Prepreg and molded products
By using a combination of urethane (meth)acrylate, specific polymerization initiator and reinforcing fiber in the prepreg, the problems of formability and storage stability of the prepreg under low temperature conditions are solved, and the 110% meter are achieved. The production of high-strength molded products below ℃ is suitable for a variety of structural materials.
Patent Information
- Application Number
- CN202080083039.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-12-25
- Filing Date
- 2020-12-03
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2040-12-03
AI Technical Summary
The existing prepregs are unstable at room temperature and require high-temperature forming, which limits their application range, especially when it is difficult to obtain high-strength molded products under low temperature conditions below 110°C.
The prepreg containing carbamate (meth)acrylate, specific polymerization initiator and reinforcing fibers is used, and the polymerization initiator is an alkyl peroxide compound with a half-life temperature of 60°C or more and less than 70°C. By optimizing the combination of polyisocyanate and compound with hydroxyl groups, the adhesion and interface shear strength of the resin are improved.
The molded product obtained has excellent formability under low temperature conditions below 110°C. The resulting molded product has excellent bending strength and interlayer shear strength, and is suitable for shells of various structural materials, including automobiles, aerospace vehicles, etc.
Smart Images

Figure BDA0003665709820000121
Abstract
Description
Technical Field
[0001] The present invention relates to a prepreg and a molded product thereof. Background Art
[0002] Fiber-reinforced resin composite materials reinforced with reinforcing fibers such as carbon fibers and glass fibers have attracted much attention for their light weight, excellent heat resistance, and excellent mechanical strength, and their use in various structural applications represented by the shells or various components of automobiles and aircraft is expanding. As a molding method for such fiber-reinforced resin composite materials, for example, the following method is used: an intermediate material called prepreg in which a thermosetting resin is impregnated in reinforcing fibers is used, and the prepreg is cured and molded by autoclave molding and pressure molding.
[0003] The resin used for prepregs usually needs to be a resin that has both stability at room temperature and curability by heating, etc., so thermosetting resins represented by epoxy resin compositions are usually used. However, prepregs using epoxy resins are cured at room temperature, so there is a problem that they need to be stored in a refrigerator.
[0004] In order to solve this problem, the development of molding materials that can achieve high productivity and stability at room temperature is underway (for example, see Patent Document 1). The molding material contains urethane (meth)acrylate having a specific structure, a polymerization initiator, and carbon fiber, but molding requires a high temperature of 130°C or more, so there is a problem that applicable uses are limited.
[0005] Therefore, there is a demand for a material that is excellent in storage stability and can produce a molded product having excellent strength and the like even under molding conditions of 110° C. or lower.
[0006] Prior art literature
[0007] Patent Literature
[0008] Patent Document 1: International Publication No. 2017 / 163899 Summary of the invention
[0009] Problems to be solved by the invention
[0010] The problem to be solved by the present invention is to provide a prepreg and a molded product thereof which are excellent in storage stability, have excellent moldability even under low temperature molding conditions of 110° C. or less, and can obtain a molded product excellent in various physical properties such as interlaminar shear strength.
[0011] Means for solving problems
[0012] The present inventors have found that a prepreg containing urethane (meth)acrylate, a specific polymerization initiator and reinforcing fibers as essential components solves the above-mentioned problems, thereby completing the present invention.
[0013] That is, it relates to a prepreg containing urethane (meth)acrylate (A), a polymerization initiator (B) and reinforcing fibers (C), characterized in that the above-mentioned polymerization initiator (B) is an alkyl peroxyester compound having a 10-hour half-life temperature of not less than 60°C and less than 70°C.
[0014] Effects of the Invention
[0015] The molded product obtained from the prepreg of the present invention has excellent bending strength and interlaminar shear strength, and can therefore be suitably used in automobile components, railway vehicle components, aerospace components, ship components, housing equipment components, sports components, light vehicle components, building civil engineering components, housings of OA equipment, etc. DETAILED DESCRIPTION
[0016] The prepreg of the present invention contains urethane (meth)acrylate (A), a polymerization initiator (B) and reinforcing fibers (C), wherein the polymerization initiator (B) is an alkyl peroxyester compound having a 10-hour half-life temperature of 60° C. or higher and lower than 70° C.
