Substrate with anti-glare layer, image display device, and method for producing substrate with anti-glare layer
By using fluorine-containing organic group-containing polysiloxane to form an anti-glare layer with an uneven structure on the glass substrate of the image display device, the problem of insufficient coating and adhesion of the anti-glare layer in the prior art is solved, and the problem of insufficient coating and adhesion of the anti-glare layer in the prior art is realized. Improves anti-glare and visual recognition, and reduces glare.
Patent Information
- Application Number
- CN202080078781.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-11-15
- Filing Date
- 2020-11-11
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2040-11-11
AI Technical Summary
The prior art has dangerous problems when etching the surface of the glass substrate using a pharmaceutical agent, and the anti-glare layer formed is insufficient in coating and adhesion, which leads to a glare phenomenon when external light is reflected in the image display device.
Polysiloxane containing fluorine organic group is used as the anti-glare coating composition, and an anti-glare layer with an uneven structure is formed on the substrate by spraying, controlling the surface coverage and haze of the convex portions, and combining high refractive rate layer to reduce reflected light.
The substrate and image display device are achieved with excellent anti-glare properties and no glare occurs, which improves visual recognition, coating and adhesion, and reduces the appearance of reflected light.
Smart Images

Figure GDA0003640275890000211 
Figure GDA0003640275890000221 
Figure GDA0003640275890000222
Abstract
Description
Technical Field
[0001] The present invention relates to a substrate with an antiglare layer which has excellent antiglare properties (antiglare function), does not cause glare (sparkling), and provides good visibility, an image display device having the substrate, and a method for producing a substrate with an antiglare layer. Background Art
[0002] When external light such as indoor lighting (fluorescent lighting, etc.) and sunlight is reflected on the display surface of an image display device (liquid crystal display, organic EL display, plasma display, etc.) included in various devices such as televisions, personal computers, and smartphones, the visibility of the image is sometimes reduced due to the reflected image.
[0003] As a method of suppressing the reflection of external light, there is a method of performing an anti-glare treatment on the display surface of an image display device. As a method of anti-glare treatment, there are proposed: etching the surface of a transparent substrate such as glass using a chemical such as fluoric acid (see Patent Document 1); and forming an organic anti-glare layer having a concave-convex surface on the surface (see Patent Document 2).
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent Document 1: Japanese Patent No. 5839134
[0007] Patent Document 2: International Publication No. 2018 / 070426 Summary of the invention
[0008] Problems to be solved by the invention
[0009] However, in the process of etching the surface of a glass substrate using chemicals, the danger of the chemicals becomes a problem, and in the process of forming an organic anti-glare layer on the surface, problems may arise in terms of coating properties on the glass substrate, coating properties when further forming a functional layer on the film, and adhesion.
[0010] Furthermore, with the recent advancement in the definition of image display devices, when an anti-glare layer is disposed on the display surface side, there is also a problem that a glare phenomenon in which random light intensity appears on the surface is likely to occur.
[0011] According to the above aspects, the object of the present invention is to provide a substrate with an anti-glare layer that has excellent anti-glare properties (anti-glare function), does not cause glare, and provides good visual recognition, and an image display device having the substrate. It also aims to provide a substrate with an anti-glare layer that has excellent coating properties and adhesion when forming a functional layer, an image display device having the substrate, and a method for manufacturing a substrate with an anti-glare layer.
[0012] Solutions for solving problems
[0013] The inventors have found that the above-mentioned problems can be solved by the following configuration, and have completed the present invention.
[0014] The present invention is as follows.
[0015] 1. A substrate with an anti-glare layer, characterized in that it comprises: a substrate; and an anti-glare layer, which is formed directly on the substrate or on the substrate with the aid of other layers, and has a concave-convex structure on the surface of the anti-glare layer, the anti-glare layer is formed by a cured product of an anti-glare film-forming composition, the anti-glare film-forming composition contains a polysiloxane having a fluorine-containing organic group, and the convex surface coverage of the anti-glare layer is 5% to 70%.
[0016] 2. The substrate with an anti-glare layer according to 1, wherein the height of the convex parts of the concavo-convex structure is 50 nm to 2000 nm.
[0017] 3. The substrate with an anti-glare layer according to 1 or 2, wherein the haze of the anti-glare layer is 0.3% to 40%.
[0018] 4. The substrate with an anti-glare layer according to any one of 1 to 3, wherein the refractive index of the anti-glare layer is in the range of 1.3 to 1.49.
[0019] 5. The substrate with an anti-glare layer according to any one of 1 to 4, wherein the anti-glare layer is formed on a high refractive index layer, and the refractive index of the high refractive index layer is higher than that of the anti-glare layer.
[0020] 6. The substrate with an anti-glare layer according to 5, wherein the refractive index of the high refractive index layer is in the range of 1.5 to 2.1.
[0021] 7. The substrate with an anti-glare layer according to any one of 1 to 6, further comprising: a functional layer formed on the anti-glare layer.
[0022] 8. An image display device comprising the substrate with an anti-glare layer according to any one of 1 to 7.
[0023] 9. A method for producing a substrate with an anti-glare layer, comprising: applying a coating liquid for forming an anti-glare film containing a polysiloxane having a fluorine-containing organic group onto a substrate to form the anti-glare layer.
[0024] Effects of the Invention
[0025] According to the present invention, a substrate with an anti-glare layer having excellent anti-glare properties (anti-glare function), no glare (flashing), and good visual recognition, and an image display device having the substrate can be provided. A substrate with an anti-glare layer having excellent coating properties and adhesion when forming a functional layer, an image display device having the substrate, and a method for manufacturing a substrate with an anti-glare layer can also be provided. DETAILED DESCRIPTION
[0026] Hereinafter, the present invention will be described in further detail.
[0027] <Anti-glare coating layer forming composition>
[0028] The anti-glare-forming composition used in the present invention comprises at least a polysiloxane having a fluorine-containing organic group (hereinafter also referred to as component (A)) and a solvent that dissolves the polysiloxane.
[0029] <Ingredients (A)>
[0030] Component (A) is a polysiloxane having an organic group substituted by a fluorine atom in the side chain. Such an organic group substituted by a fluorine atom is an organic group in which a part or all of the hydrogen atoms of an aliphatic group or an aromatic group are substituted by fluorine atoms. As for the above-mentioned organic group substituted by a fluorine atom, preferably an alkyl group in which a part or all of the hydrogen atoms are substituted by fluorine atoms, an alkyl group containing an ether bond in which a part or all of the hydrogen atoms are substituted by fluorine atoms, an organic group containing a phenyl group in which a part or all of the hydrogen atoms are substituted by fluorine atoms, etc. are preferred. The number of fluorine atoms possessed by the above-mentioned organic group substituted by a fluorine atom is also not particularly limited. The preferred number of carbon atoms of the above-mentioned organic group substituted by a fluorine atom is 1 to 20, more preferably 3 to 15, and particularly preferably 3 to 8. If their specific examples are listed, they can be listed as: trifluoropropyl, tridecafluorooctyl, heptadecafluorodecyl, pentafluorophenylpropyl.
[0031] Among these, from the viewpoint of easily obtaining a highly transparent coating film, an organic group having a perfluoroalkyl group is preferred, and an organic group represented by the following formula (F) is more preferred.
[0032] CF3(CF2) k CH2CH2-* (F)
[0033] (In the formula, k is an integer from 0 to 12. * indicates the bonding position.)
[0034] Specific examples of the organic group represented by the above formula (F) include a trifluoropropyl group, a tridecafluorooctyl group, and a heptadecafluorodecyl group.
[0035] In the present invention, a plurality of polysiloxanes having the above-mentioned side chains may be used in combination.
