A large-pore pseudo-boehmite and preparation method thereof

By using the external field strengthening method and steric hindrance effect in the mixing of simulanite and solvent, the dispersion and self-assembly of its nanosheets were improved, and the large-porous simulanite was successfully prepared, solving the existing technology The problems of insufficient mesoporous capacity and high production cost have achieved low-cost and efficient production of phthalthy aluminite.

CN114735731BActive Publication Date: 2024-11-15JIANGXI INST OF RARE EARTHS CHINESE ACAD OF SCI +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202011536131.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-12-23
Publication Date
2024-11-15
Estimated Expiration
2040-12-23

AI Technical Summary

Technical Problem

The prior art is difficult to effectively produce phthalinated alumina with large pore volume and specific pore structures, and its production cost is high and cannot meet the petrochemical industry's demand for lightweight and cleaner.

Method used

By mixing suprastic suprastic suprastic suprastic suprastic suprastic suprastic suprastic suprastic suprastic suprastic suprastic suprastic suprastic suprastic suprastic suprastic suprastic suprastic suprastic suprastic suprastic suprastic suprastic suprastic suprastic suprastic suprastic suprastic suprastic suprastic suprastic suprastic suprastic suprastic suprastic suprastic suprastic suprastic suprastic suprastic suprastic preparation.

Benefits of technology

The preparation of large pore volume is achieved, with a pore volume exceeding 0.8cm3/g, simple process, low cost, and easy recycling, achieving the purpose of green mining.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114735731B_ABST
    Figure CN114735731B_ABST
Patent Text Reader

Abstract

The present invention relates to a macroporous boehmite and a preparation method thereof, wherein the preparation method comprises the following steps: (1) mixing pseudo-boehmite and a solvent to obtain an intermediate liquid; (2) mixing the intermediate liquid and an auxiliary agent, and then grinding and drying in sequence to obtain the macroporous pseudo-boehmite. The preparation method provided by the present invention adopts a reasonable treatment process, utilizes an external field enhancement method and a steric hindrance effect to improve the dispersibility of pseudo-boehmite nanosheets, and realizes their self-assembly, thereby expanding the pore volume and pore diameter, thereby realizing the preparation of macroporous pseudo-boehmite, and the pore volume of the prepared pseudo-boehmite is greater than 0.8 cm 3 / g.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of pseudo-boehmite, and in particular to macroporous pseudo-boehmite and a preparation method thereof. Background Art

[0002] At present, pseudo-boehmite is widely used in petrochemical, nitrogen fertilizer, environmental protection and other industries as catalyst carrier, molecular sieve and raw material for producing activated alumina. In recent years, my country's petrochemical industry has faced severe challenges such as heavy and inferior crude oil, light and clean products and high costs. Processing heavy crude oil, shale oil and other residual oil has become the main task of today's refining industry. In 2017 alone, my country processed 419.2 million tons of residual oil, accounting for 73.8% of imported crude oil.

[0003] For example, CN101172631A discloses a method for preparing pseudo-boehmite, which belongs to the preparation technology of non-metallurgical alumina, including carbonation of sodium aluminate solution into gel, aging, separation, washing and drying. After the sodium aluminate solution is carbonated into gel, slurry separation is first performed, and then the filter cake is added to the washing water for mixing and slurrying, and then the temperature is raised for aging. The washing water consumption is small, the production cost is low, the product quality is easy to guarantee, and it is conducive to practical application.

[0004] CN111807396A discloses a method for producing high-purity pseudo-boehmite, comprising: a. taking metallic aluminum, smelting it with a metal catalyst, and reacting the obtained alloy aluminum with water to produce hydrogen, wherein the purity of the metallic aluminum is not less than 99.9wt%; b. separating the slurry after the aluminum-water reaction, drying the separated suspended slurry to obtain pseudo-boehmite, and optionally calcining the pseudo-boehmite to obtain alumina; c. treating the aluminum-water reaction residue after separating the slurry for recycling; the method has the advantages of simple process, short flow, and easy to achieve hydrogen preparation conditions; small amounts of catalysts gallium and indium are used in the alloy, low raw material cost and easy recycling and reuse; safe, environmentally friendly, low-cost and high-efficiency hydrogen production can be achieved, and high-value-added products of pseudo-boehmite can be obtained, with significant economic benefits.

