Lightweight reinforced composite material formulation and method for making the same

By using composite additives and solvated polymers and low-density fillers, the uniformity of color and mechanical properties in lightweight composite materials is solved, achieving uniform color of molded parts and improving mechanical properties, suitable for construction and transportation and other fields.

CN114729158BActive Publication Date: 2024-11-01CHROMAFLO TECH CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202080077873.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-09-09
Filing Date
2020-09-09
Publication Date
2024-11-01
Estimated Expiration
2040-09-09

AI Technical Summary

Technical Problem

The prior art is difficult to produce lightweight composite materials with uniform color, density and mechanical properties, especially in applications for molded parts, with conventional methods resulting in uneven color distribution and mechanical properties degradation.

Method used

Combined with composite additives and solvated polymer mixtures with low-density fillers, adjust the rheological characteristics through silane carriers and dispersants to form a combination of treated low-density fillers and polymer slurries to ensure color uniformity and mechanical properties. .

Benefits of technology

The uniform color distribution of molded parts is achieved and the mechanical properties are improved, meeting the needs of lightweight parts in construction, transportation and other applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114729158B_ABST
    Figure CN114729158B_ABST
Patent Text Reader

Abstract

Composite material formulations for lightweight molded parts include untreated low-density fillers, such as glass bubbles, solvated polymer mixtures, and polymer slurries. In one embodiment, the solvated polymer mixture is used to treat the low-density filler to form a treated low-density filler. The solvated polymer mixture may include a thermoplastic resin or a reactive resin and a composite additive. The composite additive may include a dispersant and a silane carrier composition.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] Related Applications

[0002] This application claims priority to U.S. Provisional Patent Application No. 62 / 897,645, filed on September 9, 2019, which is incorporated herein by reference in its entirety. Technical Field

[0003] The present disclosure relates to composite material formulations for use in applications requiring light, strong and durable parts, including but not limited to construction, transportation, and similar applications, and methods of making the same. Background Art

[0004] In recent years, many methods have been identified to reduce the weight of composites. Some of the proposed methods focus on fiber selection. Other methods still demonstrate the advantages and limitations of lightweight engineered fillers with a specific gravity lower than that of water. However, producing lightweight composites with uniform color properties is a completely different challenge, and one that has not yet been met. It is most important to consider that varying density and glass fiber content may affect not only color but also rheology and processing characteristics and ultimately the mechanical properties obtained. As this means, there are three specific variables: color, density and mechanical properties. It would help to identify a new method to achieve the desired combination of uniform color, density and mechanical properties. Summary of the invention

[0005] An additive package for lightweight molded parts is provided. The additive package may include about 40% to about 96% by weight of a dispersant and about 4% to about 60% by weight of a silane carrier composition. In another embodiment, the dispersant is present in an amount of about 68% to about 96%, and the silane carrier composition is present in an amount of about 4% to about 32%. In yet another embodiment, the dispersant is present in an amount of about 85%, and the silane carrier composition is present in an amount of about 15%. In one embodiment, the dispersant is composed of an alkylamine-based polymer and / or a fluorocarbon.

[0006] A solvated polymer mixture for lightweight molded parts is provided. In one embodiment, the solvated polymer mixture includes about 20% to about 97% by weight of a composite additive and about 3% to about 80% by weight of a thermoplastic resin or a reactive resin. In another embodiment, the solvated polymer mixture includes about 60% by weight of a composite additive and about 40% by weight of a thermoplastic resin or a reactive resin. In one embodiment, the solvated polymer mixture can be a thermoplastic resin, or can also be a reactive resin.

[0007] A treated low-density filler for lightweight molded parts is provided. In one embodiment, the low-density filler comprises about 0.5% to about 20% by weight of a solvated polymer mixture and about 80% to about 99.5% by weight of an untreated low-density filler. In one embodiment, the untreated low-density filler is glass bubbles.

[0008] A composite material formulation for lightweight molded parts is provided. In one embodiment, the composite material includes an untreated low-density filler, a solvated polymer mixture, and a colored polymer slurry. In another embodiment, the solvated polymer mixture is present in an amount of about 0.5% to about 20% by weight based on the weight of the untreated low-density filler.

