Polyolefin-polystyrene multi-block copolymer and preparation method thereof
Polyolefin-polyphenylene-polybenzene-based multi-block copolymers are solved by controlling the molecular weight and molecular weight distribution of polyolefin-polystyrene-based multi-block copolymers and introducing branch points into the polyolefin blocks, and polymerizing them with transition metal compound catalysts and organozinc compounds. The problem of insufficient mechanical properties of ethylene multi-block copolymers has achieved excellent tensile performance and processability.
Patent Information
- Application Number
- CN202180006719.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-04-16
- Filing Date
- 2021-04-16
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2041-04-16
AI Technical Summary
The existing polyolefin-polystyrene-based multiblock copolymers have problems with insufficient tensile strength, elongation and modulus in terms of mechanical properties, and the molecular weight and molecular weight distribution are difficult to effectively control, affecting their processability and physical properties.
The weight average molecular weight of the polyolefin-polystyrene-based multiblock copolymer is controlled to be between 100,000 and 300,000 g/mol and the molecular weight distribution is between 1.5 and 1.5 and Between 3.0, branch points were introduced into the polyolefin block, and transition metal compounds were used as catalysts, and chain transfer and anion polymerization were carried out in combination with organic zinc compounds and silicon atoms, forming a copolymer with excellent mechanical properties.
The excellent tensile strength, elongation and modulus of polyolefin-polystyrene-based multi-block copolymer is achieved, and is suitable for various industrial uses, and its processability and physical properties are improved.
Smart Images

Figure CN114746459B_ABST
Abstract
Description
Technical Field
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] This application claims priority to Korean Patent Application No. 2020-0046031, filed on Apr. 16, 2020, which is hereby incorporated by reference in its entirety. Technical Field
[0004] The invention relates to a polyolefin-polystyrene multi-block copolymer having a structure in which a polystyrene chain is connected to both ends of a polyolefin chain and a preparation method thereof. Background Art
[0005] Block copolymers are widely used in high-tech devices and general plastics, and their research and development are actively carried out. In particular, styrene-olefin copolymer resins containing polyolefin (PO) blocks and polystyrene (PS) blocks have excellent properties such as heat resistance, light resistance, and elasticity, and are used in a variety of technical fields.
[0006] Polyolefin-polystyrene block copolymers, such as styrene-ethylene-butylene-styrene (SEBS) or styrene-ethylene-propylene-styrene (SEPS), have formed a market of hundreds of thousands of tons of scale in the world. Generally, polystyrene block poly (ethylene-co-1-butylene)-block polystyrene (SEBS) triblock copolymers can be cited as a kind of styrene-olefin copolymer resin. In the structure of SEBS triblock copolymers, hard polystyrene domains are separated from soft poly (ethylene-co-1-butylene) matrix, and act as physical crosslinking sites, showing the property of thermoplastic elastomer. According to these properties, SEBS is more widely used in the product class that needs rubber and plastics, and along with the expansion of scope of use, demand significantly increases.
[0007] At the same time, the molecular weight and molecular weight distribution of copolymers are important factors that determine the mechanical properties, thermal properties, etc. of the material, and have a great influence on processability. Analyzing the molecular weight to analyze the physical properties of copolymers is considered to be the most basic and important technology. As a method for measuring molecular weight, there are viscosity method, end group analysis method, light scattering method, etc., and the most widely used typical method is the method using gel permeation chromatography (GPC).
[0008] GPC is a method of separating substances by molecular weight difference by filling a porous gel in a column, and utilizes the following phenomenon: substances with large molecular weight are discharged without passing through the pores in the gel, and have a short retention time, while substances with small molecular weight are discharged after passing through the pores in the gel, and have a long retention time. From this, the number average molecular weight, weight average molecular weight, etc. can be calculated.
[0009] Under this background, the inventors of the present invention studied methods for preparing polyolefin-polystyrene multi-block copolymers having physical properties such as tensile strength or elongation required for display, and found that by controlling the weight-average molecular weight and molecular weight distribution of the copolymer within a specific range, polyolefin-polystyrene multi-block copolymers having the required physical properties can be prepared, thus completing the present invention.
[0010] [Prior art documents]
[0011] [Patent documents]
[0012] Korean Registered Patent No. 10-1657925 Summary of the Invention
[0013] Technical Problem
[0014] An object of the present invention is to provide a polyolefin-polystyrene multi-block copolymer having a structure in which polystyrene chains are connected to both ends of a polyolefin chain. In particular, the present invention provides a polyolefin-polystyrene multi-block copolymer that exhibits excellent mechanical properties (such as tensile strength, elongation, and modulus) by maintaining a specific relationship between the weight-average molecular weight and the molecular weight distribution.
[0015] Technical Solution
[0016] To solve the above tasks, the present invention provides a polyolefin-polystyrene multi-block copolymer, which satisfies the following conditions (a) to (c) measured by gel permeation chromatography (GPC), and the following 13 condition (d) in the 13C NMR (500 MHz, tetrachloroethane-d2, standard substance TMS) spectrum:
[0017] (a) The weight-average molecular weight is 100,000 to 300,000 g / mol;
[0018] (b) The molecular weight distribution is 1.5 to 3.0;
[0019] (c) Regarding the measurement results of gel permeation chromatography, the Gaussian function modeled by a graph with the x-axis being logMw and the y-axis being dw / dlogMw is represented by the following Mathematical Formula 1. In the following Mathematical Formula 1, all constants satisfy -0.01 < A < 0.03, 4.8 < B < 5.2, 0.8 < C < 1.2, 0.6 < D < 1.2; and
[0020] (d) The polyolefin block in the polyolefin-polystyrene multi-block copolymer contains one or more branch points, the carbon atoms at the branch points show peaks at 36 ppm to 40 ppm, and the terminal carbon atoms of the branched chains starting from the branch points show peaks at 13 ppm to 15 ppm:
[0021] [Formula 1]
[0022]
[0023] (In Formula 1, Mw refers to the weight-average molecular weight of the polyolefin-polystyrene multi-block copolymer).
[0024] Advantageous Effects
[0025] The polyolefin-polystyrene multi-block copolymer provided in the present invention has excellent mechanical properties such as tensile strength, elongation at break, or modulus, and can be applied to various industrial uses. Description of the Drawings
[0026] Figure 1 Shows the 1 1H NMR spectrum and 13 13C NMR spectrum of the transition metal compound prepared in the examples. Detailed Description of the Invention
[0027] Hereinafter, the present invention will be described in more detail to help understand the present invention.
[0028] It should be understood that the words or terms used in the description and claims of the present invention should not be construed as having the meanings defined in a common dictionary. It should be understood that based on the principle that the inventor can appropriately define the meanings of the words to best explain the invention, the words or terms should be construed as having meanings consistent with their meanings in the technical concept of the present invention.