[0005] Pseudo-boehmite and its calcined activated alumina carrier must have a sufficiently large pore volume and a suitable pore structure to meet the requirements of lightweight and clean products; and since the carrier cost accounts for 60% of the catalyst raw material cost, it is also necessary to reduce the production cost of pseudo-boehmite to achieve cost reduction and efficiency improvement in the residual oil refining process. Therefore, there is an urgent need for a low-cost production and preparation method of pseudo-boehmite with large pore volume and specific pore structure. Summary of the invention

[0006] In view of the problems existing in the prior art, the present invention aims to provide a large-pore volume boehmite and a preparation method thereof, which has simple process, low price, and is easy to recycle, realizes the reuse of reaction solvent, and achieves the purpose of sustainable green mining of pseudo-boehmite. The pore volume of the obtained pseudo-boehmite is greater than 0.8 cm 3 / g.

[0007] To achieve this object, the present invention adopts the following technical solutions:

[0008] In a first aspect, the present invention provides a method for preparing macroporous pseudo-boehmite, the preparation method comprising the following steps:

[0009] (1) mixing diaspore and a solvent to obtain an intermediate solution;

[0010] (2) The intermediate liquid and the auxiliary agent are mixed, and then ground and dried in sequence to obtain the macroporous pseudo-boehmite.

[0011] The preparation method provided by the present invention adopts a reasonable treatment process, utilizes an external field enhancement method and a steric hindrance effect to improve the dispersibility of pseudo-boehmite nanosheets, and realizes their self-assembly, thereby expanding the pore volume and pore diameter, and realizing the preparation of large-pore-volume pseudo-boehmite. The pore volume of the prepared pseudo-boehmite is greater than 0.8 cm 3 / g.

[0012] As a preferred technical solution of the present invention, the solid-to-liquid ratio of the pseudo-diatomite and the solvent in step (1) is g / mL 1:(0.5-50), for example, it can be 1:0.5, 1:1, 1:2, 1:3, 1:4, 1:5, 1:6, 1:7, 1:8, 1:9, 1:10, 1:15, 1:20, 1:25, 1:30, 1:35, 1:40, 1:45 or 1:50, but is not limited to the listed values, and other values ​​not listed within the range are equally applicable.

[0013] As a preferred technical solution of the present invention, the solvent in step (1) includes one of water, an acid solution with a pH of 1-5, or an alcohol.

[0014] In the present invention, the acid solution with a pH of 1-5 may be, for example, 1, 2, 3, 4 or 5, but is not limited to the listed values, and other values ​​not listed within the range are also applicable.

[0015] Preferably, the acid solution comprises nitric acid.

[0016] Preferably, the alcohol comprises one or a combination of at least two of methanol, ethanol, n-propanol or isopropanol, preferably ethanol.

[0017] As a preferred technical solution of the present invention, the amount of the additive added in step (2) is 0.1-20% of the mass of the intermediate liquid, for example, it can be 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1%, 2%, 4%, 6%, 8%, 10%, 12%, 14%, 16%, 18% or 20%, etc., but is not limited to the listed values, and other values ​​not listed within the range are also applicable.

[0018] As a preferred technical solution of the present invention, the auxiliary agent in step (2) includes one or a combination of at least two of cetyltrimethylammonium bromide, sodium dioctyl sulfosuccinate, polyethylene glycol octylphenyl ether, sodium dodecylbenzene sulfonate, polyethylene glycol 800, anhydrous glucose, polyethylene oxide, ammonium polyacrylate or polyoxypropylene-polyoxyethylene copolymer.

[0019] In the present invention, the molecular weight of the polyethylene glycol octyl phenyl ether is 646-800 or the like.

[0020] In the present invention, the molecular weight of the polyethylene oxide is 100,000-200,000, etc.

[0021] In the present invention, the molecular weight of the ammonium polyacrylate is 89.09-200, etc.

[0022] In the present invention, the molecular weight of the polyoxypropylene-polyoxyethylene copolymer is 332.475-500, etc.

