Preparation method of oxygen reduction catalyst
By mixing carbon black with metal ion solution at room temperature and washing it centrifugally, oxygen reduction catalyst is prepared, which solves the problems of long-term preparation process, difficulty in operation and high energy consumption in the prior art, and has a high specific surface area and three-dimensionality The catalyst of the network structure simplifies operation and reduces energy consumption.
Patent Information
- Application Number
- CN202210255431.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-03-15
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2042-03-15
AI Technical Summary
The preparation process of existing oxygen reduction catalysts takes a long time, is difficult to operate and consume high energy, making it difficult to improve the cathode oxygen reduction activity.
Under a temperature of 30-40°C, the carbon black is mixed with the metal ion-solvent solution, and then the reaction is centrifuged to precipitate and wash to prepare an oxygen reduction catalyst. Ultrasonic conditions and appropriate air pressure are used to simplify the process and reduce energy Consumption.
The prepared oxygen reduction catalyst has a large specific surface area and a three-dimensional network structure, good biocompatibility, short time consumption, simple operation, low energy consumption, and is suitable for a variety of metal ions, improving the oxygen reduction activity of the cathode.
Smart Images

Figure CN114744216B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of oxygen reduction catalysts, and in particular to a method for preparing an oxygen reduction catalyst. Background Art
[0002] The reduction of oxygen on the cathode of a fuel cell requires a high activation energy. In order to improve the oxygen reduction activity of the cathode, an oxygen reduction catalyst is added to the cathode. Currently, high-temperature pyrolysis is usually performed during the preparation of oxygen reduction catalysts, which makes the preparation process time-consuming, difficult to operate, and energy-intensive. Summary of the invention
[0003] The main purpose of the present invention is to provide a method for preparing an oxygen reduction catalyst, aiming to solve the problems in the prior art that the preparation process is time-consuming, difficult to operate and has high energy consumption.
[0004] To achieve the above object, the present invention provides a method for preparing an oxygen reduction catalyst, comprising the following steps:
[0005] The carbon black is mixed with a metal ion-solvent solution, and reacted at a temperature of 30 to 40° C. to obtain a doped carbon black solution;
[0006] The doped carbon black solution is centrifuged to obtain a precipitate, which is then washed to obtain an oxygen reduction catalyst.
[0007] Optionally, the temperature condition is 35°C.
[0008] Optionally, in the metal ion-solvent solution, the solvent is methanol or ethanol.
[0009] Optionally, in the metal ion-solvent solution, the solvent is ethanol.
[0010] Optionally, in the step of mixing carbon black with a metal ion-solvent solution and reacting them at a temperature of 30 to 40° C. to obtain a doped carbon black solution, the reaction is carried out under ultrasonic conditions.
[0011] Optionally, the mass ratio of the carbon black to the metal ions is 1:(0.01-1).
[0012] Optionally, in the step of mixing carbon black with a metal ion-solvent solution and reacting at a temperature of 30 to 40° C. to obtain a doped carbon black solution, the reaction time is 1 to 5 hours.
[0013] Optionally, in the step of mixing carbon black with a metal ion-solvent solution and reacting at a temperature of 30 to 40° C. to obtain a doped carbon black solution, the reaction is carried out under an air pressure of 90 to 110 KPa.
[0014] Optionally, the metal ion-solvent solution is obtained by mixing a metal salt with a solvent, and the metal salt is at least one of silver acetate, ferric acetate, cobalt acetate, copper acetate, nickel acetate, zinc nitrate, lead nitrate, cobalt nitrate, ferric nitrate, nickel nitrate, manganese nitrate, ferric chloride, cupric chloride, potassium chloroplatinate, ferric sulfate, copper sulfate, lead sulfate, cobalt nitrate, ferric nitrate, copper nitrate and manganese nitrate.
[0015] Optionally, the metal salt is at least one of silver acetate, ferric acetate, cobalt acetate, copper acetate, cobalt nitrate, ferric nitrate, ferric chloride, copper chloride, potassium chloroplatinate, copper sulfate, cobalt nitrate, ferric nitrate, copper nitrate and manganese nitrate.
[0016] In the technical scheme of the present invention, carbon black is first reacted with metal ions to obtain carbon black doped with metal ions, and then centrifuged and washed to obtain an oxygen reduction catalyst. The obtained oxygen reduction catalyst has a large specific surface area, a three-dimensional network structure, and good biocompatibility. In addition, the reaction of carbon black and metal ions is carried out at a room temperature of 30 to 40°C. Compared with the high temperature conditions used in the past, the preparation method of the present invention is time-saving, simple to operate, and has low energy consumption. Moreover, the preparation method of the present invention can be applied to a variety of different precious metal ions and non-precious metal ions, and has a certain universality. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without paying creative work.