[0029] Polyolefin-polystyrene multi-block copolymer
[0030] The polyolefin-polystyrene multi-block copolymer of the present invention is characterized by satisfying the following conditions (a) to (c) measured by gel permeation chromatography (GPC), and the following 13 condition (d) in the 13C NMR (500 MHz, dichloroethane-d2, standard substance TMS) spectrum:
[0031] (a) The weight-average molecular weight is 100,000 to 300,000 g / mol;
[0032] (b) The molecular weight distribution is 1.5 to 3.0;
[0033] (c) Regarding the measurement result of gel permeation chromatography, the Gaussian function modeled by the graph with the x-axis as logMw and the y-axis as dw / dlogMw is represented by the following Formula 1. In the following Formula 1, all constants satisfy -0.01 < A < 0.03, 4.8 < B < 5.2, 0.8 < C < 1.2, 0.6 < D < 1.2; and
[0034] (d) The polyolefin block in the polyolefin-polystyrene-based multi-block copolymer contains one or more branch points, the carbon atoms at the branch points show a peak of 36 ppm to 40 ppm, and the terminal carbon atoms of the branches starting from the branch points show a peak of 13 ppm to 15 ppm:
[0035] [Mathematical formula 1]
[0036]
[0037] (In Mathematical Formula 1, Mw refers to the weight average molecular weight of the polyolefin-polystyrene multi-block copolymer).
[0038] The polyolefin-polystyrene multi-block copolymer of the present invention is prepared using a specific transition metal compound having a novel structure as a catalyst (to be explained below), and the weight average molecular weight, which is an important factor determining the physical properties of the copolymer, satisfies Mathematical Formula 1, thereby having a weight average molecular weight and molecular weight distribution value of a specific distribution, and achieving excellent tensile properties (e.g., tensile strength, elongation, modulus, etc.).
[0039] Regarding condition (a), the weight average molecular weight of the polyolefin-polystyrene-based multi-block copolymer may be 100,000 to 300,000 g / mol, specifically 105,000 g / mol or more, and 300,000 g / mol or less, 250,000 g / mol or less.
[0040] Regarding the condition (b), the molecular weight distribution of the polyolefin-polystyrene-based multi-block copolymer may be 1.5 to 3.0, specifically 1.5 to 2.5, or 1.5 to 2.3.
[0041] The weight average molecular weight and the number average molecular weight are polystyrene-equivalent molecular weights analyzed by gel permeation chromatography (GPC), and the molecular weight distribution is calculated from the ratio of (weight average molecular weight) / (number average molecular weight).
[0042] As described later, mathematical formula 1 of condition (c) shows a Gaussian distribution, in which constants B to D included therein are used as constants representing the weight average molecular weight and molecular weight distribution of the copolymer, and the copolymer of the present invention satisfies the numerical range of A to D while satisfying the weight average molecular weight and molecular weight distribution values of conditions (a) and (b).
[0043] Regarding condition (c), for the measurement results of gel permeation chromatography, if Mathematical Formula 1 is derived from a Gaussian function modeled by a graph with the x-axis being logMw and the y-axis being dw / dlogMw, then all the constant values included in Mathematical Formula 1 can satisfy -0.01 < A < 0.03, 4.8 < B < 5.2, 0.8 < C < 1.2, and 0.6 < D < 1.2. In particular, the constant A can be greater than -0.01, greater than -0.0099, and less than 0.03, the constant B can be greater than 4.8, greater than 4.85, and less than 5.2, less than 5.19, the constant C can be greater than 0.8, greater than 0.85, and less than 1.2, less than 1.19, and the constant D can be greater than 0.6, greater than 0.65, and less than 1.2, less than 1.19.
[0044] Mathematical Formula 1 represents a differential molecular weight distribution curve, where the horizontal axis is "log(Mw)", which is the logarithm of the weight-average molecular weight (Mw) obtained by gel permeation chromatography measurement based on polystyrene conversion, and the vertical axis is "dw / dlog(Mw)", which is the derivative of the concentration fraction (w) with respect to the logarithm of the weight-average molecular weight (log(Mw)), and can be regarded as showing the weight fraction of polymers having corresponding molecular weights according to the logarithm of the weight-average molecular weight.
[0045] That is to say, in the present invention, the Gaussian function modeled by a graph with the x-axis being logMw and the y-axis being dw / dlogMw is represented by Mathematical Formula 1, and in this case, the values of constants A to D are calculated and found to be included in specific ranges respectively.
[0046] In Mathematical Formula 1, constants A to D are constants representing the curve shown by the Gaussian distribution and show the height of the distribution curve, the width of the half-value of the maximum peak, the central position shown by the maximum peak, etc. More specifically, the constant A included in the Gaussian distribution represents the y-intercept, and the constant C represents the arithmetic meaning of the graph area. In addition, the constants B and D represent the physical properties of the copolymer corresponding to the weight-average molecular weight and the molecular weight distribution.
[0047] Regarding condition (d), the polyolefin block included in the polyolefin-polystyrene multi-block copolymer contains one or more branch points, and the carbon atoms at the branch points can show a peak of 36 ppm to 40 ppm, or a peak of 37 ppm to 40 ppm, and the terminal carbon atoms of the branched chains starting from the branch points can show a peak of 13 ppm to 15 ppm, especially a peak of 13.5 ppm to 15 ppm.
[0048] As described above, in the polyolefin-polystyrene multi-block copolymer of the present invention, the carbon atoms at the branch points have a higher peak, and the terminal carbon atoms of the branched chains have a relatively lower peak, which means that the polyolefin block of the polyolefin-polystyrene multi-block copolymer definitely includes branched chains derived from the main chain, and the branched chains are relatively long to show excellent physical properties.
[0049] The polyolefin-polystyrene multi-block copolymer can be one or more selected from the group consisting of polystyrene-poly(ethylene-co-propylene)-polystyrene block copolymer, polystyrene-poly(ethylene-co-1-butene)-polystyrene block copolymer, polystyrene-poly(ethylene-co-1-pentene)-polystyrene block copolymer, polystyrene-poly(ethylene-co-1-hexene)-polystyrene block copolymer, polystyrene-poly(ethylene-co-1-heptene)-polystyrene block copolymer and polystyrene-poly(ethylene-co-1-octene)-polystyrene block copolymer.
[0050] Preparation method of polyolefin-polystyrene multi-block copolymer
[0051] The preparation method of the polyolefin-polystyrene multi-block copolymer of the present invention is characterized in that it includes: (S1) in the presence of a catalyst composition containing a transition metal compound represented by the following formula 1, using an organic zinc compound as a chain transfer agent to polymerize olefin monomers to form polyolefin blocks; and (S2) in the presence of an alkyl lithium compound containing a silicon atom and a triamine compound, anionic polymerization of the polyolefin blocks and styrene monomers to form polystyrene blocks.