[0009] In another embodiment, a method of making a treated low density filler for lightweight molded parts includes the steps of combining about 68% to about 96% of a dispersant with about 4% to about 32% of a silane carrier, combining about 20% to about 97% by weight of a composite additive with about 3% to about 80% by weight of a thermoplastic resin or a reactive resin to form a diluted mixture, applying heat to the diluted mixture to form a solvated polymer mixture, combining about 0.5% to about 20% by weight of the solvated polymer mixture with about 80% to about 99.5% by weight of an untreated low density filler to form the treated low density filler.

[0010] In another embodiment, a method for making a composite material for lightweight molded parts includes the following steps: preparing a composite additive, wherein the composite additive includes 68% to about 96% of a dispersant and about 4% to about 32% of a silane carrier; combining about 20% to about 97% by weight of the composite additive with about 3% to about 80% by weight of a thermoplastic resin or a reactive resin to form a diluted mixture; heating the diluted mixture to form a solvated polymer mixture; combining about 0.5% to about 20% by weight of the solvated polymer mixture with about 80% to about 99.5% by weight of an untreated low-density filler to form a treated low-density filler; preparing a polymer slurry; and combining the polymer slurry with the low-density filler. BRIEF DESCRIPTION OF THE DRAWINGS

[0011] The accompanying drawings, which are incorporated in and constitute a part of the specification, show respective example configurations and data and are used only to illustrate various example embodiments. In the drawings, the same elements have the same reference numerals.

[0012] Figure 1 is a photograph of a black molded part containing a low density filler prepared by a conventional method.

[0013] Figure 2is a photograph of a black molded part containing a low density filler prepared as described in the specification below.

[0014] Figure 3 is a graphical representation of the complex viscosity of various samples of composite formulations.

[0015] Figure 4 is a 2000X microscopic image of an untreated glass bubble.

[0016] Figure 5 is a 2000X micrograph of glass bubbles treated with the solvated polymer mixture. DETAILED DESCRIPTION

[0017] It is advantageous to combine low density fillers, such as glass bubbles or other suitable low density fillers (e.g., hollow spheres or polymer spheres) with polymer slurries to manufacture molded parts for the automotive industry. For the purposes of this discussion, "low density filler" refers to any filler material having a density below 1.0. This enables manufacturers to reduce the weight of the part while maintaining the desired mechanical properties and durability. However, it has been found that simply combining hollow spheres with a colored polymer slurry results in a molded part with an uneven color distribution. For example, Figure 1 As shown in Figure 1, white swirls of glass beads can be seen on the surface of a black molded part produced by conventional methods. This uneven color distribution is unacceptable in a composite truck bed used, for example, for a consumer vehicle. Surprisingly, it has been found that treating a low-density filler with a solvated polymer mixture, either before combining with a polymer slurry or when the polymer slurry is combined with a resin, enables manufacturers to produce molded polymer parts with a completely uniform pigment distribution. It should be noted that, as an example, this description refers to glass bubbles, but it should be understood that any suitable low-density filler can be used.

[0018] In one embodiment, a lightweight reinforced colored composite material for making molded polymer parts is provided. The composite material may include a colored polymer slurry and a treated low-density filler. The treated low-density filler is typically prepared by combining an untreated low-density filler with a solvated polymer mixture. Although the following description will refer to the use of the treated low-density filler in the reinforced polymer slurry, it should be understood that the untreated low-density filler and the solvated polymer mixture can be combined with the polymer slurry in separate steps to form a reinforced polymer composite.

[0019] Composite materials for lightweight molded parts can include a colored polymer slurry and an untreated low-density filler treated with a solvated polymer mixture (i.e., a treated low-density filler). In one embodiment, the colored polymer slurry can include a polymer for sheet molding, bulk molding, pultrusion, and casting. In one embodiment, the polymer can include an unsaturated polyester. In another embodiment, the polymer slurry can also include a thickener.

[0020] To form a treated low density filler, the hollow spheres are combined with a solvated polymer mixture. The solvated polymer mixture may include a thermoplastic resin and / or a reactive resin. The solvated polymer mixture may also include a composite additive made by combining a dispersant with a silane carrier composition.

[0021] In one embodiment, the composite additive includes about 40% to about 96% by weight of a dispersant and about 4% to about 60% by weight of a silane carrier composition. In another embodiment, the dispersant is present in an amount of about 68% to about 96%, and the silane carrier composition is present in an amount of about 4% to about 32%. In yet another embodiment, the dispersant is present in an amount of about 85%, and the silane carrier composition is present in an amount of about 15%. The dispersant can be selected from any suitable dispersant or wetting agent. It is desirable that the dispersant has an affinity for both low-density fillers and colorants, and is also highly compatible with the various components of the polymer slurry. In one embodiment, suitable dispersant examples include, but are not limited to, polyimines, polyamines, amines, and fluorocarbon-based polymers.