[0036] The method for obtaining the polysiloxane having an organic group substituted with a fluorine atom in a side chain is not particularly limited, and is generally obtained by polycondensing the alkoxysilane compound having an organic group in a side chain.
[0037] Among them, polysiloxane obtained by polycondensing an alkoxysilane component containing an alkoxysilane compound represented by formula (1) is preferred.
[0038] R 11 Si(OR 12 )3 (1)
[0039] Here, R in formula (1) 11 The above-mentioned organic group substituted with a fluorine atom is represented, and the number of fluorine atoms contained in the organic group is not particularly limited.
[0040] In addition, R in formula (1) 12 It represents a hydrocarbon group having 1 to 5 carbon atoms, preferably a saturated hydrocarbon group having 1 to 5 carbon atoms, and more preferably a methyl group, an ethyl group, a propyl group or a butyl group.
[0041] Among the alkoxysilanes represented by the formula (1), R 11 is a perfluoroalkyl alkoxysilane, more preferably R 11 An alkoxysilane which is an organic group represented by the above formula (F).
[0042] Specific examples of the alkoxysilane having an organic group represented by formula (F) include trifluoropropyltrimethoxysilane, trifluoropropyltriethoxysilane, tridecafluorooctyltrimethoxysilane, tridecafluorooctyltriethoxysilane, heptadecafluorodecyltrimethoxysilane, heptadecafluorodecyltriethoxysilane, and the like.
[0043] In particular, from the viewpoint of easily obtaining a coating film having high transparency, it is preferred that k is an integer of 2 to 12.
[0044] In the present invention, at least one kind of the alkoxysilane represented by the formula (1) may be used, and a plurality of kinds may be used as necessary.
[0045] In addition, the polysiloxane having an organic group substituted by a fluorine atom in a side chain may also be a polysiloxane obtained by polycondensing the following alkoxysilane component, wherein the alkoxysilane component comprises an alkoxysilane compound other than the alkoxysilane compound shown in the above formula (1) (hereinafter, also referred to as other alkoxysilane compounds). As a specific example of other alkoxysilane compounds, at least one selected from the group consisting of the alkoxysilane compound shown in the following formula (2) and the alkoxysilane compound shown in the following formula (3) may be cited, but is not limited thereto.
[0046] Si(OR 2 )4 (2)
[0047] R 31 n Si(OR 32 ) 4-n (3)
[0048] (Where R 31 represents an organic group or a hydrogen atom not substituted by a fluorine atom, R 32 represents a hydrocarbon group having 1 to 5 carbon atoms, and n is an integer of 1 to 3. )
[0049] R in formula (2) 2 It represents a hydrocarbon group. The fewer the carbon atoms, the higher the reactivity. Therefore, it is preferably a saturated hydrocarbon group having 1 to 5 carbon atoms, and more preferably a methyl group, an ethyl group, a propyl group or a butyl group.
[0050] Specific examples of such tetraalkoxysilane include tetramethoxysilane, tetraethoxysilane, tetrapropoxysilane, tetrabutoxysilane, and the like, which are easily available as commercial products.
[0051] R in formula (3) 32 R each independently represents a hydrocarbon group having 1 to 5 carbon atoms. 32 They may be the same or different.
[0052] R in formula (3) 31 It is preferably an organic group having 1 to 20 carbon atoms, and more preferably an organic group having 1 to 15 carbon atoms. 31 They may be the same or different. Examples of the above-mentioned organic groups not substituted by fluorine atoms include: alkyl groups having 1 to 18 carbon atoms, such as methyl, ethyl, propyl, butyl, pentyl, hexyl, heptyl, octyl, and stearyl (octadecyl); alkenyl groups having 2 to 18 carbon atoms, such as vinyl; cycloalkyl groups, such as cyclohexyl; alkyl groups containing (meth)acryloyloxy groups, such as 3-(meth)acryloyloxypropyl (γ-(meth)acryloyloxypropyl); alkyl groups containing hydroxyl groups, such as 3-hydroxypropyl; γ-urea (3-urea) )propyl group; alkyl groups containing an amino group such as γ-amino(3-amino)propyl, 2-aminoethylaminomethyl, 3-(N-phenylvinylmethyl-2-aminoethylamino)propyl group; alkyl groups containing an epoxy group such as γ-glycidoxy(3-glycidyloxy)propyl, 2-(3,4-epoxycyclohexyl)ethyl group; alkyl groups containing a mercapto group such as γ-mercapto(3-mercapto)propyl group; alkyl groups containing an isocyanate group such as 3-isocyanatepropyl group; aryl groups such as phenyl group, etc.
[0053] Among these, a methyl group, an ethyl group, a propyl group, a butyl group, a pentyl group, a heptyl group, an octyl group, a dodecyl group, a hexadecyl group, an octadecyl group, a phenyl group, a vinyl group, a γ-aminopropyl group, a γ-glycidoxypropyl group, and a γ-methacryloxypropyl group are more preferable.
[0054] Specific examples of the alkoxysilane represented by the formula (3) include methyltrimethoxysilane, methyltriethoxysilane, ethyltrimethoxysilane, ethyltriethoxysilane, propyltrimethoxysilane, propyltriethoxysilane, butyltrimethoxysilane, butyltriethoxysilane, pentyltrimethoxysilane, pentyltriethoxysilane, heptyltrimethoxysilane, heptyltriethoxysilane, octyltrimethoxysilane, octyltriethoxysilane, dodecyltrimethoxysilane, dodecyltriethoxysilane, hexadecyltrimethoxysilane, hexadecyltriethoxysilane, octadecyltrimethoxysilane, octadecyltriethoxysilane, phenyltrimethoxysilane, phenyltriethoxysilane, vinyltrimethoxysilane, vinyltriethoxysilane. The present invention also includes, but is not limited to, trialkoxysilanes such as silane, 3-isocyanatepropyltrimethoxysilane, 3-isocyanatepropyltriethoxysilane, 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, γ-glycidoxypropyltrimethoxysilane, γ-glycidoxypropyltriethoxysilane, γ-mercaptopropyltrimethoxysilane, γ-mercaptopropyltriethoxysilane, 3-acryloxypropyltrimethoxysilane, 3-acryloxypropyltriethoxysilane, γ-methacryloxypropyltrimethoxysilane, γ-methacryloxypropyltriethoxysilane, γ-ureidopropyltrimethoxysilane, and γ-ureidopropyltriethoxysilane, and dialkoxysilanes such as dimethyldimethoxysilane and dimethyldiethoxysilane.
[0055] From the viewpoint of easily obtaining a coating, the total amount of the alkoxysilane compound represented by formula (1) is preferably 3 mol% or more, more preferably 5 mol% or more, relative to 100 mol% of the total alkoxysilane compound used to obtain component (A). In addition, from the viewpoint of suppressing the formation of gel and foreign matter, it is preferably 40 mol% or less, more preferably 30 mol% or less.
[0056] The upper limit of the amount of other alkoxysilane compounds used is preferably 97 mol% or less, more preferably 95 mol% or less, relative to 100 mol% of the total of all alkoxysilane compounds used to obtain component (A). The lower limit is preferably 60 mol% or more, more preferably 70 mol% or more.
[0057] (Synthesis of polysiloxane)
[0058] The method for condensing the polysiloxane used in the present invention is not particularly limited, and for example, a method of hydrolyzing / condensing the alkoxysilane in a solvent such as an alcohol or a glycol can be cited. In this case, the hydrolysis / condensation reaction can also be any of partial hydrolysis and complete hydrolysis. In the case of complete hydrolysis, in theory, 0.5 times the mole of water of all the alkoxy groups in the alkoxysilane can be added, and usually more than 0.5 times the mole of water is added.
