A forging process for a parachute clamp

Through the forging and heat treatment process, combined with the surface treatment of copper plating, nickel plating, and chromium plating, the problem of material processing during the forging process of the parachute snap ring is solved, its strength and wear resistance are improved, and it meets the high performance requirements of aviation parts.

CN114770047BActive Publication Date: 2024-10-18KUNSHAN ZHONGCHENG PRECISE FORGING CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202210508094.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-05-11
Publication Date
2024-10-18
Estimated Expiration
2042-05-11

AI Technical Summary

Technical Problem

The parachute snap ring is difficult to process during the forging process, and its material surface quality requirements are high, and existing technology cannot effectively solve its strength, wear resistance and corrosion protection problems.

Method used

A circular 30CrMnSiA steel pipe is used as the blank, which is formed through forging, normalizing, quenching and tempering processes, combined with surface treatment of copper plating, nickel plating, chromium plating, and finally grinding and polishing.

Benefits of technology

It achieves the high strength, wear resistance and corrosion resistance of the parts, ensures that the parts will not deform under a tensile force of 1200kg, and improves the appearance and durability of the parts.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114770047B_ABST
    Figure CN114770047B_ABST
Patent Text Reader

Abstract

The present invention discloses a forging process for a parachute clamp. The process comprises the following steps: (1) blank selection; (2) cutting by lathe; (3) forging; (4) normalizing; (5) cutting burrs; (6) turning the outer ring surface and the inner ring surface; (7) quenching and tempering; (8) lathe finishing; (9) surface treatment; (10) grinding and polishing, grinding and polishing the surface-treated parts to obtain the final product. The forging process of the present invention adopts a circular blank, and is formed by forging, without forging defects, and has a good forming effect. In addition, a process of turning the end surface before forging is added, which successfully solves the problem that the end surface burr is forged into the part, thereby affecting the performance of the part.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a forging process for a parachute clamp ring and belongs to the technical field of forging. Background Art

[0002] The clamp ring in the parachute is the core component of the entire device. Its working environment requires it to have high strength, wear resistance and corrosion resistance. The surface quality of the part material is high and it is not easy to process during the forging process. Summary of the invention

[0003] In order to overcome the deficiencies of the prior art, the present invention provides a forging process for a parachute clamp ring, which has a good forming effect.

[0004] The present invention is achieved through the following technical solutions:

[0005] A forging process for a parachute clamp comprises the following steps:

[0006] (1) Billet selection: select the steel pipe and then cut it into sections;

[0007] (2) Turning: The cut blank is turned on a lathe to make it blunt and cut off;

[0008] (3) Forging: The cut blank is placed in a small high frequency for heating to 950°C-1000°C, and then the forging die is started for forging at a temperature not lower than 850°C;

[0009] (4) Normalizing: The forged billet is normalized by heating it to 860-880°C, then keeping it at that temperature for 30-35 minutes, and then cooling it by air cooling;

[0010] (5) Cutting flash: Place the cooled parts in the trimming die on the punch press to cut the flash;

[0011] (6) Turning the outer and inner ring surfaces: Position and clamp the parts after flash cutting, turn the outer ring surface on a CNC lathe, and then turn the inner ring surface;

[0012] (7) Quenching and tempering: Quench and temper the parts behind the inner torus surface;

[0013] (8) Lathe finishing: Use a lathe to finish the torus surface joint marks on the quenched parts, and use sandpaper to polish to the surface roughness requirements;

[0014] (9) Surface treatment: The inspected parts are copper plated, nickel plated and chrome plated in sequence;

[0015] (10) Grinding and polishing: Grinding and polishing the surface treated parts to obtain the final product.

[0016] In the forging process of a parachute clamp, the steel pipe used in step (1) has a circular cross-section, an outer diameter of 31 mm, an inner diameter of 20 mm, and is made of 30CrMnSiA.

[0017] In the forging process of a parachute clamp, the length of the blank after cutting in step (2) is 8.5 mm.

[0018] In the forging process of a parachute clamp, the hardness HRC of the part after quenching and tempering in step (7) is 35-40.

