Resin composition, resin molded body, and method for producing the same
By combining polyimide resin with thermoplastic or thermosetting resin at a temperature below the melting point of polyimide resin and using polyimide resin particles to disperse the filler, the problems of insufficient molding processability and mechanical properties of crystalline thermoplastic and thermosetting resins are solved, and the heat resistance and mechanical properties are improved.
Patent Information
- Application Number
- CN202080079312.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-11-19
- Filing Date
- 2020-11-17
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2040-11-17
AI Technical Summary
In the existing technology, crystalline thermoplastic polyimide resins and thermosetting resins have shortcomings in terms of molding processability and mechanical properties, making it difficult to meet the requirements of high heat resistance and lightweight.
By combining polyimide resin particles with specific particle size and structural units with thermoplastic or thermosetting resins to form a resin composition, and molding it at a temperature below the melting point of the polyimide resin, the polyimide resin particles are dispersed in the resin as fillers to improve heat resistance and mechanical properties.
While maintaining the resin's lightweight properties, it significantly improves heat resistance and mechanical properties, making it suitable for a variety of molded products and composite materials.
Smart Images

Figure CN114729187B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a resin composition, a resin molded body and a method for producing the same, and more particularly to a thermoplastic polyimide resin particle, a resin composition containing a thermoplastic resin or a thermosetting resin, a resin molded body and a method for producing the same. Background Art
[0002] Polyimide resin is a useful engineering plastic with high thermal stability, high strength, and high solvent resistance due to the rigidity, resonance stabilization, and strong chemical bonding of the molecular chain, and is used in a wide range of fields. In addition, polyimide resin with crystallinity can further improve its heat resistance, strength, and chemical resistance, and therefore, it can be expected to be used as a substitute for metals, etc. However, although polyimide resin has high heat resistance, it does not show thermoplasticity on the other hand, and there is a problem of low molding processability.
[0003] As polyimide molding materials, high heat-resistant resins such as Vespel (registered trademark) are known (Patent Document 1), but their fluidity is extremely low even at high temperatures, so they are difficult to mold and must be molded for a long time under high temperature and high pressure conditions, which is also disadvantageous in terms of cost. In contrast, if a resin having a melting point and fluidity at high temperatures, such as a crystalline resin, is used, molding can be easily and inexpensively performed.
[0004] Therefore, in recent years, polyimide resins with thermoplasticity have been reported. Thermoplastic polyimide resins have excellent molding processability in addition to the heat resistance originally possessed by polyimide resins. Therefore, thermoplastic polyimide resins can also be applied to molded bodies used in harsh environments where nylon and polyester, which are general thermoplastic resins, cannot be applied.
[0005] For example, Patent Document 2 discloses a thermoplastic polyimide resin obtained by reacting a tetracarboxylic acid and / or a derivative thereof containing at least one aromatic ring, a diamine containing at least one alicyclic hydrocarbon structure, and a chain aliphatic diamine, and containing a predetermined repeating structural unit.
[0006] In the field of engineering plastics, there is also a known technique of mixing and alloying two or more thermoplastic resins for the purpose of improving physical properties, imparting functions according to the application, etc. Patent Document 3 discloses a thermoplastic polyimide resin containing a predetermined repeating unit, and also describes a scheme of using the polyimide resin in combination with other resins as a polymer alloy.
[0007] Prior art literature
[0008] Patent Literature
[0009] Patent Document 1: Japanese Patent Application Publication No. 2005-28524
[0010] Patent Document 2: International Publication No. 2013 / 118704
[0011] Patent Document 3: International Publication No. 2016 / 147996 Summary of the invention
[0012] Problem that the invention aims to solve
[0013] As mentioned above, crystalline thermoplastic polyimide resin has high heat resistance, strength, and chemical resistance, and has a specific gravity lower than that of metal. Therefore, it can also be expected to be used as a resin modifier that can improve heat resistance, mechanical properties, etc. while maintaining the lightness derived from the resin material.
[0014] The following scheme is described in the examples of Patent Document 3: a crystalline thermoplastic polyimide resin containing a predetermined repeating unit is alloyed with a polyetheretherketone resin (PEEK) to produce a resin molded body. PEEK is a thermoplastic resin having high heat resistance like a polyimide resin, and a crystalline thermoplastic polyimide resin containing a predetermined repeating unit and PEEK are heated and melted at a temperature above the melting point of the polyimide resin, and extruded and thermoformed to produce a resin molded body.
[0015] On the other hand, no research has been conducted on using the polyimide resin to improve the properties of thermoplastic resins with lower heat resistance, such as low-melting-point crystalline thermoplastic resins or low-glass-transition-temperature amorphous thermoplastic resins, or to improve the properties of thermosetting resins.
[0016] In addition, the heat resistance of cured products of thermosetting resins is generally higher than that of thermoplastic resins, but the crosslinking density is high, so there is a tendency for toughness to decrease. In aircraft, ships, etc., the strain energy release rate (G 1c ) and other factors related to the breaking strength are taken seriously, and it is expected to maintain the heat resistance of the resin cured product and improve G 1c .
[0017] An object of the present invention is to provide a resin composition, a resin molded article, and a method for producing the same, which have improved properties such as heat resistance and mechanical properties while maintaining the lightness of a thermoplastic resin or a thermosetting resin having low heat resistance.
[0018] Solutions for solving problems
[0019] The present inventors have found that the above-mentioned problems can be solved by forming a resin composition containing a crystalline thermoplastic polyimide resin having a specific polyimide structural unit in the form of resin particles having a particle size within a specific range with respect to a thermoplastic resin or a thermosetting resin.
[0020] That is, the present invention provides the following [1] to [3].
[0021] [1] A resin composition comprising: polyimide resin particles (A); and at least one selected from the group consisting of a thermoplastic resin (B) and a thermosetting resin (C), wherein the polyimide resin particles (A) comprise a repeating structural unit represented by the following formula (1) and a repeating structural unit represented by the following formula (2), wherein the content ratio of the repeating structural unit of the formula (1) is 20 to 70 mol% relative to the total of the repeating structural unit of the formula (1) and the repeating structural unit of the formula (2), and the volume average particle size D50 is 5 to 200 μm.
[0022]
[0023] (R1 is a divalent group having 6 to 22 carbon atoms and containing at least one alicyclic hydrocarbon structure. R2 is a divalent chain aliphatic group having 5 to 16 carbon atoms. X1 and X2 are each independently a tetravalent group having 6 to 22 carbon atoms and containing at least one aromatic ring.)
[0024] [2] A resin molded body comprising: polyimide resin particles (A), and at least one selected from the group consisting of cured products of thermoplastic resins (B) and thermosetting resins (C), wherein the polyimide resin particles (A) comprise a repeating structural unit represented by the aforementioned formula (1) and a repeating structural unit represented by the aforementioned formula (2), wherein the content ratio of the repeating structural unit of the formula (1) is 20 to 70 mol% relative to the total of the repeating structural units of the formula (1) and the repeating structural units of the formula (2), and the volume average particle size D50 is 5 to 200 μm.
[0025] [3] A method for producing a resin molded body as described in [2] above, wherein the method comprises the following steps: molding a resin composition containing the aforementioned polyimide resin particles (A) and at least one selected from the group consisting of the aforementioned thermoplastic resin (B) and the aforementioned thermosetting resin (C) at a temperature lower than the melting point of the polyimide resin particles (A).
[0026] Effects of the Invention
[0027] According to the present invention, it is possible to provide a resin composition, a resin molded body and a method for producing the same, which have improved properties such as heat resistance and mechanical properties while maintaining the lightness of the resin in a thermoplastic resin such as a low-melting-point crystalline thermoplastic resin, an amorphous thermoplastic resin with a low glass transition temperature, or a thermosetting resin. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1This is a microscope photograph of the resin composition (pellets) of Example 1 observed using a field emission scanning electron microscope (FE-SEM). DETAILED DESCRIPTION
[0029] [Resin composition]
[0030] The resin composition of the present invention comprises: polyimide resin particles (A) (hereinafter, also referred to as "polyimide resin particles (A)" or "component (A)"), and at least one selected from the group consisting of a thermoplastic resin (B) and a thermosetting resin (C), wherein the polyimide resin particles (A) comprise a repeating structural unit represented by the following formula (1) and a repeating structural unit represented by the following formula (2), wherein the content ratio of the repeating structural unit of the formula (1) is 20 to 70 mol% relative to the total of the repeating structural unit of the formula (1) and the repeating structural unit of the formula (2), and the volume average particle size D50 is 5 to 200 μm.
[0031]
[0032] (R1 is a divalent group having 6 to 22 carbon atoms and containing at least one alicyclic hydrocarbon structure. R2 is a divalent chain aliphatic group having 5 to 16 carbon atoms. X1 and X2 are each independently a tetravalent group having 6 to 22 carbon atoms and containing at least one aromatic ring.)
[0033] The resin composition of the present invention comprises a polyimide resin in the form of particles having a specified D50, wherein the polyimide resin combines specific different polyimide structural units at the above-mentioned specific ratio. Thus, a resin composition and a resin molded body having improved properties such as heat resistance and mechanical properties while maintaining the lightness derived from the thermoplastic resin (B) and the thermosetting resin (C) can be obtained.
[0034] Although the reason is not clear, it is believed that the polyimide resin particles (A) dispersed in the thermoplastic resin (B), the thermosetting resin (C) or their cured products act as a resin filler, thereby obtaining an improvement effect on various properties such as heat resistance and mechanical properties. In addition, the polyimide resin particles (A) act as a resin filler, and thus an effect of improving sliding properties can also be expected.
[0035] The resin composition of the present invention is a thermoplastic resin composition or a thermosetting resin composition, and its form can be appropriately selected according to the use of any of the thermoplastic resin (B) and the thermosetting resin (C). In the case where the resin composition of the present invention is a thermoplastic resin composition containing polyimide resin particles (A) and a thermoplastic resin (B), the form of the thermoplastic resin composition is preferably a pellet from the viewpoint of operability and processability. More preferably, the thermoplastic resin composition is a pellet in which the polyimide resin particles (A) described below are dispersed in a matrix composed of a thermoplastic resin (B).
[0036] <Polyimide resin particles (A)>
[0037] From the viewpoint of improving various properties such as heat resistance and mechanical properties while maintaining the lightness derived from the thermoplastic resin (B) and the thermosetting resin (C), the resin composition of the present invention contains polyimide resin particles (A), wherein the polyimide resin particles (A) include a repeating structural unit represented by the following formula (1) and a repeating structural unit represented by the following formula (2), the content ratio of the repeating structural unit of the formula (1) relative to the total of the repeating structural unit of the formula (1) and the repeating structural unit of the formula (2) is 20 to 70 mol%, and the volume average particle size D50 is 5 to 200 μm.
[0038]
[0039] (R1 is a divalent group having 6 to 22 carbon atoms and containing at least one alicyclic hydrocarbon structure. R2 is a divalent chain aliphatic group having 5 to 16 carbon atoms. X1 and X2 are each independently a tetravalent group having 6 to 22 carbon atoms and containing at least one aromatic ring.)
[0040] The polyimide resin constituting component (A) is a thermoplastic resin, which is distinguished from a polyimide resin having no glass transition temperature (Tg) and formed by, for example, molding a polyimide precursor such as polyamic acid and then closing the imide ring, or a polyimide resin that decomposes at a temperature lower than the glass transition temperature.
[0041] The polyimide resin has crystallinity, and the degree of crystallinity can be determined based on the heat of a crystallization exothermic peak observed when the polyimide resin is melted and then cooled at a temperature drop rate of 20° C. / min (crystallization heat).
[0042] The repeating structural unit of formula (1) is described in detail below.
[0043] R1 is a divalent group having 6 to 22 carbon atoms and containing at least one alicyclic hydrocarbon structure. Here, the alicyclic hydrocarbon structure refers to a ring derived from an alicyclic hydrocarbon compound, and the alicyclic hydrocarbon compound may be saturated or unsaturated and may be monocyclic or polycyclic.
[0044] Examples of the alicyclic hydrocarbon structure include, but are not limited to, cycloalkane rings such as cyclohexane ring, cycloalkene rings such as cyclohexene, bicycloalkane rings such as norbornane ring, and bicycloalkene rings such as norbornene. Among them, cycloalkane rings are preferred, cycloalkane rings having 4 to 7 carbon atoms are more preferred, and cyclohexane rings are still more preferred.
[0045] The carbon number of R1 is 6-22, preferably 8-17.
[0046] R1 contains at least one alicyclic hydrocarbon structure, and preferably contains 1 to 3 alicyclic hydrocarbon structures.
[0047] R1 is preferably a divalent group represented by the following formula (R1-1) or (R1-2).
[0048]
[0049] (m 11 and m 12 Each independently represents an integer of 0 to 2, preferably 0 or 1. 13 ~m 15 Each independently represents an integer of 0 to 2, preferably 0 or 1.)
[0050] R1 is particularly preferably a divalent group represented by the following formula (R1-3).
[0051]
[0052] In the divalent group represented by the formula (R1-3), the positional relationship of the two methylene groups with respect to the cyclohexane ring may be cis or trans, and the ratio of cis to trans may be any value.
[0053] X1 is a tetravalent group having 6 to 22 carbon atoms and containing at least one aromatic ring. The aromatic ring may be a monocyclic ring or a condensed ring, and examples thereof include a benzene ring, a naphthalene ring, an anthracene ring, and a tetracene ring, but are not limited thereto. Among them, a benzene ring and a naphthalene ring are preferred, and a benzene ring is more preferred.
[0054] X1 has 6 to 22 carbon atoms, preferably 6 to 18 carbon atoms.
[0055] X1 contains at least one aromatic ring, preferably 1 to 3 aromatic rings.
[0056] X1 is preferably a tetravalent group represented by any of the following formulae (X-1) to (X-4).
[0057]
[0058] (R 11 ~R 18 Each is independently an alkyl group having 1 to 4 carbon atoms. 11 ~p 13 Each independently represents an integer of 0 to 2, and preferably 0. 14 、p 15 、p 16 and p 18 Each independently represents an integer of 0 to 3, and preferably 0. 17 It is an integer of 0 to 4, and preferably 0. 11 ~L 13 Each is independently a single bond, an ether group, a carbonyl group or an alkylene group having 1 to 4 carbon atoms.)
[0059] It should be noted that X1 is a tetravalent group having 6 to 22 carbon atoms and containing at least one aromatic ring. Therefore, R in formula (X-2) 12 , R 13 、p 12 and p 13 The tetravalent group represented by the formula (X-2) is selected so that the number of carbon atoms in the group falls within the range of 10 to 22.
[0060] Similarly, L in formula (X-3) 11 , R 14 , R 15 、p 14 and p 15 The tetravalent group represented by formula (X-3) is selected so that the number of carbon atoms falls within the range of 12 to 22. L in formula (X-4) 12 , L 13 , R 16 , R 17 , R 18 、p 16 、p 17 and p 18 The tetravalent group represented by the formula (X-4) is selected so that the number of carbon atoms in the group falls within the range of 18 to 22.
[0061] X1 is particularly preferably a tetravalent group represented by the following formula (X-5) or (X-6).
[0062]
[0063] Next, the repeating structural unit of formula (2) is described in detail below.
[0064] R2 is a divalent chain aliphatic group having 5 to 16 carbon atoms, preferably 6 to 14 carbon atoms, more preferably 7 to 12 carbon atoms, and further preferably 8 to 10 carbon atoms. Here, the chain aliphatic group refers to a group derived from a chain aliphatic compound, and the chain aliphatic compound may be saturated or unsaturated, may be straight chain or branched, and may contain heteroatoms such as oxygen atoms.
[0065] R2 is preferably an alkylene group having 5 to 16 carbon atoms, more preferably an alkylene group having 6 to 14 carbon atoms, still more preferably an alkylene group having 7 to 12 carbon atoms, and particularly preferably an alkylene group having 8 to 10 carbon atoms. The alkylene group may be a linear or branched chain, and is preferably a linear chain chain.
[0066] R2 is preferably at least one selected from the group consisting of an octamethylene group and a decamethylene group, and an octamethylene group is particularly preferred.
[0067] In addition, another preferred embodiment of R2 is a divalent chain aliphatic group having 5 to 16 carbon atoms including an ether group. The carbon number is preferably 6 to 14, more preferably 7 to 12, and further preferably 8 to 10. Among them, a divalent group represented by the following formula (R2-1) or (R2-2) is preferred.
[0068]
[0069] (m 21 and m 22 Each independently represents an integer of 1 to 15, preferably 1 to 13, more preferably 1 to 11, and further preferably 1 to 9. 23 ~m 25 Each independently represents an integer of 1 to 14, preferably 1 to 12, more preferably 1 to 10, and further preferably 1 to 8.)