[0052] Step (S1)
[0053] Step (S1) is a step of polymerizing an olefin-based monomer using an organic zinc compound as a chain transfer agent in the presence of a catalyst composition including a transition metal compound represented by the following Formula 1 to form a polyolefin block.
[0054] [Formula 1]
[0055]
[0056] In formula 1,
[0057] M is Ti, Zr or Hf,
[0058] R 1 To R 4 Each independently represents: hydrogen; an alkyl group of 1 to 20 carbon atoms which may or may not be substituted; a cycloalkyl group of 3 to 20 carbon atoms which may or may not be substituted; or an aryl group of 6 to 20 carbon atoms which may or may not be substituted, wherein two or more adjacent groups may be connected to form a ring,
[0059] R 5 and R 6Each is independently: hydrogen; a substituted or unsubstituted alkyl group of 1 to 20 carbon atoms; a substituted or unsubstituted cycloalkyl group of 3 to 20 carbon atoms; or a substituted or unsubstituted aryl group of 6 to 20 carbon atoms, wherein the substituent is an alkyl group of 1 to 12 carbon atoms,
[0060] Each R 7 is independently a substituted or unsubstituted alkyl group of 4 to 20 carbon atoms; a substituted or unsubstituted cycloalkyl group of 4 to 20 carbon atoms; or a substituted or unsubstituted aryl group of 6 to 20 carbon atoms,
[0061] n is 1 to 5, and
[0062] Y 1 and Y 2 Each is independently a halogen group; an alkyl group having 1 to 20 carbon atoms; an alkenyl group having 2 to 20 carbon atoms; an alkynyl group having 2 to 20 carbon atoms; a cycloalkyl group having 3 to 20 carbon atoms; an aryl group having 6 to 20 carbon atoms; an alkylaryl group having 7 to 20 carbon atoms; an arylalkyl group having 7 to 20 carbon atoms; a heteroaryl group having 5 to 20 carbon atoms; an alkoxy group having 1 to 20 carbon atoms; an aryloxy group having 5 to 20 carbon atoms which may or may not have a substituent; an alkylamino group having 1 to 20 carbon atoms; an arylamino group having 5 to 20 carbon atoms; an alkylthio group having 1 to 20 carbon atoms; an arylthio group having 5 to 20 carbon atoms; an alkylsilyl group having 1 to 20 carbon atoms; an arylsilyl group having 5 to 20 carbon atoms; a hydroxyl group; an amino group; a thiol group; a silyl group; a cyano group; or a nitro group.
[0063] In particular, in Formula 1, M may be Hf.
[0064] In particular, in Formula 1, R 1 To R 4 can be independently: hydrogen; or an alkyl group of 1 to 20 carbon atoms which may or may not have a substituent, wherein two or more adjacent groups may be connected to form a ring. 1 and R 2 may each independently be an alkyl group of 1 to 20 carbon atoms, and may be linked to each other to form an aromatic ring of 5 to 20 carbon atoms, and R 3 and R 4 It may be hydrogen.
[0065] In particular, in Formula 1, R 5 and R 6 Each is independently: hydrogen; or an aryl group having 6 to 20 carbon atoms which may be substituted, wherein the substituent is an alkyl group having 1 to 6 carbon atoms.
[0066] In particular, in Formula 1, each R7 The group may independently be: a substituted or unsubstituted alkyl group having 4 to 20 carbon atoms; a substituted or unsubstituted cycloalkyl group having 4 to 20 carbon atoms; or a substituted or unsubstituted aryl group having 6 to 20 carbon atoms.
[0067] Particularly, in Formula 1, n may be 1 to 3, preferably 2.
[0068] In particular, in Equation 1, X 1 and X 2 Each independently may be an alkyl group having 1 to 20 carbon atoms.
[0069] More specifically, the transition metal compound represented by Formula 1 may be a compound represented by the following Formula 1a.
[0070] [Formula 1a]
[0071]
[0072] In formula 1a,
[0073] M.R 5 To R 7 , Y 1 and Y 2 Same as above definition.
[0074] The transition metal compound represented by Formula 1 may be selected from the following compounds, but is not limited thereto, and all transition metal compounds corresponding to Formula 1 are included in the present invention.
[0075]
[0076] In addition, the present invention provides a ligand compound represented by the following Formula 2.
[0077] [Formula 2]
[0078]
[0079] In formula 2,
[0080] R 1 To R 4 Each is independently: an alkyl group of 1 to 20 carbon atoms which may be substituted or unsubstituted; a cycloalkyl group of 3 to 20 carbon atoms which may be substituted or unsubstituted; or an aryl group of 6 to 20 carbon atoms which may be substituted or unsubstituted, wherein two or more adjacent groups may be connected to form a ring,
[0081] R 5 and R 6Each is independently: hydrogen; a substituted or unsubstituted alkyl group of 1 to 20 carbon atoms; a substituted or unsubstituted cycloalkyl group of 3 to 20 carbon atoms; or a substituted or unsubstituted aryl group of 6 to 20 carbon atoms, wherein the substituent is an alkyl group of 1 to 12 carbon atoms,
[0082] Each R 7 are independently: a substituted or unsubstituted alkyl group of 4 to 20 carbon atoms; a substituted or unsubstituted cycloalkyl group of 4 to 20 carbon atoms; or a substituted or unsubstituted aryl group of 6 to 20 carbon atoms, and
[0083] n It is 1 to 5.
[0084] That is, the transition metal compound of the present invention can be prepared by a step including reacting a ligand compound represented by Formula 2 below with a compound represented by Formula 3.
[0085] [Formula 2]
[0086]
[0087] [Formula 3]
[0088] M(Y 1 Y 2 ) 2
[0089] In the above formula,
[0090] R 1 To R 7 , M, Y 1 and Y 2 Same as above definition.
[0091] Meanwhile, during the preparation of the transition metal compound represented by Formula 1 of the present invention, the reaction may be performed through the following process.
[0092] [Reaction 1]
[0093]
[0094] [Reaction 2]
[0095]
[0096] In the present invention, the organic zinc compound is used as a chain transfer agent, which is a substance that induces the preparation of the copolymer by chain transfer during the preparation process in the polymerization reaction, and specifically, it may be a compound represented by the following Formula 4.
[0097] [Formula 4]
[0098]
[0099] In formula 4,
[0100] A is: an alkylene group of 1 to 20 carbon atoms; an arylene group of 6 to 20 carbon atoms; or an arylene group of 6 to 20 carbon atoms substituted with halogen, an alkyl group of 1 to 12 carbon atoms, a cycloalkyl group of 3 to 12 carbon atoms, an alkoxy group of 1 to 8 carbon atoms, or an aryl group of 6 to 12 carbon atoms, and
[0101] B is an arylene group of 6 to 12 carbon atoms substituted with an alkenyl group of 2 to 12 carbon atoms.