[0059] In the present invention, the amount of water used in the above reaction can be appropriately selected as desired, but is generally 0.1 to 7 times by mole, preferably 0.1 to 5 times by mole, based on all alkoxy groups in the alkoxysilane.
[0060] In addition, usually, for the purpose of promoting hydrolysis / condensation reaction, acids such as hydrochloric acid, sulfuric acid, nitric acid, acetic acid, formic acid, oxalic acid, and maleic acid; bases such as ammonia, methylamine, ethylamine, ethanolamine, and triethylamine; metal salts of hydrochloric acid, sulfuric acid, or nitric acid can also be used as catalysts. In this case, the amount of the catalyst used in the reaction is preferably about 0.001 to 0.1 times the mole of all alkoxy groups in the alkoxysilane, and more preferably 0.01 to 0.06 times the mole. Moreover, the hydrolysis / condensation reaction is also usually promoted by heating the solution in which the alkoxysilane is dissolved. At this time, the heating temperature and heating time can be appropriately selected according to the expectations. Preferably, the reaction system is set to 50°C to 180°C, and is carried out in a closed container or under reflux for tens of minutes to tens of hours in a manner that does not cause evaporation or volatilization of the liquid. For example, methods such as heating / stirring at 50°C for 24 hours and heating / stirring under reflux for 2 to 10 hours can be listed.
[0061] In addition, as other methods, for example, a method of heating a mixture of alkoxysilane, solvent and oxalic acid can be cited. Specifically, after adding oxalic acid to alcohol in advance to prepare an alcohol solution of oxalic acid, the solution is mixed with alkoxysilane and heated. At this time, the amount of oxalic acid is generally set to 0.2 to 2 moles, preferably 0.5 to 2 moles, relative to 1 mole of all alkoxy groups possessed by alkoxysilane. The heating under this method is carried out at a liquid temperature of 50°C to 180°C, preferably, in a manner that does not cause evaporation, volatilization, etc. of the liquid, for example, in a closed container or under reflux for tens of minutes to tens of hours.
[0062] In each of the above-mentioned methods, when a plurality of alkoxysilanes are used, the plurality of alkoxysilanes may be mixed in advance and used, or the plurality of alkoxysilanes may be added sequentially.
[0063] When alkoxysilane is polycondensed by the above method, the total amount of silicon atoms of the alkoxysilane charged is converted to a concentration of SiO2 (hereinafter referred to as SiO2 conversion concentration) which is usually set to 20% by mass or less, preferably 15% by mass or less. By selecting an arbitrary concentration within such a concentration range, the formation of gel can be suppressed to obtain a homogeneous polysiloxane solution.
[0064] The solvent used when polycondensing the alkoxysilane is not particularly limited as long as it dissolves the alkoxysilane compound. Generally, alcohol is generated by the polycondensation reaction of the alkoxysilane, so alcohols or organic solvents having good compatibility with alcohols are used.
[0065] Specific examples of the solvent used in the polycondensation include alcohols such as methanol, ethanol, propanol, and n-butanol; glycol ethers such as ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, diethylene glycol monomethyl ether, and diethylene glycol monoethyl ether, etc. In the present invention, a plurality of the above organic solvents may be mixed and used.
[0066] <Anti-glare film-forming composition>
[0067] The method for preparing the coating liquid (hereinafter, also referred to as coating liquid or coating liquid for anti-glare film formation) as the composition for forming an anti-glare film of the present invention is not particularly limited. As an example, the following solvent group (A), solvent group (B) and other solvent groups may be added to the polysiloxane solution obtained as described above, as well as as needed. In addition, as needed, a method for preparing the polysiloxane solution by concentrating or replacing it with other solvents may also be used.
[0068] <Solvent Group (A)>
[0069] The solvent group (A) contained in the coating liquid for forming an anti-glare coating of the present invention is at least one selected from glycol ethers and their derivatives or ketones having a boiling point of less than 160° C. Specifically, glycol ethers and their derivatives such as ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monopropyl ether, ethylene glycol monomethyl ether acetate, ethylene glycol monoethyl ether acetate, ethylene glycol dimethyl ether, ethylene glycol diethyl ether, ethylene glycol dipropyl ether, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol monomethyl ether acetate, propylene glycol dimethyl ether, and propylene glycol diethyl ether can be listed; and ketones such as acetone, methyl ethyl ketone, and methyl isobutyl ketone are preferred, among which ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol diethyl ether, ethylene glycol dipropyl ether, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol monomethyl ether acetate, and methyl isobutyl ketone are preferred from the viewpoint of coating stability.
[0070] The content of solvent group (A) in the coating liquid for forming an anti-glare coating is 0.1 to 300 parts by mass, preferably 0.3 to 100 parts by mass, and particularly preferably 0.8 to 50 parts by mass, relative to 1 part by mass of the total amount of silicon atoms possessed by component (A) converted into the mass of SiO2.
[0071] <Solvent Group (B)>
[0072] The solvent group (B) contained in the coating liquid for forming an anti-glare coating of the present invention is at least one selected from alcohols having a boiling point of 120° C. or less. Specifically, the solvent group (B) includes methanol, ethanol, 1-propanol, 2-propanol, 1-butanol, 2-butanol, 2-methyl-1-propanol, and 2-methyl-2-propanol. Among them, methanol, ethanol, 2-propanol, 2-butanol, and 2-methyl-1-propanol are preferred from the viewpoint of storage stability of the composition.
[0073] The content of solvent group (B) in the coating liquid for forming an anti-glare coating is 0.5 to 500 parts by mass, preferably 1 to 200 parts by mass, and particularly preferably 2 to 150 parts by mass, relative to 1 part by mass of the total amount of silicon atoms possessed by component (A) converted into the mass of SiO2.
[0074] <Other solvents>
[0075] The antiglare film-forming coating liquid of the present invention may contain solvents other than the solvent groups (A) and (B) (hereinafter also referred to as other solvents) as necessary from the viewpoint of the stability of the coating liquid.
[0076] Examples of other solvents include: alcohols such as hexanol, heptanol, octanol, nonanol, decanol, undecanol, dodecanol, and diacetone alcohol; glycols such as ethylene glycol, diethylene glycol, dipropylene glycol, 2-methyl-2,4-pentanediol, propylene glycol, butanediol, pentanediol, hexanediol, and heptanediol; ethylene glycol monobutyl ether, ethylene glycol dibutyl ether, propylene glycol monopropyl ether, propylene glycol monobutyl ether, propylene glycol dimethyl ether, propylene glycol diethyl ether, propylene glycol dipropyl ether, propylene glycol dibutyl ether, Glycol ethers such as diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol monopropyl ether, diethylene glycol monobutyl ether, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, diethylene glycol dipropyl ether, and diethylene glycol dibutyl ether; esters such as methyl acetate, ethyl acetate, and ethyl lactate; N-methyl-2-pyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide, γ-butyrolactone, dimethyl sulfoxide, tetramethyl urea, hexamethylphosphorotriamide, m-cresol, tetrahydrofuran, etc. Among them, ethylene glycol, diethylene glycol, 2-methyl-2,4-pentanediol, propylene glycol, butylene glycol, ethylene glycol monobutyl ether, propylene glycol monopropyl ether, propylene glycol monobutyl ether, propylene glycol dimethyl ether, propylene glycol diethyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol monopropyl ether, diethylene glycol monobutyl ether, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, diethylene glycol dipropyl ether, diethylene glycol dibutyl ether, N-methyl-2-pyrrolidone, N,N-dimethylformamide, and tetrahydrofuran are preferably used.
[0077] The total amount of silicon atoms in the component (A) in the anti-glare film-forming coating liquid is preferably 0.2 to 10% by mass, more preferably 0.5 to 8% by mass, when converted to SiO 2 (SiO 2 conversion concentration).