[0017] The urethane (meth)acrylate (A) has a urethane bond and a (meth)acryloyl group and is obtained, for example, by reacting a polyisocyanate (a1) with a compound (a2) having a hydroxyl group which contains a compound (a2-1) having a hydroxyl group and a (meth)acryloyl group as essential raw materials.
[0018] From the perspective of high adhesion and further improved interfacial shear strength with carbon fibers, the polyisocyanate (a1) preferably comprises one or more polyisocyanates selected from 2,4'-diphenylmethane diisocyanate, 4,4'-diphenylmethane diisocyanate, a carbodiimide-modified form of 4,4'-diphenylmethane diisocyanate, and polymethylene polyphenyl polyisocyanate, and more preferably comprises polymethylene polyphenyl polyisocyanate.
[0019] In addition, as the above-mentioned polyisocyanate (a1), for example, urate-modified products, biuret-modified products, urethane-imide-modified products of diphenylmethane diisocyanate, polyol-modified products obtained by modifying a polyol having a number average molecular weight of less than 1000 such as diethylene glycol and dipropylene glycol, aromatic polyisocyanates such as toluene diisocyanate (TDI), toluidine diisocyanate, xylylene diisocyanate, 1,5-naphthalene diisocyanate, and tetramethylxylene diisocyanate; alicyclic polyisocyanates such as isophorone diisocyanate (IPDI), hydrogenated diphenylmethane diisocyanate, hydrogenated xylylene diisocyanate, and norbornene diisocyanate; aliphatic polyisocyanates such as hexamethylene diisocyanate, urate-modified products, biuret-modified products, adducts, and dimer acid diisocyanate of hexamethylene diisocyanate, etc. can be used.
[0020] These polyisocyanates (a1) may be used alone or in combination of two or more.
[0021] The compound (a2) having a hydroxyl group contains a compound (a2-1) having a hydroxyl group and a (meth)acryloyl group as essential raw materials.
[0022] Examples of the compound (a2-1) having a hydroxyl group and a (meth)acryloyl group include hydroxyalkyl (meth)acrylates and epoxy (meth)acrylates. It should be noted that the compound (a2-1) having a hydroxyl group and a (meth)acryloyl group may be used alone or in combination of two or more thereof.
[0023] As the hydroxyalkyl (meth)acrylate, for example, 2-hydroxyethyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 4-hydroxy-n-butyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxy-n-butyl (meth)acrylate, 3-hydroxy-n-butyl (meth)acrylate, etc. can be mentioned, and 2-hydroxyethyl (meth)acrylate is preferred. It should be noted that these hydroxyalkyl (meth)acrylates can be used alone or in combination of two or more.
[0024] The epoxy (meth)acrylate may be obtained by reacting an epoxy resin with (meth)acrylic acid and / or (meth)acrylic anhydride.
[0025] In addition, as the compound (a2) having a hydroxyl group, it is preferred to use a polyol (a2-2) in combination with the compound (a2-1) having a hydroxyl group and a (meth)acryloyl group in order to further improve the toughness of the obtained molded article.
[0026] Examples of the other polyols (a2-2) include polyether polyols, polyester polyols, polycarbonate polyols, and polyalkylene polyols.
[0027] The molar ratio (NCO / OH) of the isocyanate group (NCO) of the isocyanate compound (a1) serving as the raw material of the urethane (meth)acrylate (A) to the hydroxyl group (OH) of the compound (a2) having a hydroxyl group is preferably 0.1 to 1.5, more preferably 0.3 to 1.2.
[0028] From the perspective of excellent storage stability of the prepreg, excellent formability even under molding conditions below 110°C, and the ability to obtain molded products with excellent interlaminar shear strength, the polymerization initiator (B) is an alkyl peroxyester compound having a 10-hour half-life temperature of 60°C or higher and less than 70°C, such as 1,1,3,3-tetramethylbutyl peroxy 2-ethylhexanoate, 2,5-dimethyl-2,5-hexanediyl-bis(2-ethylperoxyhexanoate), tert-hexyl-2-ethylhexane peroxyester, etc. It should be noted that these alkyl peroxyester compounds may be used alone or in combination of two or more.
