A continuous casting crystallizer foot roller and manufacturing method thereof
Laser cladding technology is used to form a heat-resistant, corrosion-resistant and wear-resistant cladding layer on the foot rollers of the continuous casting mold, which solves the corrosion and wear problems of the foot rollers in harsh environments in the existing technology and achieves a longer service life. Significant improvement and cost reduction.
Patent Information
- Application Number
- CN202210373525.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-04-11
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2042-04-11
AI Technical Summary
The existing continuous casting mold foot rollers are prone to corrosion, cracks and wear under harsh alternating hot and cold fatigue and corrosive environments, resulting in poor service life and high costs.
The laser cladding method is used to form a cladding layer on the surface of the substrate. A flux-cored welding wire is used to clad the rectangular spot structure generated by the laser to form a heat-resistant, corrosion-resistant and wear-resistant cladding layer. The material composition is: 0.02-0.07 %C, 12.5-15%Cr, 5-6.5%Ni, 1- 1.5% Mo, 0.2-0.4% V, 0.15-0.3% Nb, 1.7-2.5% Co, balance Fe, wire diameter 1.6-2.4mm, wire feeding speed 0.5-3m/min, process parameters 6×3mm spot and 2500-3000W power.
It significantly improves the heat resistance, corrosion resistance and wear resistance of the foot roller, reduces welding wire consumption and processing deformation, has low cost, increases the service life by 2-4 times, and is cost-effective.
Smart Images

Figure CN114752930B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of metallurgical continuous casting and surface engineering, in particular to a continuous casting crystallizer foot roller and a manufacturing method thereof. Background Art
[0002] The foot rollers of the continuous casting mold are one of the key components of slab continuous casting. During the continuous casting process, the foot rollers of the continuous casting mold are the first set of rollers to pass through after the billet emerges from the continuous casting mold. The foot rollers are in direct contact with the metal shell that has just solidified on the surface, while the interior of the shell is still molten steel. Therefore, the foot rollers need to withstand very high temperatures. At the same time, to ensure smooth casting of the continuous casting billet, water spraying is required to cool the billet surface. Therefore, after the foot rollers are separated from the billet, they will cool rapidly again. Therefore, the foot rollers are subjected to very harsh alternating hot and cold fatigue conditions. In addition, to ensure smooth continuous casting, the continuous casting process requires the use of protective slag with a very high fluorine content. The protective slag flows out of the crystallizer with the billet and forms an acidic environment when it comes into contact with water. Therefore, the surface of the foot rollers is also subject to oxidation and corrosion. This extremely harsh working environment can easily lead to serious failures such as corrosion, cracks, and wear on the foot roller surface.
[0003] Currently, foot roller design primarily utilizes composite manufacturing methods, mostly employing arc cladding, spray welding, or laser powder cladding. Cladding requires a large weld volume and significant deformation, which, depending on the material used, can lead to significant variations in service life. Spray welding requires remelting, which also results in significant deformation and higher powder prices. Service life also varies significantly depending on the powder used. Laser cladding, on the other hand, results in less deformation, but the powder is more expensive, and service life also varies significantly depending on the powder used. Summary of the Invention
[0004] In order to overcome the defects of the existing technology, the technical problem solved by the present invention is to provide a continuous casting crystallizer foot roller and a manufacturing method thereof. The laser cladding method is used to form a cladding layer on the surface of the substrate, which can significantly improve the heat resistance, corrosion resistance and wear resistance of the continuous casting crystallizer foot roller. No heat treatment and other processes are required. The production cycle is short, the production cost is low, and the service life is long. Therefore, the cost performance is high and the cost of use can be greatly reduced.
[0005] In order to achieve the above object, the present invention adopts the following technical solutions:
[0006] A continuous casting crystallizer foot roller, consisting of a substrate and a cladding layer, characterized in that the cladding layer is clad on the surface of the substrate using a laser cladding method, wherein the metal chemical composition and mass percentage of the cladding layer after cladding are: 0.02-0.07% C, 12.5-15% Cr, 5-6.5% Ni, 1-1.5% Mo, 0.2-0.4% V, 0.15-0.3% Nb, 1.7-2.5% Co, and the balance Fe.
[0007] The welding wire used in the laser cladding method is a flux-cored welding wire structure with a diameter of 1.6-2.4 mm.
[0008] The laser cladding method uses laser light generated by a laser as a heat source. The laser light is in the form of a rectangular spot structure. A welding wire is fed into the spot through a lateral wire feeding system. The welding wire is melted by the heat generated by the laser to form a welding pool, which is then solidified to form a weld bead.