[0022] Examples of such dispersants include Solsperse 24000, Solsperse 28000, Solsperse 17000, Solsperse 13940, Solsperse 3000, Solsperse 39000, Solsperse 16000 (commercially available from Lubrizol), Byk-9076 (commercially available from Byk Additives and Instruments), ADD-4276 (available from ADD), Cliqsperse PH (commercially available from Cliq), Soya Lecithin (available from multiple sources), FC 170, FC 4430 (commercially available from 3M), Afcona 7476, Afcona 7480 (commercially available from Afcona), Terwet 3780 tallow amine ethoxylate (commercially available from Terwet 3780). ethoxylate (commercially available from Huntsman) and tallow amine oleate (available from a variety of sources).

[0023] It will be appreciated that the choice of dispersant will be determined by the nature of the colorant or resin to be used, the filler, and the polymers and monomers present in the polymer slurry. It will also be appreciated that the ratio of dispersant to silane carrier composition may vary depending on the desired rheology of the selected dispersant and additive package.

[0024] Silane carrier compositions may include, but are not limited to, vinyltrimethoxysilane (AP-Silane 21, available from Advanced Polymer, Inc.), y-methacryloxypropyltrimethoxysilane (AP-Silane 71T, available from Advanced Polymer, Inc.), amino-modified propyltrimethoxysilane (Silquest A-1130, available from Momentive), methacryloxypropyltriethoxysilane (available from multiple sources), and y-aminopropyltriethoxysilane (Silquest A-1100, available from Momentive).

[0025] The composite additive can be combined with one or more resins, including thermoplastic resins and reactive resins. One suitable resin includes Elvacite 2013. In one embodiment, about 20% to about 97% of the composite additive can be combined with about 3% to about 80% by weight of the resin to form a diluted mixture. In another embodiment, about 60% of the composite additive is combined with about 40% of the resin. And, in yet another embodiment, about 5% of the resin is combined with about 95% by weight of the composite additive. The diluted mixture is then heated and stirred to form a solvated polymer mixture.

[0026] Example

[0027] Example 1

[0028] In one example, a 100 g sample of the additive package is prepared by combining about 85% by weight of BYK-9076 dispersant with about 15% by weight of AP-Silane 21 in a DAC orbital mixing cup and processing for about 30 seconds. 95 g of the resulting additive package is then combined with 5 g of Elvacite 2013 to form a 5% diluted mixture. The diluted mixture is then heated at about 60° C. for approximately 24 hours. The sample is then scraped off and mixed using a high shear mixing blade and allowed to stand at room temperature for about 12 hours to form a solvated polymer mixture.

[0029] About 1.32 grams of the 5% solvated polymer mixture (approximately 0.88% by weight) (EXP 1) was then combined with about 148.68 g of IM16K glass bubbles (approximately 99.12% by weight, commercially available from 3M) in a one quart jar. The jar was then sealed and placed on a horizontal roller for about 3 days to coat the bubbles with the solvated polymer mixture. Additional samples of treated glass bubbles were prepared using 1.76% (EXP 2) and 3.52% (EXP 3) by weight of the solvated polymer mixture.

[0030] About 15 g of each of the three samples of treated glass bubbles were then combined with about 30 g of Arotra n 805 polymer syrup (commercially available from Ashland Chemical).

[0031] Rheological data for each of the resulting reinforced composite samples (Examples 1, 2, and 3) and control samples of polymer slurries and untreated glass bubbles were obtained using a TA Instruments Discovery HR 1 rheometer. The rheometer was equipped with a 50 mm cone and plate geometry with a 56 micron gap at the tip of the cone. A controlled frequency sweep was performed at a constant temperature of 25°C from 0.1 to 100 radians per second with a maximum strain of 5%. Prior to data collection, a brief conditioning time of ten (10) seconds was applied to each sample at the start of the experiment.

[0032] Data collection was recorded logarithmically over the specified frequency range, with ten data points collected per decade of frequency range, for a total of thirty-one (31) data points per sample. The instrument was set to collect sixty-four (64) data measurements per waveform. The equilibrium and integration times were each set to five (5) seconds per data point over the measurement range.