[0078] <Other ingredients>
[0079] In the present invention, other components other than the component (A) and the solvent group (A) and (B), for example, inorganic fine particles, metalloxane oligomers, metalloxane polymers, leveling agents, surfactants and the like may be contained.
[0080] The inorganic particles are preferably particles such as silicon dioxide particles, aluminum oxide particles, titanium dioxide particles, and magnesium fluoride particles, and colloidal solutions of these inorganic particles are particularly preferred. The colloidal solution may be a colloidal solution obtained by dispersing inorganic particle powder in a dispersion medium, or a commercially available colloidal solution.
[0081] In the present invention, by containing inorganic particles, the surface shape and other functions of the formed cured film can be given. As inorganic particles, the average particle size is preferably 0.001 to 0.2 μm, and more preferably 0.001 to 0.1 μm. When the average particle size of the inorganic particles exceeds 0.2 μm, the transparency of the cured film formed using the coating solution to be prepared may be reduced.
[0082] Examples of the dispersion medium for the inorganic fine particles include water and organic solvents. As the colloidal solution, the pH or pKa is preferably adjusted to 1 to 10, and more preferably 2 to 7, from the viewpoint of the stability of the coating solution for forming a coating film.
[0083] As the organic solvent used in the dispersion medium of the colloidal solution, there can be listed: alcohols such as methanol, ethanol, propanol, butanol, ethylene glycol, propylene glycol, butanediol, pentanediol, 2-methyl-2,4-pentanediol, diethylene glycol, dipropylene glycol, ethylene glycol monopropyl ether; ketones such as methyl ethyl ketone and methyl isobutyl ketone; aromatic hydrocarbons such as toluene and xylene; amides such as dimethylformamide, dimethylacetamide, N-methylpyrrolidone; esters such as ethyl acetate, butyl acetate, γ-butyrolactone; ethers such as tetrahydrofuran and 1,4-dioxane. Among these, alcohols and ketones are preferred. These organic solvents can be used as dispersion medium alone or in a mixture of two or more.
[0084] As metalloxane oligomers or metalloxane polymers, single or composite oxide precursors of silicon, titanium, zirconium, aluminum, tantalum, antimony, bismuth, tin, indium, zinc, etc. are used. As metalloxane oligomers or metalloxane polymers, commercial products may be used, or substances obtained by conventional methods such as hydrolysis of monomers such as metal alkoxides, nitrates, hydrochlorides, and carboxylates.
[0085] <Anti-glare layer and formation of anti-glare layer>
[0086] The antiglare layer of the present invention can be obtained by applying the above-mentioned antiglare film-forming coating liquid to a substrate and thermally curing the coating liquid. That is, the antiglare layer is formed from a cured product of the polysiloxane having a fluorine-containing organic group contained in the antiglare film-forming coating liquid.
[0087] Here, the anti-glare layer has a concavo-convex structure on the surface. The concavo-convex structure is a fine concavo-convex structure in which the height of the convex part is 50nm to 2000nm. The overall thickness of the anti-glare layer is 50nm to 3000nm, and the surface side of the anti-glare layer becomes a fine concavo-convex structure. That is, a fine concavo-convex structure is formed on a uniform and flat coating, so it can also be expressed as convex parts intermittently formed on a flat coating. It should be noted that, in this case, the part where the convex part is not formed is a concave part. The convex part surface coverage, which is the proportion of the convex parts of the fine concavo-convex structure, is 5% to 70%, preferably 10% to 60%.
[0088] Specifically, the surface coverage of the convex portion can be measured by the following method. That is, the surface shape is measured using a white light interference optical microscope (ContourGT, manufactured by BRUKER), and the shape analysis is further performed. The surface shape measurement is performed under the following appropriate conditions: using the VSI measurement method and using a high-density CCD camera, the zoom lens magnification is 0.55 times, the object lens magnification is 50 times, the measurement area is 230μm×170μm, the light source is a white light source, and in terms of light intensity and threshold (Threshhold), noise is not allowed to enter the measurement as much as possible. Moreover, as a shape analysis, after color filtering in Terms Removal (Cylinder and Tilt), the image is processed into a grayscale of 256 levels. The above-mentioned convex surface coverage is measured at any part of the film surface, the processed image is divided into 1900 parts, the brightness of the area is calculated, the area with high brightness is the convex part, the area with low brightness and uniformity is the flat part, and the value calculated by convex part / flat part × 100 is the convex surface coverage of the film surface. The environment during the measurement is 23°C and 30RH%.
[0089] The anti-glare layer has a haze of preferably 0.3% to 40%, more preferably 0.5% to 30%, from the viewpoint of suppressing glare and obtaining an image display device with high visual recognition. It should be noted that in this specification and claims, the haze can be measured according to JIS K7163 using a haze meter (manufactured by SUGA Testing Instruments Co., Ltd., haze meter HZ-V3).
[0090] The flat coating portion and the fine concavo-convex structure can be formed by one coating, but the fine concavo-convex structure can also be formed after the flat coating portion is formed. In addition, the coating liquid for forming the anti-glare coating that forms the flat coating portion and the coating liquid for forming the anti-glare coating that forms the fine concavo-convex structure can be set to the same coating liquid, or the coating liquids of the two can be set to different coating liquids. For example, it can be set that: the composition of the solid components of the two is the same, but the solid component concentration of the coating liquid that forms the fine concavo-convex structure is higher than the solid component concentration of the coating liquid that forms the flat coating portion, or the composition of the solid components of the two can be set to be different. Moreover, it can also be set that the composition of the solid components of the two is the same, but the solvent composition of the two is different, but it is not limited to this.
[0091] As for the fine concave-convex structure, for example, after the anti-glare coating forming coating liquid is applied and before curing, air can be blown on the surface to form fine concave-convex structures on the surface. After the flat coating portion is formed, a coating liquid with a slightly higher concentration can be sprayed to partially form a convex portion. During spraying, the flow rate of the anti-glare coating forming coating liquid and the gas flow rate described later can be adjusted to form fine concave-convex structures, but the invention is not limited to this.
[0092] From the viewpoint of suppressing reflected light, the refractive index of the antiglare layer is selected from the range of, for example, 1.3 to 1.49.
[0093] The coating of the anti-glare film-forming coating liquid for forming an anti-glare layer can also be applied to, for example, a dip coating method, a flow coating method, a spin coating method, a flexographic printing method, an inkjet coating method, a rod coating method, a gravure roll coating method, a roll coating method, a knife coating method, an air doctor coat method, an air knife coating method, a wire doctor coat method, a reverse coating method, a transfer roll coating method, a micro gravure coating method, a kiss coat method, a cast coating method, a slot orifice coating method, a calender coating method, a die coating method and the like known or well-known methods, but the anti-glare film-forming coating liquid of the present invention is characterized in that it is particularly suitable for a spray coating method.
[0094] Examples of the substrate include known or well-known substrates such as plastics, glass, and ceramics. Examples of the plastic include plates and films of polycarbonate, poly(meth)acrylate, polyethersulfone, polyarylate, polyurethane, polysulfone, polyether, polyetherketone, trimethylpentene, polyolefin, polyethylene terephthalate, (meth)acrylonitrile, triacetyl cellulose, diacetyl cellulose, and cellulose acetate butyrate.
[0095] The uniform film thickness obtained by the spray coating method as described above can be adjusted by adjusting the amount of chemical solution, nozzle / stage distance (the distance between the nozzle and the stage), coating speed, gas flow rate or gas pressure, etc.
[0096] The amount of the chemical solution is a parameter that determines the film thickness. The film thickness increases as the amount of the chemical solution increases, and the film thickness decreases as the amount of the chemical solution decreases. In spraying, the amount of the chemical solution is, for example, 0.5 to 20 mL (milliliters) / min, preferably 0.8 to 12 mL / min.