[0029] The content of the polymerization initiator (B) is preferably in the range of 0.3 to 3% by mass in the prepreg components excluding the reinforcing fibers (C) from the viewpoint of excellent balance between storage stability and curing characteristics.
[0030] It should be noted that, in the prepreg of the present invention, other polymerization initiators other than the above-mentioned polymerization initiator (B) can be used in combination within the scope of not impairing the effect of the present invention. As other polymerization initiators, for example, diacyl peroxide compounds, peroxyester compounds, hydroperoxide compounds, ketone peroxide compounds, alkyl perester compounds, percarbonate compounds, peroxyketals, etc. can be cited.
[0031] As the reinforcing fiber (C), organic fibers such as carbon fiber, glass fiber, silicon carbide fiber, alumina fiber, boron fiber, metal fiber, aramid fiber, vinylon fiber, polyester fiber, etc. can be cited. From the aspect of obtaining a molded product with higher strength and high elasticity, carbon fiber or glass fiber is preferred, and carbon fiber is more preferred. These reinforcing fibers (C) can be used alone or in combination of two or more.
[0032] As the carbon fiber, various carbon fibers such as polyacrylonitrile-based, pitch-based, and rayon-based carbon fibers can be used. Among them, polyacrylonitrile-based carbon fibers are preferred because high-strength carbon fibers can be easily obtained.
[0033] The shape of the reinforcing fibers (C) is not particularly limited, and examples thereof include reinforcing fiber bundles obtained by bundling reinforcing fiber filaments, unidirectional materials obtained by aligning reinforcing fiber bundles in one direction, woven fabrics, or short reinforcing fibers cut, or nonwoven fabrics and papers formed from short reinforcing fibers cut. It is preferred to use unidirectional materials as reinforcing fibers and laminate them to obtain high mechanical properties.
[0034] When using short-cut reinforcing fibers, it is preferred to use carbon fibers cut to 2.5 to 50 mm in order to further improve the flowability in a mold during molding and the appearance of the molded product.
[0035] In the case of woven fabrics, examples include plain weave, twill weave, satin weave, or non-crimped fabrics, sheets in which fiber bundles are paralleled in one direction, and sewn sheets in which sheets stacked at different angles are sewn together so as not to unravel.
[0036] As the unit area weight of reinforcing fiber (per 1m 2 The weight of the fiber is not particularly limited, but is preferably 10 g / m 2 ~650g / m 2 If 10g / m 2 If the weight per unit area is 650 g / m 2 The weight per unit area is preferably 50 to 500 g / m2, because the resin impregnation becomes good. 2 , particularly preferably 50 to 300 g / m 2 .
[0037] In order to further improve the mechanical strength of the obtained molded product, the content of the reinforcing fibers (C) in the prepreg of the present invention is preferably in the range of 20 to 85% by mass, more preferably in the range of 40 to 80% by mass.
[0038] As components of the prepreg of the present invention, components other than those mentioned above can be used, for example, it can contain free radical polymerizable monomers, thermosetting resins, thermoplastic resins, inhibitors, curing accelerators, fillers, low shrinkage agents, release agents, thickeners, thickeners, pigments, antioxidants, plasticizers, flame retardants, antibacterial agents, ultraviolet stabilizers, reinforcing materials, photocuring agents, etc.