[0033] like Figure 3 As shown, the use of composite additives allows manufacturers to control or adjust complex fluid behavior, including but not limited to the degree of plasticity, pseudoplasticity, thixotropy and pseudothixotropy present in the composite formulation. Specifically, the complex viscosity of the composite formulation using the composite additive remains lower and more stable at increasing angular frequency.

[0034] Figure 4 and 5 Microscopic images of unmodified and surface-treated glass bubbles, magnified 2000X. Figure 5As can be seen, after the glass bubble was treated, multiple submicron particles were found to adhere to the surface of the bubble. Without being bound by theory, it is likely that as the silane bonded to the glass, the polymethylmethacrylate lost solubility and formed the observed particles on the surface. Those particles then acted as a binding sight for the color additive to bond to the glass and help wet the glass. It should also be noted that in the images collected on the untreated glass bubble ( Figure 4 ) are relatively few particles visible in FIG. Again, without being bound by theory, it is possible that the few particles that appear in this image may be submicron contaminants.

[0035] Example 2

[0036] In a second example, white, red, and yellow molded part formulations (MCFs) were formulated with and without treated glass bubbles. For each formulation presented in this section, the formulation was reduced to 100.00 + / - 0.02 g, the ingredients were weighed and mixed for forty-five (45) seconds using an orbital mixer at 2700 RPM. Temperature was measured before and after the mixing process. Viscosity measurements were made using an RVT spindle appropriate for the slurry viscosity over a period of time, from mixing until a fully mature viscosity of at least 20 million cP was reached. Typically, mature viscosity was reached in two to three days; however, samples were retained for several weeks to continue viscosity measurements. The following table details each slurry formulation for each color.

[0037] White MPF Formula

[0038] Three batches of white MPF were prepared as detailed in Table 1 below:

[0039] Table 1

[0040]

[0041]

[0042] As can be seen from the above formulation, commercial DPG-Iso resins generally have strong mechanical properties. A commercial saturated low shrinkage additive is used to provide the necessary shrinkage characteristics. Because this formulation is intended and designed to be weatherable, UVS-10476 is used to provide color and weatherability. Peroxide initiators and inhibitors are used to provide control over the cure characteristics. Commercial grade zinc stearate is used as a release agent. Am-9033 was used as a thickener to achieve the necessary molding viscosity over time. For consistency purposes, one inch chopped commercial grade glass was used at a constant volume percentage of 10.5% when molding the final part. The fibers were introduced into the slurry at molding viscosity under high temperature and shear conditions.

[0043] The differences among the three groups can be found in the fillers. Specifically, the control group was made with aluminum trihydrate, while Group A used untreated glass bubbles and Group B used treated glass bubbles. The treated bubbles (experimental filler 20200423d) included 96.648% glass bubble filler, 2.667% Sartomer SR350 resin material, 0.582% Byk9076 dispersant, and 0.103% Silane AP 21 silane carrier.

[0044] Yellow MPF Formula

[0045] Two batches of yellow MPF were prepared as detailed in Table 2 below:

[0046] Table 2

[0047]

[0048] If the colorant is changed, a fundamental difference between the yellow and white formulations occurs. Specifically, UVS-80637 is used to achieve a bright, weather-resistant yellow color. With regard to fillers, group A includes untreated glass bubbles, while group B includes the above-described treated glass bubbles.

[0049] Red MPF Formula

[0050] Two batches of red MPF were prepared as detailed in Table 3A below:

[0051] Table 3A

[0052]

[0053]

[0054] The principle difference between the red formulation and the white and yellow formulations is the change in colorant. Specifically, UVS-70388 is used to achieve a bright, weather-resistant red color. Regarding fillers, Group A includes untreated glass bubbles, while Group B includes treated glass bubbles as described above.

[0055] Once the formulation is prepared, sections of twelve inch square panels can be molded. Panels are cut to 125 x 65 mm for appearance measurements and viscosity testing.

[0056] Color measurements were made using an X-Rite Color-Eye 7000A instrument under the following conditions:

[0057] 1. Large area view.

[0058] 2.10° observer.

[0059] 3.D65 cold luminescence.

[0060] 4. Includes reflected light (specular).

[0061] 5. CIE (1976) L*a*b* color space.

[0062] Tables 3B, 4 and 5 below detail the color data for the white, yellow and red panels, respectively, where L* is a measurement from light to dark, a* is a measurement from red to green, and b* is a measurement of yellow. Table 6 includes viscosity data for the samples.