[0019] In the forging process of a parachute clamp, in step (9), the copper plating layer has a thickness of 12-18 microns, the nickel plating layer has a thickness of 8-12 microns, and the chrome plating layer has a thickness of 0.5-2 microns.

[0020] The forging process of a parachute clamp has an area of ​​0.12 square decimeters.

[0021] In the forging process of a parachute clasp, in step (10), the specific step of grinding is: placing the part and the abrasive in a ratio of 1:3-4 into the drum of a roller polishing grinder, and then adding abrasive and water, and the working speed is 30 Hz.

[0022] In the forging process of a parachute clamp, the abrasive accounts for 5%-10% of the total amount of the parts and the abrasive.

[0023] In the forging process of a parachute clamp, the total amount of the parts and abrasive does not exceed 3 / 4 of the height of the drum.

[0024] In the forging process of a parachute clamp, the abrasive is a ceramic abrasive and has a diameter of 3 mm.

[0025] The beneficial effects achieved by the present invention are:

[0026] The forging process of the present invention adopts a circular ring-shaped blank, and forms it through forging without producing forging defects, and has a good forming effect; an end face turning process before forging is added, which successfully solves the problem that the end face burrs are forged into the parts and thus affect the performance of the parts.

[0027] The process of the present invention reduces the hardness of parts by normalizing, which is beneficial to subsequent part processing; quenching and tempering can increase the strength of parts, meeting the requirement that parts can withstand a tensile force of 1200kg without deformation; in addition, the combination of copper plating, nickel plating and chrome plating makes the parts both beautiful and corrosion-resistant. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 It is a schematic diagram of the structure of the blank after cutting;

[0029] Figure 2 It is a schematic diagram of the structure of the blank after forging.

[0030] Figure 3 It is a schematic diagram of the structure of the blank after the flash is cut off.

[0031] Figure 4 It is a structural diagram of the product. DETAILED DESCRIPTION

[0032] The present invention is further described below. The following examples are only used to more clearly illustrate the technical solution of the present invention, and are not intended to limit the protection scope of the present invention.

[0033] A forging process for a parachute clasp comprises the following steps:

[0034] (1) Billet selection: select a ring-shaped steel pipe made of 30CrMnSiA with an outer diameter of 31 mm and an inner diameter of 20 mm, and then cut it into sections;

[0035] (2) Turn the material, turn the end face of the cut blank on a lathe, make it blunt, and cut it to ensure that the length of the blank is 8.5 mm. Figure 1 As shown;

[0036] (3) Forging: put the cut blank into a small high frequency for heating to 950℃-1000℃, and then start forging with a forging die at a temperature not lower than 850℃. Figure 2 As shown;

[0037] (4) Normalizing: normalizing the forged billet, heating it to 860-880°C, then keeping it warm for 30-35 minutes, and cooling it by air cooling;

[0038] (5) Cut the flash. Place the parts after normalizing and cooling in the trimming die on the punch press to cut the flash. Ensure that the residual flash is no larger than 0.3 mm. Figure 3 As shown;

[0039] (6) Turn the outer ring surface, position and clamp the parts after cutting the flash, and turn the outer ring surface on the CNC lathe

[0040] (7) Turn the inner ring surface, position and clamp the parts after turning the outer ring surface, and start turning the inner ring surface on the CNC lathe to ensure that the two semicircular ring surfaces are turned smoothly;

[0041] (8) Quenching and tempering: quench and temper the parts behind the inner ring surface; quenching temperature 890℃±10℃, oil quenching, tempering: heating temperature 480℃±20℃, keep warm for 90-120 minutes, air cooling;

[0042] (9) Lathe finishing: Use a lathe to finish the machining marks on the torus surface of the quenched parts, and use sandpaper to polish to the surface roughness requirements;

[0043] (10) Inspection: Use a pin as a measuring tool to check the magnetism of the polished parts;

[0044] (11) Surface treatment: The inspected parts are subjected to copper plating, nickel plating and chrome plating in sequence, with a plating area of ​​0.12 square decimeter, of which the copper plating thickness is 12 to 18 microns, the nickel plating thickness is 8 to 12 microns, and the chrome plating thickness is 0.5 to 2 microns; the inner circle of the hanging is electroplated, and the contact point is moved half of the time to separate it from the nickel-plated contact point.