[0039] Examples of the radical polymerizable monomer include styrene compounds such as styrene, methylstyrene, halogenated styrene, and divinylbenzene; monofunctional (meth)acrylate compounds such as methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, cyclohexyl (meth)acrylate, isobornyl (meth)acrylate, benzyl (meth)acrylate, methylbenzyl (meth)acrylate, phenoxyethyl (meth)acrylate, methylphenoxyethyl (meth)acrylate, phenylbenzyl (meth)acrylate, phenyl methacrylate, dicyclopentenyl (meth)acrylate, dicyclopentenyloxyethyl (meth)acrylate, and dicyclopentanyl methacrylate; (meth)acrylate compounds containing hydroxyl groups such as hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, and hydroxybutyl (meth)acrylate; di(meth)acrylate compounds such as ethylene glycol di(meth)acrylate, propylene glycol di(meth)acrylate, 1,4-butanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, bisphenol di(meth)acrylate, polytetramethylene glycol di(meth)acrylate, ethoxylated bisphenol A di(meth)acrylate, and 1,4-cyclohexanedimethanol di(meth)acrylate; and polyfunctional di(meth)acrylate compounds such as trimethylolpropane tri(meth)acrylate, ethoxylated isocyanuric acid tri(meth)acrylate, and pentaerythritol tri(meth)acrylate. These may be used alone or in combination of two or more.
[0040] Among these radical polymerizable monomers, monofunctional and bifunctional (meth)acrylates having a molecular weight of 150 to 1000 are preferred from the viewpoint of further improving the odor in the working environment and the mechanical strength of the molded article. Phenoxyethyl (meth)acrylate, methylphenoxyethyl (meth)acrylate, benzyl (meth)acrylate, methylbenzyl (meth)acrylate, polytetramethylene glycol di(meth)acrylate, and ethoxylated bisphenol A di(meth)acrylate are more preferred. Phenoxyethyl (meth)acrylate, benzyl (meth)acrylate, and ethoxylated bisphenol A di(meth)acrylate are further preferred.
[0041] From the perspective of further improving the operability in the working environment and the mechanical strength of the molded body, the mass ratio of the urethane (meth) acrylate (A) to the radical polymerizable monomer (urethane (meth) acrylate (A) / radical polymerizable monomer) is preferably 95 / 5 to 50 / 50, more preferably 95 / 5 to 70 / 30.
[0042] Examples of the thermosetting resin include vinyl ester resins, unsaturated polyester resins, phenol resins, melamine resins, furan resins, etc. These thermosetting resins may be used alone or in combination of two or more.
[0043] As the above-mentioned thermoplastic resin, for example, polyamide resin, polyethylene terephthalate resin, polybutylene terephthalate resin, polycarbonate resin, carbamate resin, polypropylene resin, polyethylene resin, polystyrene resin, acrylic resin, polybutadiene resin, polyisoprene resin and resins obtained by modifying them by copolymerization etc. can be listed. Among them, polyamide resin and polyurethane resin are preferred. In addition, these thermoplastic resins can be used alone or in combination of two or more. In addition, the thermoplastic resin can be added in the form of particles or melt mixed. When using a thermoplastic resin in the form of particles, from the viewpoint of dispersibility in the fiber, the particle system is preferably less than 30 μm, more preferably 20 μm.
[0044] Examples of the polymerization inhibitor include hydroquinone, trimethylhydroquinone, p-tert-butylcatechol, tert-butylhydroquinone, toluhydroquinone, p-benzoquinone, naphthoquinone, hydroquinone monomethyl ether, phenothiazine, copper naphthenate, copper chloride, etc. These polymerization inhibitors may be used alone or in combination of two or more.
[0045] Examples of the curing accelerator include metal soaps such as cobalt naphthenate, cobalt octenate, vanadyl octenate, copper naphthenate, and barium naphthenate, and metal chelate compounds such as vanadyl acetoacetate, cobalt acetoacetate, and iron acetylacetonate. In addition, examples of amines include N,N-dimethylamino-p-benzaldehyde, N,N-dimethylaniline, N,N-diethylaniline, N,N-dimethyl-p-toluidine, N-ethyl-m-toluidine, triethanolamine, m-toluidine, diethylenetriamine, pyridine, phenylmorpholine, piperidine, and diethanolaniline. These curing accelerators may be used alone or in combination of two or more.
[0046] The filler includes inorganic compounds and organic compounds, and can be used to adjust the physical properties of the molded product, such as strength, elastic modulus, impact strength, and fatigue durability.