[0063] Table 3B

[0064]

[0065] Table 4

[0066]

[0067] Table 5

[0068]

[0069] Table 6

[0070]

[0071] Contrary to intuitive assumptions, light-colored fillers (such as aluminum trihydrate) can and do affect the color of white composites—and not necessarily in a positive way. In fact, data show that in highly filled composite systems, fillers can and will limit the color brightness that can be achieved in the white color space. In addition, even at low fiber volumes, control white formulations have been shown to have a color change of about one unit of L* (dL*1.0) on the surface of white molded parts.

[0072] Surprisingly, our data show that when untreated glass filler is added to the formulation to replace aluminum trihydrate, L* increases by about one unit (dL*1.0) and the change in L* increases to about 1.5 units (dL*1.5).

[0073] In the white color space, the use of untreated glass filler (white Formulation B) was associated with a significant improvement in color consistency compared to the control and Formulation A.

[0074] In the yellow and red color space, the use of treated fillers was associated with increased color and / or chroma and improved color uniformity. Regarding processing characteristics, we did not see a meaningful impact on initial slurry viscosity within the first few hours of thickening. However, after the first 24-48 hours, the use of treated fillers appeared to be associated with higher, firmer molded viscosities.

[0075] Example 3

[0076] In a third example, three batches of the MPF formulations detailed in Table 7 below were prepared. In general, the formulations were reduced to 100.00 + / - 0.02 g, the ingredients were weighed and mixed using an orbital mixer at 2700 RPM for forty-five (45) seconds. Temperature was measured before and after the mixing process. Viscosity measurements were made using an RVT spindle appropriate for the viscosity of the slurry over a period of time from mixing until a fully mature viscosity of at least 20 million cP was achieved. Typically, mature viscosity was achieved within two to three days; however, samples were retained for several weeks for continued viscosity measurements.

[0077] Table 7

[0078]

[0079]

[0080] The first MPF formulation shown in this table is a control. The second experiment "Group A" includes a lightweight engineered glass filler, which was introduced into the formulation in an attempt to reduce the specific gravity of the compound. For the third experiment "Group B", an experimental rheology modifier (Experimental Filler Additive 1) was included to affect the behavior of the engineered glass filler. Experimental Filler Additive 1 included 85% Byk 9076 and 15% AP Silane 21.

[0081] In these examples, the MPF slurry was mixed for approximately ten (10) minutes using a Cowles mixer under moderate (1100 RPM) agitation. After mixing, the MPF was compounded on a 24 inch MPF machine using conventional compounding methods. Using a glass drop, the target was 37% fiber by volume and 55% fiber by weight to prepare a control formulation with a specific gravity of 1.75. For the experimental formulations, the target fiber volume was maintained at 37% and the weight percentage of fiber was increased to approximately 62% as a function of weight and density. After compounding, the MPF was rolled into reels and allowed to mature to a slurry viscosity of 240,000-400,000 cP over a period of seven (7) to ten (10) days. For each compound, about ten (10) untextured 12" x 12" panels were molded at 290-310°F for three minutes using a 100 ton hydraulic press. The average panel thickness was three (3) millimeters.

[0082] Appearance and appearance measurement

[0083] Color measurements were made using an X-Rite Color-Eye 7000A instrument under the following conditions:

[0084] 1. Large area view.

[0085] 2.10° Observer

[0086] 3.D65 cold luminescence

[0087] 4. Including reflected light.

[0088] 5. CIE (1976) L*a*b* color space.

[0089] Gloss measurements were made using a BYK-Gardner Micro-Tri-Glossmeter capable of taking readings simultaneously at 20°, 60°, and 85°. For this example, the results were focused on the 60° geometry. The color and gloss data presented represent the average of three (3) readings on each panel.

[0090] For the weathering evaluation, each data point provided in this example represents the average of three (3) color and three (3) gloss readings per panel. For the starting point data, the average of all readings was used as a control for L*, a*, b*, and 60° gloss. Table 8 provides a table of our starting point data, including standard deviations.

[0091] Table 8

[0092]

[0093] Weathering test solution

[0094] The resulting panels were subjected to 2000 hours of Xenon Arc exposure per SAE J2527 using an Atlas Ci4000 Weather-O-Meter with borosilicate internal and external filters. This exposure is approximately equivalent to two (2) years of exposure per SAE J1976 at five degrees (5°) south facing in southern Florida. The test period is described in Table 9.

