

[0049] A low-dielectric mobile phone middle frame substrate comprises the following components in parts by weight:

[0050] 60 parts of polycarbonate, 10 parts of polyethylene terephthalate, 12 parts of modified hollow glass microspheres, 10 parts of toughening agent, 5 parts of dispersant, 0.6 parts of antioxidant and 0.8 parts of lubricant.

[0051] Furthermore, the toughening agent is M521.

[0052] Furthermore, the dispersant is magnesium stearate.

[0053] Furthermore, the antioxidant is antioxidant B225.

[0054] Furthermore, the lubricant is vinyl bisstearamide and polysiloxane, and the weight ratio of the lubricant is 1:1.

[0055] Furthermore, the method for preparing the modified hollow glass microspheres comprises the following steps:

[0056] (1) At room temperature, 5 parts of tetraethyl silicate were added to 15 parts of anhydride curing agent and stirred for 60 minutes, followed by adding 0.6 parts of KH550 coupling agent and 10 parts of epoxy resin in sequence, and stirring was continued for 40 minutes to obtain a mixed solution;

[0057] (2) diluting the mixed solution of step (1) by 70 times with deionized water, slowly adding 60 parts of hollow glass microspheres while stirring, stirring for 50 minutes, drying at 120°C for 6 hours, and sieving to obtain modified hollow glass microspheres.

[0058] Furthermore, the hollow glass microspheres have a particle size of 20-30 μm and a specific gravity of 0.4-0.5 g / cm 3 , strength 12000-18000psi.

[0059] The preparation method of the low-dielectric mobile phone middle frame substrate is detailed in Example 1.

[0060] Example 4

[0061] A low-dielectric mobile phone middle frame substrate comprises the following components in parts by weight:

[0062] 65 parts of polycarbonate, 20 parts of polyethylene terephthalate, 12 parts of modified hollow glass microspheres, 10 parts of toughening agent, 5 parts of dispersant, 0.8 parts of antioxidant and 1.0 parts of lubricant.

[0063] Furthermore, the toughening agent is EM-500.

[0064] Furthermore, the dispersant is magnesium stearate.

[0065] Furthermore, the antioxidant is antioxidant 1010.

[0066] Furthermore, the lubricant is pentaerythritol stearate.

[0067] Furthermore, the method for preparing the modified hollow glass microspheres comprises the following steps:

[0068] (1) At room temperature, 4 parts of tetraethyl silicate were added to 14 parts of anhydride curing agent and stirred for 50 minutes, followed by adding 0.5 parts of KH550 coupling agent and 15 parts of epoxy resin in sequence, and stirring was continued for 50 minutes to obtain a mixed solution;

[0069] (2) diluting the mixed solution of step (1) by 80 times with deionized water, slowly adding 80 parts of hollow glass microspheres while stirring, stirring for 50 minutes, drying at 140° C. for 4 hours, and sieving to obtain modified hollow glass microspheres.

[0070] Furthermore, the hollow glass microspheres have a particle size of 20-30 μm and a specific gravity of 0.4-0.5 g / cm 3 , strength 12000-18000psi.

[0071] The preparation method of the low-dielectric mobile phone middle frame substrate is detailed in Example 1.

[0072] Example 5

[0073] A low-dielectric mobile phone middle frame substrate comprises the following components in parts by weight:

[0074] 63 parts of polycarbonate, 22 parts of polyethylene terephthalate, 15 parts of modified hollow glass microspheres, 12 parts of toughening agent, 6 parts of dispersant, 0.6 parts of antioxidant and 1.2 parts of lubricant.

[0075] Furthermore, the toughening agent is M521.

[0076] Furthermore, the dispersant is zinc stearate.

[0077] Furthermore, the antioxidant is antioxidant 1076.

[0078] Furthermore, the lubricant is polysiloxane.

[0079] Furthermore, the method for preparing the modified hollow glass microspheres comprises the following steps:

[0080] (1) At room temperature, 5 parts of tetraethyl silicate were added to 16 parts of anhydride curing agent and stirred for 60 minutes, followed by adding 0.7 parts of KH550 coupling agent and 18 parts of epoxy resin in sequence, and stirring was continued for 50 minutes to obtain a mixed solution;

[0081] (2) diluting the mixed solution of step (1) by 60 times with deionized water, slowly adding 70 parts of hollow glass microspheres while stirring, stirring for 30 minutes, drying at 120° C. for 8 hours, and sieving to obtain modified hollow glass microspheres.

[0082] Furthermore, the hollow glass microspheres have a particle size of 20-30 μm and a specific gravity of 0.4-0.5 g / cm 3 , strength 12000-18000psi.

[0083] The preparation method of the low-dielectric mobile phone middle frame substrate is detailed in Example 1.

[0084] Example 6

[0085] A low-dielectric mobile phone middle frame substrate comprises the following components in parts by weight:

[0086] 70 parts of polycarbonate, 25 parts of polyethylene terephthalate, 18 parts of modified hollow glass microspheres, 15 parts of toughening agent, 7 parts of dispersant, 1.0 part of antioxidant and 1.5 parts of lubricant.

[0087] Furthermore, the toughening agent is EM-500A.

[0088] Furthermore, the dispersant is calcium stearate.

[0089] Furthermore, the antioxidant is antioxidant B225.

[0090] Furthermore, the lubricant is vinyl bisstearamide and polysiloxane, and the weight ratio of the lubricant is 1:1.