[0070] It should be noted that R2 is a divalent chain aliphatic group having 5 to 16 carbon atoms (preferably 6 to 14 carbon atoms, more preferably 7 to 12 carbon atoms, and even more preferably 8 to 10 carbon atoms). Therefore, m in formula (R2-1) is 21 and m 22 The divalent group represented by formula (R2-1) is selected so that the number of carbon atoms in the group falls within the range of 5 to 16 (preferably 6 to 14, more preferably 7 to 12, and even more preferably 8 to 10). 21 +m 22 It is 5 to 16 (preferably 6 to 14, more preferably 7 to 12, and further preferably 8 to 10).
[0071] Similarly, m in formula (R2-2) 23 ~m 25The divalent group represented by formula (R2-2) is selected so that the number of carbon atoms falls within the range of 5 to 16 (preferably 6 to 14, more preferably 7 to 12, and even more preferably 8 to 10). 23 +m 24 +m 25 The carbon number is 5 to 16 (preferably 6 to 14 carbon atoms, more preferably 7 to 12 carbon atoms, and still more preferably 8 to 10 carbon atoms).
[0072] X2 is defined similarly to X1 in formula (1), and preferred embodiments are also the same.
[0073] The content ratio of the repeating structural unit of formula (1) is preferably 20 to 70 mol% relative to the total of the repeating structural unit of formula (1) and the repeating structural unit of formula (2). When the content ratio of the repeating structural unit of formula (1) is within the above range, the polyimide resin can be fully crystallized in a normal injection molding cycle. If the content ratio is 20 mol% or more, the molding processability is good, and if it is 70 mol% or less, good heat resistance can be maintained.
[0074] From the viewpoint of achieving high crystallinity, the content ratio of the repeating structural unit of formula (1) is preferably 65 mol% or less, more preferably 60 mol% or less, and further preferably 50 mol% or less, relative to the total of the repeating structural unit of formula (1) and the repeating structural unit of formula (2).
[0075] Among them, from the viewpoint of obtaining a resin composition having high crystallinity and better heat resistance, the content ratio of the repeating structural unit of formula (1) is preferably 20 mol% or more and less than 40 mol% relative to the total of the repeating structural unit of formula (1) and the repeating structural unit of formula (2). The above content ratio is more preferably 25 mol% or more, further preferably 30 mol% or more, and further preferably 32 mol% or more from the viewpoint of molding processability, and further preferably 35 mol% or less from the viewpoint of embodying high crystallinity.
[0076] The total content ratio of the repeating structural units of the formula (1) and the repeating structural units of the formula (2) is preferably 50 to 100 mol %, more preferably 75 to 100 mol %, further preferably 80 to 100 mol %, and further preferably 85 to 100 mol %, relative to all repeating structural units constituting the above-mentioned polyimide resin.
[0077] The polyimide resin may further contain a repeating structural unit of the following formula (3). In this case, the repeating structural unit of formula (3) preferably contains 25 mol% or less relative to the total of the repeating structural unit of formula (1) and the repeating structural unit of formula (2). On the other hand, the lower limit is not particularly limited as long as it exceeds 0 mol%.
[0078] The content ratio is preferably 5 mol % or more, more preferably 10 mol % or more from the viewpoint of improving heat resistance, and is preferably 20 mol % or less, more preferably 15 mol % or less from the viewpoint of maintaining crystallinity.
[0079]
[0080] (R3 is a divalent group having 6 to 22 carbon atoms and containing at least one aromatic ring. X3 is a tetravalent group having 6 to 22 carbon atoms and containing at least one aromatic ring.)
[0081] R3 is a divalent group having 6 to 22 carbon atoms and containing at least one aromatic ring. The aromatic ring may be a monocyclic ring or a condensed ring, and examples thereof include a benzene ring, a naphthalene ring, an anthracene ring, and a tetracene ring, but are not limited thereto. Among them, a benzene ring and a naphthalene ring are preferred, and a benzene ring is more preferred.
[0082] The carbon number of R3 is 6-22, preferably 6-18.
[0083] R3 contains at least one aromatic ring, preferably 1 to 3 aromatic rings.
[0084] In addition, a monovalent or divalent electron-withdrawing group may be bonded to the aromatic ring. Examples of the monovalent electron-withdrawing group include a nitro group, a cyano group, a p-toluenesulfonyl group, a halogen group, a haloalkyl group, a phenyl group, an acyl group, and the like. Examples of the divalent electron-withdrawing group include fluorinated alkylene groups (e.g., -C(CF3)2-, -(CF2) p -(herein, p is an integer of 1 to 10))) and other halogenated alkylene groups, such as -CO-, -SO2-, -SO-, -CONH-, and -COO- can also be mentioned.
[0085] R3 is preferably a divalent group represented by the following formula (R3-1) or (R3-2).
[0086]
[0087] (m 31 and m 32 Each independently represents an integer of 0 to 2, preferably 0 or 1. 33 and m 34 Each independently represents an integer of 0 to 2, preferably 0 or 1. 21 , R 22 and R 23 Each is independently an alkyl group having 1 to 4 carbon atoms, an alkenyl group having 2 to 4 carbon atoms, or an alkynyl group having 2 to 4 carbon atoms. 21 、p 22 and p 23 It is an integer of 0 to 4, and preferably 0. 21is a single bond, an ether group, a carbonyl group, or an alkylene group having 1 to 4 carbon atoms.
[0088] It should be noted that R3 is a divalent group having 6 to 22 carbon atoms and containing at least one aromatic ring. Therefore, m in formula (R3-1) 31 、m 32 , R 21 and p 21 The divalent group represented by the formula (R3-1) is selected so that the number of carbon atoms in the group falls within the range of 6 to 22.
[0089] Similarly, L in formula (R3-2) 21 、m 33 、m 34 , R 22 , R 23 、p 22 and p 23 The divalent group represented by the formula (R3-2) is selected so that the number of carbon atoms in the group falls within the range of 12 to 22.
[0090] X3 is defined similarly to X1 in formula (1), and preferred embodiments are also the same.
[0091] The polyimide resin may further contain a repeating structural unit represented by the following formula (4).
[0092]
[0093] (R4 is -SO2- or -Si(R x )(R y )O- divalent group, R x and R y Each independently represents a chain aliphatic group having 1 to 3 carbon atoms or a phenyl group. X4 is a tetravalent group having 6 to 22 carbon atoms and containing at least one aromatic ring.
[0094] X4 is defined similarly to X1 in formula (1), and preferred embodiments are also the same.
[0095] There is no particular restriction on the terminal structure of the polyimide resin. For example, the polyimide resin constituting the polyimide resin particles (A) may be an uncapped polyimide resin. An uncapped polyimide resin refers to a polyimide resin whose terminal structure is only a terminal amino group and a terminal carboxyl group derived from the tetracarboxylic acid component and the diamine component as its raw materials.
[0096] If the polyimide resin constituting the polyimide resin particles (A) is not end-capped, the terminal amino group and the terminal carboxyl group in the polyimide resin particles (A) can be cross-linked with the thermoplastic resin (B) or the thermosetting resin (C), and the mechanical properties such as toughness can be further improved. From this viewpoint, in the resin composition of the present invention, the polyimide resin particles (A) composed of the unend-capped polyimide resin are more preferably used in combination with the thermosetting resin (C).
[0097] On the other hand, when the polyimide resin is end-capped, the polyimide resin preferably has a chain aliphatic group having 5 to 14 carbon atoms at the end.
[0098] The chain aliphatic group may be saturated or unsaturated, and may be linear or branched. If the polyimide resin has the above-mentioned specific group at the terminal, a resin composition having excellent heat aging resistance can be obtained.
[0099] Examples of the saturated chain aliphatic group having 5 to 14 carbon atoms include n-pentyl, n-hexyl, n-heptyl, n-octyl, n-nonyl, n-decyl, n-undecyl, lauryl, n-tridecyl, n-tetradecyl, isopentyl, neopentyl, 2-methylpentyl, 2-methylhexyl, 2-ethylpentyl, 3-ethylpentyl, isooctyl, 2-ethylhexyl, 3-ethylhexyl, isononyl, 2-ethyloctyl, isodecyl, isododecyl, isotridecyl and isotetradecyl.
[0100] Examples of the unsaturated linear aliphatic group having 5 to 14 carbon atoms include 1-pentenyl, 2-pentenyl, 1-hexenyl, 2-hexenyl, 1-heptenyl, 2-heptenyl, 1-octenyl, 2-octenyl, nonenyl, decenyl, dodecenyl, tridecenyl and tetradecenyl.
[0101] Among them, the above-mentioned chain aliphatic group is preferably a saturated chain aliphatic group, and more preferably a saturated straight-chain aliphatic group. In addition, from the viewpoint of obtaining heat aging resistance, the above-mentioned chain aliphatic group preferably has a carbon number of 6 or more, more preferably a carbon number of 7 or more, and further preferably a carbon number of 8 or more, and preferably has a carbon number of 12 or less, more preferably a carbon number of 10 or less, and further preferably a carbon number of 9 or less. The above-mentioned chain aliphatic group may be only one kind, or may be two or more kinds.
[0102] The above-mentioned chain aliphatic group is particularly preferably at least one selected from the group consisting of n-octyl, isooctyl, 2-ethylhexyl, n-nonyl, isononyl, n-decyl, and isodecyl, further preferably at least one selected from the group consisting of n-octyl, isooctyl, 2-ethylhexyl, n-nonyl, and isononyl, and most preferably at least one selected from the group consisting of n-octyl, isooctyl, and 2-ethylhexyl.
[0103] Furthermore, when the polyimide resin has a chain aliphatic group having 5 to 14 carbon atoms at the terminal, it is preferred that the terminal has only a chain aliphatic group having 5 to 14 carbon atoms in addition to a terminal amino group and a terminal carboxyl group from the viewpoint of heat aging resistance. When a group other than the above is present at the terminal, the content thereof is preferably 10 mol% or less, more preferably 5 mol% or less, relative to the chain aliphatic group having 5 to 14 carbon atoms.
[0104] When the polyimide resin has a carbon chain aliphatic group having 5 to 14 carbon atoms at the terminal, the content of the carbon chain aliphatic group having 5 to 14 carbon atoms in the polyimide resin is preferably 0.01 mol% or more, more preferably 0.1 mol% or more, and further preferably 0.2 mol% or more, relative to 100 mol% of the total of all repeating structural units constituting the polyimide resin, from the viewpoint of exhibiting excellent heat aging resistance. In addition, in order to ensure a sufficient molecular weight and obtain good mechanical properties, the content of the carbon chain aliphatic group having 5 to 14 carbon atoms in the polyimide resin is preferably 10 mol% or less, more preferably 6 mol% or less, and further preferably 3.5 mol% or less, relative to 100 mol% of the total of all repeating structural units constituting the polyimide resin.
[0105] The content of the linear aliphatic group having 5 to 14 carbon atoms in the polyimide resin can be determined by depolymerizing the polyimide resin.
[0106] The polyimide resin preferably has a melting point of 360° C. or lower and a glass transition temperature of 150° C. or higher.
[0107] The melting point of the polyimide resin is preferably 280° C. or higher, more preferably 290° C. or higher from the viewpoint of heat resistance, and is more preferably 345° C. or lower, further preferably 340° C. or lower, and further preferably 335° C. or lower from the viewpoint of achieving high molding processability.
[0108] The glass transition temperature of the polyimide resin is preferably 160°C or higher, further preferably 170°C or higher, from the viewpoint of heat resistance, and is preferably 250°C or lower, more preferably 230°C or lower, further preferably 200°C or lower, from the viewpoint of achieving high molding processability.
[0109] Furthermore, for the polyimide resin, from the viewpoint of improving crystallinity, heat resistance, mechanical strength, and chemical resistance, the heat of the crystallization exothermic peak observed when the polyimide resin is melted and cooled at a temperature drop rate of 20° C. / min (hereinafter, also referred to as “crystallization exothermic heat”) is preferably 5.0 mJ / mg or more, more preferably 10.0 mJ / mg or more, and further preferably 17.0 mJ / mg or more, as measured by a differential scanning calorimeter. The upper limit of the crystallization exothermic heat is not particularly limited, but is usually 45.0 mJ / mg or less.
[0110] The melting point, glass transition temperature and crystallization heat of the polyimide resin can be measured using a differential scanning calorimeter, and specifically, can be measured by the method described in Examples.
[0111] The logarithmic viscosity of the 5 mass % concentrated sulfuric acid solution of the polyimide resin at 30°C is preferably in the range of 0.2 to 2.0 dL / g, more preferably 0.3 to 1.8 dL / g. If the logarithmic viscosity is above 0.2 dL / g, sufficient mechanical strength can be obtained when the obtained resin composition is made into a molded body, and if it is below 2.0 dL / g, the molding processability and operability become good. The logarithmic viscosity μ is obtained as follows: using a Cannon-Fenske viscometer, the time for concentrated sulfuric acid and the polyimide resin solution to flow at 30°C are measured respectively, and the logarithmic viscosity μ is obtained by the following formula.
[0112] μ=ln(ts / t0) / C
[0113] t0: time for concentrated sulfuric acid to flow
[0114] ts: Flow time of polyimide resin solution
[0115] C: 0.5 (g / dL)
[0116] The weight average molecular weight Mw of the polyimide resin constituting the polyimide resin particles (A) is preferably 10,000 to 150,000, more preferably 15,000 to 100,000, further preferably 20,000 to 80,000, further preferably 30,000 to 70,000, further preferably 35,000 to 65,000. In addition, when the weight average molecular weight Mw of the polyimide resin is 10,000 or more, the mechanical strength of the obtained molded body becomes good, when it is 40,000 or more, the mechanical strength stability becomes good, and when it is 150,000 or less, the molding processability becomes good.
[0117] The weight average molecular weight Mw of the polyimide resin can be measured by gel filtration chromatography (GPC) using polymethyl methacrylate (PMMA) as a standard sample.
[0118] (Volume average particle size D50)
[0119] The polyimide resin particles (A) have a volume average particle size D50 of 5 to 200 μm, more preferably 5 to 150 μm, further preferably 5 to 100 μm, and further preferably 5 to 40 μm, from the viewpoint of obtaining a resin composition and a resin molded product having improved properties such as heat resistance and mechanical properties while maintaining the lightness derived from the thermoplastic resin (B) and the thermosetting resin (C), and from the viewpoint of dispersibility.
[0120] D50 of the polyimide resin particles (A) can be measured by a laser diffraction light scattering particle size distribution analyzer, and specifically, can be measured by the method described in Examples.
[0121] The shape of the polyimide resin particles (A) is not particularly limited, preferably porous. If the polyimide resin particles (A) are porous, the heat resistance, mechanical properties and other characteristics of the resin composition and the resin molded body obtained can be improved, and further lightweight. In addition, it is also possible to expect the low dielectric constant of the resin composition and the resin molded body. From the viewpoint of obtaining these effects, the polyimide resin particles (A) are preferably present in the resin composition and the resin molded body in the state of porous particles. Therefore, as described later, preferably in the case of not applying the thermal history above the melting point of the polyimide resin particles (A), the resin composition and the resin molded body are manufactured. It should be noted that "in the case of not applying the thermal history above the melting point of the polyimide resin particles (A), the resin composition and the resin molded body" refers to, when manufacturing the resin composition and the resin molded body of the present invention, all manufacturing processes are carried out under the temperature condition lower than the melting point of the polyimide resin particles (A).
[0122] The fact that the polyimide resin particles (A) are porous can be confirmed by observation using a scanning electron microscope (SEM).
[0123] In addition, the polyimide resin particles (A) can be produced by the production method described later to adjust the D50 of the polyimide resin particles (A) to the above range and to have a porous state.
[0124] (proportion)
[0125] From the viewpoint of obtaining a resin composition and a resin molded product having improved properties such as heat resistance and mechanical properties while maintaining the lightness derived from the thermoplastic resin (B) and the thermosetting resin (C), the specific gravity of the polyimide resin particles (A) is preferably 0.8 to 1.7, more preferably 0.9 to 1.5, further preferably 1.0 to 1.4, and further preferably 1.05 to 1.25.
[0126] The specific gravity of the polyimide resin particles (A) is a value measured at 23° C., and can be specifically measured by the method described in Examples.
[0127] (True density)
[0128] From the viewpoint of obtaining a resin composition and a resin molded product having improved properties such as heat resistance and mechanical properties while maintaining the lightness derived from the thermoplastic resin (B) and the thermosetting resin (C), the true density of the polyimide resin particles (A) measured by a gas phase method is preferably 1.0 to 1.8 g / cm 3 , more preferably 1.1 to 1.6 g / cm 3 , more preferably 1.2 to 1.5 g / cm 3 From the above viewpoints, the true density of the polyimide resin particles (A) measured by a liquid phase method is preferably 0.8 to 1.7 g / cm 3 , more preferably 0.9 to 1.5 g / cm 3 , more preferably 1.0 to 1.4 g / cm 3 .