[0097] The gas flow rate is a parameter for forming fine droplets. Examples of the gas used include N2 and dry air, but are not particularly limited thereto. In spraying, the gas flow rate is, for example, 3 to 70 L (liters) / min, preferably 6 to 60 L / min. The gas pressure is 30 to 700 kPa, preferably 50 to 650 kPa.
[0098] As a preferred gas flow rate from the viewpoint of forming fine projections and depressions, it is preferred that the gas be ventilated in an atmospheric atmosphere at a flow rate of 150 to 140,000 times, preferably 500 to 75,000 times, relative to the flow rate of the coating liquid for forming an anti-glare coating, so as to refine the droplets of the coating liquid for forming an anti-glare coating and apply it to the surface of the substrate.
[0099] The nozzle / table distance is a parameter related to film thickness, coating properties, and the amount of convex portion coverage on the surface. For example, the film thickness becomes thicker as the distance approaches, and the film thickness becomes thinner as the distance moves away. The preferred nozzle / table distance is, for example, 30 to 200 mm, and more preferably 50 to 150 mm.
[0100] The coating speed is a parameter related to the film thickness and the amount of convex portion coverage on the surface. For example, the film thickness becomes thinner as the speed increases, and the film thickness becomes thicker as the speed decreases. In spray coating, the coating speed is, for example, 50 to 2000 mm / sec, preferably 100 to 1500 mm / sec.
[0101] The thickness of the coating formed on the substrate can be adjusted by the above-mentioned parameters during coating, and can also be easily adjusted by the SiO2 conversion concentration of the coating liquid.
[0102] The coating film formed on the substrate is heated to obtain a coating film. In consideration of the heat resistance of the substrate, etc., the calcination temperature is preferably in the range of 80°C to 300°C, and more preferably in the range of 100°C to 250°C.
[0103] A high refractive index layer having a refractive index higher than that of the anti-glare layer can also be provided under the anti-glare layer of the present invention. In this case, by appropriately adjusting the refractive indices of the anti-glare layer and the high refractive index layer, the reflected light reflected by the surface of the anti-glare layer and the reflected light reflected by the surface of the high refractive index layer interfere with each other in opposite phases, thereby further adding the effect of reducing reflected light.
[0104] Here, the high refractive index layer is not particularly limited as long as it has a higher refractive index than the anti-glare layer. However, in consideration of adhesion with the anti-glare layer, it is preferably a cured product of a coating solution containing a metal alkoxide and an alkoxysilane. For example, a coating disclosed in International Publication No. WO2012-057165 can be used.
[0105] Examples of the high refractive index layer disclosed in the above publication include films obtained by applying and curing a coating liquid containing one or more metal alkoxides of the following formula (A), alkoxysilanes of the formula (B), or condensates thereof.
[0106] M1(OR 1 )n (A)
[0107] (Wherein, M1 represents metals such as silicon (Si), titanium (Ti), tantalum (Ta), zirconium (Zr), boron (B), aluminum (Al), magnesium (Mg), tin (Sn) and zinc (Zn), and R 1 represents an alkyl group having 1 to 5 carbon atoms, and n represents the valence of M1. )
[0108] (R 102 ) n Si(OR 103 ) 4-n (B)
[0109] (Where R 102 represents an alkyl group, an alkenyl group, a cycloalkyl group, an aryl group, or a heteroatom-containing group including the following groups: a group having a heteroatom between carbon atoms of the alkyl group, alkenyl group, cycloalkyl group, and aryl group. Part or all of the hydrogen atoms in the above-mentioned alkyl group, alkenyl group, cycloalkyl group, aryl group, and heteroatom-containing group may be substituted by a substituent, and part of the above-mentioned alkyl group and alkenyl group may also have a cycloalkyl group or an aryl group. R 103 represents an alkyl group having 1 to 5 carbon atoms, and n represents an integer of 1 or 2. )
[0110] Examples of the above-mentioned group having a hetero atom include a group having at least one hetero atom selected from the group consisting of an oxygen atom, a nitrogen atom and a sulfur atom, and examples thereof include: -O-, -NR- (R represents a hydrogen atom or an alkyl group having 1 to 6 carbon atoms), -CO-, -S-, -CO-, and groups formed by combining these.
[0111] Examples of the substituent include halogen atoms such as a fluorine atom, a chlorine atom, a bromine atom, and an iodine atom, a cyano group, a nitro group, a hydroxyl group, an amino group, a urea group, an isocyanate group, and a mercapto group.
[0112] Representative examples of the metal alkoxide represented by formula (A) include, when M1 is titanium, alkoxytitanium such as tetramethoxytitanium, tetraethoxytitanium, tetraisopropoxytitanium, tetra-n-propoxytitanium, tetra-n-butoxytitanium, tetraisobutoxytitanium, tetra-tert-butoxytitanium and tetrapentoxytitanium.
[0113] When M1 is silicon, alkoxysilanes such as tetramethoxysilane, tetraethoxysilane, tetrapropoxysilane, and tetrabutoxysilane may be mentioned.
[0114] As R in formula (B) 102 Specific examples include: alkyl groups having 1 to 18 carbon atoms, such as methyl, ethyl, propyl, butyl, pentyl, hexyl, heptyl, octyl, and stearyl; alkenyl groups such as vinyl; cycloalkyl groups such as cyclohexyl; alkyl groups containing (meth)acryloyloxy groups, such as 3-(meth)acryloyloxypropyl; alkyl groups containing halogen atoms, such as 3-chloropropyl, trifluoropropyl, tridecafluorooctyl, and heptadecafluorodecyl; alkyl groups containing hydroxyl groups, such as 3-hydroxypropyl; γ-ureido (3-ureido)propyl Alkyl groups containing a urea group; alkyl groups containing an amino group such as γ-amino (3-amino) propyl, 2-aminoethylaminomethyl, and 3-(N-phenylvinylmethyl-2-aminoethylamino) propyl; alkyl groups containing an epoxy group such as γ-glycidoxy (3-glycidyloxy) propyl and 2-(3,4-epoxycyclohexyl) ethyl; alkyl groups containing a mercapto group such as γ-mercapto (3-mercapto) propyl; alkyl groups containing an isocyanate group such as 3-isocyanate propyl; and aromatic groups such as phenyl.
[0115] Specific examples of the formula (B) include alkoxysilanes such as trialkoxysilane and dialkoxysilane.
[0116] Specific examples of trialkoxysilanes include methyltrimethoxysilane, methyltriethoxysilane, ethyltrimethoxysilane, ethyltriethoxysilane, propyltrimethoxysilane, propyltriethoxysilane, butyltrimethoxysilane, butyltriethoxysilane, pentyltrimethoxysilane, pentyltriethoxysilane, heptyltrimethoxysilane, heptyltriethoxysilane, octyltrimethoxysilane, octyltriethoxysilane, dodecyltrimethoxysilane, dodecyltriethoxysilane, hexadecyltrimethoxysilane, hexadecyltriethoxysilane, octadecyltrimethoxysilane, octadecyltriethoxysilane, phenyltrimethoxysilane, phenyltriethoxysilane, vinyltrimethoxysilane, vinyltriethoxysilane, 2-aminoethylaminomethyltrimethoxysilane, γ-aminopropyltrimethoxysilane, 3-(2-aminoethylaminopropyl)trimethoxysilane, 3-(2-aminoethylaminopropyl)trimethoxysilane, triethoxysilane, γ-aminopropyl triethoxysilane, γ-glycidoxypropyl trimethoxysilane, γ-glycidoxypropyl triethoxysilane, 2-(3,4-epoxycyclohexyl)ethyl trimethoxysilane, styrylethyl triethoxysilane, 3-(N-styrylmethyl-2-aminoethylamino)propyl trimethoxysilane, p-styryl trimethoxysilane, γ-mercaptopropyl trimethoxysilane, γ-mercaptopropyl Triethoxysilane, γ-methacryloxypropyl trimethoxysilane, γ-methacryloxypropyl triethoxysilane, γ-ureidopropyl trimethoxysilane, γ-ureidopropyl triethoxysilane, trifluoropropyl trimethoxysilane, trifluoropropyl triethoxysilane, tridecafluorooctyl trimethoxysilane, tridecafluorooctyl triethoxysilane, heptadecafluorodecyl trimethoxysilane, heptadecafluorodecyl triethoxysilane, 3-isocyanate propyl triethoxysilane.