[0095] Table 9

[0096]

[0097] Mechanical Testing

[0098] Flexural and tensile properties were determined by ASTM D790 using an Instron Model 3366 extensometer. Five (5) composite specimens of each sample were evaluated for flexural and tensile properties. Flexural tests were performed using a three-point probe with a maximum load capacity of 50 KN at a crosshead speed of 0.05 in / min. Test results were generated using Bluehill 2 software.

[0099] Notched Izod testing was performed according to ASTM D236 to determine the impact strength of various formulations.

[0100] Weathering results

[0101] After weathering exposure, the panels were rinsed in warm water and dried using a soft cotton cloth. Each panel was then subjected to an average of three readings for color and gloss as described in the experimental section. A table of the exposure and subsequent weathering results can be found in Table 10.

[0102] Table 10. Irradiation and appearance data after completing SAE J2527 (boron / boron) irradiation

[0103]

[0104] As described above, the weathering properties of the panels were evaluated per SAEJ2527 at 2000 hours of Xenon Arc exposure using borosilicate internal and external filters. It is important to understand that the Ci4000 is calibrated at a UV irradiance of 340nm, achieving 0.55 Watts per square meter. Under these conditions, approximately 660kJ of UV exposure (measured at 340nm) was achieved over approximately 500 hours of testing. Per SAE 1976, 1320kJ, or 1000 hours of Xenon Arc exposure, was determined to be roughly equivalent to one (1) year of exposure at five degrees (5°) south Florida.

[0105] Typical shipping specifications require that weatherable materials undergo no meaningful, visible change to an observer after exposure to exposure in South Florida for a period of time. Typically, the minimum acceptable exposure period is two (2) to five (5) years, depending on the manufacturer and application [3-5]. In dark spaces, changes in appearance can be expressed in two (2) ways.

[0106] A. There can be color changes, measured by L*a*b*;

[0107] B. Surface erosion may also occur, resulting in subsequent loss of gloss.

[0108] Typically, in the black color space, color changes exceeding 2.0 dE* will begin to be noticeable to the observer. This is especially true for materials that lose more than 50% of their original gloss when measured at 60°.

[0109] Based on these appearance criteria, none of the formulations experienced an objectionable change in appearance during testing. However, some differences between the formulations emerged. During irradiation, the control formulation retained nearly seventy percent (70%) of its original gloss, remaining below 1.0 dE* from the original color. However, after 2000 hours, Experimental Formulation A had over twice the dE* of the control formulation and only retained approximately fifty percent (50%) of its gloss. We attribute this to the effect of the untreated glass filler used to reduce the weight or density of the composite. Experimental Formulation B also retained approximately fifty percent (50%) of its gloss while remaining within approximately 1.0 dE* of the original color. Therefore, it appears that using Experimental Filler Additive 1 as an additive to change the rheology of the formulation was able to reduce the effect of the treated glass filler on color retention.

[0110] Mechanical properties

[0111] The key properties of the formulation are identified in Tables 11, 12 and 13 below:

[0112] Table 11. Physical properties of MPF composites.

[0113]

[0114] Table 12. Tensile properties of MPF composites

[0115]

[0116] Table 13. Flexural properties of MPF composites

[0117]

[0118]

[0119] The results in Tables 11 and 12 show the tensile and flexural properties of Experimental Formulations 1 and 2 relative to the control. Related to the tensile properties, the addition of lightweight glass fillers to the composites appears to have a detrimental effect on tensile strength (approximately 17%). This is supported by the observed decrease in percent elongation at break, which is similar to the introduction of lightweight engineering glass fillers into the formulation. However, the tensile modulus for all three formulations are within standard deviations of each other.

[0120] A slightly different story emerges regarding the flexural properties. The flexural strength of experimental formulation A is approximately one standard deviation lower than that of the control. This is consistent with the data generated for the tensile properties. However, the flexural strength and modulus of experimental formulation B are several standard deviations higher than the control. To explain this, the flexural and tensile properties of the formulations were analyzed in relation to the amount of glass fiber volume as reinforcement.

[0121] Table 14. Comparison of tensile and flexural properties with percent volume of glass fiber reinforcement

[0122]

[0123] The mechanical properties achieved in these formulations may depend on the fiber reinforcement used. To realize the benefits of fiber reinforcement, it may be beneficial to have the reinforcing fibers uniformly wetted and dispersed in the resin matrix.