[0018] Figure 1 This is a scanning electron microscope photograph (SEM) of the oxygen reduction catalyst prepared in Example 1 of the present invention;
[0019] Figure 2 This is a scanning electron microscope photograph (SEM) of the oxygen reduction catalyst prepared in Example 2 of the present invention;
[0020] Figure 3 This is a scanning electron microscope photograph (SEM) of the oxygen reduction catalyst prepared in Example 3 of the present invention.
[0021] The realization of the purpose, functional features and advantages of the present invention will be further explained in conjunction with embodiments and with reference to the accompanying drawings. DETAILED DESCRIPTION
[0022] To make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them.
[0023] It should be noted that, in the embodiments, those without specifying specific conditions are carried out according to normal conditions or conditions recommended by the manufacturer. Those without specifying the manufacturer of reagents or instruments used are conventional products that can be purchased commercially. In addition, the meaning of "and / or" appearing in the full text includes three parallel schemes, and "A and / or B" is taken as an example, including schemes A, B, or A and B that meet the same time. In addition, the technical schemes between the various embodiments can be combined with each other, but must be based on the ability of ordinary technicians in the field to achieve. When the combination of the technical schemes is contradictory or cannot be achieved, it should be considered that the combination of such technical schemes does not exist, and is not within the scope of protection required by the present invention. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in the field without making creative work, all belong to the scope of protection of the present invention.
[0024] The reduction of oxygen on the cathode of a fuel cell requires a high activation energy. In order to improve the oxygen reduction activity of the cathode, an oxygen reduction catalyst is added to the cathode. Currently, high-temperature pyrolysis is usually performed during the preparation of oxygen reduction catalysts, which makes the preparation process time-consuming, difficult to operate, and energy-intensive.
[0025] In view of this, the present invention provides a method for preparing an oxygen reduction catalyst, the method for preparing the oxygen reduction catalyst comprising the following steps:
[0026] Step S10, mixing carbon black with a metal ion-solvent solution, and reacting them at a temperature of 30 to 40° C. to obtain a doped carbon black solution.
[0027] Carbon black is a highly dispersible black powdery substance obtained by incomplete combustion of hydrocarbon substances. Its main component is carbon. The carbon black particles are nearly spherical and have a large specific surface area. Under the temperature condition of 30-40°C, carbon black and metal ions will react to obtain carbon black doped with metal ions. Therefore, what is obtained by step S10 is a solution containing carbon black doped with metal ions, that is, a doped carbon black solution.
[0028] Furthermore, the temperature condition is in the range of 30-40°C, and can be 30°C, 35°C or 40°C, etc. In the embodiment of the present invention, the temperature condition is preferably 35°C.
[0029] In an embodiment of the present invention, in the metal ion-solvent solution, the solvent is methanol or ethanol. Preferably, the solvent is ethanol.
[0030] Furthermore, in step S10, the reaction is carried out under ultrasonic conditions. In this way, the carbon black and the metal ion-solvent solution are mixed more evenly, that is, the carbon black and the metal ions are mixed more evenly, and the obtained carbon black doped with metal ions has better doping effect and higher quality.
[0031] Wherein, the mass ratio of the carbon black to the metal ion is 1:(0.01-1). For example, the mass ratio of carbon black to metal ion is 1:0.01, the mass ratio of carbon black to metal ion is 1:0.1, the mass ratio of carbon black to metal ion is 1:1, and so on, which are not limited in the present invention. Preferably, the mass ratio of carbon black to metal ion is 1:0.1.
[0032] In step S10, the reaction time is 1 to 5 hours, for example, 1 hour, 3 hours or 5 hours, etc. In the embodiment of the present invention, the preferred reaction time is 3 hours.
[0033] In step S10, the reaction is carried out under a pressure of 90 to 110 KPa, such as 90 KPa, 100 KPa or 110 KPa. In the embodiment of the present invention, the preferred reaction time is 100 KPa, and 100 KPa is a normal pressure condition. Compared with the previous preparation method requiring high pressure, the preparation method of the present invention has mild reaction conditions, lower cost and more stable operation.