[0023] In the present invention, by selecting specific reagents, utilizing external field enhancement method and steric hindrance effect to improve the dispersibility of pseudo-boehmite nanosheets, realize their self-assembly, and regulate the pore size, pore volume and specific surface area of ​​pseudo-boehmite, thereby obtaining pseudo-boehmite with large pore volume.

[0024] As a preferred technical solution of the present invention, the grinding speed in step (2) is 100-2000r / min, for example, it can be 100r / min, 200r / min, 400r / min, 600r / min, 800r / min, 1000r / min, 1200r / min, 1400r / min, 1600r / min, 1800r / min or 2000r / min, but is not limited to the listed values, and other values ​​not listed within the range are also applicable.

[0025] Preferably, the grinding time in step (2) is 0.5-8 h, for example, it can be 0.5 h, 1 h, 1.5 h, 2 h, 2.5 h, 3 h, 3.5 h, 4 h, 4.5 h, 5 h, 5.5 h, 6 h, 6.5 h, 7 h, 7.5 h or 8 h, but is not limited to the listed values, and other values ​​not listed within the range are also applicable.

[0026] As a preferred technical solution of the present invention, the drying method in step (2) includes heat drying and / or cold drying.

[0027] As a preferred technical solution of the present invention, the temperature of the thermal drying is 60-95°C, for example, it can be 60°C, 65°C, 70°C, 75°C, 80°C, 85°C, 90°C or 95°C, but is not limited to the listed values, and other unlisted values ​​within the range are also applicable.

[0028] Preferably, the heat drying time is 6-30 hours, for example, 6 hours, 10 hours, 15 hours, 20 hours, 25 hours or 30 hours, etc., but is not limited to the listed values, and other values ​​not listed within the range are also applicable.

[0029] Preferably, the cold drying temperature T is -50°C ≤ T ≤ -40°C, for example, it can be -50°C, -49°C, -48°C, -47°C, -46°C, -45°C, -44°C, -43°C, -42°C, -41°C or -40°C, etc., but is not limited to the listed values, and other unlisted values ​​within the range are also applicable.

[0030] Preferably, the cold drying time is 6-30 h, for example, 6 h, 10 h, 15 h, 20 h, 25 h or 30 h, etc., but is not limited to the listed values, and other values ​​not listed within the range are also applicable.

[0031] As a preferred technical solution of the present invention, the preparation method comprises the following steps:

[0032] (1) mixing pseudo-boehmite and a solvent to obtain an intermediate solution; the solid-liquid ratio of the pseudo-boehmite to the solvent is 1:(0.5-50) g / mL; the solvent comprises one of water, an acid solution with a pH of 1-5, or an alcohol;

[0033] (2) The intermediate liquid and the auxiliary agent are mixed, and then ground and dried in sequence to obtain the macroporous pseudo-boehmite; the amount of the auxiliary agent added is 0.1-20% of the mass of the intermediate liquid; the auxiliary agent includes one or a combination of at least two of cetyl trimethylamine bromide, sodium dioctyl succinate sulfonate, polyethylene glycol octylphenyl ether, sodium dodecylbenzene sulfonate, polyethylene glycol 800, anhydrous glucose, polyethylene oxide, ammonium polyacrylate or polyoxypropylene-polyoxyethylene copolymer; the grinding speed is 100-2000r / min; the grinding time is 0.5-8h.

[0034] In a second aspect, the present invention provides a large-pore pseudo-boehmite, wherein the large-pore pseudo-boehmite is obtained by the preparation method described in the first aspect, and the pore volume of the pseudo-boehmite is greater than 0.8 cm3 / g.

[0035] Compared with the prior art solutions, the present invention has at least the following beneficial effects:

[0036] (1) The solvent used in the present invention is ethanol, which has a simple process, low price, and is easy to recycle, thereby realizing the reuse of the reaction solvent and achieving the purpose of sustainable green mining of pseudo-boehmite.

[0037] (2) The pore volume of the pseudo-boehmite obtained in the present invention is greatly improved compared with the prior art. The pore volume obtained in the present invention is greater than 0.8 cm 3 / g. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] Figure 1 It is a schematic diagram of the method for preparing large-pore pseudo-boehmite provided in Example 1 of the present invention.