[0009] The process parameters of the laser cladding method are as follows: the spot structure size generated by the laser is 6×3 mm, the laser power is 2500-3000 W, and the wire feeding speed is 0.5-3 m / min.
[0010] A method for manufacturing a continuous casting crystallizer foot roller comprises the following steps:
[0011] 1) Preparation of base material: Select suitable pipes or rods and process them to a diameter smaller than the finished product by 1-3mm according to design requirements, leaving a working layer thickness of 0.5-1.5mm;
[0012] 2) Inspection: Make sure that the processed base material has no defects that affect its use, such as cracks, pores, slag inclusions, etc.
[0013] 3) A professional laser wire cladding welding bed is used for laser cladding operations. The welding wire is fed into the laser spot using a side wire feeding system. The cladding is performed in two layers, with each layer controlled to have a cladding thickness of approximately 0.5-1.2 mm. The final cladding layer size is Φ1 mm larger than the finished product diameter as a margin for subsequent processing.
[0014] 4) After slowly cooling to room temperature, it is machined to the design requirements of size, finish and coaxiality, which is the continuous casting mold foot roller to be inspected;
[0015] 5) Non-destructive testing: Confirm that the foot roll of the continuous casting mold to be inspected after processing has no defects such as cracks, pores, slag inclusions, etc. that affect its use.
[0016] Compared with the prior art, the present invention has the following beneficial effects:
[0017] 1) The invention adopts welding wire and laser wire electrode cladding technology to clad the continuous casting mold foot roller, and the heat resistance, corrosion resistance and wear resistance of the clad material are significantly improved;
[0018] 2) Since the laser cladding method used in this invention has a low dilution rate, the designed weld layer thickness can be significantly reduced compared to overlay welding. Therefore, the consumption of welding wire for making full rollers using this invention is much lower than that used for overlay welding, which can save a lot of welding wire and reduce costs.
[0019] 3) The deformation of the continuous casting mold foot roller produced by the present invention after cladding is very small, which is about 1 / 5 of the deformation of cladding, so the processing allowance can be very small, saving processing costs;
[0020] 4) The price of the continuous casting mold foot roller welding wire produced by the present invention is 2-5 times lower than that of laser powder cladding, and the consumption can be saved by 30%-50% compared with powder;
[0021] 5) Practice has proved that the service life of the continuous casting crystallizer foot roller produced by the present invention is significantly improved, which is 2-4 times that of other methods, thereby increasing the service life and reducing the cost of use. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 It is a schematic diagram of the structural principle of the present invention;
[0023] Figure 2 yes Figure 1 A magnified schematic diagram of the local structure of the X portion;
[0024] Figure 3 It is a schematic structural diagram of the laser cladding process of the present invention.
[0025] In the figure: 1- cladding layer 2- substrate 3- annular groove 4- bearing platform 6- lateral wire feeding system 7- laser DETAILED DESCRIPTION
[0026] The specific embodiments of the present invention will be further described below with reference to the accompanying drawings:
[0027] See Figure 1-Figure 3 As shown, the present invention relates to a continuous casting crystallizer foot roller, which consists of a substrate 2 and a cladding layer 1. The cladding layer 1 is clad on the surface of the substrate 2 by a laser cladding method, wherein the metal chemical composition and mass percentage of the cladding layer 1 after cladding are: 0.02-0.07% C, 12.5-15% Cr, 5-6.5% Ni, 1-1.5% Mo, 0.2-0.4% V, 0.15-0.3% Nb, 1.7-2.5% Co, and the balance Fe.
[0028] The welding wire used in the laser cladding method is a flux-cored welding wire structure with a diameter of 1.6-2.4 mm.
[0029] The laser cladding method uses laser light generated by a laser 7 as a heat source. The laser light is in the form of a rectangular spot structure. The welding wire is fed into the spot through a lateral wire feeding system 6. The welding wire is melted by the heat generated by the laser to form a welding pool, which is then solidified to form a weld bead.
[0030] The process parameters of the laser cladding method are as follows: the spot structure size generated by the laser 7 is 6×3 mm, the laser power is 2500-3000 W, and the wire feeding speed is 0.5-3 m / min.