[0045] (12) Grinding and polishing: Grind and polish the surface treated parts. Put the parts and abrasives into the drum of a roller polishing machine in a ratio of 1:3-4, with the total amount not exceeding 3 / 4 of the drum height. Then add 5% to 10% of the total weight of the parts and abrasives and an appropriate amount of water. The working speed is 30Hz, polishing for 10-15min, and the abrasive is a ceramic abrasive with a diameter of 3mm. The final parts are as follows: Figure 4 shown.

[0046] The present invention selects pipe materials of reasonable specifications, which can save raw materials to the maximum extent; turning the end surface of the blank before forging is conducive to placing the blank into the forging die for forging and forming, preventing corners from overflowing, and preventing burrs from being pressed into the interior of the part. Forging can increase the strength of the part, make the internal structure tighter, and prevent the raw materials from being loose and having pores. Normalizing can reduce the hardness of the part, which is beneficial to the subsequent part processing and the heat treatment of the final part. Quenching and tempering can increase the strength of the part and meet the requirement that the part can withstand a tensile force of 1200kg without deformation; surface treatment makes the part beautiful in appearance and meets the requirements of corrosion resistance and wear resistance.

[0047] The parts of the present invention are subjected to magnetic inspection and can be used as aviation parts to prevent electromagnetic interference. The surface of the present invention is not only chrome-plated, but also copper-plated and nickel-plated to increase the adhesion between the chrome layer and the parts and prevent the chrome layer from falling off.

[0048] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the technical principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A forging process for a parachute clasp, characterized in that: The following steps are involved: (1) Billet selection: select the steel pipe and then cut it into sections; (2) Turning: The cut blank is turned on a lathe to make it blunt and cut off; (3) Forging: The cut blank is placed in a small high frequency for heating to 950°C-1000°C, and then the forging die is started for forging at a temperature not lower than 850°C; (4) Normalizing: The forged billet is normalized by heating it to 860-880°C, then keeping it warm for 30-35 minutes, and cooling it by air cooling; (5) Cutting flash: Place the cooled parts in the trimming die on the punch press to cut the flash; (6) Turning the outer and inner ring surfaces: Position and clamp the parts after flash cutting, turn the outer ring surface on a CNC lathe, and then turn the inner ring surface; (7) Quenching and tempering: Quench and temper the parts behind the inner torus surface; (8) Lathe finishing: Use a lathe to finish the joint marks on the torus surface of the quenched parts, and use sandpaper to polish to the surface roughness requirements; (9) Inspection: Use a pin as a measuring tool to check the magnetism of the polished parts; (10) Surface treatment: The inspected parts are copper plated, nickel plated and chrome plated in sequence; (11) Grinding and polishing: Grind and polish the surface treated parts. Place the parts and abrasive in a ratio of 1:3-4 into the drum of a roller polishing grinder, add abrasive and water, and operate at a speed of 30 Hz to obtain the final product.

2. The forging process of the parachute clamp according to claim 1 is characterized in that: The steel pipe used in step (1) has a circular cross-section, an outer diameter of 31 mm, an inner diameter of 20 mm, and is made of 30CrMnSiA.

3. The forging process of the parachute clamp according to claim 1 is characterized in that: The length of the blank after cutting in step (2) is 8.5 mm.

4. The forging process of the parachute clamp according to claim 1 is characterized in that: The abrasive is 5%-10% of the total amount of the parts and the abrasive.

5. The forging process of the parachute clamp according to claim 1 is characterized in that: The total amount of the parts and abrasives shall not exceed 3 / 4 of the height of the drum.

6. The forging process of the parachute clamp according to claim 1 is characterized in that: The abrasive is a ceramic abrasive with a diameter of 3 mm.

Citation Information