[0039] The present invention is further described in detail below. However, the following examples are only simplified examples of the present invention and do not represent or limit the scope of protection of the present invention. The scope of protection of the present invention shall be subject to the claims. DETAILED DESCRIPTION

[0040] To better illustrate the present invention and facilitate understanding of the technical solution of the present invention, typical but non-limiting embodiments of the present invention are as follows:

[0041] Example 1

[0042] This embodiment provides a method for preparing macroporous pseudo-boehmite. Figure 1 As shown, it includes the following: take 10g of pseudo-boehmite and 120mL of dilute nitric acid (pH=5), add 0.5g of polyethylene oxide (molecular weight of 100000) in a beaker and stir, then sand grind and set the speed of the sand grinder to 500r / min, the time is 40min, and the sand-milled liquid is blown dried at 65°C for 24h, and then kept at 65°C for 24h and vacuum dried at a vacuum degree of -30kPa to obtain macroporous pseudo-boehmite.

[0043] The performance indicators of the obtained large-pore pseudo-boehmite are shown in Table 1.

[0044] Example 2

[0045] The present embodiment provides a preparation method of macroporous pseudo-boehmite, comprising the following steps: taking 10 g of pseudo-boehmite and 120 mL of dilute nitric acid (pH=5), and then adding 0.5 g of sodium dioctyl sulfonate succinate in a beaker and stirring, and then sand-milling the mixture, setting the speed of the sand mill to 500 r / min and the time to 40 min, and drying the sand-milled liquid by blast drying at 65° C. for 24 h, and then drying the mixture by vacuum drying at 65° C. for another 24 h and at a vacuum degree of -30 kPa to obtain macroporous pseudo-boehmite.

[0046] The performance indicators of the obtained large-pore pseudo-boehmite are shown in Table 1.

[0047] Example 3

[0048] The present embodiment provides a preparation method of large-pore volume pseudo-boehmite, comprising the following steps: taking 10 g of pseudo-boehmite and 120 mL of water, and then adding 0.5 g of sodium dioctyl sulfonate succinate in a beaker and stirring, and then sand-milling the sand mill at a speed of 500 r / min for 40 min, and drying the sand-milled liquid by blast drying at 65° C. for 24 h, and then drying the liquid by vacuum drying at 65° C. for another 24 h and at a vacuum degree of -30 kPa to obtain pseudo-boehmite.

[0049] The performance indicators of the obtained large-pore pseudo-boehmite are shown in Table 1.

[0050] Example 4

[0051] The present embodiment provides a preparation method of macroporous pseudo-boehmite, comprising the following steps: taking 10 g of pseudo-boehmite and 120 mL of water, adding 0.68 g of polyethylene glycol octylphenyl ether (molecular weight 646) and stirring in a beaker, and then sand milling the mixture. The speed of the sand mill is set to 500 r / min and the time is 40 min. The sand milled liquid is dried by blast drying at 65° C. for 24 h, and then dried under vacuum at 65° C. for 24 h and a vacuum degree of -30 kPa to obtain pseudo-boehmite.

[0052] The performance indicators of the obtained large-pore pseudo-boehmite are shown in Table 1.

[0053] Example 5

[0054] The present embodiment provides a preparation method of macroporous pseudo-boehmite, comprising the following steps: taking 10 g of pseudo-boehmite and 120 mL of ethanol, adding 0.5 g of sodium dodecylbenzene sulfonate and stirring in a beaker, and then sand-milling the sand mill at a speed of 500 r / min for 40 min, blowing and drying the sand-milled liquid at 65° C. for 24 h, and then drying the liquid at 65° C. for another 24 h under a vacuum degree of -30 kPa to obtain macroporous pseudo-boehmite.

[0055] The performance indicators of the obtained large-pore pseudo-boehmite are shown in Table 1.

[0056] Example 6

[0057] The present embodiment provides a preparation method of macroporous pseudo-boehmite, comprising the following steps: taking 10 g of pseudo-boehmite and 120 mL of ethanol, and then adding 0.5 g of polyethylene oxide (molecular weight of 100,000) and stirring in a beaker, and then sand-milling the mixture, setting the speed of the sand mill to 500 r / min and the time to 40 min, and drying the sand-milled liquid by blast drying at 65° C. for 24 h, and then drying the mixture by vacuum drying at 65° C. for 24 h and at a vacuum degree of -30 kPa to obtain macroporous pseudo-boehmite.