[0102] In addition, A may be: an alkylene group of 1 to 12 carbon atoms; an arylene group of 6 to 12 carbon atoms; or an arylene group of 6 to 12 carbon atoms substituted with halogen, an alkyl group of 1 to 12 carbon atoms, a cycloalkyl group of 3 to 12 carbon atoms, an alkoxy group of 1 to 8 carbon atoms, or an aryl group of 6 to 12 carbon atoms, and
[0103] B may be an arylene group of 6 to 12 carbon atoms substituted with an alkenyl group of 2 to 8 carbon atoms.
[0104] Formula 4 may have a structure in which both terminals of the formula have double bonds. For example, if B is an arylene group substituted with an alkenyl group, the arylene group may be connected to A, and the double bond of the alkenyl group substituted on the arylene group may be located outermost in Formula 4.
[0105] In the case where the organozinc compound reacts with one or more olefinic monomers in the presence of the catalyst composition, polymerization can be performed with the olefinic monomer interposed between zinc (Zn) of the organozinc compound and the organic group (A).
[0106] The mixing amount of the organic zinc compound may be 1 to 200 equivalents based on 1 equivalent of the transition metal compound of Formula 1, and specifically, the mixing amount may be 10 to 100 equivalents based on 1 equivalent of the transition metal compound of Formula 1.
[0107] The organozinc compound does not contain THF and impurities (such as a large amount of magnesium salt), can be used in high purity, and therefore, can be used as a chain transfer agent and is advantageously used in olefin polymerization.
[0108] In addition, the catalyst composition may further include a compound represented by the following Formula 5, and the compound represented by Formula 5 may function as a co-catalyst and a scavenger at the same time.
[0109] [Formula 5]
[0110] -[Al(R a )-O] m -
[0111] In formula 5,
[0112] Each R a are independently: a halogen group; a hydrocarbon group of 1 to 20 carbon atoms; or a halogen-substituted hydrocarbon group of 1 to 20 carbon atoms, and
[0113] M is an integer greater than or equal to 2.
[0114] The compound represented by Formula 5 is not particularly limited as long as it is an alkylaluminoxane. Preferred examples may be modified methylaluminoxane (MMAO), methylaluminoxane (MAO), ethylaluminoxane, isobutylaluminoxane, butylaluminoxane, etc., and a particularly preferred compound may be modified methylaluminoxane (MMAO).
[0115] The compound represented by Formula 5 is a compound of the oligomer type generated by the reaction of alkyl aluminum and water, and if used as a co-catalyst, chain transfer can be reduced. Therefore, a copolymer with a high molecular weight can be prepared, and the formation of homopolyolefins by side reactions can be prevented. Therefore, finally, a polyolefin-polystyrene multi-block copolymer showing excellent physical properties such as high tensile strength can be prepared.
[0116] Meanwhile, the compound represented by Formula 5 can inhibit chain transfer as described above, whereas, for example, when a compound such as alkylaluminum is used as a co-catalyst, chain transfer occurs in large amounts, the molecular weight of the copolymer may decrease, the production of homopolyolefins may increase, and the physical properties of the block copolymer may deteriorate.
[0117] In this way, by using the transition metal compound represented by Formula 1 and the compound represented by Formula 5 in combination, a polyolefin-polystyrene-based multi-block copolymer having the conditions (a) to (d) can be prepared.
[0118] In addition, the transition metal compound represented by Formula 1 and the compound represented by Formula 5 may be used in a supported form via a carrier. As the carrier, silica or alumina may be used without limitation.
[0119] In addition, the catalyst composition may further include a compound represented by Formula 6 below.
[0120] [Formula 6]
[0121] [LH] + [Z(A) 4 ] - or [L] + [Z(A) 4 ] -
[0122] In formula 6,
[0123] Z is an element of group 13,
[0124] Each A is independently: an aryl group of 6 to 20 carbon atoms, in which one or more hydrogen atoms may be substituted by a substituent; or an alkyl group of 1 to 20 carbon atoms, and
[0125] The substituent of A is: halogen; a hydrocarbon group of 1 to 20 carbon atoms; an alkoxy group of 1 to 20 carbon atoms; or an aryloxy group of 6 to 20 carbon atoms.
[0126] In step (S1), the olefin monomer injected as the reaction material can be ethylene, propylene, 1-butene, 1-pentene, 4-methyl-1-pentene, 1-hexene, 1-heptene, 1-octene, 1-decene, 1-undecene, 1-dodecene, 1-tetradecene, 1-hexadecene, 1-eicosene or a mixture thereof. The olefin monomer can be used alone or as a mixture of two or more.
[0127] For example, step (S1) can be carried out in a homogeneous solution state. In this case, a hydrocarbon solvent can be used as a solvent, or the olefin monomer itself can be used as a medium. The hydrocarbon solvent can include an aliphatic hydrocarbon solvent of 4 to 20 carbon atoms, particularly isobutane, hexane, cyclohexane, methylcyclohexane, etc. The solvent can be used alone, or a mixture of two or more thereof can be used.
[0128] The polymerization temperature of step (S1) may vary according to reaction materials, reaction conditions, etc., and may be specifically 70 to 170° C., particularly 80 to 150° C., or 90 to 120° C. Within the above range, the solubility of the polymer may increase and the catalyst may have thermal stability.
[0129] The polymerization in step (S1) may be performed by a batch system or a continuous system, or may be performed by two or more steps having different reaction conditions.
[0130] The compound prepared in the above step (S1) can serve as a precursor for preparing the polyolefin-polystyrene multi-block copolymer of the present invention by an anionic polymerization reaction in the step (S2) described later.
[0131] Step (S2)
[0132] Step (S2) is a step of preparing a polyolefin-polystyrene multiblock copolymer by anionic polymerization of a polyolefin block and a styrene monomer in the presence of an alkyl lithium compound containing a silicon atom and a triamine compound to form a polystyrene block.
[0133] In step (S2), the styrene monomers can be continuously inserted into the (polyolefin group) contained in the compound formed in step (S1) 2The zinc-carbon bonds of Zn are formed between the Zn groups, and the styrene groups present at the ends of the compound formed by step (S1) can be used as copolymer sites to participate in the styrene monomers and thus be connected to the styrene chains. In addition, the multi-block copolymer produced by this method can be easily quenched by the reaction of the end groups with water, oxygen or organic acids, and thereby can be converted into industrially useful polyolefin-polystyrene multi-block copolymers.
[0134] The styrene-based monomer may be a styrene-based monomer having 6 to 20 carbon atoms. More specifically, a styrene-based monomer including ethylene substituted with an aromatic group having 6 to 20 carbon atoms, ethylene substituted with a phenyl group, etc., such as styrene, may be used.