[0129] The true density measurement by the gas phase method can be performed in accordance with the "Determination of density and specific gravity by gas replacement method" specified in JIS Z8807: 2012. Furthermore, the true density measurement by the liquid phase method (densimeter method) can be performed using n-butanol as the medium solution and a wet true density measuring instrument.
[0130] The true density can be specifically measured by the method described in the Examples.
[0131] Furthermore, the difference (D1-D2) between the true density D1 measured by a gas phase method and the true density D2 measured by a liquid phase method of the polyimide resin particles (A) is preferably 0.05 to 0.7 g / cm 3 , more preferably 0.08 to 0.5 g / cm 3 , more preferably 0.08 to 0.4 g / cm 3 It is speculated that (D1-D2) indicates the presence of fine pores into which the medium solution used in the true density measurement by the liquid phase method cannot enter.
[0132] (Specific surface area)
[0133] From the viewpoint of workability and obtaining a resin composition having excellent fluidity, the specific surface area of the polyimide resin particles (A) is preferably 1.0 to 50 m 2 / g, more preferably 2.0 to 40 m 2 / g, more preferably 5.0 to 25 m 2It is estimated that both D50 and pore volume of the polyimide resin particles (A) have an influence on the above-mentioned specific surface area.
[0134] The above-mentioned specific surface area can be obtained by the BET method, and specifically, can be measured by the method described in Examples.
[0135] (Total pore volume)
[0136] When the polyimide resin particles (A) are porous, the total pore volume is preferably 0.005 to 0.50 cc / g, more preferably 0.01 to 0.30 cc / g, and further preferably 0.015 to 0.20 cc / g, from the viewpoint of obtaining a resin composition and a resin molded body having improved properties such as heat resistance and mechanical properties while maintaining the lightness derived from the thermoplastic resin (B) and the thermosetting resin (C).
[0137] Specifically, the total pore volume can be measured by the method described in Examples.
[0138] (Average hole diameter)
[0139] When the polyimide resin particles (A) are porous, the average pore diameter is preferably 5 to 85 nm, more preferably 10 to 80 nm, and further preferably 20 to 70 nm, from the viewpoint of obtaining a resin composition and a resin molded body having improved properties such as heat resistance and mechanical properties while maintaining the lightness derived from the thermoplastic resin (B) and the thermosetting resin (C).
[0140] Specifically, the average pore diameter can be measured by the method described in Examples.
[0141] The aforementioned D50, specific gravity, true density, specific surface area, total pore volume and average pore diameter of the polyimide resin particles (A) are preferably the values measured using the polyimide resin particles (A) before being mixed with the resin composition and the resin molded body, which are in the aforementioned range. It should be noted that it is considered that: in the present invention, when the resin composition and the resin molded body are manufactured without applying a thermal history above the melting point of the polyimide resin particles (A), the shape of the polyimide resin particles (A) in the resin composition and the resin molded body can maintain the shape of the polyimide resin particles (A) used as long as there is no deformation caused by shear stress. "The shape of the polyimide resin particles (A) used" refers to the D50 and porous state of the polyimide resin particles (A) before being mixed with the resin composition and the resin molded body.
[0142] (Method for producing polyimide resin particles (A))
[0143] The polyimide resin particles (A) can be produced by reacting a tetracarboxylic acid component containing a tetracarboxylic acid having at least one aromatic ring and / or a derivative thereof with a diamine component containing a diamine having at least one alicyclic hydrocarbon structure and a chain aliphatic diamine.
[0144] The tetracarboxylic acid containing at least one aromatic ring is preferably a compound obtained by directly bonding four carboxyl groups to the aromatic ring, and may contain an alkyl group in the structure. Moreover, the aforementioned tetracarboxylic acid preferably has 6 to 26 carbon atoms. As the aforementioned tetracarboxylic acid, pyromellitic acid, 2,3,5,6-toluenetetracarboxylic acid, 3,3',4,4'-benzophenonetetracarboxylic acid, 3,3',4,4'-biphenyltetracarboxylic acid, 1,4,5,8-naphthalenetetracarboxylic acid, etc. are preferred. Among them, pyromellitic acid is more preferred.
[0145] As the derivative of tetracarboxylic acid containing at least one aromatic ring, anhydride or alkyl ester of tetracarboxylic acid containing at least one aromatic ring can be mentioned. The above-mentioned tetracarboxylic acid derivative preferably has a carbon number of 6 to 38. As the anhydride of tetracarboxylic acid, pyromellitic acid monoanhydride, pyromellitic acid dianhydride, 2,3,5,6-toluenetetracarboxylic dianhydride, 3,3',4,4'-diphenylsulfonetetracarboxylic dianhydride, 3,3',4,4'-benzophenonetetracarboxylic dianhydride, 3,3',4,4'-biphenyltetracarboxylic dianhydride, 1,4,5,8-naphthalenetetracarboxylic dianhydride, etc. can be mentioned. Examples of the alkyl esters of tetracarboxylic acids include dimethyl pyromellitate, diethyl pyromellitate, dipropyl pyromellitate, diisopropyl pyromellitate, dimethyl 2,3,5,6-toluenetetracarboxylate, dimethyl 3,3',4,4'-diphenylsulfonetetracarboxylate, dimethyl 3,3',4,4'-benzophenonetetracarboxylate, dimethyl 3,3',4,4'-biphenyltetracarboxylate, and dimethyl 1,4,5,8-naphthalenetetracarboxylate. In the alkyl esters of the tetracarboxylic acids, the number of carbon atoms in the alkyl group is preferably 1 to 3.
[0146] As the tetracarboxylic acid and / or its derivative containing at least one aromatic ring, at least one compound selected from the above may be used alone or in combination of two or more compounds.
[0147] The carbon number of the diamine containing at least one alicyclic hydrocarbon structure is preferably 6 to 22, and examples thereof include 1,2-bis(aminomethyl)cyclohexane, 1,3-bis(aminomethyl)cyclohexane, 1,4-bis(aminomethyl)cyclohexane, 1,2-cyclohexanediamine, 1,3-cyclohexanediamine, 1,4-cyclohexanediamine, 4,4'-diaminodicyclohexylmethane, 4,4'-methylenebis(2-methylcyclohexylamine), carvonediamine, limonenediamine, isophoronediamine, norbornanediamine, bis(aminomethyl)tricyclo[5.2.1.0 2,6] decane, 3,3'-dimethyl-4,4'-diaminodicyclohexylmethane, 4,4'-diaminodicyclohexylpropane, etc. These compounds can be used alone or in combination with two or more compounds selected from them. Among them, 1,3-bis(aminomethyl)cyclohexane can be used appropriately. It should be noted that the diamines containing alicyclic hydrocarbon structures usually have structural isomers, but the ratio of cis-isomers / trans-isomers is not limited.
[0148] The chain aliphatic diamine may be straight chain or branched, and the carbon number is preferably 5 to 16, more preferably 6 to 14, and further preferably 7 to 12. In addition, if the carbon number of the chain part is 5 to 16, an ether bond may be included therebetween. As the chain aliphatic diamine, for example, 1,5-pentamethylenediamine, 2-methylpentane-1,5-diamine, 3-methylpentane-1,5-diamine, 1,6-hexamethylenediamine, 1,7-heptamethylenediamine, 1,8-octamethylenediamine, 1,9-nonamethylenediamine, 1,10-decamethylenediamine, 1,11-undemethylenediamine, 1,12-dodecamethylenediamine, 1,13-tridecamethylenediamine, 1,14-tetradecamethylenediamine, 1,16-hexadecamethylenediamine, 2,2'-(ethylenedioxy)bis(ethylamine) and the like are preferred.
[0149] The chain aliphatic diamine may be used alone or in combination of two or more. Among them, chain aliphatic diamines having 8 to 10 carbon atoms are preferably used, and at least one selected from the group consisting of 1,8-octamethylenediamine and 1,10-decamethylenediamine is particularly preferably used.
[0150] When the polyimide resin particles (A) are produced, the molar ratio of the amount of the diamine containing at least one alicyclic hydrocarbon structure to be charged is preferably 20 to 70 mol% relative to the total amount of the diamine containing at least one alicyclic hydrocarbon structure and the chain aliphatic diamine. The molar amount is more preferably 25 mol% or more, further preferably 30 mol% or more, and further preferably 32 mol% or more. From the viewpoint of achieving high crystallinity, it is more preferably 60 mol% or less, further preferably 50 mol% or less, further preferably less than 40 mol%, and further preferably 35 mol% or less.
[0151] The diamine component may contain a diamine containing at least one aromatic ring. The diamine containing at least one aromatic ring preferably has 6 to 22 carbon atoms, and examples thereof include o-phenylenediamine, m-phenylenediamine, p-phenylenediamine, 1,2-diethynylphenylenediamine, 1,3-diethynylphenylenediamine, 1,4-diethynylphenylenediamine, 1,2-diaminobenzene, 1,3-diaminobenzene, 1,4-diaminobenzene, 4,4'-diaminodiphenyl ether, 3,4'-diaminodiphenyl ether, 4,4'-diaminodiphenylmethane, α,α'-bis(4-aminophenyl)1,4-diisopropylbenzene, α,α'-bis(3-aminophenyl)-1,4-diisopropylbenzene, 2,2-bis[4-(4-aminophenoxy)phenyl]propane, 2,6-diaminonaphthalene, and 1,5-diaminonaphthalene.
[0152] In the above, the molar ratio of the amount of the diamine containing at least one aromatic ring to be charged is preferably 25 mol% or less relative to the total amount of the diamine containing at least one alicyclic hydrocarbon structure and the chain aliphatic diamine.
[0153] The molar ratio is preferably 5 mol% or more, more preferably 10 mol% or more from the viewpoint of improving heat resistance, and is preferably 20 mol% or less, more preferably 15 mol% or less from the viewpoint of maintaining crystallinity.
[0154] From the viewpoint of reducing coloration of the polyimide resin particles (A), the molar ratio is preferably 12 mol% or less, more preferably 10 mol% or less, further preferably 5 mol% or less, and further preferably 0 mol%.
[0155] When producing the polyimide resin particles (A), the charging amount ratio of the tetracarboxylic acid component to the diamine component is preferably 0.9 to 1.1 mol of the diamine component relative to 1 mol of the tetracarboxylic acid component.
[0156] Moreover, when manufacturing the polyimide resin particles (A), in addition to the aforementioned tetracarboxylic acid component and the aforementioned diamine component, an end-capping agent may also be mixed. As the end-capping agent, at least one selected from the group consisting of monoamines and dicarboxylic acids is preferred. When using an end-capping agent, the amount used is as long as the amount of the end group that can be introduced into the polyimide resin constituting the polyimide resin particles (A) can be an amount, relative to 1 mol of the aforementioned tetracarboxylic acid and / or its derivative, preferably 0.0001 to 0.1 mol, more preferably 0.001 to 0.06 mol, further preferably 0.002 to 0.035 mol, further preferably 0.002 to 0.020 mol, further preferably 0.002 to 0.012 mol.
[0157] Among them, as the end-capping agent, a monoamine end-capping agent is preferred. From the viewpoint of introducing the aforementioned chain aliphatic group having 5 to 14 carbon atoms into the terminal of the polyimide resin constituting the polyimide resin particles (A) to improve the heat aging resistance, a monoamine having a chain aliphatic group having 5 to 14 carbon atoms is more preferred, and a monoamine having a saturated straight-chain aliphatic group having 5 to 14 carbon atoms is further preferred.
[0158] The blocking agent is particularly preferably at least one selected from the group consisting of n-octylamine, isooctylamine, 2-ethylhexylamine, n-nonylamine, isononylamine, n-decylamine, and isodecylamine, further preferably at least one selected from the group consisting of n-octylamine, isooctylamine, 2-ethylhexylamine, n-nonylamine, and isononylamine, and most preferably at least one selected from the group consisting of n-octylamine, isooctylamine, and 2-ethylhexylamine.
[0159] As the polymerization method for producing the polyimide resin particles (A), known polymerization methods can be applied without particular limitation, and examples thereof include solution polymerization, melt polymerization, solid phase polymerization, suspension polymerization, and the like. Among them, suspension polymerization under high temperature conditions using an organic solvent is particularly preferred. When suspension polymerization is performed under high temperature conditions, the polymerization is preferably performed at 150° C. or higher, and more preferably at 180 to 250° C. The polymerization time can be appropriately selected according to the monomers used, but is preferably about 0.1 to 6 hours.
[0160] The method for producing polyimide resin particles (A) preferably includes the step of reacting the tetracarboxylic acid component and the diamine component in the presence of a solvent containing an alkylene glycol solvent represented by the following formula (I). In this way, porous polyimide resin particles having a D50 of 5 to 200 μm can be easily obtained.
[0161]
[0162] (Ra1 is a hydrogen atom or an alkyl group having 1 to 4 carbon atoms, Ra2 is a linear alkylene group having 2 to 6 carbon atoms, and n is an integer of 1 to 3.)
[0163] Ra1 in formula (I) is a hydrogen atom or an alkyl group having 1 to 4 carbon atoms, preferably an alkyl group having 1 to 4 carbon atoms, and more preferably a methyl group or an ethyl group.
[0164] Ra2 in the formula (I) is a linear alkylene group having 2 to 6 carbon atoms, preferably a linear alkylene group having 2 to 3 carbon atoms, and more preferably an ethylene group.
[0165] In the formula (I), n is an integer of 1 to 3, and preferably 2 or 3.
[0166] As specific examples of the aforementioned alkylene glycol-based solvents, ethylene glycol monomethyl ether, diethylene glycol monomethyl ether (another name: 2-(2-methoxyethoxy) ethanol), triethylene glycol monomethyl ether, ethylene glycol monoethyl ether, diethylene glycol monoethyl ether (another name: 2-(2-ethoxyethoxy) ethanol), ethylene glycol monoisopropyl ether, diethylene glycol monoisopropyl ether, triethylene glycol monoisopropyl ether, ethylene glycol monobutyl ether, diethylene glycol monobutyl ether, triethylene glycol monobutyl ether, ethylene glycol monoisobutyl ether, diethylene glycol monoisobutyl ether, ethylene glycol monoisobutyl ether, ethylene glycol, 1,3-propylene glycol, etc. can be cited. These solvents can be used alone or in combination with two or more solvents selected from them. Among these solvents, it is preferred to select at least one of the group consisting of 2-(2-methoxyethoxy) ethanol, triethylene glycol monomethyl ether, 2-(2-ethoxyethoxy) ethanol and 1,3-propylene glycol.
[0167] As a suitable method for producing the polyimide resin particles (A), for example, there can be mentioned a method in which a solution (a) comprising a tetracarboxylic acid component in a solvent comprising the above-mentioned alkylene glycol-based solvent and a solution (b) comprising a diamine component in a solvent comprising the above-mentioned alkylene glycol-based solvent are separately prepared, and then the solution (b) is added to the solution (a), or the solution (a) is added to the solution (b) to prepare a solution (c) containing a polyamic acid, and then the solution (c) is heated to imidize the polyamic acid and precipitate the polyimide resin particles in the solution (c), thereby obtaining the polyimide resin particles (A).
[0168] The reaction of the tetracarboxylic acid component and the diamine component may be performed under normal pressure or under pressure, but is preferably performed under normal pressure because a pressure-resistant container is not required.
[0169] When a capping agent is used, it is preferred to mix solution (a) and solution (b), mix the capping agent in the mixed solution to prepare a solution (c) containing polyamic acid, and then heat the solution (c). It is more preferred to add the capping agent to solution (a) after the solution (b) is added to prepare a solution (c) containing polyamic acid, and then heat the solution (c).
[0170] <Thermoplastic resin (B)>
[0171] The thermoplastic resin (B) (hereinafter also referred to as "component (B)") is a thermoplastic resin other than the above-mentioned component (A).
[0172] When the polyimide resin particles (A) are produced, they can be contained in the resin composition and the resin molded body in a state of maintaining the shape of the polyimide resin particles (A) used, without applying a thermal history above the melting point, as long as there is no deformation caused by shear stress. From this viewpoint, the thermoplastic resin (B) is preferably at least one selected from the group consisting of the following (B1) and (B2).
[0173] (B1) Amorphous thermoplastic resin having a glass transition temperature lower than the melting point of the polyimide resin particles (A)
[0174] (B2) a crystalline thermoplastic resin having a melting point lower than that of the polyimide resin particles (A) or a glass transition temperature lower than that of the polyimide resin particles (A)
[0175] It should be noted that in this specification, "amorphous thermoplastic resin" refers to a thermoplastic resin having a glass transition temperature but no melting point, and "thermoplastic resin without melting point" more specifically refers to a thermoplastic resin having a crystallization exothermic peak heat (crystallization heat) of less than 5 mJ / mg when the resin is melted and then cooled at a temperature drop rate of 20°C / min as measured by a differential scanning calorimeter. Furthermore, "crystalline thermoplastic resin" refers to a thermoplastic resin having a melting point and a crystallization heat of 5 mJ / mg or more.