[0031] A method for manufacturing a continuous casting crystallizer foot roller comprises the following steps:
[0032] 1) Preparation of substrate 2 material: Select appropriate tubes or rods and process them to a diameter Φ1-3mm smaller than the finished product according to design requirements, leaving a working layer thickness of 0.5-1.5mm;
[0033] 2) Inspection: Determine that the processed substrate 2 material has no defects that affect its use, such as cracks, pores, slag inclusions, etc.;
[0034] 3) A professional laser wire cladding welding bed is used for laser cladding operations. The welding wire is fed into the laser spot using a side wire feeding system 6. The cladding is performed in two layers, with each layer controlled to have a cladding thickness of approximately 0.5-1.2 mm. The final cladding layer size is Φ1 mm larger than the finished product diameter as a margin for subsequent processing.
[0035] 4) After slowly cooling to room temperature, it is machined to the design requirements of size (such as the annular groove 3 with a certain distance D on the outer surface, the bearing platform 4 for mounting bearings at both ends, etc.), finish and coaxiality, and then it is the continuous casting crystallizer foot roller to be inspected;
[0036] 5) Non-destructive testing: Confirm that the foot roll of the continuous casting mold to be inspected after processing has no defects such as cracks, pores, slag inclusions, etc. that affect its use.
[0037] [Example 1]
[0038] The base material 2 of the continuous casting crystallizer foot roller is 42CrMo bar with a size of Ф100×635mm. The manufacturing method is as follows:
[0039] Step 1: Preparation of substrate 2: Turn the substrate material to Ø98×640mm.
[0040] Step 2: Pre-cladding flaw detection: Perform color flaw detection or magnetic particle flaw detection on the processed continuous casting crystallizer foot roller base 2 to confirm that there are no defects that affect use, such as cracks, pores, slag inclusions, etc.
[0041] Step 3: Laser wire cladding: A laser wire cladding welding bed is used to weld the cladding layer 1. A side wire feeding system 6 is used, and the welding wire is fed from the front to the laser spot. The cladding is divided into two layers, and the cladding thickness of each layer is controlled to be about 0.75-1mm. The final cladding layer size is 1mm larger than the finished product diameter.
[0042] Step 4: Finished product processing: The continuous casting crystallizer foot roller slowly cooled to room temperature is machined. The size after processing is: Ф100±0.05×635mm, the spacing of the annular groove 3 is D=40mm, and the roughness is Ra3.2, meeting the design requirements of size, tolerance and roughness.
[0043] Step 5: Finished product flaw detection: The processed continuous casting mold foot roller needs to be subjected to non-destructive testing to ensure that there are no defects that affect its use, such as cracks, pores, slag inclusions, etc.
[0044] The composition and weight percentage of the welding wire cladding metal used in step 3 are: 0.05% C, 13.5% Cr, 6.0% Ni, 1.2% Mo, 0.2% V, 0.20% Nb, 2.1% Co, and the balance Fe.
[0045] The process parameters of laser wire cladding in step 3 are: a rectangular 6×3 mm spot generated by the laser 7, a power of 2500-3000 W, a wire feeding speed of 0.5 m / min, a spot moving speed of 600 mm / min, an overlap of 50%, and a wire diameter of Ф2.4 mm.
[0046] In this embodiment, the outer diameter of the substrate is designed to be Ø98 mm based on the following reasons: the substrate material is 42CrMo rod, and the bending deformation after cladding is very small, or almost no deformation, and the thickness of the cladding layer will not change after processing; in addition, the corrosion environment of the foot roller of the continuous casting crystallizer is relatively weak, and the wear amount in a normal cycle generally does not exceed Ø0.7 mm, and the cladding layer thickness of 1 mm fully meets the requirements.
[0047] [Example 2]
[0048] The base material of the crystallizer foot roller is Q345D pipe with a size of Ф100×730mm. Its manufacturing method is as follows:
[0049] Step 1: Prepare the substrate 2 and turn the substrate 2 material to Ø97×735mm.
[0050] Step 2: Pre-cladding flaw detection: perform color flaw detection or magnetic particle flaw detection on the processed continuous casting crystallizer foot roller base 2 to confirm that there are no defects that affect use, such as cracks, pores, slag inclusions, etc.
[0051] Step 3: Laser wire cladding. A laser wire cladding welding bed is used to weld the cladding layer 1. A side wire feeding system 6 is used. The welding wire is fed from the front to the laser spot. The cladding is performed in two layers. The cladding thickness of each layer is controlled to be about 1-1.2 mm. The final cladding layer size is 1 mm larger than the finished product diameter.
[0052] Step 4: Finished product processing: The continuous casting crystallizer foot roller that is slowly cooled to room temperature is machined. The size after processing is: Ф100±0.05×730mm, the spacing between the annular grooves 3 is D=40mm, and the roughness is Ra3.2, meeting the design requirements of size, tolerance and roughness.