[0058] The performance indicators of the obtained large-pore pseudo-boehmite are shown in Table 1.

[0059] Example 7

[0060] The present embodiment provides a preparation method of macroporous pseudo-boehmite, comprising the following steps: taking 10 g of pseudo-boehmite and 120 mL of ethanol, and then adding 0.5 g of ammonium polyacrylate (molecular weight 89.09) and stirring in a beaker, and then sand-milling the mixture, setting the speed of the sand mill to 500 r / min and the time to 40 min, and drying the sand-milled liquid by blast drying at 65° C. for 24 h, and then drying the mixture by vacuum drying at 65° C. for 24 h and at a vacuum degree of -30 kPa to obtain macroporous pseudo-boehmite.

[0061] The performance indicators of the obtained large-pore pseudo-boehmite are shown in Table 1.

[0062] Example 8

[0063] The present embodiment provides a preparation method of macroporous pseudo-boehmite, comprising the following steps: taking 10 g of pseudo-boehmite and 120 mL of ethanol, adding 0.5 g of hexadecyltrimethylamine bromide and stirring in a beaker, and then sand-milling the mixture with the speed of the sand mill set to 500 r / min for 2 h, and drying the sand-milled liquid by blast drying at 65° C. for 24 h, and then drying the mixture under vacuum at 65° C. for another 24 h and a vacuum degree of -30 kPa to obtain macroporous pseudo-boehmite.

[0064] The performance indicators of the obtained large-pore pseudo-boehmite are shown in Table 1.

[0065] Example 9

[0066] The present embodiment provides a preparation method of large-pore pseudo-boehmite, comprising the following steps: taking 10 g of pseudo-boehmite and 120 mL of ethanol, adding 0.5 g of sodium dioctyl sulfonate succinate and stirring in a beaker, and then sand-milling them together at a speed of 500 r / min for 2 h, blowing and drying the sand-milled liquid at 65° C. for 24 h, and then drying it under vacuum at 65° C. for another 24 h at a vacuum degree of -30 kPa to obtain large-pore pseudo-boehmite.

[0067] The performance indicators of the obtained large-pore pseudo-boehmite are shown in Table 1.

[0068] Example 10

[0069] The present embodiment provides a preparation method of macroporous pseudo-boehmite, comprising the following steps: taking 10 g of pseudo-boehmite and 120 mL of ethanol, adding 0.5 g of sodium dodecylbenzene sulfonate and stirring in a beaker, and then sand-milling the sand mill at a speed of 500 r / min for 2 h, blowing and drying the sand-milled liquid at 65° C. for 24 h, and then drying the liquid at 65° C. for another 24 h under a vacuum degree of -30 kPa to obtain macroporous pseudo-boehmite.

[0070] The performance indicators of the obtained large-pore pseudo-boehmite are shown in Table 1.

[0071] Embodiment 11

[0072] The present embodiment provides a preparation method of macroporous pseudo-boehmite, comprising the following steps: taking 10 g of pseudo-boehmite and 120 mL of ethanol, and then adding 0.5 g of polyethylene glycol 800 and stirring in a beaker, and then sand-milling the sand mill at a speed of 500 r / min for 2 h, and drying the sand-milled liquid by blast drying at 65° C. for 24 h, and then drying the liquid by vacuum drying at 65° C. for another 24 h and at a vacuum degree of -30 kPa to obtain macroporous pseudo-boehmite.

[0073] The performance indicators of the obtained large-pore pseudo-boehmite are shown in Table 1.

[0074] Example 12

[0075] The present embodiment provides a preparation method of macroporous pseudo-boehmite, comprising the following steps: taking 10 g of pseudo-boehmite and 120 mL of ethanol, and then adding 0.5 g of anhydrous glucose and stirring in a beaker, and then sand-milling the mixture with the speed of the sand mill set to 500 r / min for 2 h, and drying the sand-milled liquid by blast drying at 65° C. for 24 h, and then drying the mixture by vacuum drying at 65° C. for another 24 h and at a vacuum degree of -30 kPa to obtain macroporous pseudo-boehmite.