[0117] Specific examples of the dialkoxysilane include dimethyldimethoxysilane and dimethyldiethoxysilane.
[0118] Specific examples of the above-mentioned condensation products include: methyl silicate (Silicate) 51, methyl silicate 53, ethyl silicate 40, ethyl silicate 48 (trade name, manufactured by COLCOAT), MKC silicate (trade name, manufactured by Mitsubishi Chemical Corporation), silicone resins manufactured by Toray / Dow Corning, silicone resins manufactured by Momentive Performance Materials Japan, silicone resins manufactured by Shin-Etsu Chemical Co., Ltd., hydroxyl-containing polydimethylsiloxane manufactured by Dow Corning / Asia, silicon oligomers such as silicon oligomers manufactured by Toray / Dow Corning; titanium oligomers such as titanium tetra-n-butoxide and tetramer (manufactured by Kanto Chemical Co., Ltd.), etc.
[0119] The refractive index of the high refractive index layer is higher than that of the anti-glare layer, and is preferably set to a refractive index in which the reflected light reflected from the surface of the anti-glare layer and the reflected light reflected from the surface of the high refractive index layer serving as the interface between the anti-glare layer and the high refractive index layer are in opposite phases, for example, selected from the range of 1.5 to 2.1, more preferably selected from the range of 1.5 to 1.8.
[0120] The refractive index of the high refractive index layer can also be adjusted by adjusting the curing temperature. In this case, it is preferred in the following aspects: the higher the curing temperature, the higher the refractive index of the high refractive index layer. From the viewpoint of considering the heat resistance of the substrate, the sintering temperature is preferably in the range of 100°C to 300°C, and more preferably in the range of 150°C to 250°C.
[0121] The high refractive index layer may be further irradiated with ultraviolet light (UV) after curing to adjust the refractive index of the obtained high refractive index layer. In the high refractive index layer, the ultraviolet irradiation for obtaining the desired refractive index may be performed using, for example, a high pressure mercury lamp. When a high pressure mercury lamp is used, it is preferred that the total light irradiation is 1000 mJ / cm at 365 nm. 2 The irradiation dose is more preferably 2000 mJ / cm 2 ~10000mJ / cm 2 In addition, the UV light source is not particularly specified, and other UV light sources may be used. When other light sources are used, it is sufficient to irradiate the same amount of accumulated light as when the high-pressure mercury lamp is used.
[0122] Next, a functional layer obtained from a specific coating agent may be formed on the surface of the antiglare layer. In the present invention, the antiglare layer is formed from the above-mentioned coating liquid, so the coating property of the coating liquid forming the functional layer on the antiglare layer and the adhesion with the functional layer become good.
[0123] In the present invention, the functional layer provided on the anti-glare layer is not particularly limited. Specific examples include functional layers obtained from antifouling agents, coatings, adhesives, antireflection agents, hydrophobic agents, hydrophilic agents, oleophobic agents, oleophilic agents, hard coating agents, antiskid agents, etc.
[0124] The thickness of the antiglare layer and the functional layer is preferably 5 to 1000 nm, more preferably 10 to 400 nm.
[0125] The coating liquid for forming a coating of the present invention has excellent coating properties and can form a coating with high transmittance. In addition, the coating efficiency in the case of spraying is also excellent. Therefore, it can be preferably used in the fields of displays such as televisions, computers, car navigation, and mobile phones.
[0126] Example
[0127] The present invention will be described in further detail below with reference to examples, but the present invention is not limited thereto.
[0128] The abbreviations used below are as follows.
[0129] TEOS: tetraethoxysilane.
[0130] F13: tridecafluorooctyltrimethoxysilane.
[0131] UPS: γ-ureidopropyltriethoxysilane.
[0132] TTE: Tetraethoxytitanium.
[0133] AN: Aluminum nitrate nonahydrate.
[0134] MeOH: methanol.
[0135] EtOH: ethanol.
[0136] IPA: Isopropyl alcohol.
[0137] PGME: Propylene glycol monomethyl ether.
[0138] BCS: Butyl Cellosolve.
[0139] PB: Propylene glycol monobutyl ether.
[0140] PG: Propylene glycol.
[0141] HG: 2-methyl-2,4-pentanediol.
[0142] NMP: N-methyl-2-pyrrolidone.
[0143] <Synthesis example 1>
[0144] TEOS (31.6 g), F13 (6.2 g), and MeOH (30.3 g) were added to a 200 mL four-necked flask equipped with a reflux tube and stirred. MeOH (15.1 g), water (15.0 g), and oxalic acid (0.8 g) were added thereto, and stirred for 30 minutes in an ice bath at 10° C. Then, the mixture was stirred at 65° C. for 2 hours, and then UPS (0.5 g) and MeOH (0.5 g) were added, and the mixture was further reacted at 65° C. for 2 hours. Then, the mixture was cooled to room temperature to obtain a solution K1.
[0145] <Synthesis example 2>
[0146] AN (2.9 g), water (2.6 g) and EtOH (50.6 g) were added to a 200 mL flask and stirred to obtain an AN solution. TEOS (21.2 g) was added to the AN solution and stirred at room temperature for 30 minutes. Then, TTE (10.0 g) and EtOH (12.7 g) were added and stirred at room temperature for further 30 minutes to obtain a solution K2.
[0147] <Synthesis Example 3>
[0148] AN (2.8 g), water (2.6 g) and EtOH (51.2 g) were added to a 200 mL flask and stirred to obtain an AN solution. TEOS (17.7 g) was added to the AN solution and stirred at room temperature for 30 minutes. Then, TTE (12.9 g) and EtOH (12.8 g) were added and further stirred at room temperature for 30 minutes to obtain a solution K3.
[0149] <Synthesis example 4>
[0150] AN (2.7 g), water (2.5 g) and EtOH (51.8 g) were added to a 200 mL flask and stirred to obtain an AN solution. TEOS (14.3 g) was added to the AN solution and stirred at room temperature for 30 minutes. Then, TTE (15.7 g) and EtOH (13.0 g) were added and further stirred at room temperature for 30 minutes to obtain a solution K4.
[0151] <Synthesis Example 5>
[0152] TEOS (33.0 g) and MeOH (32.5 g) were added to a 200 mL four-necked flask equipped with a reflux tube and stirred. MeOH (13.8 g), water (15.0 g) and oxalic acid (0.9 g) were added thereto and stirred for 30 minutes in an ice bath at 10° C. Then, the mixture was stirred at 60° C. for 2 hours, and then UPS (2.4 g) and MeOH (2.4 g) were added and reacted at 60° C. for further 30 minutes. Then, the mixture was cooled to room temperature to obtain a solution K5.
[0153] <Preparation Example 1>
[0154] PGME (20 g) and EtOH (20 g) were added to the K1 and K5 solutions (60 g) to obtain solutions KL1-1 and KM2-1, respectively.
[0155] <Preparation Example 2>
[0156] PG (5 g), NMP (20 g) and MeOH (63 g) were added to the K1 solution (12 g) to obtain a solution KL1-2.