[0176] (Amorphous thermoplastic resin (B1))
[0177] When the thermoplastic resin (B) is an amorphous thermoplastic resin, it is preferably an amorphous thermoplastic resin (B1) (hereinafter also referred to as "amorphous thermoplastic resin (B1)" or "component (B1)") having a glass transition temperature lower than the melting point of the polyimide resin particles (A). Component (B1) can be melted and molded at a temperature lower than the melting point of component (A), so a resin composition and a resin molded body can be obtained in which the shape of the component (A) used is maintained.
[0178] As component (B1), for example, polystyrene resin; polyvinyl chloride; polyvinylidene chloride; polymethyl methacrylate; acrylonitrile-butadiene-styrene resin; polycarbonate resin; polysulfone resin; polyphenylsulfone resin; polyarylate resin; polyphenylene ether resin; polyethersulfone resin; polyetherimide resin; polyamideimide resin; polyurethane resin; and the like, and a non-crystalline thermoplastic resin having a glass transition temperature lower than the melting point of component (A). These may be used alone or in combination of two or more.
[0179] From the viewpoint of making it easy to include the component (A) in the resin composition and the resin molded article while maintaining the shape of the component (A) used, the melting point of the component (A) is set to Tm A (°C), the glass transition temperature Tg of component (B1) B1 (℃) preferably (Tm A -30)°C or less, preferably (Tm A -50)°C or less, more preferably (Tm A -100)℃ or less. Glass transition temperature Tg B1 The lower limit of Tg is not particularly limited, and may be, for example, -125°C or higher. B1 It is preferably -50°C or higher, more preferably 0°C or higher, and further preferably 50°C or higher.
[0180] (Crystalline thermoplastic resin (B2))
[0181] When the thermoplastic resin (B) is a crystalline thermoplastic resin, it is preferably a crystalline thermoplastic resin (B2) (hereinafter also referred to as "crystalline thermoplastic resin (B2)" or "component (B2)") having a melting point lower than the melting point of the polyimide resin particles (A) or a glass transition temperature lower than the glass transition temperature of the polyimide resin particles (A). Component (B2) can also be melted and molded at a temperature lower than the melting point of component (A) or a temperature lower than the glass transition temperature. Therefore, component (A) can be contained in the resin composition and the resin molded body in a state where the shape of component (A) used is maintained.
[0182] As component (B2), for example, polyolefin resins such as polyethylene, polypropylene, and cyclic polyolefins; polyamide resins; polyacetal resins; polyphenylene sulfide resins; polyester resins such as polyethylene terephthalate, polyethylene naphthalate, polycyclohexylene dimethylene terephthalate, and polyglycolic acid; liquid crystal polymers; fluororesins such as polytetrafluoroethylene and polyvinylidene fluoride; polymethylpentene resins; polyurethane resins; and crystalline thermoplastic resins having a glass transition temperature lower than the glass transition temperature of component (A) or a melting point lower than the melting point of component (A) can be mentioned. These can be used alone or in combination of two or more.
[0183] Melting point Tm of component (B2) B2 The temperature (°C) is not particularly limited as long as it is lower than the melting point of component (A), but is preferably 320°C or lower, more preferably 300°C or lower, further preferably 280°C or lower, and further preferably 250°C or lower from the viewpoint of moldability. Melting point Tm B2The lower limit of is also not particularly limited, but from the viewpoint of heat resistance, it is preferably 50° C. or higher, more preferably 100° C. or higher, further preferably 120° C. or higher, and further preferably 140° C. or higher.
[0184] Furthermore, the glass transition temperature Tg of component (B2) B2 The temperature (°C) is not particularly limited as long as it is lower than the glass transition temperature of component (A), but is preferably 170°C or lower, more preferably 150°C or lower, further preferably 120°C or lower, and further preferably 100°C or lower from the viewpoint of moldability. B2 The lower limit of Tg is not particularly limited, and can be, for example, -125°C or higher. B2 It is preferably -50°C or higher, more preferably -20°C or higher, and further preferably 0°C or higher.
[0185] As the thermoplastic resin (B) used in the present invention, one or more species selected from the group consisting of the components (B1) and (B2) can be used.
[0186] From the viewpoint of including the component (A) in the resin composition and the resin molded article while maintaining the shape of the component (A) to be used, and from the viewpoint of improving heat resistance, mechanical properties, etc., the thermoplastic resin (B) is preferably selected from polystyrene resins, polyvinyl chloride, polyvinylidene chloride, polymethyl methacrylate, acrylonitrile-butadiene-styrene resins, polycarbonate resins, polysulfone resins, polyphenylsulfone resins, polyarylate resins, polyphenylene ether resins, polyethersulfone resins, polyetherimide resins, polyamideimide resins, polyolefin resins, polyamide resins, polyacetal resins, polyphenylene sulfide resins, polyester resins, liquid crystal polymers, fluororesins, polymethylpentene resins, and polyurethanes. At least one selected from the group consisting of resins, more preferably at least one selected from the group consisting of polystyrene resins, polyvinyl chloride, polyvinylidene chloride, polymethyl methacrylate, acrylonitrile-butadiene-styrene resins, polycarbonate resins, polyphenylene sulfone resins, polyphenylene ether resins, polyether sulfone resins, polyetherimide resins, polyamideimide resins, polyolefin resins, polyamide resins, polyacetal resins, polyphenylene sulfide resins, polyester resins, fluororesins, and polyurethane resins, further preferably at least one selected from the group consisting of polycarbonate resins, polyolefin resins, polyamide resins, and polyphenylene sulfide resins, further preferably polyolefin resins, and further preferably polypropylene resins.
[0187] In addition, the terminal amino group may remain in the polyimide resin particles (A), and if a thermoplastic resin (B) having a structure capable of reacting with the terminal amino group is used, the toughness of the obtained resin composition and resin molded product can be improved. From this viewpoint, the thermoplastic resin (B) is preferably at least one selected from the group consisting of polyamide resins and polyamide-imide resins, and more preferably a polyamide resin.
[0188] The improvement in toughness here means that the elongation until the resin molded body breaks when tensile stress is applied thereto becomes larger, and can be evaluated by, for example, measuring the tensile breaking strain.
[0189] Examples of the polyamide resin used as the thermoplastic resin (B) include aromatic ring-containing polyamides and aliphatic polyamides.
[0190] As the aromatic ring-containing polyamide, from the viewpoint of satisfying the characteristics of the aforementioned component (B2), a polyamide derived from an aromatic ring-containing diamine and an aliphatic dicarboxylic acid is preferred, and examples thereof include polymeta-phenylenediamine adipamide (MXD6), polymeta-phenylenediamine sebacate (MXD10), polypara-phenylenediamine adipamide (PXD6), polypara-phenylenediamine sebacate (PXD10), polymeta-phenylenediamine adipamide / para-phenylenediamine adipamide (MPXD6), and polymeta-phenylenediamine sebacate / para-phenylenediamine sebacate (MPXD10), and one or more thereof can be used.
[0191] Examples of aliphatic polyamides include polycaproamide (polyamide 6), polyhexamethylene adipamide (polyamide 66), polyundecanamide (polyamide 11), polydodecaneamide (polyamide 12), and polyhexamethylene dodecanamide (polyamide 612). One or more of these may be used.
[0192] Among the above, aliphatic polyamides are more preferred from the viewpoint of obtaining a toughness improvement effect in the obtained resin composition and resin molded article.
[0193] <Thermosetting resin (C)>
[0194] The thermosetting resin (C) (hereinafter also referred to as "component (C)") is not particularly limited as long as it is a thermosetting resin that can disperse the polyimide resin particles (A), and for example, at least one selected from the group consisting of epoxy resins, phenolic resins, urea resins, melamine resins, unsaturated polyimide resins, bismaleimide resins, silicone resins, carbamate resins, casein resins, furan resins, alkyd resins, and xylene resins can be cited. Among them, from the viewpoint of being included in the resin composition and the resin molded body in a state of maintaining the shape of the component (A) used, and from the viewpoint of the dispersibility of the component (A), the component (C) is preferably at least one selected from the group consisting of epoxy resins, carbamate resins, and bismaleimide resins, more preferably at least one selected from the group consisting of epoxy resins and carbamate resins, and even more preferably epoxy resins.
[0195] The epoxy resin used as the component (C) may be a two-component curing type epoxy resin composition containing an epoxy group-containing compound as a main component and a curing agent.
[0196] The epoxy group-containing compound as the main agent is preferably a polyfunctional epoxy compound having two or more epoxy groups. From the viewpoint of the mechanical strength of the cured product, the polyfunctional epoxy compound is more preferably a polyfunctional epoxy compound containing an aromatic ring or an alicyclic structure in the molecule.
[0197] Specific examples of the polyfunctional epoxy compound include a polyfunctional epoxy compound having a glycidylamino group derived from m-phenylenediamine; a polyfunctional epoxy compound having a glycidylamino group derived from p-phenylenediamine; a polyfunctional epoxy compound having a glycidylamino group derived from 1,3-bis(aminomethyl)cyclohexane; a polyfunctional epoxy compound having a glycidylamino group derived from 1,4-bis(aminomethyl)cyclohexane; a polyfunctional epoxy compound having a glycidylamino group derived from diaminodiphenylmethane such as tetraglycidyldiaminodiphenylmethane; The present invention also includes a polyfunctional epoxy compound having a glycidylamino group; a polyfunctional epoxy compound having a glycidylamino group and / or a glycidyloxy group derived from p-aminophenol; a polyfunctional epoxy compound having a glycidyloxy group derived from bisphenol A such as bisphenol A diglycidyl ether; a polyfunctional epoxy compound having a glycidyloxy group derived from bisphenol F such as bisphenol F diglycidyl ether; a polyfunctional epoxy compound having a glycidyloxy group derived from phenol novolac; and a polyfunctional epoxy compound having a glycidyloxy group derived from resorcinol; etc. The above-mentioned polyfunctional epoxy compounds may be used in combination of two or more.
[0198] Among the above, from the viewpoint of obtaining a cured product having high heat resistance, the polyfunctional epoxy compound used as the main agent is preferably at least one selected from the group consisting of a polyfunctional epoxy compound having a glycidylamino group derived from m-xylylenediamine, a polyfunctional epoxy compound having a glycidylamino group derived from p-xylylenediamine, a polyfunctional epoxy compound having a glycidylamino group derived from diaminodiphenylmethane, a polyfunctional epoxy compound having a glycidyloxy group derived from bisphenol A, and a polyfunctional epoxy compound having a glycidyloxy group derived from bisphenol F as the main component. From the viewpoint of obtaining a cured product having high heat resistance, and from the viewpoint of availability and economic efficiency, a polyfunctional epoxy compound having a glycidylamino group derived from diaminodiphenylmethane such as tetraglycidyldiaminodiphenylmethane is more preferred.
[0199] The curing agent used in the epoxy resin composition may have two or more active hydrogen atoms that can react with the epoxy group in the main agent, and is preferably a polyamine compound or a modified product thereof from the viewpoint of curability.
[0200] Specifically, there can be mentioned chain aliphatic polyamine compounds such as ethylenediamine, diethylenetriamine, triethylenetetramine, tetraethylenepentamine, pentaethylenehexamine, hexamethylenediamine, 2-methylpentamethylenediamine, and trimethylhexamethylenediamine; 1,2-bis(aminomethyl)cyclohexane, 1,3-bis(aminomethyl)cyclohexane, 1,4-bis(aminomethyl)cyclohexane, menthanediamine, isophoronediamine, norbornanediamine, tricyclodecanediamine, adamantanediamine, diaminocyclohexane, 1,4-diamino-2-methylcyclohexane, 1,4-diamino-3,6-diethylcyclohexane, diaminodiethylmethyl Cyclohexane, 3,3'-dimethyl-4,4'-diaminodicyclohexylmethane, 4,4'-diaminodicyclohexylmethane and other polyamine compounds having an alicyclic structure; o-phenylenediamine, m-phenylenediamine (MXDA), p-phenylenediamine (PXDA), phenylenediamine, diaminodiphenylmethane, diaminodiphenylsulfone and other polyamine compounds having an aromatic ring; N-aminomethylpiperazine, N-aminoethylpiperazine and other polyamine compounds having a heterocyclic structure; polyether polyamine compounds, and their Mannich modified products, epoxy modified products, Michael adducts, Michael adduct / condensation products, styrene modified products, polyamide modified products, etc. These can be used alone or in combination of two or more.
[0201] Among the above, from the viewpoint of obtaining a resin composition and a resin molded article having high heat resistance and high breaking strength, the epoxy resin used as component (C) is more preferably a two-component curing type epoxy resin composition in which the main agent is tetraglycidyldiaminodiphenylmethane and the curing agent is diaminodiphenyl sulfone. This is because the cured product of the resin composition containing the polyimide resin particles (A) and the epoxy resin composition as the thermosetting resin (C) has excellent heat resistance and a high strain energy release rate (G 1c ) is improved, which can reflect high fracture strength.
[0202] The strain energy release rate (G1C) is based on ASTM D5045-99, which is derived from the plane strain fracture toughness (K 1C ) can be calculated specifically by the method described in the embodiments.
[0203] The content of the curing agent in the epoxy resin composition is an amount in which the ratio of the number of active amine hydrogen atoms in the curing agent to the number of epoxy groups in the main agent (number of active amine hydrogen atoms in the curing agent / number of epoxy groups in the main agent) is preferably 1 / 0.5 to 1 / 2, more preferably 1 / 0.6 to 1 / 1.8, and even more preferably 1 / 0.75 to 1 / 1.5.
[0204] Examples of the urethane resin used as the component (C) include a two-component curable urethane resin composition containing a polyol compound such as polyester polyol and polyether polyol and a polyisocyanate compound.
[0205] Examples of the bismaleimide resin used as the component (C) include a two-component curable bismaleimide resin composition containing a bismaleimide such as 4,4′-bis(maleimide)diphenylmethane and a cyanate compound such as bis(3,5-dimethyl-4-cyanatephenyl)methane.
[0206] (content)
[0207] The resin composition of the present invention may contain polyimide resin particles (A) and at least one selected from the group consisting of a thermoplastic resin (B) and a thermosetting resin (C), and may use the thermoplastic resin (B) and the thermosetting resin (C) in combination.
[0208] From the viewpoint of improving various properties such as heat resistance and mechanical properties while maintaining the lightness derived from the thermoplastic resin (B) and the thermosetting resin (C), the mass ratio of the polyimide resin particles (A) to the total amount of the thermoplastic resin (B) and the thermosetting resin (C) [(A) / {(B)+(C)}] is preferably in the range of 1 / 99 to 99 / 1, more preferably 5 / 95 to 95 / 5, and even more preferably 5 / 95 to 90 / 10.
[0209] From the viewpoint of obtaining a resin composition or resin molded body in which the polyimide resin particles (A) are dispersed in a matrix composed of a thermoplastic resin (B), a thermosetting resin (C) or a cured product thereof, the mass ratio [(A) / {(B)+(C)}] is more preferably in the range of 5 / 95 to 80 / 20, more preferably 5 / 95 to 70 / 30, more preferably 5 / 95 to 60 / 40, more preferably 5 / 95 to 50 / 50, and still more preferably 5 / 95 to 40 / 60.
[0210] When the resin composition of the present invention is a thermoplastic resin composition containing polyimide resin particles (A) and a thermoplastic resin (B), the mass ratio is preferably in the range of 5 / 95 to 60 / 40, and further in the range of 5 / 95 to 50 / 50, in order to achieve good strand extrusion properties from an extruder and to easily produce pellets.
[0211] And in the resin composition, from the viewpoint of obtaining the effect of the present invention, the total content of the polyimide resin particles (A), the thermoplastic resin (B) and the thermosetting resin (C) is preferably 70% by mass or more, more preferably 80% by mass or more, and further preferably 90% by mass or more. In addition, the upper limit is 100% by mass.
[0212] <Additives>
[0213] The resin composition of the present invention may contain additives such as fillers, matting agents, nucleating agents, plasticizers, antistatic agents, anti-coloring agents, anti-gelling agents, flame retardants, colorants, slip improvers, antioxidants, conductive agents, and resin modifiers as needed.
[0214] The content of the above-mentioned additives is not particularly limited. From the viewpoint of maintaining the physical properties derived from component (A), component (B) and component (C) and achieving the effects of the additives, the content is usually 50% by mass or less, preferably 0.0001 to 30% by mass, more preferably 0.0001 to 15% by mass, further preferably 0.001 to 10% by mass, and further preferably 0.01 to 8% by mass in the resin composition.