[0034] Further, the metal ion-solvent solution is obtained by mixing a metal salt with a solvent, and the metal salt is at least one of silver acetate, ferric acetate, cobalt acetate, copper acetate, nickel acetate, zinc nitrate, lead nitrate, cobalt nitrate, ferric nitrate, nickel nitrate, manganese nitrate, ferric chloride, copper chloride, potassium chloroplatinate, ferric sulfate, copper sulfate, lead sulfate, cobalt nitrate, ferric nitrate, copper nitrate and manganese nitrate. Metal ions are provided by a metal salt dissolved in a solvent such as ethanol or methanol, thereby achieving doping of metal ions on carbon black. In an embodiment of the present invention, preferably, the metal salt is at least one of silver acetate, ferric acetate, cobalt acetate, copper acetate, cobalt nitrate, ferric nitrate, ferric chloride, copper chloride, potassium chloroplatinate, copper sulfate, cobalt nitrate, ferric nitrate, copper nitrate and manganese nitrate.
[0035] Step S20, centrifuging the doped carbon black solution to obtain a precipitate, washing the precipitate, and obtaining an oxygen reduction catalyst.
[0036] By centrifugation and washing, free metal ions are removed to obtain relatively pure carbon black doped with metal ions, namely, oxygen reduction catalyst.
[0037] It should be noted that deionized water is preferably used for washing in step S20. Deionized water is pure water from which ions such as sodium, magnesium, calcium, zinc and iron have been removed. This helps prevent the introduction of other impurity ions.
[0038] In the technical scheme of the present invention, carbon black is first reacted with metal ions to obtain carbon black doped with metal ions, and then centrifuged and washed to obtain an oxygen reduction catalyst. The obtained oxygen reduction catalyst has a large specific surface area, a three-dimensional network structure, and good biocompatibility. In addition, the reaction of carbon black and metal ions is carried out at a room temperature of 30 to 40°C. Compared with the high temperature conditions used in the past, the preparation method of the present invention is time-saving, simple to operate, and has low energy consumption. Moreover, the preparation method of the present invention can be applied to a variety of different precious metal ions and non-precious metal ions, and has a certain universality.
[0039] The technical solution of the present invention is further described in detail below in conjunction with specific embodiments and drawings. It should be understood that the following embodiments are only used to explain the present invention and are not used to limit the present invention.
[0040] Example 1
[0041] (1) Carbon black is mixed with a potassium chloroplatinate-ethanol solution, and reacted for 3 hours under a temperature condition of 35° C., a gas pressure condition of 100 KPa, and ultrasonic conditions to obtain a doped carbon black solution, wherein the mass ratio of carbon black to platinum ions is 1:0.1.
[0042] (2) The doped carbon black solution is centrifuged to obtain a precipitate, which is then washed three times with deionized water to obtain an oxygen reduction catalyst.
[0043] The oxygen reduction catalyst prepared in Example 1 was subjected to electron microscope scanning to obtain a scanning electron microscope photo (SEM) as shown in FIG. Figure 1 As shown in the figure, the oxygen reduction catalyst has a three-dimensional network structure, which means that the specific surface area is large and the catalytic activity is good.
[0044] Example 2
[0045] (1) Carbon black is mixed with an iron nitrate-ethanol solution, and reacted for 3.5 hours under a temperature condition of 30° C., a gas pressure condition of 101 KPa, and ultrasonic conditions to obtain a doped carbon black solution, wherein the mass ratio of carbon black to iron ions is 1:0.01.
[0046] (2) The doped carbon black solution is centrifuged to obtain a precipitate, which is then washed three times with deionized water to obtain an oxygen reduction catalyst.
[0047] The oxygen reduction catalyst prepared in Example 2 was subjected to electron microscope scanning to obtain a scanning electron microscope photo (SEM) as shown in FIG. Figure 2 As shown in the figure, the oxygen reduction catalyst has a three-dimensional network structure, which means that the specific surface area is large and the catalytic activity is good.
[0048] Example 3
[0049] (1) Carbon black is mixed with a cobalt nitrate-ethanol solution, and reacted for 2.5 hours under a temperature condition of 40° C., a gas pressure condition of 99 KPa, and an ultrasonic condition to obtain a doped carbon black solution, wherein the mass ratio of carbon black to cobalt ions is 1:1.
[0050] (2) The doped carbon black solution is centrifuged to obtain a precipitate, which is then washed three times with deionized water to obtain an oxygen reduction catalyst.
[0051] The oxygen reduction catalyst prepared in Example 3 was subjected to electron microscope scanning to obtain a scanning electron microscope photo (SEM) as shown in FIG. Figure 3 As shown in the figure, the oxygen reduction catalyst has a three-dimensional network structure, which means that the specific surface area is large and the catalytic activity is good.
[0052] Example 4
[0053] (1) Carbon black is mixed with a silver acetate-ethanol solution, and reacted for 1 hour under a temperature condition of 34° C., a gas pressure condition of 110 KPa and ultrasonic conditions to obtain a doped carbon black solution, wherein the mass ratio of carbon black to silver ions is 1:0.05.