[0135] The alkyl lithium compound including a silicon atom may be a compound represented by Formula 7 below.
[0136] [Formula 7]
[0137] (CH 3 ) 3 Si(CH 2 )Li
[0138] Such an alkyl lithium compound containing a silicon atom is a material widely used as an anionic polymerization initiator and easily available, and is advantageously used in the present invention.
[0139] The triamine compound may be a compound represented by Formula 8 below.
[0140] [Formula 8]
[0141]
[0142] The triamine compound is a compound that is easily coordinated with lithium and is used to improve the reactivity of the alkyl lithium compound as a base or as a nucleophilic agent. It is easily available and has a low unit price.
[0143] The present invention novel uses compounds of formula 7 and formula 8 (for example, Me 3 SiC 2 Li·(PMDETA)) as the initiator of step (S2) can suppress the production of polystyrene homopolymer, polyolefin homopolymer and polyolefin-polystyrene diblock copolymer while maximizing the production of the polyolefin-polystyrene multiblock copolymer which is the object of the present invention.
[0144] The alkyllithium compound containing silicon atoms represented by Formula 7 and the triamine compound represented by Formula 8 may be mixed in an aliphatic hydrocarbon solvent and then injected, or the alkyllithium compound containing silicon atoms represented by Formula 7 and the triamine compound represented by Formula 8 may be sequentially injected into the reactor.
[0145] The anionic polymerization temperature of step (S2) may vary according to the reaction materials, reaction conditions, etc., and may be specifically performed at 40°C to 170°C, more specifically, 80°C to 120°C.
[0146] The anionic polymerization of step (S2) may be performed by a batch system, a semi-continuous system, or a continuous system, or may be performed by two or more steps having different reaction conditions.
[0147] The anionic polymerization time of step (S2) can be changed according to the reaction materials, reaction conditions, etc., and can be specifically 0.5 to 10 hours, 0.5 to 8 hours, 0.5 to 5 hours or 0.5 to 2 hours. Within the above range, the conversion of the total amount of styrene monomers injected into the multi-block copolymer may be favorable.
[0148] As described above, in the preparation method of the present invention, a polyolefin-polystyrene multi-block copolymer can be prepared by propagating a polyolefin chain through olefin polymerization using the above-mentioned organic zinc compound represented by Formula 4 and continuously performing styrene anion polymerization, and thereby a polyolefin-polystyrene multi-block copolymer having better physical properties than before and easily used in industry can be efficiently prepared.
[0149] Example
[0150] Hereinafter, the present invention will be explained in more detail with reference to Examples. However, the Examples are for illustrating the present invention, and the scope of the present invention is not limited thereto.
[0151] Reagents and experimental conditions
[0152] All experiments were performed under inert atmosphere using a standard glove box and Schlenk technique. Toluene, hexane, and tetrahydrofuran (THF) were distilled from benzophenone ketyl radical and used. Methylcyclohexane (anhydrous grade) used for polymerization was purchased from Tokyo Chemical Industry (TCI) and used after purification using Na / K alloy. Sublimation grade HfCl 4 Purchased from Streme and used as received. Ethylene-propylene gas mixture was purified using trioctylaluminum (0.6 M in mineral spirits) in a bomb reactor (2.0 L).
[0153] Recorded using ECZ 600 equipment (JOEL) 1 H NMR (600 MHz) and 13 C NMR (150 MHz) spectrum.
[0154] Elemental analyses were performed at the Asia University Analytical Center.
[0155] GPC data were analyzed in 1,2,4-trichlorobenzene at 160°C using a PL-GPC 220 system equipped with a refractive index detector and two columns (Plarian Mixed-B 7.5x300 mm Varian [Polymer Lab]).
[0156] Preparation of transition metal compounds
[0157] [Formula 1-1]
[0158]
[0159] (i) Preparation of ligand compound
[0160]
[0161] 2,6-dicyclohexylaniline (0.772 g, 3.00 mmol) and 6-bromo-2-pyridinecarboxaldehyde (0.558 g, 3.00 mmol) were dissolved in toluene (5 mL), and molecular sieves were injected therein. The mixture thus obtained was heated to 70 ° C overnight under stirring. After filtering, the solvent was removed using a rotary evaporator. A yellow solid (1.07 g, 84%) was obtained.
[0162] 1 H NMR (C 6 D 6 ): δ8.41(s,1H,NCH),8.09(d,J=7.8Hz,1H),7.53(m,3H),6.85(d,J=7.8Hz,1H),6.63(t,J=7.8Hz,1H),2.74(m,2H), 1.87(d,J=12Hz,4H), 1.64(d,J=12.6Hz,4H), 1.54(d,J=10.8Hz,2H), 1.39(quartet,J=10.2Hz,4H), 1.11(m,6H)ppm.
[0163] 13 C NMR (C 6 D 6 ): δ26.55,27.33,34.25,39.30,119.42,124.32,125.21,129.83,136.68,138.82,142.54,148.94,155.95,162.06ppm.
[0164] HRMS(EI): m / z calculated ([M + ]C 24 H 29 Bn 2)424.1514. Measured value: 424.1516.
[0165] Under nitrogen, the above compound (1.07 g, 2.51 mmol), 1-naphthaleneboronic acid (0.453 g, 2.64 mmol), Na 2 CO 3 (0.700 g, 6.60 mmol) and toluene (5 mL) were placed in a schlenk flask. Degassed H 2 O / EtOH (1 mL, volume ratio, 1:1) and (Ph 3 P) 4 A toluene (1 mL) solution of Pd (7.83 mg, 0.00678 mmol) was subjected to column chromatography on silica gel using hexane and ethyl acetate (volume ratio, 90:3:1) containing a small amount of triethylamine to obtain a lemon yellow oil (0.712 g, 60%).
[0166] 1 H NMR (C 6 D 6 ): δ8.70(s,1H,NCH),8.41(d,J=7.8Hz,1H),8.31(d,J=7.8Hz,1H),7.68(d,J=7.2Hz,1H),7.65(d,J=7.8Hz,1H),7.54(d,J=7.2Hz,1H),7. 27(m,4H),7.20(m,4H),2.93(m,2H),1.90(d,J=12Hz,4H),1.61(d,J=13.2Hz,4H),1.50(d,J=12.6Hz,2H),1.38(m,4H),1.11(m,6H),ppm.
[0167] 13 C NMR (C 6 D 6 ): δ26.63,27.38,34.35,39.36,119.21,124.32,124.98,125.50,126.15,126.21,126.64,126.75,12 8.15,128.73,129.38,131.81,134.52,136.94,137.14,138.52,149.48,155.13,159.79,164.05ppm.