[0215] [Method for producing resin composition]
[0216] The method for producing the resin composition of the present invention is not particularly limited. From the viewpoint of including the polyimide resin particles (A) in the resin composition in a state where the shape of the polyimide resin particles (A) is maintained, it is preferred to produce the resin composition by mixing the polyimide resin particles (A) with the thermoplastic resin (B) or the thermosetting resin (C) without applying a thermal history above the melting point of the polyimide resin particles (A). As mentioned above, "producing the resin composition without applying a thermal history above the melting point of the polyimide resin particles (A)" means that when producing the resin composition of the present invention, all the production steps are carried out under temperature conditions lower than the melting point of the polyimide resin particles (A).
[0217] Specifically, resin combination of the present invention is in the case of a thermoplastic resin composition containing polyimide resin particles (A) and a thermoplastic resin (B). When manufacturing the resin combination, preferably at a temperature lower than the melting point of polyimide resin particles (A), polyimide resin particles (A) and thermoplastic resin (B) are mixed. For example, in an extruder, at a set temperature lower than the melting point of polyimide resin particles (A), the resin combination containing polyimide resin particles (A) and thermoplastic resin (B) is mixed. When the set temperature of the extruder is multistage, preferably all set temperatures are made to be lower than the melting point of polyimide resin particles (A). In addition, in the mixing process of the resin combination, preferably the mode of the temperature above the melting point that the resin temperature does not become the polyimide resin particles (A) is adjusted.
[0218] From the viewpoint of maintaining the shape of the component (A) used, the melting point of the component (A) is set to Tm A (°C), the kneading temperature is preferably (Tm A -10)°C or lower, preferably (Tm A -20)°C or lower, more preferably (Tm A -30)℃ or below.
[0219] When the thermoplastic resin (B) is an amorphous thermoplastic resin (B1), the kneading temperature is preferably a temperature not lower than the glass transition temperature of the component (B1), and the glass transition temperature of the component (B1) is Tg. B1 In the case of (°C), from the viewpoint of easy extrusion, (Tg B1 +5)℃ or more, more preferably (Tg B1 When the thermoplastic resin (B) is a crystalline thermoplastic resin (B2), the temperature is preferably at least the melting point of the component (B2), and the melting point of the component (B2) is defined as Tm. B2 In the case of (°C), from the viewpoint of easy extrusion, (Tm B2 +5)℃ or more, more preferably (TmB2 +10)℃ or above.
[0220] Preferably, the resin composition is kneaded under the above temperature conditions and then extruded into strands, whereby pellets of the thermoplastic resin composition containing the polyimide resin particles (A) to be used can be produced in a state where the shapes thereof are maintained.
[0221] After the pellets are produced, a drying step may be performed as necessary. In this case, the drying temperature is also preferably a temperature lower than the melting point of the polyimide resin particles (A).
[0222] When the resin composition of the present invention is a thermosetting resin composition containing polyimide resin particles (A) and a thermosetting resin (C), when producing the resin composition, the polyimide resin particles (A) and the thermosetting resin (C) can be mixed under a temperature condition lower than the melting point of the polyimide resin particles (A). From the viewpoint of maintaining the shape of the component (A) used and suppressing the decomposition of the thermosetting resin (C) before curing, the melting point of the component (A) is set to Tm A (°C), the mixing temperature is preferably (Tm A -10)°C or lower, preferably (Tm A -20)°C or lower, more preferably (Tm A -30)°C or lower, more preferably (Tm A -50)°C or lower, more preferably (Tm A -100)°C or lower, more preferably (Tm A The lower limit of the mixing temperature can be selected according to the curing speed of the thermosetting resin composition and the like.
[0223] When the resin composition of the present invention is produced, the melting point of the component (A) is set to Tm from the viewpoint of maintaining the shape of the component (A) used. A (°C), more preferably (Tm A All the manufacturing steps are carried out under the temperature condition of -10)°C or below, and more preferably under (Tm A All the manufacturing steps are carried out under the temperature condition of -20)°C or below, and more preferably under (Tm A All manufacturing processes are carried out under temperature conditions below -30)°C.
[0224] [Resin molded body]
[0225] The resin molded article of the present invention comprises: polyimide resin particles (A), and at least one selected from the group consisting of cured products of thermoplastic resins (B) and thermosetting resins (C), wherein the polyimide resin particles (A) comprise a repeating structural unit represented by the following formula (1) and a repeating structural unit represented by the following formula (2), wherein the content ratio of the repeating structural unit of the formula (1) is 20 to 70 mol% relative to the total of the repeating structural unit of the formula (1) and the repeating structural unit of the formula (2), and the volume average particle size D50 is 5 to 200 μm.
[0226]
[0227] (R1 is a divalent group having 6 to 22 carbon atoms and containing at least one alicyclic hydrocarbon structure. R2 is a divalent chain aliphatic group having 5 to 16 carbon atoms. X1 and X2 are each independently a tetravalent group having 6 to 22 carbon atoms and containing at least one aromatic ring.)
[0228] The component (A), the component (B) and the component (C), and suitable embodiments thereof are the same as those described in the resin composition.
[0229] The resin molded article of the present invention is preferably a resin molded article in which polyimide resin particles (A) are dispersed in a matrix composed of a cured product of a thermoplastic resin (B) or a thermosetting resin (C). It is believed that the polyimide resin particles (A) function as a resin filler, thereby achieving an improvement effect in various properties such as heat resistance and mechanical properties.
[0230] [Method for producing resin molded article]
[0231] When manufacturing the resin molded body of the present invention, it is preferred to manufacture the resin molded body without applying a thermal history above the melting point of the polyimide resin particles (A) in order to maintain the shape of the polyimide resin particles (A) used and contain them in the resin molded body. From the above viewpoint, the method for manufacturing the resin molded body of the present invention preferably comprises the step of molding a resin composition containing the polyimide resin particles (A) and at least one selected from the group consisting of a thermoplastic resin (B) and a thermosetting resin (C) at a temperature lower than the melting point of the polyimide resin particles (A).
[0232] When producing a resin molded body, the resin composition of the present invention can be used.
[0233] When a resin molded article is produced using a thermoplastic resin composition containing polyimide resin particles (A) and a thermoplastic resin (B), it is preferred to use pellets of the resin composition produced by the above-described method.
[0234] Before the pellets are provided for molding, a step of drying the pellets may be performed as required. From the viewpoint of including the polyimide resin pellets (A) in the resin molded body in a state of maintaining the shape of the pellets to be used, the drying temperature of the pellets is preferably a temperature lower than the melting point of the polyimide resin pellets (A). From the viewpoint of preventing the degradation of the thermoplastic resin (B), it is more preferably 200°C or less, further preferably 150°C or less, and further preferably 120°C or less. The lower limit of the drying temperature is not particularly limited, but from the viewpoint of drying efficiency, it is preferably 40°C or more, and more preferably 60°C or more.
[0235] The drying time of the pellets can be appropriately selected depending on the type of the thermoplastic resin (B) used, the drying temperature, etc., and is preferably 0.5 to 10 hours, more preferably 2 to 8 hours.
[0236] When a thermoplastic resin composition containing polyimide resin particles (A) and a thermoplastic resin (B) is used as the resin composition, the molding method of the resin molded body includes injection molding, extrusion molding, blow molding, hot press molding, vacuum molding, pressure molding, laser molding, ultrasonic heating molding, welding, and fusion bonding. Among them, injection molding is preferred because it can be molded without setting the molding temperature and the mold temperature during molding to high temperatures.
[0237] When a thermoplastic resin composition containing polyimide resin particles (A) and a thermoplastic resin (B) is used as the resin composition, the thermoplastic resin (B) is preferably at least one selected from the group consisting of the following (B1) and (B2).
[0238] (B1) Amorphous thermoplastic resin having a glass transition temperature lower than the melting point of the polyimide resin particles (A)
[0239] (B2) a crystalline thermoplastic resin having a melting point lower than that of the polyimide resin particles (A) or a glass transition temperature lower than that of the polyimide resin particles (A)
[0240] The amorphous thermoplastic resin (B1) and the crystalline thermoplastic resin (B2), and suitable embodiments thereof are the same as those described in the resin composition.
[0241] When the thermoplastic resin (B) is an amorphous thermoplastic resin (B1), from the viewpoint of maintaining the shape of the polyimide resin particles (A) used, the method for producing a resin molded body preferably comprises the following step: extruding a resin composition containing polyimide resin particles (A) and an amorphous thermoplastic resin (B1) at a temperature lower than the melting point of the polyimide resin particles (A) and higher than the glass transition temperature of the amorphous thermoplastic resin (B1).
[0242] From the viewpoint of maintaining the shape of the component (A) used, the melting point of the component (A) is set to Tm A (°C), the temperature is preferably (T mA -10)℃ or less, more preferably (T mA -20)℃ or less, more preferably (T mA The lower limit of the temperature is not particularly limited as long as it is a temperature equal to or higher than the glass transition temperature of the component (B1), and the glass transition temperature of the component (B1) is Tg B1 In the case of (°C), from the viewpoint of easy extrusion, (Tg B1 +5)℃ or more, more preferably (Tg B1 +10)℃ or above.
[0243] When manufacturing the resin molded body, it is preferred that at least the set temperature during extrusion is set to the above range, and when the set temperature is multi-stage, it is preferred that all the set temperatures are set to the above range. In addition, it is more preferred to adjust the resin temperature during extrusion to the above range.
[0244] Moreover, when the thermoplastic resin (B) is a crystalline thermoplastic resin (B2), from the viewpoint of maintaining the shape of the polyimide resin particles (A) used, the method for producing a resin molded body preferably comprises the following step: extruding a resin composition containing polyimide resin particles (A) and a crystalline thermoplastic resin (B2) at a temperature lower than the melting point of the polyimide resin particles (A) and higher than the melting point of the crystalline thermoplastic resin (B2).
[0245] From the viewpoint of maintaining the shape of the component (A) used, the melting point of the component (A) is set to Tm A (°C), the temperature is preferably (Tm A -10)℃ or less, more preferably (Tm A -20)°C or less, more preferably (Tm A The lower limit of the temperature is not particularly limited as long as it is a temperature equal to or higher than the melting point of the component (B2), and the melting point of the component (B2) is Tm. B2 In the case of (°C), from the viewpoint of easy extrusion, (Tm B2 +5)℃ or more, more preferably (Tm B2 +10)℃ or above.
[0246] As mentioned above, when manufacturing resin molded body, preferably at least the setting temperature when extruding is set to the above-mentioned range, and when this setting temperature is multi-stage, preferably all setting temperatures are set to the above-mentioned range. In addition, it is more preferable to adjust the resin temperature when extruding to the mode of the above-mentioned range.
[0247] When a thermoplastic resin composition containing polyimide resin particles (A) and a thermoplastic resin (B) is used as the resin composition, specific procedures of the method for producing the resin molded article of the present invention include, for example, the following method.
[0248] First, polyimide resin pellets (A), thermoplastic resin (B), and various optional components as required are added and dry-mixed, and then introduced into an extruder, kneaded and extruded at a temperature lower than the melting point of the polyimide resin pellets (A), preferably at a temperature within the aforementioned range, to produce pellets. Alternatively, the thermoplastic resin (B) is introduced into an extruder, melted at a temperature lower than the melting point of the polyimide resin pellets (A), preferably at a temperature within the aforementioned range, and then polyimide resin pellets (A) and various optional components as required are introduced therein, and then kneaded and extruded in an extruder, thereby producing the pellets.
[0249] The pellets are dried under the aforementioned drying conditions as required, and then introduced into various molding machines such as injection molding machines, and molded at a temperature lower than the melting point of the polyimide resin particles (A) to produce a resin molded body having a desired shape. After molding, short-term heating using ultrasound as required may be performed, and post-processing such as melting and bonding at the interface of component (A) and component (B) may also be performed.
[0250] When a thermosetting resin composition containing polyimide resin particles (A) and a thermosetting resin (C) is used as the resin composition, from the viewpoint of maintaining the shape of the component (A) used, the method for producing a resin molded body preferably cures and molds the resin composition at a temperature lower than the melting point of the polyimide resin particles (A), preferably at a temperature in the above range. From the viewpoint of maintaining the shape of the component (A) used and suppressing the decomposition of the thermosetting resin (C) before curing, the melting point of the component (A) is set to Tm A (°C), the temperature (curing temperature) is preferably (Tm A -10)°C or lower, preferably (Tm A -20)°C or lower, more preferably (Tm A -30)℃ or less, more preferably (Tm A -50)℃ or less, more preferably (Tm A The lower limit of the temperature is not particularly limited as long as it is a temperature at which the thermosetting resin composition can be cured.
[0251] <Purpose>
[0252] The resin composition and resin molded body of the present invention improve various properties such as heat resistance and mechanical properties while maintaining the lightness derived from the resin, and can be used for industrial intermediate products such as prepregs, resin adhesives, matrix resins for fiber reinforced plastics (FRP), coating agents, laminating adhesives, 3D printing materials, etc.; sliding components, structural components or engine components for aircraft, ships, or vehicles, cooking utensils, stationery, headphone vibration plates, air pillows, connectors, and other molded products.
[0253] When the resin composition of the present invention is used for structural members for aircraft, ships, or vehicles, from the viewpoint of simultaneously improving the elastic modulus, strength, and toughness, the material constituting the structural member is preferably a fiber-reinforced composite material containing the resin composition of the present invention or a cured product thereof, and reinforcing fibers.
[0254] As the reinforcing fiber used in the fiber reinforced composite material, for example, glass fiber, carbon fiber, boron fiber and metal fiber can be cited, and one or more of them can be used. Among them, from the viewpoint of the strength and lightness of the obtained composite material, carbon fiber is preferred. That is, the aforementioned fiber reinforced composite material is preferably a carbon fiber reinforced composite material (CFRP) comprising the aforementioned resin composition or its cured product, and carbon fiber.
[0255] The carbon fiber used in CFRP is manufactured using rayon, polyacrylonitrile (PAN) and the like as raw materials, or can be manufactured by spinning asphalt such as petroleum and coal as raw materials. In addition, a regenerated product of the end material of the carbon fiber or a regenerated carbon fiber from which the resin is removed from the CFRP can also be used. The form of the carbon fiber can include, for example, a single filament or multifilament simply arranged in a unidirectional or alternating manner, a woven fabric or other fabric, a non-woven fabric or a mat, and the like. Among them, the form of a single filament, a fabric, a non-woven fabric or a mat is preferred, and the form of a fabric is more preferred.
[0256] The average fiber diameter of the carbon fiber is preferably 1 to 100 μm, more preferably 3 to 50 μm, and further preferably 4 to 20 μm. If the average fiber diameter is within this range, processing is easy, and the elastic modulus and strength of the obtained CFRP become excellent. It should be noted that the average fiber diameter can be measured by observation based on a scanning electron microscope (SEM) or the like. More than 50 fibers are randomly selected to measure the length, and the number average fiber diameter can be calculated.
[0257] The fineness of the carbon fiber is preferably 20 to 4500 tex, more preferably 50 to 4000 tex. If the fineness is within this range, the resin composition is easily impregnated, and the elastic modulus and strength of the obtained composite material become excellent. It should be noted that the fineness can be obtained as follows: the weight of long fibers of any length is obtained and converted to the weight per 1000 m, so that it can be obtained. The number of filaments can usually preferably use carbon fibers of about 500 to 60,000.
[0258] The fiber-reinforced composite material can be produced by impregnating reinforcing fibers with the resin composition of the present invention by a conventional method and then molding the impregnated fibers into a desired shape.
[0259] Example
[0260] Next, the present invention will be described in more detail with reference to Examples, but the present invention is not limited thereto. In addition, various measurements and evaluations in each of the production examples and Examples were performed as follows.
[0261] <Infrared spectroscopy (IR measurement)>
[0262] The IR measurement of the polyimide resin pellets was performed using “JIR-WINSPEC50” manufactured by JEOL Ltd.
[0263] <Logarithmic viscosity μ>
[0264] After the polyimide resin pellets were dried at 190 to 200° C. for 2 hours, a polyimide resin solution prepared by dissolving 0.100 g of the polyimide resin in 20 mL of concentrated sulfuric acid (96%, manufactured by Kanto Chemical Co., Ltd.) was used as a measurement sample and measured at 30° C. using a Cannon-Fenske viscometer. The logarithmic viscosity μ was determined according to the following formula.
[0265] μ=ln(ts / t0) / C
[0266] t0: time for concentrated sulfuric acid to flow
[0267] ts: Flow time of polyimide resin solution
[0268] C: 0.5 g / dL
[0269] <Melting point, glass transition temperature, crystallization temperature, crystallization heat>
[0270] The melting point Tm and glass transition temperature Tg of the polyimide resin particles and thermoplastic resin described in the production examples, and the crystallization temperature Tc and crystallization heat ΔHm of the polyimide resin particles described in the production examples were measured using a differential scanning calorimeter (“DSC-6220” manufactured by SII NanoTechnology Inc.).