[0124] In the table above, it is observed that the total mechanical properties per unit volume of fiber reinforcement decreased by fifteen percent (15%) between the control and Experimental Formulation A. This suggests that when lightweight fillers are added to the formulation in place of more traditional fillers (such as aluminum trihydrate), the interface between the fiber and polymer matrix is ​​adversely affected. In contrast, when rheological additives and modifiers are introduced into the formulation (such as Experimental Filler Additive 1 in Experimental Formulation B), the adverse effects appear to be minimized, or reversed to some extent. Likewise, in MPF ​​formulations, modifying the rheology and wetting characteristics of the polymer matrix relative to the reinforcing fibers will improve or weaken the mechanical properties of the compounding and molding formulations.

[0125] Thus, the addition of less than four percent (4%) by weight of an untreated glass filler having a theoretical specific gravity of 0.46 is sufficient to reduce the density of a sheet molding compound having thirty-seven percent (37%) by volume of glass fibers from a specific gravity of about 1.75 to less than 1.60. However, even the addition of this small amount of untreated glass filler had a significant impact on the mechanical properties and weatherability of the compound. The effect of the filler (Experimental Formulation A) is believed to be an effect on the matrix rheology during processing, which has an adverse effect on the interface between the fiber and the polymer matrix. This observation is supported by the weathering results, where an increased degradation in gloss and L* is associated with the addition of the untreated glass sphere filler.

[0126] Therefore, in Experimental Formulation B, a rheological composite additive was introduced to reverse the effect of the untreated glass filler on the load transfer of the polymer composite matrix. Although the addition of this additive did not improve the tensile strength, it did improve the flexural properties of the resulting material. Furthermore, the inclusion of a rheological modifier in the glass bubbles appeared to minimize the effect of the untreated glass filler on the weathering properties.

[0127] While the invention has been described with respect to specific examples including presently preferred modes of carrying out the invention, those skilled in the art will appreciate that there are numerous variations and permutations of the above described systems and techniques that fall within the spirit and scope of the invention as defined in the appended claims.

Claims

1. A composite material formulation for lightweight molded parts, wherein the composite material include: untreated low-density fillers comprising hollow spheres; A solvated polymer mixture, wherein the solvated polymer mixture comprises: a thermoplastic resin or a reactive resin, and a composite additive, wherein the composite additive comprises a dispersant and a silane carrier composition; wherein 0.5% to 20% by weight of the solvated polymer mixture is combined with 80% to 99.5% by weight of the untreated low density filler to form a treated low density filler; combining the treated low density filler with a polymer slurry to form a polymer slurry mixture; and The polymer syrup mixture is combined with additional compounds to form a composite material.

2. The composite material formulation according to claim 1, wherein the solvated polymer mixture comprises 20% to 97% by weight of the composite additive and 3% to 80% by weight of the thermoplastic resin or reactive resin.

3. The composite material formulation according to claim 2, wherein the solvated polymer mixture comprises 60% of the composite additive and 40% of the thermoplastic resin or reactive resin.

4. The composite material formulation according to claim 1, wherein the composite additive comprises 68% to 96% of a dispersant and 4% to 32% of a silane carrier.

5. The composite material formulation according to claim 4, wherein the composite additive comprises 85% by weight of the dispersant and 15% by weight of the silane carrier composition.

6. The composite formulation of claim 1, wherein the polymer slurry comprises a low density sheet molding compound, a bulk molding compound, a pultrusion compound, or a casting polymer compound.

7. The composite formulation of claim 1, wherein the dispersant is an alkylamine based or a fluorocarbon based polymer.

8. A method for producing a polymer slurry mixture comprising a treated low-density filler for lightweight molded parts, the method comprising: The following steps are involved: combining 85% by weight of a dispersant with 15% by weight of a silane carrier composition to form an additive package; combining 20% ​​to 97% by weight of the compounding additive with 3% to 80% by weight of the thermoplastic resin or reactive resin to form a diluted mixture; heating the diluted mixture to form a solvated polymer mixture; combining 0.5% to 20% by weight of the solvated polymer mixture with 80% to 99.5% by weight of an untreated low density filler to form a treated low density filler; The treated low density filler is combined with a polymer slurry to form a polymer slurry mixture.

9. The method according to claim 8, wherein the method further The following steps are involved: The polymer syrup mixture is combined with additional composite materials to form a material.