[0157] <Preparation Example 3>
[0158] EtOH (2.5 g), IPA (42 g), BCS (9.4 g), PB (9.4 g) and HG (18.7 g) were added to solutions K2 to K4 (18 g) to obtain solutions KL2 to KL4, respectively.
[0159] <Preparation Example 4>
[0160] To the K1 solution (40 g) were added PGME (20 g) and EtOH (40 g) to obtain solution KM1.
[0161] <Preparation Example 5>
[0162] MeOH (1.8 g), EtOH (18.5 g), PGME (18.5 g), PB (27.7 g) and HG (18.5 g) were added to the K5 solution (15 g) to obtain a solution KM2-2.
[0163] [Spraying conditions]
[0164] The spraying was performed using the following equipment and conditions.
[0165] Device name: Sprayer API-240-3D manufactured by Apeiros Corporation.
[0166] <Coating conditions I-1>
[0167] Nozzle model: LPVN45, nozzle height: 100mm, Y-axis spacing: 2mm, air pressure: 550kPa, liquid flow rate 1.0mL / min, nozzle speed: 900mm / sec.
[0168] <Coating Conditions I-2>
[0169] The coating condition I-1 was changed to a Y-axis spacing of 3 mm, with the other conditions remaining the same.
[0170] <Coating conditions I-3>
[0171] The coating condition I-1 was changed to Y-axis spacing: 5 mm, and other conditions remained the same.
[0172] <Coating conditions I-4>
[0173] The coating condition I-1 was changed to a Y-axis spacing of 1.4 mm, with the other conditions remaining the same.
[0174] <Coating conditions II-1>
[0175] Nozzle model: LPVN12, nozzle height: 100mm, Y-axis spacing: 7mm, air pressure: 560kPa, liquid flow rate 4.9mL / min, nozzle speed: 500mm / sec.
[0176] <Coating conditions II-2>
[0177] The coating condition II-1 was changed to a nozzle speed of 550 mm / sec, and the other conditions remained the same.
[0178] <Coating Conditions III>
[0179] Nozzle model: LPVN45, nozzle height: 100mm, Y-axis spacing: 7mm, air pressure: 470kPa, liquid flow rate 4.9mL / min, nozzle speed: 170mm / sec.
[0180] <Coating Condition IV>
[0181] Nozzle model: LPVN45, nozzle height: 100mm, Y-axis spacing: 7mm, air pressure: 365kPa, liquid flow rate 4.9mL / min, nozzle speed: 500mm / sec.
[0182] <Coating Conditions V>
[0183] Nozzle model: LPVN45, nozzle height: 50mm, Y-axis spacing: 3mm, air pressure: 550kPa, liquid flow rate 1.0mL / min, nozzle speed: 700mm / sec.
[0184] [Firing conditions]
[0185] <Firing Condition A>
[0186] The resulting product was dried on a hot plate at 70° C. for 5 minutes and baked in a hot air circulation oven at 160° C. for 30 minutes.
[0187] <Firing Condition B>
[0188] Dry in a hot air circulation oven at 130°C for 3 minutes and irradiate with UV at 3000mJ / cm 2 (365 nm conversion, high pressure mercury lamp), and calcined in a hot air circulation oven at 160°C for 30 minutes.
[0189] <Firing Condition C>
[0190] The resulting film was dried on a hot plate at 40° C. for 5 minutes and baked in a hot air circulation oven at 160° C. for 30 minutes.
[0191] <Various evaluation conditions>
[0192] [Haze]
[0193] Soda lime glass was used as the substrate, and a film was formed by spray coating under the same coating conditions as in the examples and comparative examples. The haze of the obtained film-coated substrate was measured using a haze meter HZ-V3 manufactured by SUGA Test Instruments Co., Ltd.
[0194] [Surface observation]
[0195] Soda lime glass was used as the substrate, and the produced substrate with a coating was observed using a three-dimensional white interference microscope Contour GT manufactured by BRUKER JAPAN Co., Ltd.
[0196] [Convex surface coverage]
[0197] The convex surface coverage is calculated by calculating the area ratio of the convex portion and the flat portion in any measurement location from the brightness component of the image analysis based on the image acquired by surface observation. The convex surface coverage is calculated in the same way as the calculation method of the convex surface coverage described above.
[0198] [Reflectivity]
[0199] <Specular reflection, reflected color>
[0200] The substrate was made of soda-lime glass, and the reflectance of the produced substrate with a coating was measured at a wavelength of 380nm to 800nm at an incident angle of 5° using an ultraviolet-visible-near-infrared spectrophotometer UV-3600 manufactured by Shimadzu Corporation. The average visual reflectance (regular reflection) and reflection color a were calculated based on the obtained spectral reflectance curve in accordance with JIS R 3106. * , b * .
[0201] <SCI、SCE>
[0202] The substrate was made of soda-lime glass, and the reflectance of the produced substrate with a coating was measured at a wavelength range of 360nm to 740nm at an incident angle of 8° using a spectrophotometer CM-3700A manufactured by Konica Minolta Co., Ltd., and the average visual reflectance of SCI and SCE was calculated in accordance with JIS Z 8722. It should be noted that SCI (Specular Component Include: including specular regular reflection light) is a measurement that takes regular reflection light into account, and SCE (Specular Component Exclude: excluding specular regular reflection light) is a measurement that does not take regular reflection light into account.
[0203] [sparkling]
[0204] In a liquid crystal display with a pixel density of 350ppi, yellow-green is displayed on the front surface with maximum brightness. A substrate with a coating is placed directly on the screen. The case where flickering occurs is evaluated as ×, the case where some flickering can be confirmed is evaluated as △, and the case where no flickering occurs is evaluated as 0.
[0205] [Refractive index]
[0206] A silicon substrate (100) was used as the substrate, and solutions KL2 to 4 were formed into films by spin coating in a manner such that the film thickness after firing was 100 nm. The films were fired under the above-mentioned firing condition B. The obtained substrate with a coating was used to measure the refractive index at a wavelength of 633 nm using an ellipsometer (DVA-FLVW, manufactured by Sojiri Optical Industry Co., Ltd.).
[0207] <Example 1>
[0208] The substrate was made of soda-lime glass, and the solution KL1-2 obtained in the above-mentioned Preparation Example 2 was sprayed under coating condition III, and then fired under firing condition A to form a lower layer. The solution KL1-1 obtained in the above-mentioned Preparation Example 1 was sprayed on the obtained substrate under coating condition I-1, and then fired under firing condition C to obtain a substrate with a coating.
[0209] Various evaluations were performed using the obtained substrate with a coating film. The evaluation results are shown in Table 1-2.
[0210] <Examples 2 to 3, Comparative Examples 1 to 4>
[0211] A substrate with a coating film was obtained in the same manner as in Example 1 except that the solutions and conditions used were changed as shown in Table 1-1 below. In Comparative Examples 2 and 4, a substrate with a coating film was obtained only by forming the lower layer.
[0212] Various evaluations were performed using the obtained substrate with a coating film. The evaluation results are shown in Table 1-2.
[0213] [Table 1-1]
[0214]
[0215] [Table 1-2]
[0216]
[0217] As shown in Table 1-2, in Examples 1 to 3, regular reflection and SCI values were suppressed to low levels, and no glare occurred. Moreover, compared to Comparative Example 2, SCE, which is a light scattering component in the reflectivity, was generated, so that an anti-glare function could be achieved, which provided the following suggestion: an anti-glare functional film with an anti-reflection function could be constructed.
[0218] In Comparative Example 1, the SCI value was extremely large and flashing occurred.
[0219] Comparative Example 3 is a case where a solution without a fluoroalkyl component is used, and a shape with a low convex surface coverage cannot be obtained, and the SCI value becomes higher. In addition, as for Comparative Example 4, there is no anti-glare property, but the reflection color is small. However, both SCI and regular reflection become higher.