[0271] In a nitrogen atmosphere, the polyimide resin particles or thermoplastic resin were subjected to a thermal history of the following conditions: first heating (heating rate 10°C / min), followed by cooling (temperature drop rate 20°C / min), and then second heating (heating rate 10°C / min).
[0272] The melting point Tm is determined by reading the peak top value of the endothermic peak observed in the second heating. The glass transition temperature Tg is determined by reading the value observed in the second heating. The crystallization temperature Tc is determined by reading the peak top value of the exothermic peak observed during cooling.
[0273] The crystallization heat amount ΔHm (mJ / mg) was calculated from the area of the exothermic peak observed during cooling.
[0274] <Half crystallization time>
[0275] The half crystallization time of the polyimide resin particles is measured using a differential scanning calorimeter ("DSC-6220" manufactured by SII NanoTechnology Inc.).
[0276] In a nitrogen atmosphere, the polyimide resin was completely melted by maintaining the temperature at 420°C for 10 minutes, and then a rapid cooling operation was performed at a cooling rate of 70°C / min, and the time taken from the appearance of the crystallization peak observed at this time to the peak top was calculated. It should be noted that in Table 1, when the half-crystallization time is less than 20 seconds, it is recorded as "<20".
[0277] <Weight Average Molecular Weight>
[0278] The weight average molecular weight (Mw) of the polyimide resin particles was measured using a gel filtration chromatography (GPC) measuring apparatus "Shodex GPC-101" manufactured by Showa Denko K.K. under the following conditions.
[0279] Column: Shodex HFIP-806M
[0280] Mobile phase solvent: HFIP containing 2 mM sodium trifluoroacetate
[0281] Column temperature: 40°C
[0282] Mobile phase flow rate: 1.0 mL / min
[0283] Sample concentration: about 0.1 mass%
[0284] Detector: IR detector
[0285] Injection volume: 100μm
[0286] Standard curve: Standard PMMA
[0287] <Volume average particle size (D50)>
[0288] D50 of the polyimide resin particles and the resin particles used in the comparative examples was determined by laser diffraction particle size distribution measurement.
[0289] The laser diffraction light scattering particle size distribution measuring instrument "LMS-2000e" manufactured by Malvern was used as the measuring device. In the D50 measurement of the resin particles, water was used as the dispersion medium, and the resin particles were dispersed under ultrasonic conditions under conditions where they were more fully dispersed. The measuring range was set to 0.02 to 2000 μm.
[0290] <True density (gas phase method)>
[0291] The true density of the polyimide resin pellets was measured by a gas phase method using VM-100 manufactured by Seishin Enterprise Co., Ltd. as a measuring apparatus and helium as a gas in accordance with “Measurement method of density and specific gravity by gas replacement method” specified in JIS Z8807:2012.
[0292] <True density (liquid phase method)>
[0293] The true density of the polyimide resin pellets by a liquid phase method (densimeter method) is determined by using an automatic wet true density measuring device "AUTO TRUE DENSER MAT-7000" manufactured by Seishin Enterprise Co., Ltd. as a measuring device and n-butanol as a medium solution, and the true density is determined by the following formula.
[0294]
[0295] Pd: true density of the sample
[0296] Wa: Determine the quality of the cuvette
[0297] Wb: (measurement cuvette + sample) mass
[0298] Wc: (measurement cuvette + sample + medium solution) mass
[0299] Wd: (measurement cuvette + medium solution) mass
[0300] Ld: Density of medium solution
[0301] <Specific surface area>
[0302] The specific surface area of the polyimide resin particles was determined by measuring the nitrogen adsorption under the following conditions and obtaining an adsorption isotherm (vertical axis: nitrogen adsorption, horizontal axis: relative pressure P / P0) according to the BET method. The sample used for the measurement was pre-treated by heating at 180°C and vacuum degassing for 6 hours.
[0303] Measuring device: Continuous surface area / pore distribution measuring device NOVA-TOUCH manufactured by Quantachrome
[0304] Gas used: Nitrogen
[0305] Refrigerant: Liquid nitrogen (temperature 77.35K)
[0306] Relative pressure measurement: 5×10 -3 <P / P0<0.99
[0307] Isotherm data used in calculation of specific surface area: 0.05 <P / P0<0.3
[0308] <Total pore volume>
[0309] The total pore volume of the polyimide resin particles is calculated as follows: Assuming that the pores are filled with liquid nitrogen, the P / P 0,max Calculate the amount of adsorbed nitrogen under.
[0310] <Average pore diameter>
[0311] The average pore diameter of the polyimide resin particles is determined according to the following formula.
[0312] Average pore diameter Dave = (4V total / S)
[0313] V total : Total pore volume
[0314] S: Specific surface area (BET method)
[0315] <State of the thread>
[0316] The thermoplastic resin compositions of Examples 1 to 3 were evaluated based on the following criteria by visually observing the state of the strands extruded from the extruder.
[0317] A: Good
[0318] B: Can extrude strands, but easy to chop
[0319] C: Unable to extrude strands
[0320] <Specific Gravity>
[0321] The thermoplastic resin (B) used in Examples 1 to 3 alone or the thermoplastic resin composition obtained in Examples 1 to 3 was used to prepare a molded body of 80 mm×10 mm×4 mm in thickness according to the method described below, and the specific gravity at 23° C. was determined using an electronic densimeter (“MDS-300” manufactured by Alfa Mirage Co., Ltd.).
[0322] In this example, the specific gravity of the polyimide resin particles (A) is the absolute value of the true density (liquid phase method) measured by the above method. The specific gravity of the polyimide resin particles 1 obtained in Production Example 1 was 1.19.
[0323] The specific gravity of the polyimide resin pellets 1 obtained in Production Example 1 was measured by the following method by melt-kneading at a temperature not lower than the melting point thereof.
[0324] The polyimide resin pellets 1 obtained in Preparation Example 1 were melt-kneaded using Labplast Mill (manufactured by Toyo Seiki Seisaku-sho, Ltd.) at a barrel setting temperature of 350° C. and a screw speed of 70 rpm, and strands were extruded and air-cooled, and pelletized using a pelletizer (“Fan cutter FC-Mini-4 / N” manufactured by Star Plastics Co., Ltd.). The pellets were dried at 150° C. for 12 hours, and the true density (liquid phase method) was measured according to the above method, and the value was used as the specific gravity. The specific gravity was 1.29.
[0325] <Specific Gravity of Component (A) in Resin Molded Article>
[0326] The specific gravity of the component (A) in the resin molded products obtained in Examples 1 to 3 was calculated according to the following formula.
[0327] [(Specific gravity of resin molded body) - (Specific gravity of component (B)) × (Mass fraction of component (B))] / (Mass fraction of component (A))
[0328] <Tensile Strength, Tensile Elastic Modulus, and Tensile Fracture Strain>
[0329] Using the thermoplastic resin (B) used alone in each example or the thermoplastic resin composition obtained in each example, a 1A type test piece specified in JIS K7161-2: 2014 was prepared according to the method described below and used for measurement. A tensile test was performed using a tensile tester ("Strograph VG-1E" manufactured by Toyo Seiki Co., Ltd.) in accordance with JIS K7161-1: 2014 and K7161-2: 2014 at a temperature of 23° C., a clamp distance of 50 mm, and a test speed of 20 mm / min to measure tensile strength, tensile elastic modulus, and tensile breaking strain.
[0330] <Flexural modulus>
[0331] Using the thermoplastic resin (B) used alone in each example or the thermoplastic resin composition obtained in each example, a molded body of 80 mm×10 mm×4 mm thickness specified in ISO316 was prepared according to the method described below and used for measurement. A bending test was performed at a temperature of 23° C. and a test speed of 2 mm / min using Bendgraph (manufactured by Toyo Seiki Seisaku-sho, Ltd.) in accordance with ISO178 to measure the flexural modulus.
[0332] <Heat Deformation Temperature (HDT)>
[0333] Using the thermoplastic resin (B) used alone in each example or the thermoplastic resin composition obtained in each example, a resin molded body of 80 mm×10 mm×4 mm in thickness was produced according to the method described below and used for measurement.
[0334] The measurement was carried out in a flat-lay test in accordance with JIS K7191-1, 2: 2015. Specifically, the heat deformation temperature was measured using an HDT tester "Auto-HDT3D-2" (manufactured by Toyo Seiki Seisaku-sho, Ltd.) at a support distance of 64 mm, a load of 1.80 MPa, and a heating rate of 120°C / hour.
[0335] <Weightlessness Temperature>
[0336] The thermoplastic resin (B) used alone in each example, or pellets of the thermoplastic resin composition or cured product of the thermosetting resin composition obtained in each example were used for the measurement.
[0337] A thermogravimetric analyzer ("TG / DTA6200" manufactured by Seiko Instruments Inc.) was used for the measurement. About 10 mg of the sample was collected and heated from room temperature to 450°C under the conditions of a nitrogen flow rate of 100 mL / min and a heating rate of 10°C / min. The temperature at which the weight decreased by 1% by mass relative to the sample weight of 100% by mass at 100°C was taken as the 1% weight loss temperature, the temperature at which the weight decreased by 5% by mass was taken as the 5% weight loss temperature, and the temperature at which the weight decreased by 10% by mass was taken as the 10% weight loss temperature.
[0338] <Dynamic friction coefficient>
[0339] Using the thermoplastic resin (B) used alone in each example or the thermoplastic resin composition obtained in each example, resin molded bodies were produced according to the method described below, and those cut into 30 mm×30 mm×3 mm thick were used for measurement.
[0340] The measurement was performed using a friction and wear tester (MODELE MF-III-F) manufactured by A&D Co., Ltd. According to JIS K7218 (1986)-A method, the material on the other side was an S45C ring (contact area 2 cm 2 ), a sliding wear test was carried out under the conditions of initial load: 50N, test speed: 0.5m / s, and sliding distance: 3km, and the dynamic friction coefficient was measured.
[0341] <Plane strain fracture toughness (K 1C ), Poisson's ratio, strain energy release rate (G 1C )>
[0342] The plane strain fracture toughness K is determined according to the following "bending fracture toughness test" 1C , the Poisson's ratio and tensile elastic modulus were determined according to the following "Tensile Test".
[0343] (Bending fracture toughness test)
[0344] Using the cured product of the thermosetting resin composition described in Table 7, resin molded bodies of 60 mm×12 mm×6 mm in thickness were manufactured according to the method described below. After notching with a 30° t1.0-equiangular milling cutter, the test pieces obtained by pre-crack processing were used for measurement.
[0345] The measurement was performed using a universal material testing machine (Model 5966) manufactured by Instron Inc. A bending fracture toughness test (n=5) was performed in accordance with ASTM D5045-99 at 23°C, a test speed of 1 mm / min, and a support distance of 48 mm (initial).
[0346] (Tensile test)
[0347] Using the cured products of the thermosetting resin compositions listed in Table 7, resin molded bodies were produced according to the method described below, and the resulting test pieces were cut into 150 mm×12 mm×3 mm thick, and used for measurement.
[0348] The measurement was performed using a universal material testing machine (Model 5966) manufactured by Instron. The tensile test was performed in accordance with JIS K7161-2:2014 at a temperature of 23°C, a chuck distance of 115 mm, and a test speed of 1 mm / min (n=3). A uniaxial strain gauge (KFGS-5-120-C1-23 manufactured by Kyowa Electric Co., Ltd.) was attached to the center of one side of the test piece to perform strain measurement.
[0349] Next, the stress diffusion coefficient K is calculated according to the following formula: Q .
[0350]
[0351]
[0352] K Q :Stress diffusion coefficient (MPa·m 1 / 2 )
[0353] P Q : For K Q Load (kN)
[0354] B: Test piece thickness (cm)
[0355] W: Test piece width (cm)
[0356] a: Crack length
[0357] x:a / W
[0358] In addition, S is set to be the distance between supporting points (cm), and S / W=4.
[0359] Here, when the following formula (1) is satisfied, P is used. Q Find K Q .
[0360] P max / P Q <1.1···(1)
[0361] P max : Maximum load
[0362] In addition, if the following condition (2) is satisfied, K Q =K 1C .
[0363] B, a, Wa>2.5(K Q / σ y ) 2 ···(2)
[0364] σ y :Bending deviation 0.2% stress (MPa)
[0365] K obtained by the above method 1C , Poisson's ratio, and tensile elastic modulus, the strain energy release rate (G 1C ).
[0366]
[0367] G 1C : Strain energy release rate (J / m 2 )
[0368] ν: Poisson's ratio
[0369] E: tensile elastic modulus (MPa)
[0370] <Glass transition temperature (Tg)>
[0371] Tg of the cured product of the thermosetting resin composition described in Table 7 was determined by dynamic viscoelasticity measurement (DMA). Using the thermosetting resin composition described in Table 7, a resin molded body of 50 mm×10 mm×3 mm thick was produced by the method described below and used for measurement.
[0372] A dynamic viscoelasticity measuring device ("XSTARDMS6100" manufactured by Hitachi High-Tech Science Corporation) was used for the measurement. According to JIS K7244:1998, the storage modulus E', loss modulus E" and tanδ were measured in a nitrogen flow (300 mL / min), a measurement temperature of room temperature to 300°C, a heating rate of 4.0°C / min, a frequency of 1 Hz, and a measurement mode of bending mode. The peak temperature (°C) on the high temperature side of tanδ is shown in Table 7 as Tg.
[0373] <Tensile strength, tensile elastic modulus, maximum elongation, and elongation at break of film>
[0374] Using the thermoplastic resin compositions having the compositions shown in Table 8, films were prepared according to the methods described below, and cut into pieces with a width of 10 mm to be used for measurement.
[0375] A tensile test was performed using a tensile testing machine ("Strograph VG-1E" manufactured by Toyo Seiki Co., Ltd.) in accordance with JIS K7161-1:2014 and K7161-2:2014 at a temperature of 23°C, a clamp distance of 50 mm, and a test speed of 50 mm / min to measure tensile strength, tensile elastic modulus, maximum elongation, and breaking elongation.
[0376] Production Example 1 (Production of Polyimide Resin Pellets 1)
[0377] In a 2L separable flask equipped with a Dean-Stark trap, a Liebig condenser, a thermocouple, and four paddles, 500 g of 2-(2-methoxyethoxy)ethanol (manufactured by Nippon Emulsifier Co., Ltd.) and 218.12 g (1.00 mol) of pyromellitic dianhydride (manufactured by Mitsubishi Gas Chemical Co., Ltd.) were introduced, and after nitrogen gas was flowed, stirring was performed at 150 rpm so as to form a uniform suspension solution. On the other hand, using a 500 mL beaker, 49.79 g (0.35 mol) of 1,3-bis(aminomethyl)cyclohexane (manufactured by Mitsubishi Gas Chemical Co., Ltd., cis / trans ratio = 7 / 3) and 93.77 g (0.65 mol) of 1,8-octamethylenediamine (manufactured by Kanto Chemical Co., Ltd.) were dissolved in 250 g of 2-(2-methoxyethoxy)ethanol to prepare a mixed diamine solution. The mixed diamine solution was slowly added using a plunger pump. Heat was released by the addition, but the internal temperature was adjusted to fall within the range of 40 to 80°C. During the addition of the mixed diamine solution, all nitrogen was flowed and the stirring blade speed was set to 250 rpm. After the addition was completed, 130 g of 2-(2-methoxyethoxy)ethanol and 1.284 g (0.010 mol) of n-octylamine (manufactured by Kanto Chemical Co., Ltd.) as an end-capping agent were added and further stirred. At this stage, a light yellow polyamic acid solution was obtained. Next, after the stirring speed was set to 200 rpm, the polyamic acid solution in the 2L detachable flask was heated to 190°C. During the gradual heating process, the precipitation of polyimide resin particles and dehydration accompanied by imidization were confirmed when the solution temperature was between 120 and 140°C. After being kept at 190°C for 30 minutes, it was cooled to room temperature and filtered. The obtained polyimide resin particles were washed with 300 g of 2-(2-methoxyethoxy)ethanol and 300 g of methanol, filtered, and then dried in a dryer at 180° C. for 10 hours to obtain 317 g of polyimide resin particles 1.
[0378] The IR spectrum of the polyimide resin particles 1 was measured. The results showed that ν(C=O) was 1768, 1697 (cm -1 ) The characteristic absorption of the imide ring was confirmed at . The logarithmic viscosity was 1.30 dL / g, Tm was 323°C, Tg was 184°C, Tc was 266°C, the crystallization heat was 21.0 mJ / mg, the half crystallization time was less than 20 seconds, and the Mw was 55,000.
[0379] The composition of the polyimide resin pellets 1 obtained in Production Example 1 is shown in Table 1. In addition, the mol% of the tetracarboxylic acid component and the diamine component in Table 1 are values calculated from the input amount of each component when producing the polyimide resin pellets.