[0047] Examples of the inorganic compound include calcium carbonate, magnesium carbonate, barium sulfate, mica, talc, kaolin, clay, diatomaceous earth, asbestos, barite, barium oxide, silicon dioxide, silica sand, dolomite, limestone, gypsum, aluminum powder, hollow spheres, aluminum oxide, glass powder, aluminum hydroxide, calcite, zirconium oxide, antimony trioxide, titanium oxide, molybdenum dioxide, and iron powder.
[0048] As the above-mentioned organic compound, there are natural polysaccharide powders such as cellulose and chitin, synthetic resin powders, etc., and as synthetic resin powders, organic powders such as hard resins, soft rubbers, elastomers or polymers (copolymers) can be used, and particles with multilayer structures such as core-shell type can be used. Specifically, particles formed by acrylic particles, polyamide particles, butadiene rubber and / or acrylic rubber, urethane rubber, silicone rubber, etc., polyimide resin powders, fluororesin powders, phenolic resin powders, etc. can be cited. These fillers can be used alone or in combination of two or more.
[0049] Examples of the release agent include zinc stearate, calcium stearate, paraffin wax, polyethylene wax, carnauba wax, etc. Preferably, paraffin wax, polyethylene wax, carnauba wax, etc. These release agents may be used alone or in combination of two or more.
[0050] As the above-mentioned thickener, for example, metal oxides such as magnesium oxide, magnesium hydroxide, calcium oxide, calcium hydroxide, metal hydroxides, etc., acrylic resin-based microparticles, etc. can be mentioned, and it can be appropriately selected according to the handleability of the prepreg of the present invention. These thickeners can be used alone or in combination of two or more.
[0051] The prepreg of the present invention is obtained, for example, by steps 1 and 2: the reinforcing fiber (C) is impregnated with a resin solution prepared by mixing the polyisocyanate (a1), the compound (a2-1) having a hydroxyl group and a (meth)acryloyl group, the other polyol (a2-2), and the polymerization initiator (B) using a known mixer such as a planetary mixer and a kneader, and then sandwiched with a release PET film from the upper surface and rolled using a rolling mill to obtain a sheet; and the step 2 is left to stand at room temperature to 50° C. to react the isocyanate group of the polyisocyanate (a1) with the hydroxyl group of the compound (a2-1) having a hydroxyl group and a (meth)acryloyl group and the other polyol (a2-2). In step 1, a substance obtained by preliminarily partially reacting the polyisocyanate (a1), the compound having a hydroxyl group and a (meth)acryloyl group (a2-1), and other polyols (a2-2) may be used within a range that does not impair the impregnation property into the fiber.
[0052] The thickness of the prepreg of the present invention is preferably 0.02 to 1.0 mm. A thickness of 0.02 mm or more is preferred because handling for lamination becomes easy, and a thickness of 1 mm or less is preferred because resin impregnation becomes good. In addition, 0.05 to 0.5 mm is more preferred.
[0053] As a method for obtaining a molded product from the prepreg obtained above, for example, the following method can be used: peeling off the above-mentioned demoulding PET film from the prepreg, stacking 8 to 16 sheets of prepreg, and then putting it into a mold preheated to 100°C to 120°C, using a compression molding machine to close the mold, shaping the prepreg, maintaining a molding pressure of 0.1 to 10 MPa, thereby curing the prepreg, and then taking out the molded product to obtain a molded product. In this case, the following manufacturing method is preferred: in a mold with a shearing edge, at a mold temperature of 100°C to 120°C, maintaining a predetermined time of 1 to 2 minutes per 1 mm thickness of the molded product, and a molding pressure of 1 to 8 MPa, and performing heating compression molding.
[0054] The molded product obtained from the prepreg of the present invention has excellent bending strength, interlaminar shear strength, etc., and can therefore be suitably used in automobile parts, railway vehicle parts, aerospace parts, ship parts, housing equipment parts, sports parts, light vehicle parts, building civil engineering parts, housings of OA equipment, etc.