[0220] <Examples 4 to 6, Comparative Examples 5 to 7>
[0221] A substrate with a coating film was obtained in the same manner as in Example 1 except that the solution and conditions used were changed as shown in Table 2-1 below.
[0222] Various evaluations were performed using the obtained substrate with a coating film. The evaluation results are shown in Table 2-2.
[0223] [Table 2-1]
[0224]
[0225] [Table 2-2]
[0226]
[0227] As shown in Table 2-2, in Examples 4 to 6, the SCI value can be suppressed to a low level, and no glare occurs. Moreover, when compared with Comparative Examples 5 to 7, the absolute value of the reflected color value can be reduced, and SCE is generated, so the anti-glare function can be demonstrated, which suggests that an anti-glare coating with an anti-reflection function can be formed.
[0228] Industrial Applicability
[0229] By using the coating liquid for forming an anti-glare coating of the present invention and the coating structure using the coating liquid, a laminate having excellent anti-reflection and anti-glare properties (anti-glare function) can be provided, which can be formed on a glass substrate. Thus, it can contribute to improving the display quality level of image display devices (liquid crystal display, organic EL display, plasma display, etc.) possessed by various devices such as televisions, personal computers, and smart phones.
Claims
1. A substrate with an anti-glare layer, characterized in that: have: Base material; as well as The anti-glare layer is directly formed on the substrate or formed on the substrate with the aid of other layers, and has a concavo-convex structure on the surface of the anti-glare layer. The anti-glare layer is formed of a cured product of an anti-glare film-forming composition, wherein the anti-glare film-forming composition contains a polysiloxane having a fluorine-containing organic group. The polysiloxane is obtained by polycondensing an alkoxysilane component containing an alkoxysilane compound represented by the following formula (1): The anti-glare film-forming composition contains at least one selected from ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol diethyl ether, ethylene glycol dipropyl ether, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol monomethyl ether acetate and methyl isobutyl ketone. In the concavo-convex structure on the surface of the anti-glare layer, the convex surface coverage, which is the proportion of convex portions, is 5% to 70%. R 11 Si(OR 12 )3(1) R 11 represents an organic group substituted by a fluorine atom, R 12 It represents a hydrocarbon group having 1 to 5 carbon atoms.
2. The substrate with an anti-glare layer according to claim 1, wherein The polysiloxane is further obtained by polycondensing an alkoxysilane component containing at least one selected from the group consisting of an alkoxysilane compound represented by the following formula (2) and an alkoxysilane compound represented by the following formula (3), Si(OR 2 )4(2) R 31 n Si(OR 32 ) 4-n (3) In the formula, R 2 Represents a hydrocarbon group; R 31 represents an organic group or a hydrogen atom not substituted by a fluorine atom, R 32 It represents a hydrocarbon group having 1 to 5 carbon atoms, and n is an integer of 1 to 3.
3. The substrate with an anti-glare layer according to claim 2, wherein: The organic group not substituted by fluorine atoms is selected from: an alkyl group having 1 to 18 carbon atoms, an alkenyl group having 2 to 18 carbon atoms, a cycloalkyl group, an alkyl group containing a (meth)acryloyloxy group, an alkyl group containing a hydroxyl group, an alkyl group containing a urea group, an alkyl group containing an amino group, an alkyl group containing an epoxy group, an alkyl group containing a mercapto group, an alkyl group containing an isocyanate group, or an aryl group.
4. The substrate with an anti-glare layer according to claim 2, wherein The alkoxysilane compound represented by the formula (2) is tetramethoxysilane, tetraethoxysilane, tetrapropoxysilane or tetrabutoxysilane.
5. The substrate with an anti-glare layer according to claim 2, wherein The alkoxysilane compound represented by the formula (3) is methyltrimethoxysilane, methyltriethoxysilane, ethyltrimethoxysilane, ethyltriethoxysilane, propyltrimethoxysilane, propyltriethoxysilane, butyltrimethoxysilane, butyltriethoxysilane, pentyltrimethoxysilane, pentyltriethoxysilane, heptyltrimethoxysilane, heptyltriethoxysilane, octyltrimethoxysilane, octyltriethoxysilane, dodecyltrimethoxysilane, dodecyltriethoxysilane, hexadecyltrimethoxysilane, hexadecyltriethoxysilane, octadecyltrimethoxysilane, octadecyltriethoxysilane, phenyltrimethoxysilane, phenyltriethoxysilane, ethyltrimethoxysilane, ethyl ...ethyltrimethoxysilane, ethyltriethoxysilane, ethyltrimethoxysilane, ethyltriethoxysilane, ethyltrimethoxysilane, ethyltriethoxysilane, ethyltrimethoxysilane, ethyltriethoxysilane, ethyltrimethoxysilane, ethyltriethoxysilane, ethyltrimethoxysilane, ethyltriethoxysilane, ethyltrimethoxysilane, ethyltriethoxysilane, Alkenyltrimethoxysilane, vinyltriethoxysilane, 3-isocyanatepropyltrimethoxysilane, 3-isocyanatepropyltriethoxysilane, 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, γ-glycidoxypropyltrimethoxysilane, γ-glycidoxypropyltriethoxysilane, γ-mercaptopropyltrimethoxysilane, γ-mercaptopropyltriethoxysilane, 3-acryloxypropyltrimethoxysilane, 3-acryloxypropyltriethoxysilane, γ-methacryloxypropyltrimethoxysilane, γ-methacryloxypropyltriethoxysilane, γ-ureidopropyltrimethoxysilane or γ-ureidopropyltriethoxysilane.
6. The substrate with an anti-glare layer according to any one of claims 1 to 5, wherein The polysiloxane having a fluorine-containing organic group further includes a polysiloxane containing an organic group represented by the following formula (F): CF3(CF2) k CH2CH2-*(F) In the formula, k is an integer of 0 to 12, and * represents a bonding position.
7. The substrate with an anti-glare layer according to any one of claims 1 to 5, wherein The anti-glare film-forming composition contains at least one selected from methanol, ethanol, 2-propanol, 2-butanol, and 2-methyl-1-propanol.
8. The substrate with an anti-glare layer according to any one of claims 1 to 5, wherein The haze of the anti-glare layer is 0.3% to 40%.
9. The substrate with an anti-glare layer according to any one of claims 1 to 5, wherein The refractive index of the anti-glare layer is in the range of 1.3 to 1.
49.
10. The substrate with an anti-glare layer according to any one of claims 1 to 5, characterized in that The anti-glare layer is formed on a high-refractive-index layer, and the refractive index of the high-refractive-index layer is higher than that of the anti-glare layer.
11. The substrate with an anti-glare layer according to claim 10, wherein The refractive index of the high refractive index layer is in the range of 1.5 to 2.
1.
12. The substrate with an anti-glare layer according to any one of claims 1 to 5, characterized in that The substrate with an anti-glare layer further includes: a functional layer formed on the anti-glare layer.
13. An image display device, characterized in that: A substrate with an antiglare layer according to any one of claims 1 to 12.
14. A method for manufacturing a substrate with an anti-glare layer, comprising: A step of obtaining a substrate with an anti-glare layer by using the anti-glare film-forming composition according to any one of claims 1 to 12 as a coating liquid for forming an anti-glare film, and applying the coating liquid for forming an anti-glare film on a substrate to form an anti-glare layer.
Citation Information
Patent Citations
Touch panel
WO2012057165A1
Anti-glare hard coat laminate
WO2018070426A1
Anti-dazzle property optical stacking body
CN101163994A
Anti-glare hard coat laminate
CN109791225A
Formation of hydrophilic coating film and coated article
JP2000262963A