[0380] The polyimide resin particles 1 had a D50 of 17 μm and a specific gravity of 1.19, and were porous. Table 1 also shows the analysis results of the true density, specific surface area, total pore volume, and average pore diameter of the polyimide resin particles 1.
[0381] Production Example 2 (Production of Polyimide Resin Particles 2)
[0382] Polyimide resin particles 2 were produced in the same manner as in Production Example 1 except that n-octylamine was not used as a terminal blocking agent, and were analyzed by the above-described method. Table 1 shows the composition and analysis results of the polyimide resin particles 2.
[0383] [Table 1]
[0384]
[0385] The abbreviations in Table 1 are as follows.
[0386] PMDA; pyromellitic dianhydride
[0387] 1,3-BAC; 1,3-bis(aminomethyl)cyclohexane
[0388] OMDA; 1,8-octamethylenediamine
[0389] n-OcA: n-octylamine
[0390] Production Example 3 (Production of Modified Polyethylene Terephthalate Resin 1)
[0391] A mixture of 6449.5 g (33.2 mol) of dimethyl terephthalate (DMT), 2747.1 g (44.2 mol) of ethylene glycol (EG), 4727.4 g (15.5 mol) of 3,9-bis(1,1-dimethyl-2-hydroxyethyl)2,4,8,10-tetraoxaspiro〔5,5〕undecane (SPG), and 0.03 mol of manganese acetate tetrahydrate per 100 mol of dimethyl terephthalate was heated to 200° C. in a nitrogen atmosphere to carry out an ester exchange reaction. After the amount of methanol distilled reached 90% or more relative to the theoretical amount, 0.02 mol of antimony (III) oxide and 0.05 mol of triphenyl phosphate were added per 100 mol of dimethyl terephthalate, the temperature was gradually raised and the pressure was reduced, and finally polymerization was carried out at 280° C. and 0.1 kPa or less. The reaction was terminated when the melt viscosity reached an appropriate level, thereby preparing a polyester containing 44 mol % of SPG residues and 56 mol % of EG residues in the diol component and 100 mol % of terephthalic acid residues in the dicarboxylic acid component.
[0392] Example 1 (Production and Evaluation of Thermoplastic Resin Composition and Resin Molded Article)
[0393] The polyimide resin pellets 1 obtained in Preparation Example 1 and pellets of polypropylene (PP) resin as a crystalline thermoplastic resin (B2-1) ("Novatec FY6" manufactured by Japan Polypropylene Corporation, melting point 150-160°C, glass transition temperature 0°C) were used in the proportions shown in Table 2. The PP resin pellets were introduced from the hopper on the inlet side of a co-rotating twin-screw kneading extruder ("HK-25D" manufactured by Parker Corporation, screw diameter D=25 mmΦ, L / D=41 (L: screw length)), and the polyimide resin pellets 1 were introduced into the extruder from a side feeder, and kneaded under the conditions of a barrel setting temperature of 200°C, a feed rate of 6 kg / hour, and a screw speed of 200 rpm to extrude strands. At this time, the resin temperature, torque, resin pressure, and the state of the strands were confirmed. The resin temperature is the temperature at the outlet of the extruder.
[0394] The strands extruded from the extruder were water-cooled, pelletized using a pelletizer ("Fan cutter FC-Mini-4 / N" manufactured by Star Plastics Co., Ltd.), and used for injection molding.
[0395] Injection molding was performed using an injection molding machine ("ROBOSHOT α-S30iA" manufactured by FANUC Corporation) at a barrel setting temperature of 200°C, a mold temperature of 50°C, and an injection speed of 62.5 mm / sec to produce resin molded bodies of predetermined shapes used in various evaluations.
[0396] The obtained pellets and resin molded bodies were used to perform various evaluations according to the above-mentioned methods.
[0397] Examples 2-3, Comparative Example 1
[0398] Except for changing the composition of the resin composition, the strand extrusion conditions, and the molding conditions as shown in Table 2, pellets and resin molded bodies were produced in the same manner as in Example 1, and various evaluations were performed by the aforementioned methods.
[0399] [Table 2]
[0400] Table 2
[0401]
[0402] *: “-” means not determined
[0403] According to Table 2, the following situations are determined.
[0404] The resin molded bodies of Examples 1 to 3 containing polyimide resin particles 1 as component (A) and PP resin as crystalline thermoplastic resin (B2-1) have improved tensile elastic modulus, flexural modulus, HDT and 1% weight loss temperature compared to the resin molded body of Comparative Example 1 consisting only of PP resin.
[0405] In the resin molded bodies of Examples 1 to 3, the specific gravity of the component (A) in the molded bodies is 1.19 to 1.22. This specific gravity is lower than the specific gravity (1.29) of the pellets obtained by melt-kneading the polyimide resin pellets 1, and is the same as or slightly higher than the specific gravity (1.19) of the polyimide resin pellets 1 compounded in the resin composition. It is therefore believed that the component (A) is not melted during the production process of the resin composition and the resin molded bodies of Examples 1 to 3, and is contained in the resin composition and the resin molded bodies in a state of maintaining the shape of the polyimide resin pellets 1 used.
[0406] The resin composition (pellets) obtained in Example 1 was cut with a microtome ("ULTRACUT E" manufactured by REICHERT-JUNG LIMITED), smoothed, and then stained with a ruthenium-based stain. The cut surface ( Figure 1 ).Depend on Figure 1 It is understood that in the resin composition obtained in Example 1, the polyimide resin particles 1 are dispersed in the matrix formed of the PP resin.
[0407] In addition, the extrusion property of the strands was confirmed in the production of the resin compositions (pellets) of Examples 1 to 3. As shown in Table 2, the resin compositions of Examples 1 to 3 were all capable of being extruded into strands, but in Example 3, compared with Examples 1 and 2, increases in resin temperature, torque, and resin pressure were observed, and the obtained strands were also brittle. Therefore, it can be said that the resin compositions of Examples 1 and 2 were excellent in strand extrusion property.
[0408] Example 4 (Production and Evaluation of Thermoplastic Resin Composition and Resin Molded Article)
[0409] The polyimide resin pellets 1 obtained in Production Example 1 and a polycarbonate (PC) resin ("Upiron S2000" manufactured by Mitsubishi Engineering-Plastics Corporation, glass transition temperature 145-150°C) as an amorphous thermoplastic resin (B1-1) were used in the ratio shown in Table 3. The PC resin was dried in a dryer at 120°C for 5 hours, and then introduced from the hopper on the inlet side of a co-rotating twin-screw kneading extruder ("HK-25D" manufactured by Parker Corporation), and the polyimide resin pellets 1 were introduced into the extruder from a side feeder, and kneading was performed under the conditions of a barrel setting temperature of 275°C, a feed rate of 6 kg / hour, and a screw speed of 150 rpm to extrude strands.
[0410] The strands extruded from the extruder were air-cooled, pelletized using a pelletizer ("Fancutter FC-Mini-4 / N" manufactured by Star Plastics Co., Ltd.), and used for injection molding.
[0411] The obtained pellets were dried in a dryer at 120°C for 4 hours, and then injection molded using an injection molding machine ("ROBOSHOTα-S30iA" manufactured by FANUC Corporation) under the conditions of a barrel setting temperature of 270°C, a mold temperature of 100°C, and an injection speed of 62.5 mm / sec to produce resin molded bodies of specified shapes for various evaluations.
[0412] The obtained pellets and resin molded body were used to perform HDT measurement according to the above method.
[0413] Comparative Example 2
[0414] A polycarbonate resin as the amorphous thermoplastic resin (B1-1) was used alone and dried in a dryer at 120° C. for 4 hours, followed by the same method as in Example 4 to prepare a resin molded body.
[0415] The HDT of the obtained resin molded product was measured by the above method.
[0416] Example 5 (Production and Evaluation of Thermoplastic Resin Composition and Resin Molded Article)
[0417] The polyimide resin pellets 1 obtained in Preparation Example 1 and polyphenylene sulfide (PPS) resin (Torelina A900 manufactured by Toray Industries, Ltd., melting point 278°C, glass transition temperature 90°C) as a crystalline thermoplastic resin (B2-2) were used in the proportions shown in Table 3. The PPS resin was introduced from a hopper on the inlet side of a co-rotating twin-screw kneading extruder (HK-25D manufactured by Parker Corporation), and the polyimide resin pellets 1 were introduced into the extruder from a side feeder, and kneading was performed under the conditions of a barrel setting temperature of 290°C, a feed rate of 6 kg / hour, and a screw rotation speed of 200 rpm to extrude strands.
[0418] The strands extruded from the extruder were water-cooled, pelletized using a pelletizer ("Fan cutter FC-Mini-4 / N" manufactured by Star Plastics Co., Ltd.), and used for injection molding.
[0419] The obtained pellets were dried in a dryer at 130°C for 3 hours, and then injection molded using an injection molding machine ("ROBOSHOTα-S30iA" manufactured by FANUC Corporation) under the conditions of a barrel setting temperature of 310°C, a mold temperature of 150°C, and an injection speed of 62.5 mm / sec to produce resin molded bodies of specified shapes for various evaluations.
[0420] The HDT of the obtained resin molded product was measured by the above method.
[0421] Comparative Example 3
[0422] A PPS resin was used alone as the crystalline thermoplastic resin (B2-2), and dried in a dryer at 130° C. for 3 hours, followed by the same method as in Example 5 to prepare a resin molded body.
[0423] The HDT of the obtained resin molded product was measured by the above method.
[0424] [Table 3]
[0425] Table 3
[0426]
[0427] Example 6 (Manufacture and evaluation of thermoplastic resin composition and resin molded article)
[0428] The polyimide resin pellets 1 obtained in Preparation Example 1 and polyamide resin PA6 ("UBE Nylon 1030B" manufactured by Ube Industries, Ltd., melting point 215-225°C, glass transition temperature 50°C) as a crystalline thermoplastic resin (B2-3) were used in the proportions shown in Table 4. PA6 was introduced from the hopper on the lower side of a co-rotating twin-screw kneading extruder ("HK-25D" manufactured by Parker Corporation), and the polyimide resin pellets 1 were introduced into the extruder from a side feeder, and kneading was performed under the conditions of a barrel setting temperature of 260°C, a feed rate of 6 kg / hour, and a screw speed of 200 rpm to extrude strands.
[0429] The strands extruded from the extruder were water-cooled, pelletized using a pelletizer ("Fan cutter FC-Mini-4 / N" manufactured by Star Plastics Co., Ltd.), and used for injection molding.
[0430] The obtained pellets were dried in a dryer at 80°C for 6 hours, and then injection molded using an injection molding machine ("ROBOSHOTα-S30iA" manufactured by FANUC Corporation) at a barrel setting temperature of 250°C, a mold temperature of 80°C, and an injection speed of 62.5 mm / sec. The obtained injection molded product was annealed in a dryer at 120°C for 1 hour to produce a resin molded body of a predetermined shape for various evaluations.
[0431] The obtained resin molded body was used to perform HDT measurement and tensile test according to the above-mentioned method.
[0432] Example 7
[0433] In Example 6, except having changed the compounding amounts (mass parts) of the polyimide resin particles 1 and the polyamide resin PA6 into the amounts described in Table 4, a resin molded body was produced in the same manner as in Example 6.
[0434] The obtained resin molded body was used to perform HDT measurement and tensile test according to the above-mentioned method.
[0435] Comparative Example 4
[0436] A polyamide resin PA6 was used alone as a crystalline thermoplastic resin (B2-3), and after drying in a dryer at 80° C. for 6 hours, a resin molded body was prepared in the same manner as in Example 6.
[0437] The obtained resin molded body was used to perform HDT measurement and tensile test according to the above-mentioned method.
[0438] [Table 4]
[0439] Table 4
[0440]
[0441] According to Table 4, the resin molded bodies of Examples 6 and 7 containing polyimide resin particles 1 and polyamide resin PA6 have improved HDT and significantly improved tensile breaking strain compared to the resin molded body of Comparative Example 4 consisting of PA6 alone.
[0442] Example 8 (Manufacture and evaluation of thermoplastic resin composition and resin molded article)
[0443] The polyimide resin pellets 1 obtained in Production Example 1 and polyethylene terephthalate (PET) resin ("RT553C" manufactured by Mitsubishi Chemical Corporation, melting point 250°C, glass transition temperature 81°C) as a crystalline thermoplastic resin (B2-4) were used in the ratio shown in Table 5. The PET resin was introduced from the hopper on the lower side of a co-rotating twin-screw kneading extruder ("HK-25D" manufactured by Parker Corporation), and the polyimide resin pellets 1 were introduced into the extruder from a side feeder, and kneading was performed under the conditions of a barrel setting temperature of 280°C, a feed rate of 6 kg / hour, and a screw speed of 200 rpm to extrude strands.
[0444] The strands extruded from the extruder were water-cooled, pelletized using a pelletizer ("Fan cutter FC-Mini-4 / N" manufactured by Star Plastics Co., Ltd.), and used for injection molding.
[0445] The obtained pellets were dried in a dryer at 80°C for 6 hours, and then injection molded using an injection molding machine ("ROBOSHOTα-S30iA" manufactured by FANUC Corporation) under the conditions of a barrel setting temperature of 250°C, a mold temperature of 80°C, and an injection speed of 62.5 mm / sec to produce resin molded bodies of specified shapes for various evaluations.
[0446] The obtained resin molded body was used to perform various evaluations by the above-mentioned methods.
[0447] Comparative Example 5
[0448] A PET resin was used alone as the crystalline thermoplastic resin (B2-4), and dried in a dryer at 130° C. for 3 hours, followed by the same method as in Example 8 to prepare a resin molded body.
[0449] The obtained resin molded body was used to perform various evaluations by the above-mentioned methods.
[0450] Example 9 (Production and Evaluation of Thermoplastic Resin Composition and Resin Molded Article)
[0451] The polyimide resin pellets 1 obtained in Preparation Example 1 and the modified polyethylene terephthalate (PET) resin 1 (melting point 220-230°C, glass transition temperature 110°C) as the crystalline thermoplastic resin (B2-5) obtained in Preparation Example 3 were used in the ratio shown in Table 5. The PET resin was introduced from the hopper on the lower side of a co-rotating twin-screw kneading extruder ("HK-25D" manufactured by Parker Corporation), and the polyimide resin pellets 1 were introduced into the extruder from a side feeder, and kneading was performed under the conditions of a barrel setting temperature of 265°C, a feed rate of 6 kg / hour, and a screw speed of 200 rpm to extrude strands.
[0452] The strands extruded from the extruder were water-cooled, pelletized using a pelletizer ("Fan cutter FC-Mini-4 / N" manufactured by Star Plastics Co., Ltd.), and used for injection molding.
[0453] The obtained pellets were dried in a dryer at 80°C for 6 hours, and then injection molded using an injection molding machine ("ROBOSHOTα-S30iA" manufactured by FANUC Corporation) under the conditions of a barrel setting temperature of 250°C, a mold temperature of 80°C, and an injection speed of 62.5 mm / sec to produce resin molded bodies of specified shapes for various evaluations.
[0454] The obtained resin molded body was used to perform various evaluations by the above-mentioned methods.
[0455] Comparative Example 6
[0456] A PET resin was used alone as the crystalline thermoplastic resin (B2-5), and after drying in a dryer at 130° C. for 3 hours, a resin molded body was prepared in the same manner as in Example 9.
[0457] The obtained resin molded body was used to perform various evaluations by the above-mentioned methods.
[0458] [Table 5]
[0459] Table 5
[0460]
[0461] According to Table 5, the resin molded bodies of Examples 8 and 9 containing polyimide resin particles 1 and PET resin or modified PET resin 1 show improvements in HDT, flexural strength and flexural modulus compared to the resin molded bodies of Comparative Examples 5 and 6 consisting only of PET resin or modified PET resin 1.
[0462] Example 10 (Production and Evaluation of Thermosetting Resin Composition and Resin Molded Article)
[0463] Using a two-component curable epoxy resin composition (C-1) as a thermosetting resin (C), a thermosetting resin composition and a cured product were prepared and evaluated by the following method.
[0464] In a 100cc disposable cup, 18.6g of bisphenol A type liquid epoxy resin ("jER828" manufactured by Mitsubishi Chemical Corporation, epoxy equivalent 186g / equivalent) as a main agent, which was adjusted to 40°C, was added. 9.5g of the polyimide resin particles 1 obtained in Production Example 1 was added thereto, and then 3.55g of 1,3-bis(aminomethyl)cyclohexane ("1,3-BAC" manufactured by Mitsubishi Gas Chemical Co., Ltd.) as a curing agent was added, and mixed with a wooden spatula at a rotation speed of 200rpm / min for 1 minute to prepare a thermosetting resin composition containing the polyimide resin particles 1 and a two-component curable epoxy resin composition (C-1) composed of the above-mentioned main agent and curing agent. In the two-component curable epoxy resin composition (C-1), the molar ratio of the number of epoxy groups in the main agent to the number of active amine hydrogens in the curing agent was 1 / 1.