[0076] The performance indicators of the obtained large-pore pseudo-boehmite are shown in Table 1.

[0077] Embodiment 13

[0078] The present embodiment provides a preparation method of large-pore pseudo-boehmite, comprising the following steps: taking 10 g of pseudo-boehmite and 120 mL of n-propanol, and then adding 0.5 g of polyethylene glycol octylphenyl ether (molecular weight 646) and stirring in a beaker, and then sand-milling them together at a speed of 500 r / min for 2 hours, and drying the sand-milled liquid by blast drying at 65° C. for 24 hours, and then drying them under vacuum at 65° C. for 24 hours and a vacuum degree of -30 kPa to obtain large-pore pseudo-boehmite.

[0079] The performance indicators of the obtained large-pore pseudo-boehmite are shown in Table 1.

[0080] Embodiment 14

[0081] The present embodiment provides a preparation method of macroporous pseudo-boehmite, comprising the following steps: taking 10 g of pseudo-boehmite and 120 mL of glycerol, adding 0.1 g of cetyltrimethylammonium bromide and stirring in a beaker, and then sand-milling the mixture with the speed of the sand mill set to 500 r / min for 2 h, and drying the sand-milled liquid by blast drying at 65° C. for 24 h, and then drying the mixture under vacuum at 65° C. for another 24 h and a vacuum degree of -30 kPa to obtain macroporous pseudo-boehmite.

[0082] The performance indicators of the obtained large-pore pseudo-boehmite are shown in Table 1.

[0083] Embodiment 15

[0084] The present embodiment provides a preparation method of large-pore pseudo-boehmite, comprising the following steps: taking 10 g of pseudo-boehmite and 120 mL of methanol, and then adding 0.1 g of polyethylene glycol octylphenyl ether (molecular weight 646) and stirring in a beaker, and then sand-milling them together, setting the speed of the sand mill to 500 r / min and the time to 2 h, blowing and drying the sand-milled liquid at 65° C. for 24 h, and then drying it under vacuum at 65° C. for 24 h and a vacuum degree of -30 kPa to obtain large-pore pseudo-boehmite.

[0085] The performance indicators of the obtained large-pore pseudo-boehmite are shown in Table 1.

[0086] Example 16

[0087] The present embodiment provides a preparation method of macroporous pseudo-boehmite, comprising the following steps: taking 10 g of pseudo-boehmite and 120 mL of isopropanol, and then adding 0.1 g of polyoxypropylene-polyoxyethylene copolymer solution (molecular weight 332.475) and stirring in a beaker, and then sand-grinding the mixture together, and drying the sand-grinded liquid by blast drying at 65° C. for 24 h, and then drying the mixture under vacuum at 65° C. for 24 h and a vacuum degree of -30 kPa to obtain macroporous pseudo-boehmite.

[0088] The performance indicators of the obtained large-pore pseudo-boehmite are shown in Table 1.

[0089] Comparative Example 1

[0090] The only difference from Example 1 is that the dilute nitric acid is replaced by an equal amount of sodium hydroxide with an equimolar concentration, that is, a sodium hydroxide solution with a pH of 9. The performance indicators of the obtained pseudo-boehmite are shown in Table 1.

[0091] Comparative Example 2

[0092] The only difference from Example 3 is that water is replaced by an equal amount of sodium hydroxide solution with a pH of 10. The performance indicators of the obtained pseudo-boehmite are shown in Table 1.

[0093] Comparative Example 3

[0094] The only difference from Example 5 is that ethanol is replaced by an equal amount of sodium hydroxide solution with a pH of 12. The performance indicators of the obtained pseudo-boehmite are shown in Table 1.

[0095] Comparative Example 4

[0096] The only difference from Example 5 is that in step (2), stirring is performed instead of grinding after adding polyethylene oxide. The performance indicators of the obtained pseudo-boehmite are shown in Table 1.

[0097] Comparative Example 5

[0098] The only difference from Example 5 is that the amount of the additive added is 35% of the mass of the intermediate liquid. The performance indicators of the obtained pseudo-boehmite are shown in Table 1.