[0053] Step 5: Finished product flaw detection. The processed continuous casting mold foot roller needs to be subjected to non-destructive testing to ensure that there are no defects that affect its use, such as cracks, pores, slag inclusions, etc.
[0054] The composition and weight percentage of the welding wire cladding metal used in step 3 are: 0.04% C, 13% Cr, 6.0% Ni, 1.1% Mo, 0.25% V, 0.19% Nb, 1.9% Co, and the balance Fe.
[0055] The process parameters of laser wire cladding in step 3 are: a rectangular 6×3 mm spot generated by the laser 7, a power of 2500-3000 W, a wire feeding speed of 0.5 m / min, a spot moving speed of 600 mm / min, an overlap of 50%, and a wire diameter of Ф2.4 mm.
[0056] In this embodiment, the outer diameter of the substrate 2 is designed to be 97 mm in diameter because the substrate material is Q345D pipe, which has a slightly large bending deformation after cladding. The cladding layer 1 will change in thickness in the circumferential direction after processing, so the cladding thickness needs to be increased to compensate. In addition, the corrosive environment of the foot roller of the continuous casting crystallizer is relatively strong, and the wear in a normal cycle can generally reach 1 mm in diameter. Therefore, a cladding layer thickness of 1.5 mm is required to ensure usage requirements.
[0057] The continuous casting crystallizer foot rollers of the two embodiments have been used in practice and their service life is 2-3 times longer than that of ordinary cladding rollers.
[0058] The present invention provides a simple manufacturing method for the continuous casting mold foot roller. The flux-cored welding wire is easy to manufacture, achieving a wire utilization rate of over 98% during the cladding process and reducing wire costs. The cladding mold foot roller does not require heat treatment or other processes, resulting in a short production cycle. The continuous casting mold foot roller manufactured using the present invention offers high cost-effectiveness.
[0059] The above description is only a preferred specific embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any technician familiar with the technical field, within the technical scope disclosed by the present invention, who makes equivalent replacements or changes based on the technical solution and inventive concept of the present invention, should be covered by the scope of protection of the present invention.
Claims
1. A continuous casting crystallizer foot roller, consisting of a base and a cladding layer, characterized in that: The cladding layer is clad on the surface of the substrate by a laser cladding method, wherein the metal chemical composition and mass percentage of the cladding layer after cladding are: 0.02-0.07% C, 12.5-15% Cr, 5-6.5% Ni, 1-1.5% Mo, 0.2-0.4% V, 0.15-0.3% Nb, 1.7-2.5% Co, and the remainder is Fe. The thickness of the cladding layer is 1-1.5 mm.
2. A continuous casting crystallizer foot roller according to claim 1, characterized in that: The welding wire used in the laser cladding method is a flux-cored welding wire structure with a diameter of 1.6-2.4 mm.
3. A continuous casting crystallizer foot roller according to claim 1, characterized in that: The laser cladding method uses laser light generated by a laser as a heat source. The laser light is in the form of a rectangular spot structure. A welding wire is fed into the spot through a lateral wire feeding system. The welding wire is melted by the heat generated by the laser to form a welding molten pool, which is then solidified to form a weld bead.
4. A continuous casting crystallizer foot roller according to claim 1 or 3, characterized in that: The process parameters of the laser cladding method are: the spot structure size generated by the laser is 6×3mm, the laser power is 2500-3000w, and the wire feeding speed of the welding wire is 0.5-3m / min.
5. The method for manufacturing a continuous casting crystallizer foot roller according to claim 1, characterized in that: The following steps are involved: 1) Preparation of base material: Select suitable pipes or bars and process them to a diameter smaller than Φ1-3mm according to design requirements; 2) Inspection: Make sure that the processed base material has no defects that affect its use, such as cracks, pores or slag inclusions; 3) Use a professional laser wire electrode cladding welding bed for laser cladding operations, use a side wire feeding system to feed the welding wire into the laser spot, and clad in two layers. The thickness of each layer is controlled at 0.5-1.2mm; 4) After slowly cooling to room temperature, it is machined to the size, finish and coaxiality required by the design, which is the continuous casting crystallizer foot roller to be inspected; 5) Nondestructive testing: Confirm that the processed continuous casting mold foot roller has no cracks, pores or slag inclusion defects that affect its use.
Citation Information
Patent Citations
Wear-resisting heat-resisting alloy material used for small profile roll laser alloying
CN106498308A
Flux-cored wire used for repairing continuous casting hollow foot roller sleeve, and cladding process of flux-cored wire
CN109604858A