[0168] HRMS(EI): m / z calculated ([M + ]C 34 H 36 N 2 )472.2878. Measured value: 472.2878.
[0169] 2-isopropylphenyl lithium (0.114 g, 0.904 mmol) dissolved in ether (8 mL) was added dropwise to a schlenk flask containing the above compound (0.247, 0.523 mmol) in ether (20 mL). After stirring for 3 hours, an aqueous solution of ammonium chloride (0.30 g) (10 mL) was added and the product was extracted with ether (3 x 10 mL). The resulting oil was dried overnight at 60 ° C under high vacuum. A yellow solid (0.257 g, 83%) was obtained.
[0170] H NMR (C 6 D 6 ): δ8.24(m,1H),7.90(m,1H),7.64(m,1H),7.62(d,J=7.8Hz,1H),7.56(d,J=7.2H z,1H),7.26(m,3H),7.22(m,4H),7.11(m,5H),5.62(d,J=5.4Hz,1H,NCH),4.59(d ,J=5.4Hz,1H,NH),3.31(septet,J=7.2Hz,1H,CH),2.74(m,2H),1.79(d,J=7.8Hz ,2H),1.64(m,4H),1.54(m,4H),1.32(m,4H),1.08(m,2H),1.03(d,J=6.6Hz,3H,CH 3 ),1.00(m,1H),0.980(d,J=6.6Hz,3H,CH 3 ),0.921(m,3H)ppm.
[0171] 13 C NMR (C 6 D 6 ): δ23.78,24.45,26.63,27.42,27.54,28.96,34.77,35.08,39.01,67.64,119.99,122.89,124.13,124.80,125.36,125.77,126.08,1 26.46,126.56,126.71,127.58,128.55,129.35,131.84,134.64,136.94,138.77,141.88,142.24,144.97,146.32,159.28,163.74ppm.
[0172] HRMS(EI): m / z calculated ([M + ]C 43 H 48 N2 )592.3817. Measured value: 592.3819.
[0173] (ii) Preparation of transition metal compounds
[0174] The ligand compound (0.150 g, 0.253 mmol) in toluene (1.5 g) was placed in a schlenk flask, and n-BuLi (0.17 mL, 1.6 M hexane solution, 0.27 mmol) was added dropwise at room temperature. After stirring for 1 hour, HfCl 4 (0.814 g, 0.254 mmol) was added thereto as a solid. The reaction mixture was heated at 100°C and stirred for 2 hours. After cooling, MeMgBr (0.29 mL, 3.1 M ether solution, 0.89 mmol) was injected and stirred at room temperature overnight. After removing volatile substances through a vacuum line, the product was extracted with toluene (1.5 g). The extract was filtered through diatomaceous earth filtration. The solvent was removed through a vacuum line, and the residue was softened in hexane (2 mL) to obtain a yellow solid (0.128 g, 63%). It was analyzed 1 H NMR spectra and 13 CNMR spectrum, the results show Figure 1 middle.
[0175] 1 H NMR (C 6 D 6 ): δ8.58(d,J=7.8Hz,1H),8.29(d,J=8.4Hz,1H),7.79(d,J=7.8Hz,1H),7.71(d,J=7.2Hz,1H ),7.54(d,J=7.8Hz,1H),7.46(m,1H),7.30(m,2H),7.15(m,3H),7.09(m,3H),6.88(t,J=7.8H z,1H),6.62(d,J=8.4Hz,1H),6.48(s,1H,NCH),3.39(m,1H),2.92(m,2H),2.15(d,J=13.8Hz ,1H),2.10(d,J=13.8Hz,2H),1.80(m,2H),1.65(m,3H),1.29(m,6H),1.17(d,J=7.2Hz,3H,CH 3 ),1.07(m,3H),0.99(s,3H,HfCH 3 ),0.95(m,2H),0.73(d,J=7.2Hz,3H,CH 3 ),0.70(s,3H,HfCH 3 ),0.23(m,1H)ppm.
[0176] 13 C NMR (C 6 D 6 ): δ23.31,25.04,26.63,26.74,27.70,27.76,27.81,28.29,28.89,35.00,35.66,36. 62,37.02,38.13,40.88,62.53,67.00,77.27,119.30,120.30,124.29,125.52,125.6 0,125.97,126.95,127.06,127.73,129.91,130.00,130.09,130.85,134.36,135.80, 140.73,140.89,144.02,145.12,146.31,146.38,146.49,164.46,170.79,206.40ppm.
[0177] Analytical calculation value (C 45 H 52 HkDJ 2 ): C, 67.61; H, 6.56; N, 3.50%. Measured value: C, 67.98; H, 6.88; N, 3.19%.
[0178] Preparation of organozinc compounds
[0179]
[0180] Borane dimethyl sulfide (1.6mL, 3.2mmol) was slowly injected into triethylborane (0.6g) under stirring and reacted for 90 minutes. The resulting product was slowly injected into divinylbenzene (3.8g) dissolved in anhydrous ether (10mL) cooled to -20°C, and then stirred overnight. After removing the solvent using a vacuum pump, diethyl zinc (0.8g) was added. In the case of removing the triethylborane produced by distillation under reduced pressure, the reaction was carried out at 0°C for 5 hours. Excess divinylbenzene and diethyl zinc were removed by distillation under reduced pressure at 40°C. Methylcyclohexane (150mL) was added and the resulting product was dissolved again. The solid compound generated as a by-product was filtered using diatomaceous earth to prepare the organic zinc compound represented by the above formula.
[0181] Preparation of polyolefin-polystyrene multi-block copolymers
[0182] Example 1
[0183] The parr reactor (600 mL) was dried under vacuum at 120° C. for 2 hours. A solution of MMAO (813 mg, 2020 μmol-Al) in methylcyclohexane (200 g) was injected into the reactor as a scavenger. The mixture thus obtained was stirred at 120° C. for 1 hour using a heating mantle and the solution was removed using a catheter.
[0184] The reactor was filled with methylcyclohexane (1200 g) containing MMAO (2020 μmol-Al) as a scavenger, and 1-hexene (560 g) was charged as an olefin monomer, and then the temperature was set to 90° C. A solution of an organic zinc compound (2800 μmol) in methylcyclohexane (1.58 g) was charged as a chain transfer agent, and a mixture containing [(C 18 H 37 ) 2 N(H)Me] + [B(C 6 F 5 ) 4 ] - (1.0 equivalent) of an activated transition metal compound (12 μmol-Hf) in methylcyclohexane. The valve of the ethylene tank was opened, while the pressure in the reactor was maintained at 25 bar, and polymerization was carried out in the range of 90°C to 120°C for 40 minutes. After the polymerization, the ethylene gas was exhausted and the temperature of the reactor was controlled to 90°C again.