[0055] Example
[0056] The present invention will be described in more detail below with reference to specific examples. The gel time was measured using CURELASTOMETER 7 TYPE P (manufactured by JSR Trading Co., Ltd.).
[0057] (Preparation Example 1: Preparation of prepreg resin composition (1))
[0058] A mixture of polymethylene polyphenyl polyisocyanate and MDI ("MILLIONATE MR-200" manufactured by Tosoh Corporation) 50 parts by mass, 4,4'-diphenylmethane diisocyanate 50 parts by mass, 66 parts by mass of HEMA, 25 parts by mass of NEWPOL BPE-20 (manufactured by Sanyo Chemical Co., Ltd.: EO adduct of bisphenol A, hydroxyl equivalent; 164 g / eq), 31 parts by mass of NEWPOL BPE-40 (manufactured by Sanyo Chemical Co., Ltd.: EO adduct of bisphenol A, hydroxyl equivalent; 204 g / eq), and 3 parts by mass of a polymerization initiator ("KAYAESTER TMPO-70" manufactured by KAYAKU NOURYON Co., Ltd., 1,1,3,3-tetramethylbutyl peroxy 2-ethylhexanoate) were mixed to obtain a resin composition (1) for prepreg.
[0059] (Preparation Example 2: Preparation of prepreg resin composition (R1))
[0060] A mixture of polymethylene polyphenyl polyisocyanate and MDI ("MILLIONATE MR-200" manufactured by Tosoh Corporation) 50 parts by mass, 4,4'-diphenylmethane diisocyanate 50 parts by mass, 66 parts by mass of HEMA, NEWPOL BPE-20 (manufactured by Sanyo Chemical Co., Ltd.: EO adduct of bisphenol A, hydroxyl equivalent; 164 g / eq) 25 parts by mass, NEWPOL BPE-40 (manufactured by Sanyo Chemical Co., Ltd.: EO adduct of bisphenol A, hydroxyl equivalent; 204 g / eq) 31 parts by mass, and a polymerization initiator ("KAYAESTER O" manufactured by KAYAKU NOURYON Co., Ltd., tert-butylperoxy-2-ethylhexanoate) 3 parts by mass were mixed to obtain a prepreg resin composition (R1).
[0061] (Preparation Example 3: Preparation of prepreg resin composition (R2))
[0062] A mixture of polymethylene polyphenyl polyisocyanate and MDI ("MILLIONATE MR-200" manufactured by Tosoh Corporation) 50 parts by mass, 4,4'-diphenylmethane diisocyanate 50 parts by mass, 66 parts by mass of HEMA, NEWPOL BPE-20 (manufactured by Sanyo Chemical Co., Ltd.: EO adduct of bisphenol A, hydroxyl equivalent; 164 g / eq) 25 parts by mass, NEWPOL BPE-40 (manufactured by Sanyo Chemical Co., Ltd.: EO adduct of bisphenol A, hydroxyl equivalent; 204 g / eq) 31 parts by mass, and a polymerization initiator ("Trigonox 122-80C" manufactured by KAYAKU NOURYON Co., Ltd., 1,1-di(tert-amylperoxy)cyclohexane) 3 parts by mass were mixed to obtain a prepreg resin composition (R2).
[0063] (Example 1: Preparation and evaluation of prepreg (1))
[0064] The resin composition for prepreg (1) was applied to one side of a polyethylene terephthalate film subjected to a mold release treatment, and then impregnated with carbon fibers ("T-700-12K-50C" manufactured by Toray Industries, Inc.) by a hand lay-up method so that the carbon fiber content was 50% by mass, and then covered with the same film, and aged at 25°C for 1 week to prepare a prepreg (1). The gel time of the prepreg (1) was 90 seconds at 100°C and 30 seconds at 110°C.
[0065] [Evaluation of storage stability]
[0066] The prepreg (1) obtained above was stored at 25°C for 4 weeks, and the gel time at 110°C was measured, and the storage stability was evaluated according to the following criteria.