[0465] The obtained thermosetting resin composition was cured by keeping it in a hot air dryer at 80°C for 1 hour, and the 5% weight loss temperature and 10% weight loss temperature of the cured product were measured according to the above method.
[0466] Embodiment 11
[0467] In Example 10, except that the amount of polyimide resin particles 1 added was changed to 22.1 g, a thermosetting resin composition and a cured product thereof were prepared in the same manner as in Example 10, and the 5% weight loss temperature and 10% weight loss temperature of the cured product were measured according to the aforementioned method. The results are shown in Table 6.
[0468] [Table 6]
[0469] Table 6
[0470]
[0471] Example 12 (Preparation and Evaluation of Thermosetting Resin Composition and Resin Molded Body)
[0472] Using a two-component curable epoxy resin composition (C-2) as the thermosetting resin (C), a thermosetting resin composition and a cured product were prepared and evaluated by the following method.
[0473] In a 500 mL detachable flask, tetraglycidyldiaminodiphenylmethane (TGDDM) ("SUMIEPOXY ELM-434" manufactured by Sumitomo Chemical Co., Ltd.), an epoxy-containing compound as a main agent, is measured and melted in an oil bath at 130°C. Next, the amount of polyimide resin particles 1 previously dried at 150°C for 1 hour as described in Table 7 is added, and stirring is continued for 3 hours while heating. After stirring, it is cooled to 110°C, transferred to a disposable cup and measured. Thereto, 4,4'-diaminodiphenyl sulfone (DDS) as a curing agent is added in an equivalent ratio of the number of active amine hydrogens in the curing agent to the number of epoxy groups in the main agent (the number of active amine hydrogens in the curing agent / the number of epoxy groups in the main agent) = 1 / 1.43, and stirred and mixed in an oven at 110°C to prepare an epoxy resin composition.
[0474] The obtained epoxy resin composition was degassed under reduced pressure, and the epoxy resin composition was injected into a casting mold of a specified shape preheated to 110°C, and the temperature was increased to 150°C at a heating rate of 2°C / min. After heating for 2 hours, the temperature was increased to 180°C, and further heated for 2 hours to cure, thereby obtaining a test piece of the desired shape.
[0475] The test piece dimensions are as follows.
[0476] For bending fracture toughness test: 125mm×115mm×6mm
[0477] For dynamic viscoelasticity and Poisson's ratio measurement: 220mm×100mm×3mm
[0478] The obtained test pieces were used to measure the plane strain fracture toughness (K 1C ), strain energy release rate (G 1C ), Poisson's ratio, and glass transition temperature based on DMA. The results are shown in Table 7.
[0479] Examples 13 to 15, Comparative Examples 7 to 9
[0480] Except for changing the type, amount, and drying conditions of the resin particles used as described in Table 7, an epoxy resin composition and a cured product were prepared and evaluated in the same manner as in Example 12. The results are shown in Table 7.
[0481] [Table 7]
[0482] Table 7
[0483]
[0484] *: “-” means not determined
[0485] The components described in Table 7 are as follows.
[0486] (A1) Polyimide resin particles 1: polyimide resin particles obtained in Production Example 1
[0487] (A2) Polyimide resin particles 2: polyimide resin particles obtained in Production Example 2 (uncapped)
[0488] (a1) Polyethersulfone resin particles: "SUMIKAEXCEL 4800P" manufactured by Sumitomo Chemical Co., Ltd., D50 = 560 μm
[0489] (a2) Polyetheretherketone resin particles: "330UPF" manufactured by Jilin Joinature Polymer Co., Ltd., D50 = 14 μm
[0490] (C-2) Two-component curable epoxy resin composition: An epoxy resin composition prepared by mixing tetraglycidyldiaminodiphenylmethane (TGDDM), an epoxy group-containing compound as a main agent, and 4,4'-diaminodiphenyl sulfone (DDS), a curing agent, at an equivalent ratio of the number of active amine hydrogens in the curing agent to the number of epoxy groups in the main agent (number of active amine hydrogens in the curing agent / number of epoxy groups in the main agent) = 1 / 1.43
[0491] According to Table 7, it is determined that the cured products of the thermosetting resin compositions of Examples 12 to 15 can maintain heat resistance and can also improve plane strain fracture toughness and strain energy release rate compared to the cured products of the comparative examples. In addition, by using uncapped polyimide resin particles 2 as polyimide resin particles, plane strain fracture toughness and strain energy release rate are further improved.
[0492] Reference Examples 1 and 2 (Production of Thermoplastic Resin Film)
[0493] The polyimide resin pellets 1 obtained in Production Example 1 and pellets of polypropylene (PP) resin ("Novatec FY6" manufactured by Japan Polypropylene Corporation) as the crystalline thermoplastic resin (B2-1) were used in the ratio shown in Table 8. The PP resin was dried in advance with hot air at 80°C for 6 hours or more before use.
[0494] PP resin pellets were introduced from the hopper on the inlet side of a co-rotating twin-screw kneading extruder ("HK-25D" manufactured by Parker Corporation, screw diameter D = 25 mmΦ, L / D = 41 (L: screw length)), and polyimide resin pellets 1 were introduced into the extruder from a side feeder, and kneading was performed under the conditions of a barrel setting temperature of 200°C, a feed rate of 6 kg / hour, and a screw speed of 200 rpm to extrude strands. The strands extruded from the extruder were water-cooled and pelletized using a pelletizer ("Fan cutter FC-Mini-4 / N" manufactured by Star Plastics Co., Ltd.), and the pellets were used to produce a single-layer film by extrusion molding.
[0495] Extrusion molding was performed under the following conditions using a LABO PLASTOMILLT die extrusion molding apparatus (manufactured by Toyo Seiki Seisaku-sho, Ltd.) equipped with an extruder, a T-die, a cooling roll, and a winder.
[0496] Extruder
[0497] Screw diameter D: 20mmΦ, L / D=25 (L: screw length)
[0498] Screw speed: 14rpm
[0499] Set temperature: 190~210℃
[0500] T-die
[0501] Die width: 150mm, die lip width: 0.4mm
[0502] Set temperature: 205℃
[0503] Cooling roller
[0504] Set temperature: 50℃
[0505] Winding machine
[0506] Winding speed: 1.0m / min
[0507] The obtained film was used to evaluate the film according to the above method. The results are shown in Table 8.
[0508] Reference Examples 3 to 7 (Production of Thermoplastic Resin Film)
[0509] The polyimide resin pellets 1 obtained in Production Example 1 and the polyamide resin PA6 ("UBE Nylon 1030B" manufactured by Ube Industries, Ltd.) as the crystalline thermoplastic resin (B2-3) were used in the ratio shown in Table 8. PA6 was pre-dried at 80°C for 10 hours or more before use.
[0510] PA6 was introduced from the hopper on the lower side of a co-rotating twin-screw kneading extruder ("HK-25D" manufactured by Parker Corporation), and polyimide resin pellets 1 were introduced into the extruder from a side feeder, and kneading was performed under the conditions of a barrel setting temperature of 260°C, a feed rate of 6 kg / hour, and a screw speed of 200 rpm to extrude strands. The strands extruded from the extruder were water-cooled and pelletized using a pelletizer ("Fan cutter FC-Mini-4 / N" manufactured by Star Plastics Co., Ltd.), and the pellets were used to produce a single-layer film by extrusion molding.
[0511] Extrusion molding was performed under the following conditions using a LABO PLASTOMILLT die extrusion molding apparatus (manufactured by Toyo Seiki Seisaku-sho, Ltd.) equipped with an extruder, a T-die, a cooling roll, and a winder.
[0512] Extruder
[0513] Screw diameter D: 20mmΦ, L / D=25
[0514] Screw speed: 16rpm
[0515] Set temperature: 240~265℃
[0516] T-die
[0517] Die width: 150mm, die lip width: 0.4mm
[0518] Set temperature: 260℃
[0519] Cooling roller
[0520] Set temperature: 48℃
[0521] Winding machine
[0522] Winding speed: 1.0m / min
[0523] The obtained film was used to evaluate the film according to the above method. The results are shown in Table 8.
[0524] Reference Examples 8 to 9 (Production of Thermoplastic Resin Film)
[0525] The polyimide resin particles 1 obtained in Preparation Example 1 and the polyamide resin MXD6 as the crystalline thermoplastic resin (B2-6): poly(m-xylylene adipamide), "S6011" manufactured by Mitsubishi Gas Chemical Co., Ltd., melting point 237°C, glass transition temperature 85°C were used in the proportions shown in Table 8. MXD6 was pre-dried at 80°C for 10 hours or more before use.
[0526] MXD6 was introduced from the hopper on the lower side of a co-rotating twin-screw kneading extruder ("HK-25D" manufactured by Parker Corporation), and polyimide resin pellets 1 were introduced into the extruder from a side feeder, and kneading was performed under the conditions of a barrel setting temperature of 260°C, a feed rate of 6 kg / hour, and a screw speed of 200 rpm to extrude strands. The strands extruded from the extruder were water-cooled and pelletized using a pelletizer ("Fan cutter FC-Mini-4 / N" manufactured by Star Plastics Co., Ltd.), and a single-layer film was produced by extrusion molding using the pellets.
[0527] Extrusion molding was performed under the following conditions using a LABO PLASTOMILLT die extrusion molding apparatus (manufactured by Toyo Seiki Seisaku-sho, Ltd.) equipped with an extruder, a T-die, a cooling roll, and a winder.
[0528] Extruder
[0529] Screw diameter D: 20mmΦ, L / D=25
[0530] Screw speed: 40rpm
[0531] Set temperature: 240~260℃
[0532] T-die
[0533] Die width: 150mm, die lip width: 0.4mm
[0534] Set temperature: 260℃
[0535] Cooling roller
[0536] Set temperature: 75℃
[0537] Winding machine
[0538] Winding speed: 1.8m / min (reference example 8), 1.2m / min (reference example 9)
[0539] The obtained film was used to evaluate the film according to the above method. The results are shown in Table 8.
[0540] [Table 8]
[0541] Table 8
[0542]
[0543] The components described in Table 8 are as follows.
[0544] (A1) Polyimide resin particles 1: polyimide resin particles obtained in Production Example 1
[0545] (B2-1) Polypropylene resin: "Novatec FY6" manufactured by Japan Polypropylene Corporation
[0546] (B2-3) Polyamide resin PA6: Ube Industries, Ltd. "UBE Nylon 1030B"
[0547] (B2-6) Polyamide resin MXD6: poly(m-xylylene adipamide), "S6011" manufactured by Mitsubishi Gas Chemical Co., Ltd.
[0548] Industrial Applicability
[0549] According to the present invention, it is possible to provide a resin composition, a resin molded body and a method for producing the same, which have improved properties such as heat resistance and mechanical properties while maintaining the lightness of the resin in a thermoplastic resin such as a low-melting-point crystalline thermoplastic resin, an amorphous thermoplastic resin with a low glass transition temperature, or a thermosetting resin.
Claims
1. A resin composition comprising: polyimide resin particles (A), and a thermoplastic resin (B) or a thermoplastic resin (B) and a thermosetting resin (C), wherein the polyimide resin particles (A) comprise a repeating structural unit represented by the following formula (1) and a repeating structural unit represented by the following formula (2), wherein the content ratio of the repeating structural unit of the formula (1) is 20 to 70 mol% relative to the total of the repeating structural unit of the formula (1) and the repeating structural unit of the formula (2), and the volume average particle size D50 is 5 to 200 μm, in, The polyimide resin particles (A) are porous, with an average pore diameter of 5 to 85 nm. R 1 is a divalent group having 6 to 22 carbon atoms and containing at least one alicyclic hydrocarbon structure, R 2 is a divalent chain aliphatic group having 5 to 16 carbon atoms, X 1 and X 2 are each independently a tetravalent group having 6 to 22 carbon atoms and containing at least one aromatic ring, The mass ratio (A) / {(B)+(C)} of the polyimide resin particles (A) to the total amount of the thermoplastic resin (B) and the thermosetting resin (C) is in the range of 15 / 85 to 80 / 20.
2. The resin composition according to claim 1, in, The mass ratio (A) / {(B)+(C)} of the polyimide resin particles (A) to the total amount of the thermoplastic resin (B) and the thermosetting resin (C) is in the range of 30 / 70 to 80 / 20.
3. The resin composition according to claim 1 or 2, in, The thermoplastic resin (B) is at least one selected from the group consisting of the following (B1) and (B2), (B1) an amorphous thermoplastic resin having a glass transition temperature lower than the melting point of the polyimide resin particles (A); (B2) A crystalline thermoplastic resin having a melting point lower than that of the polyimide resin particles (A), or a glass transition temperature lower than the glass transition temperature of the polyimide resin particles (A).
4. The resin composition according to claim 1 or 2, in, The thermoplastic resin (B) is at least one selected from the group consisting of polystyrene resin, polyvinyl chloride, polyvinylidene chloride, polymethyl methacrylate, acrylonitrile-butadiene-styrene resin, polycarbonate resin, polysulfone resin, polyphenylsulfone resin, polyarylate resin, polyphenylene ether resin, polyethersulfone resin, polyetherimide resin, polyamideimide resin, polyolefin resin, polyamide resin, polyacetal resin, polyphenylene sulfide resin, polyester resin, liquid crystal polymer, fluororesin, polymethylpentene resin, and polyurethane resin.
5. The resin composition according to claim 1 or 2, in, The thermosetting resin (C) is at least one selected from the group consisting of epoxy resin, phenolic resin, urea resin, melamine resin, unsaturated polyimide resin, bismaleimide resin, silicone resin, urethane resin, casein resin, furan resin, alkyd resin, and xylene resin.
6. The resin composition according to claim 5, in, The epoxy resin is a two-component curing epoxy resin composition in which the main agent is tetraglycidyl diaminodiphenylmethane and the curing agent is diaminodiphenyl sulfone.
7. The resin composition according to claim 1 or 2, in, The polyimide resin constituting the polyimide resin particles (A) is a non-terminated polyimide resin.
8. A resin molded article comprising: polyimide resin particles (A), and a thermoplastic resin (B) or a cured product of a thermoplastic resin (B) and a thermosetting resin (C), wherein the polyimide resin particles (A) comprise a repeating structural unit represented by the following formula (1) and a repeating structural unit represented by the following formula (2), wherein the content ratio of the repeating structural unit of the formula (1) is 20 to 70 mol % relative to the total of the repeating structural unit of the formula (1) and the repeating structural unit of the formula (2), and the volume average particle size D50 is 5 to 200 μm, in, The polyimide resin particles (A) are porous, with an average pore diameter of 5 to 85 nm. R 1 is a divalent group having 6 to 22 carbon atoms and containing at least one alicyclic hydrocarbon structure, R 2 is a divalent chain aliphatic group having 5 to 16 carbon atoms, X 1 and X 2 are each independently a tetravalent group having 6 to 22 carbon atoms and containing at least one aromatic ring, The mass ratio (A) / {(B)+(C)} of the polyimide resin particles (A) to the total amount of the thermoplastic resin (B) and the thermosetting resin (C) is in the range of 15 / 85 to 80 / 20.
9. A method for producing a resin molded body according to claim 8, in, The manufacturing method comprises the following steps: The resin composition containing the polyimide resin particles (A) and the thermoplastic resin (B) or the thermoplastic resin (B) and the thermosetting resin (C) is molded at a temperature lower than the melting point of the polyimide resin particles (A).
10. The method for producing a resin molded body according to claim 9, in, The thermoplastic resin (B) is at least one selected from the group consisting of the following (B1) and (B2), (B1) an amorphous thermoplastic resin having a glass transition temperature lower than the melting point of the polyimide resin particles (A); (B2) A crystalline thermoplastic resin having a melting point lower than that of the polyimide resin particles (A), or a glass transition temperature lower than the glass transition temperature of the polyimide resin particles (A).
11. The method for producing a resin molded body according to claim 10, in, The thermoplastic resin (B) is the amorphous thermoplastic resin (B1), and the production method comprises the following steps: extruding a resin composition containing the polyimide resin particles (A) and the amorphous thermoplastic resin (B1) at a temperature lower than the melting point of the polyimide resin particles (A) and higher than the glass transition temperature of the amorphous thermoplastic resin (B1).
12. The method for producing a resin molded body according to claim 10, in, The thermoplastic resin (B) is the crystalline thermoplastic resin (B2), and the production method comprises the following steps: extruding a resin composition containing the polyimide resin particles (A) and the crystalline thermoplastic resin (B2) at a temperature lower than the melting point of the polyimide resin particles (A) and higher than the melting point of the crystalline thermoplastic resin (B2).