[0185] If the temperature reaches 90°C, add Me(III) (3.85 g) mixed in methylcyclohexane. 3 SiC 2 Me prepared from Li (3.080 mmol) and PMDETA (3.388 mmol) 3 SiC 2 Li(PMDETA) solution. After the temperature was maintained at 90°C for 30 minutes while stirring, styrene (132 g) was injected. The temperature was controlled in the range of 90°C to 100°C using a heating mantle. The viscosity gradually increased and reached an almost invisible state within 5 hours. 1 H NMR analysis confirmed the complete conversion of styrene. After the complete conversion of styrene, 2-ethylhexanoic acid and ethanol were injected continuously. The polymer mass thus obtained was dried in a vacuum oven at 80°C overnight.
[0186] Examples 2 to 15
[0187] The same method as in Example 1 was carried out except that the reaction conditions were changed as shown in Table 1 below.
[0188] Comparative Examples 1 to 4
[0189] As commercially available SEBS, G1650, G1651, G1652 and G1654 from Kraton were used respectively.
[0190] Comparative Example 5
[0191] The preparation was carried out by the following method using a compound represented by the following formula as a transition metal compound.
[0192] [Comparison formula 1]
[0193]
[0194] A solution of trimethylaluminum (14.4 mg, 200 μmol-Al) dissolved in methylcyclohexane (17 g) was injected into the autoclave. The autoclave was purged of catalyst poisons at 100° C. for 1 hour, and the solution was removed using a cannula.
[0195] The organozinc compound (49.1 mg, 150 μmol) was dissolved in methylcyclohexane (40 g) and injected into the high-pressure reactor, and then the temperature was raised to 80° C. 18 H 37 )N(Me)H + [B(C 6 F 5 ) 4 ] - A solution obtained by stirring trioctylaluminum (4.0 μmol) in benzene for 2 hours was diluted in a solution (1.0 g) obtained by dissolving trioctylaluminum (50 μmol, 18.3 mg) in methylcyclohexane (15 g). The catalyst solution was injected into a high-pressure reactor, and then an ethylene-propylene mixed gas was injected at a pressure of 20 bar. The temperature was controlled in the range of 95° C. to 115° C. The pressure was slowly reduced as the monomer was consumed, and after a polymerization process of 55 minutes at 45° C., the remaining gas was discharged.
[0196] Will Me 3 SiC 2 Li (150 μmol, 14.1 mg) and PMDETA (150 μmol, 26 mg) were mixed in methylcyclohexane (1.0 g), then injected into the reactor and stirred for 30 minutes. The stirring temperature was maintained at 90°C to 100°C. After styrene (7.8 g) was injected into the high pressure reactor, the reaction was carried out for 5 hours while the temperature was maintained at 90°C to 100°C to convert all styrene monomers. After the styrene monomers were fully converted, acetic acid and ethanol were continuously injected. After obtaining the polymer, it was dried overnight at 180°C in a vacuum oven.
[0197] Comparative Examples 6 to 9
[0198] A copolymer was prepared by the same method as in Comparative Example 5, except that the polymerization conditions were changed as shown in Table 1 below.
[0199] [Table 1]
[0200]
[0201]
[0202] Experimental Example 1
[0203] For the polyolefin-polystyrene-based multi-block copolymers of Examples and Comparative Examples, the following physical properties of the copolymers were measured.
[0204] (1) Measurement of ethylene, α-olefin and styrene content
[0205] The measurement was performed by NMR. The measurement was performed using a Bruker 600MHz AVANCE III HD NMR instrument under the conditions of ns=16, d1=3s, solvent=TCE-d2 and 373K. 1 H NMR, and the solvent peak of TCE-d2 was calibrated to 6.0 ppm. 3 At 1 ppm, CH 3 The relevant peak (triplet) was at about 0.96 ppm and the content was calculated. In addition, the styrene content was calculated from the aromatic peak at about 6.5 ppm to 7.5 ppm.
[0206] (2) Weight average molecular weight (Mw, g / mol) and molecular weight distribution (polydispersity index, PDI)
[0207] The weight average molecular weight (Mw, g / mol) and number average molecular weight (Mn, g / mol) were measured separately, and the molecular weight distribution (polydispersity index, PDI) was calculated by dividing the weight average molecular weight by the number average molecular weight.
[0208] Column: PL Olexis
[0209] Solvent: Trichlorobenzene (TCB)
[0210] Flow rate: 1.0ml / min
[0211] Sample concentration: 1.0mg / ml
[0212] Injection volume: 200 μl
[0213] Column temperature: 160°C
[0214] Detector: Agilent high temperature RI detector
[0215] Standard: Styrene
[0216] The Mark-Houwink equation (K = 40.8 × 10 -5 , α = 0.7057) were used to calculate the molecular weight by universal calibration.
[0217] (3) Calculate the value of constant AD in equation 1
[0218] To calculate the value of the constant AD, the GPC measurement data were fitted with a Gaussian function using Origin's nonlinear curve fitting.
[0219] [Table 2]
[0220]
[0221] Experimental Example 2
[0222] For the polyolefin-polystyrene-based multi-block copolymers of Examples and Comparative Examples, the peak values of carbon atoms at branch points and terminal carbon atoms of branches starting from the branch points are summarized and recorded in Table 3 below.
[0223] Specifically, using a Bruker AVANCEIII 500MHz NMR instrument, about 50 mg of a sample was placed in 1.2 mL of TCE-d2 (tetrachloroethane-d2) solvent and then heated in a heater at 100°C for 1 hour while vortexing two or three times. After checking for uniform dissolution, the sample was transferred to an NMR tube and measured at 100°C. 13 C NMR spectrum.
[0224] [Table 3]
[0225] Branch point carbon atom The terminal carbon atom of the branch Example 1 38 14 Example 2 38 14 Example 3 38 14 Example 4 38 14 Example 5 38 14 Example 6 38 14 Example 7 38 14 Example 8 38 14 Example 9 38 14 Example 10 38 14 Embodiment 11 38 14 Example 12 38 14 Embodiment 13 38 14 Embodiment 14 38 14 Embodiment 15 38 14 Comparative Example 1 34 11 Comparative Example 2 34 11 Comparative Example 3 34 11 Comparative Example 4 34 11 Comparative Example 5 30 23 Comparative Example 6 30 23 Comparative Example 7 30 23 Comparative Example 8 38 14 Comparative Example 9 38 14
[0226] Experimental Example 3
[0227] Each test specimen was formed based on the ASTM D412 tensile test method, and the tensile strength, elongation, and 300% modulus were measured.
[0228] [Table 4]
[0229]
[0230] As shown in Table 4 above, it is confirmed that the block copolymers of Examples 1 to 15 that meet all of the conditions (a) to (d) set forth in the present invention exhibit the same excellent tensile properties, including tensile strength, elongation and 300% modulus, at a certain level compared to the copolymers of Comparative Examples that do not meet all of the conditions.