[0067] ○: The difference in gel time at 110°C between 1 week after production and 4 weeks after production is less than 5 seconds
[0068] △: The difference in gel time at 110°C between 1 week after production and 4 weeks after production is 5 seconds or more and less than 10 seconds
[0069] ×: The difference in gel time at 110°C between one week after production and four weeks after production is 10 seconds or more
[0070] [Production of molded products]
[0071] Twelve sheets of the above-obtained prepreg (1) were stacked and heated and pressed using a plate-shaped mold to obtain a molded product. The heating and pressing conditions were a mold temperature of 105°C and a mold closing pressure of 4 MPa for 5 minutes, and the mold was opened and taken out, and allowed to cool at room temperature to obtain a molded product (1).
[0072] [Evaluation of Formability]
[0073] The surface of the molded article (1) obtained above was evaluated according to the following criteria.
[0074] ○: No expansion or uncured parts
[0075] ×: There is swelling or uncured part
[0076] [Evaluation of flexural strength and flexural modulus]
[0077] A test piece having a width of 5 mm and a length of 100 mm was cut out from the molded product (1) obtained above, and the flexural strength and flexural modulus were measured in accordance with JIS K7074.
[0078] [Evaluation of interlaminar shear strength]
[0079] A test piece having a width of 10 mm and a length of 22 mm was cut out from the molded product (1) obtained above, and the interlaminar shear strength of the test piece was measured in accordance with JIS K7078.
[0080] (Comparative Example 1: Preparation and Evaluation of Prepreg (R1))
[0081] The same operation as in Example 1 was carried out except that the prepreg resin composition (1) used in Example 1 was changed to the prepreg resin composition (R1), and the prepreg (R1) was prepared and each evaluation was performed. The gel time of the prepreg (R1) was 300 seconds at 100° C. and 110 seconds at 110° C. It should be noted that under the above molding conditions, uncured portions existed and a molded product could not be obtained.
[0082] (Comparative Example 2: Preparation and Evaluation of Prepreg (R2))
[0083] The same operation as in Example 1 was carried out except that the prepreg resin composition (1) used in Example 1 was changed to the prepreg resin composition (R2), and the prepreg (R2) was prepared and each evaluation was performed. The gel time of the prepreg (R2) could not be measured because it was not cured at 100 to 110° C., but was 50 seconds at 140° C. It should be noted that under the above molding conditions, an uncured portion existed and a molded product could not be obtained.
[0084] Table 1 shows the evaluation results of the prepregs (1), (R1) and (R2) obtained above.
[0085] [Table 1]
[0086]
[0087] The prepreg of the present invention in Example 1 was excellent in storage stability and moldability, and the obtained molded product was excellent in strength.
[0088] On the other hand, Comparative Examples 1 and 2 are examples in which an alkyl peroxyester compound having a 10-hour half-life temperature of 60° C. or higher and less than 70° C. was not used as a polymerization initiator. It was confirmed that no curing occurred at 100 to 110° C., and no molded product could be obtained.
Claims
1. A method for producing a prepreg, characterized in that: The invention relates to a method for producing a prepreg containing urethane (meth)acrylate (A), a polymerization initiator (B) and reinforcing fibers (C). The urethane (meth)acrylate (A) is a reaction product of a polyisocyanate (a1) and a compound (a2) having a hydroxyl group, which has a compound (a2-1) having a hydroxyl group and a (meth)acryloyl group as an essential raw material. The polymerization initiator (B) is one or more selected from 1,1,3,3-tetramethylbutyl peroxy 2-ethylhexanoate and tert-hexyl-2-ethylhexane peroxyester. The production method comprises the step of impregnating the reinforcing fiber (C) with a resin solution obtained by mixing the polyisocyanate (a1), the compound (a2-1), a polyol (a2-2) other than the compound (a2-1), and the polymerization initiator (B).
2. The method for producing a prepreg according to claim 1, wherein: The polyisocyanate (a1) comprises polymethylene polyphenyl polyisocyanate.
3. The method for producing a prepreg according to claim 1 or 2, wherein: The reinforcing fiber (C) is carbon fiber.
4. A molded product, characterized in that: This is a cured product of a prepreg obtained by the production method according to any one of claims 1 to 3.