[0091] Furthermore, the method for preparing the modified hollow glass microspheres comprises the following steps:

[0092] (1) At room temperature, 6 parts of tetraethyl silicate were added to 20 parts of anhydride curing agent and stirred for 50 minutes, followed by the addition of 1.0 parts of KH550 coupling agent and 20 parts of epoxy resin, and stirring was continued for 60 minutes to obtain a mixed solution;

[0093] (2) diluting the mixed solution of step (1) by 80 times with deionized water, slowly adding 50 parts of hollow glass microspheres while stirring, stirring for 40 minutes, drying at 120° C. for 8 hours, and sieving to obtain modified hollow glass microspheres.

[0094] Furthermore, the hollow glass microspheres have a particle size of 20-30 μm and a specific gravity of 0.4-0.5 g / cm 3 , strength 12000-18000psi.

[0095] The preparation method of the low-dielectric mobile phone middle frame substrate is detailed in Example 1.

[0096] Comparative Example 1

[0097] The low dielectric mobile phone middle frame substrate of this embodiment is basically the same as that of embodiment 5, and the similarities are not repeated here. Some differences are: no modified hollow glass microspheres are added.

[0098] Comparative Example 2

[0099] The low dielectric mobile phone middle frame substrate of this embodiment is basically the same as that of embodiment 5, and the similarities are not repeated here. Some differences are: 25 parts of modified hollow glass microspheres.

[0100] Comparative Example 3

[0101] The low dielectric mobile phone middle frame substrate of this embodiment is basically the same as that of embodiment 5, and the similarities are not repeated here. Some differences are: no toughening agent is added.

[0102] The low dielectric mobile phone middle frame substrates prepared in Examples 1-6 of the present invention and Comparative Examples 1-3 were subjected to performance testing, and the test results are shown in Table 1.

[0103] Table 1 Performance test results of low dielectric mobile phone middle frame substrate of the present invention

[0104]

[0105] As shown in Table 1, when no modified hollow glass microspheres are added to Comparative Example 1, the dielectric properties of the substrate deteriorate, the density of the substrate increases, and it is not easy to process; when more modified hollow glass microspheres are added to Comparative Example 2, the impact strength of the substrate deteriorates; when no toughening agent is added to Comparative Example 3, the impact strength of the substrate deteriorates. After adding 10-18 parts of modified hollow glass microspheres and 5-15 parts of toughening agent to the present invention, the raw materials work synergistically, and the dielectric constant of the obtained substrate is 2.601-2.723, the dielectric loss is 0.00257-0.0036, and the dielectric properties are excellent; the notched impact strength is 20.22-24.40KJ / m 2 , tensile strength is 36-45MPa, flexural strength is 58-70MPa, mechanical properties are excellent, and specific gravity is 0.956-0.993g / cm 3 , small specific gravity and light weight.

[0106] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Other modifications or equivalent substitutions made to the technical solution of the present invention by ordinary technicians in the field should be included in the scope of the claims of the present invention as long as they do not depart from the spirit and scope of the technical solution of the present invention.

Claims

1. A low dielectric mobile phone middle frame substrate, characterized in that: According to weight parts, it includes the following ingredients: 55-70 parts of polycarbonate, 10-25 parts of polyethylene terephthalate, 10-18 parts of modified hollow glass microspheres, 5-15 parts of toughening agent, 3-8 parts of dispersant, 0.4-1 parts of antioxidant and 0.5-1.5 parts of lubricant; The toughening agent is one or more of EM-500, EM-500A, and M521; The modified hollow glass microsphere preparation method comprises the following steps: (1) At room temperature, add 2-6 parts of tetraethyl silicate to 10-20 parts of anhydride curing agent and stir for 30-60 minutes, then add 0.2-1.0 parts of KH550 coupling agent and 10-20 parts of epoxy resin in sequence, and continue stirring for 30-60 minutes to obtain a mixed solution; (2) diluting the mixed solution of step (1) by 50-80 times with deionized water, slowly adding 50-80 parts of hollow glass microspheres while stirring, stirring for 30-60 minutes, drying, and sieving to obtain modified hollow glass microspheres; The hollow glass microspheres have a particle size of 20-30 μm and a specific gravity of 0.4-0.5 g / cm 3 , strength 12000-18000psi.

2. According to claim 1, the low dielectric mobile phone middle frame substrate is characterized in that: The dispersant is one or more of zinc stearate, calcium stearate and magnesium stearate.

3. The low dielectric mobile phone middle frame substrate according to claim 1, characterized in that: The antioxidant is one or more of antioxidant 1010, antioxidant 1076 and antioxidant B225.

4. The low dielectric mobile phone middle frame substrate according to claim 1, characterized in that: The lubricant is one or more of pentaerythritol stearate, vinyl bisstearamide and polysiloxane.

5. According to claim 1, the low-dielectric mobile phone middle frame substrate, the drying conditions are: drying temperature 120-140°C, time 4-8h.

6. A method for preparing a low-dielectric mobile phone middle frame substrate according to any one of claims 1 to 5, characterized in that: The steps include: The modified hollow glass microspheres, polyethylene terephthalate, polycarbonate, toughening agent, antioxidant, lubricant and dispersant are uniformly mixed according to the weight proportions, and granulated to obtain master batches containing hollow glass microspheres, and the master batches are added into an injection molding machine for injection molding.

7. The method for preparing a low-dielectric mobile phone middle frame substrate according to claim 6, characterized in that: The injection molding temperature of the injection molding machine is 280-300° C., and the injection molding pressure is 80-120 bar.

Citation Information

Patent Citations

  • Polyamide composition for 5G mobile phone middle frame and preparation method thereof

    CN112409789A

  • Flame-retardant PET and PC composite material and preparation method thereof

    CN106905674A

  • Thermosetting resin composition, prepreg, laminated board and printed circuit board

    CN109233244A

  • Material for preparing radome and preparation method thereof

    CN112646344A