[0231] Experimental Example 4
[0232] The complex viscosity was measured using the Advanced Rheometric Expansion System (ARES) from TA Instruments. The sample gap was set to 2.0 mm using a 25.0 mm diameter parallel plate at 160°C. The measurement was performed at a frequency of 0.05 rad / s to 500 rad / s using a dynamic strain frequency sweep mode and a strain of 5%, with 10 points measured per decade and a total of 41 points measured.
[0233] The complex viscosities at frequencies of 0.5 rad / s and 125 rad / s are summarized and reported in Table 5 below.
[0234] [Table 5]
[0235]
[0236] As shown in the results, it was confirmed that the polyolefin-polystyrene-based multi-block copolymer of the present invention exhibited a low complex viscosity in a high frequency region, particularly at a frequency of 125 rad / s, and excellent processability.
Claims
1. A method for preparing a polyolefin-polystyrene multi-block copolymer, the method comprising: (S1) polymerizing an olefin monomer using an organic zinc compound as a chain transfer agent in the presence of a catalyst composition comprising a transition metal compound represented by the following Formula 1 to form a polyolefin block; and (S2) anion polymerizing the polyolefin block and a styrene monomer in the presence of an alkyl lithium compound containing a silicon atom and a triamine compound to form a polystyrene block: [Formula 1] In formula 1, M is Ti, Zr or Hf, R1 to R4 are each independently: hydrogen; an alkyl group of 1 to 20 carbon atoms which may be substituted or unsubstituted; a cycloalkyl group of 3 to 20 carbon atoms which may be substituted or unsubstituted; or an aryl group of 6 to 20 carbon atoms which may be substituted or unsubstituted, wherein two or more adjacent groups may be connected to form a ring, R5 and R6 are each independently: hydrogen; a substituted or unsubstituted alkyl group of 1 to 20 carbon atoms; a substituted or unsubstituted cycloalkyl group of 3 to 20 carbon atoms; or a substituted or unsubstituted aryl group of 6 to 20 carbon atoms, wherein the substituent is an alkyl group of 1 to 12 carbon atoms, Each R7 is independently: a cycloalkyl group having 6 to 20 carbon atoms which may be substituted or unsubstituted, n is 1 to 5, and Y1 and Y2 are each independently: a halogen group; an alkyl group of 1 to 20 carbon atoms; an alkenyl group of 2 to 20 carbon atoms; an alkynyl group of 2 to 20 carbon atoms; a cycloalkyl group of 3 to 20 carbon atoms; an aryl group of 6 to 20 carbon atoms; an alkylaryl group of 7 to 20 carbon atoms; an arylalkyl group of 7 to 20 carbon atoms; a heteroaryl group of 5 to 20 carbon atoms; an alkoxy group of 1 to 20 carbon atoms; an aryloxy group of 5 to 20 carbon atoms which may or may not have a substituent; an alkylamino group of 1 to 20 carbon atoms; an arylamino group of 5 to 20 carbon atoms; an alkylthio group of 1 to 20 carbon atoms; an arylthio group of 5 to 20 carbon atoms; an alkylsilyl group of 1 to 20 carbon atoms; an arylsilyl group of 5 to 20 carbon atoms; a hydroxyl group; an amino group; a thiol group; a silyl group; a cyano group; or a nitro group.
2. The method for preparing a polyolefin-polystyrene multi-block copolymer according to claim 1, wherein: The transition metal compound represented by Formula 1 is selected from the following compounds:
3. The method for preparing a polyolefin-polystyrene multi-block copolymer according to claim 1, wherein: The organic zinc compound is a compound represented by the following formula 4: [Formula 4] In formula 4, A is: an alkylene group of 1 to 20 carbon atoms; an arylene group of 6 to 20 carbon atoms; or an arylene group of 6 to 20 carbon atoms substituted with halogen, an alkyl group of 1 to 12 carbon atoms, a cycloalkyl group of 3 to 12 carbon atoms, an alkoxy group of 1 to 8 carbon atoms, or an aryl group of 6 to 12 carbon atoms, and B is an arylene group of 6 to 12 carbon atoms substituted with an alkenyl group of 2 to 12 carbon atoms.
4. A polyolefin-polystyrene multi-block copolymer prepared by the method of claim 1, wherein the copolymer satisfies the following conditions (a) to (c) measured by gel permeation chromatography (GPC) and the following conditions (a) to (c) using 500 MHz, tetrachloroethane-d2, standard substance TMS. 13 Condition (d) in C NMR spectroscopy: (a) a weight average molecular weight of from greater than 150,000 g / mol to 300,000 g / mol; (b) a molecular weight distribution of 1.5 to 3.0; (c) Regarding the measurement results by gel permeation chromatography, the Gaussian function modeled by a graph with the x-axis being logMw and the y-axis being dw / dlogMw is represented by the following Mathematical Formula 1. In the following Mathematical Formula 1, all constants satisfy -0.01 < A < 0.03, 4.8 < B < 5.2, 0.8 < C < 1.2, and 0.6 < D < 1.2; and (d) The polyolefin block in the polyolefin-polystyrene multi-block copolymer contains one or more branch points. The carbon atoms at the branch points show peaks at 36 ppm to 40 ppm, and the terminal carbon atoms of the side chains starting from the branch points show peaks at 13 ppm to 15 ppm; [Mathematical Formula 1] In Mathematical Formula 1, Mw refers to the weight-average molecular weight of the polyolefin-polystyrene multi-block copolymer.
5. The polyolefin-polystyrene multi-block copolymer according to claim 4, wherein: The polyolefin-polystyrene multi-block copolymer is one or more selected from the group consisting of polystyrene-poly(ethylene-co-propylene)-polystyrene block copolymer, polystyrene-poly(ethylene-co-1-butene)-polystyrene block copolymer, polystyrene-poly(ethylene-co-1-pentene)-polystyrene block copolymer, polystyrene-poly(ethylene-co-1-hexene)-polystyrene block copolymer, polystyrene-poly(ethylene-co-1-heptene)-polystyrene block copolymer, and polystyrene-poly(ethylene-co-1-octene)-polystyrene block copolymer.
Citation Information
Patent Citations
Organozinc compound including polyolefin-polystyrene block copolymers and method for manufacturing thereof
KR101657925B1
Cross-copolymer, and resin composition
CN106133016A
Polyolefin-polystyrene multi-block copolymer, organozinc compound for preparing same, and method for preparing polyolefin-polystyrene multi-block copolymer
CN110475795A
Polyolefin-polystyrene-based multiblock copolymer and preparation method therefor
CN113631604A
Polyolefin-polystyrene multiblock copolymer, organozinc compound and method for manufacturing the polyolefin-polystyrene multiblock copolymer
KR101829382B1