[0054] (2) The doped carbon black solution is centrifuged to obtain a precipitate, which is then washed three times with deionized water to obtain an oxygen reduction catalyst.
[0055] The oxygen reduction catalyst prepared in Example 4 was subjected to electron microscope scanning, and the obtained SEM image showed that the oxygen reduction catalyst had a three-dimensional network structure.
[0056] Example 5
[0057] (1) Carbon black is mixed with potassium chloroplatinate-silver acetate-ethanol solution, and reacted for 3 hours under a temperature condition of 36° C., a gas pressure condition of 100 KPa and ultrasonic conditions to obtain a doped carbon black solution, wherein the mass ratio of carbon black to metal ions (platinum ions and silver ions) is 1:0.15.
[0058] (2) The doped carbon black solution is centrifuged to obtain a precipitate, which is then washed three times with deionized water to obtain an oxygen reduction catalyst.
[0059] The oxygen reduction catalyst prepared in Example 5 was subjected to electron microscope scanning, and the obtained SEM image showed that the oxygen reduction catalyst had a three-dimensional network structure.
[0060] Example 6
[0061] (1) Carbon black is mixed with an iron nitrate-cobalt nitrate-ethanol solution, and reacted for 5 hours under a temperature condition of 35° C., an air pressure condition of 90 KPa and ultrasonic conditions to obtain a doped carbon black solution, wherein the mass ratio of carbon black to metal ions (iron ions and cobalt ions) is 1:0.1.
[0062] (2) The doped carbon black solution is centrifuged to obtain a precipitate, which is then washed three times with deionized water to obtain an oxygen reduction catalyst.
[0063] The oxygen reduction catalyst prepared in Example 6 was subjected to electron microscope scanning, and the obtained SEM image showed that the oxygen reduction catalyst had a three-dimensional network structure.
[0064] Example 7
[0065] (1) Carbon black is mixed with a potassium chloroplatinate-methanol solution, and reacted for 3 hours under a temperature condition of 35° C., a gas pressure condition of 100 KPa, and ultrasonic conditions to obtain a doped carbon black solution, wherein the mass ratio of carbon black to platinum ions is 1:0.1.
[0066] (2) The doped carbon black solution is centrifuged to obtain a precipitate, which is then washed three times with deionized water to obtain an oxygen reduction catalyst.
[0067] The oxygen reduction catalyst prepared in Example 7 was subjected to electron microscope scanning, and the obtained SEM image showed that the oxygen reduction catalyst had a three-dimensional network structure.
[0068] The above are only preferred embodiments of the present invention, and do not limit the patent scope of the present invention. For those skilled in the art, the present invention may have various changes and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the patent protection scope of the present invention.
Claims
1. A method for preparing an oxygen reduction catalyst, characterized in that: The following steps are involved: The carbon black and the metal ion-solvent solution are mixed and reacted at a temperature of 30 to 40° C. to obtain a doped carbon black solution; the doped carbon black solution is centrifuged to obtain a precipitate, and the precipitate is washed to obtain an oxygen reduction catalyst; In the metal ion solvent solution, the solvent is methanol or ethanol; The reaction time is 1 to 5 hours; The reaction is carried out under a gas pressure of 90 to 110 KPa; The metal salt is at least one of silver acetate, ferric acetate, cobalt acetate, copper acetate, nickel acetate, zinc nitrate, lead nitrate, cobalt nitrate, ferric nitrate, nickel nitrate, ferric chloride, cupric chloride, potassium chloroplatinate, ferric sulfate, copper sulfate, lead sulfate, cobalt nitrate, copper nitrate and manganese nitrate.
2. The method for preparing an oxygen reduction catalyst according to claim 1, wherein: The temperature condition is 35°C.
3. The method for preparing an oxygen reduction catalyst according to claim 1, characterized in that: In the metal ion-solvent solution, the solvent is ethanol.
4. The method for preparing an oxygen reduction catalyst according to claim 1, wherein: In the step of mixing carbon black with a metal ion-solvent solution and reacting them at a temperature of 30 to 40° C. to obtain a doped carbon black solution, the reaction is carried out under ultrasonic conditions.
5. The method for preparing an oxygen reduction catalyst according to claim 1, characterized in that: The mass ratio of the carbon black to the metal ions is 1:(0.01-1).
6. The method for preparing an oxygen reduction catalyst according to claim 1, characterized in that: The metal salt is at least one of silver acetate, ferric acetate, cobalt acetate, copper acetate, cobalt nitrate, ferric nitrate, ferric chloride, copper chloride, potassium chloroplatinate, copper sulfate, cobalt nitrate, copper nitrate and manganese nitrate.