[0099] Comparative Example 6

[0100] The only difference from Example 5 is that the grinding time is 12 hours. The performance indicators of the obtained pseudo-boehmite are shown in Table 1.

[0101] Table 1 Performance indexes of pseudo-boehmite

[0102]

[0103]

[0104] It can be seen from the results of the above embodiments and comparative examples that the present invention improves the dispersibility of pseudo-boehmite nanosheets by rationally selecting reagents and steps in the preparation process, utilizing external field enhancement method and steric hindrance effect, and realizes self-assembly thereof, thereby expanding the pore volume and pore diameter, and realizing the preparation of large-pore-volume pseudo-boehmite.

[0105] The applicant declares that the present invention illustrates the detailed structural features of the present invention through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned detailed structural features, that is, it does not mean that the present invention must rely on the above-mentioned detailed structural features to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of the components selected by the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

[0106] The preferred embodiments of the present invention are described in detail above. However, the present invention is not limited to the specific details in the above embodiments. Within the technical concept of the present invention, a variety of simple modifications can be made to the technical solution of the present invention, and these simple modifications all belong to the protection scope of the present invention.

[0107] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.

[0108] In addition, various embodiments of the present invention may be arbitrarily combined, and as long as they do not violate the concept of the present invention, they should also be regarded as the contents disclosed by the present invention.

Claims

1. A method for preparing macroporous pseudo-boehmite, characterized in that: The preparation method comprises the following steps: (1) mixing diaspore and a solvent to obtain an intermediate solution; The solvent is alcohol; (2) mixing the intermediate liquid and the auxiliary agent, and then grinding and drying in sequence to obtain the macroporous pseudo-boehmite; The additive is added in an amount of 0.1-20% of the mass of the intermediate liquid; the additive includes one or a combination of at least two of cetyl trimethylamine bromide, sodium dioctyl sulfosuccinate, polyethylene glycol octylphenyl ether, sodium dodecylbenzene sulfonate, polyethylene glycol 800, anhydrous glucose, polyethylene oxide, ammonium polyacrylate or polyoxypropylene-polyoxyethylene copolymer; The grinding time is 0.5-8h.

2. The preparation method according to claim 1, characterized in that The solid-to-liquid ratio of the pseudo-diatomite to the solvent in step (1) is 1:(0.5-50) g / mL.

3. The preparation method according to claim 1, characterized in that: The alcohol includes one or a combination of at least two of methanol, ethanol, n-propanol or isopropanol.

4. The preparation method according to claim 1, characterized in that: The grinding speed in step (2) is 100-2000r / min.

5. The preparation method according to claim 1, characterized in that: The drying method in step (2) includes heat drying and / or cold drying.

6. The preparation method according to claim 5, characterized in that: The temperature of the thermal drying is 60-95°C.

7. The preparation method according to claim 5, characterized in that: The thermal drying time is 6-30h.

8. The preparation method according to claim 5, characterized in that: The cold drying temperature T is -50°C≤T≤-40°C.

9. The preparation method according to claim 5, characterized in that: The cold drying time is 6-30h.

10. The preparation method according to claim 1, characterized in that: The preparation method comprises the following steps: (1) mixing pseudo-boehmite and a solvent to obtain an intermediate solution; the solid-liquid ratio of the pseudo-boehmite to the solvent is 1:(0.5-50) g / mL; and the solvent is alcohol; (2) The intermediate liquid and the auxiliary agent are mixed, and then ground and dried in sequence to obtain the macroporous pseudo-boehmite; the amount of the auxiliary agent added is 0.1-20% of the mass of the intermediate liquid; the auxiliary agent includes one or a combination of at least two of cetyl trimethylamine bromide, sodium dioctyl succinate sulfonate, polyethylene glycol octylphenyl ether, sodium dodecylbenzene sulfonate, polyethylene glycol 800, anhydrous glucose, polyethylene oxide, ammonium polyacrylate or polyoxypropylene-polyoxyethylene copolymer; the grinding speed is 100-2000r / min; the grinding time is 0.5-8h.

11. A macroporous pseudo-boehmite, characterized in that: The large-pore pseudo-boehmite is obtained by the preparation method according to any one of claims 1 to 10, and the pore volume of the pseudo-boehmite is greater than 0.8 cm 3 / g.