Polyester film, method for preparing the same and method for using the same for recycling polyethylene terephthalate containers
By controlling the composition and processing technology of copolyester resin and homopolymer polyethylene terephthalate resin, a polyester film with excellent seam characteristics and recyclability was prepared. This solved the problems of uneven shrinkage of polyester film in the heat shrink process and agglomeration during the recycling process, and improved the quality and production efficiency of recycled polyester chips.
Patent Information
- Application Number
- CN202110549031.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2021-01-22
- Filing Date
- 2021-05-19
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2041-05-19
AI Technical Summary
Existing polyester films suffer from uneven shrinkage or distortion during heat shrinking processes, and are difficult to recycle effectively, especially during high-temperature heat treatment when they tend to clump together, affecting recyclability and production efficiency.
By preparing a polyester film comprising copolyester resin and homopolymer polyethylene terephthalate resin, controlling its melting enthalpy and melting point within a specific range, and combining appropriate stretching and heat setting processes, the film is ensured to have excellent crystallinity and solvent adhesion strength, and the agglomeration rate is reduced.
It achieves excellent seam characteristics and recyclability of polyester film in heat shrink process, reduces agglomeration in recycling process, improves the quality and productivity of recycled polyester chips, and reduces environmental pollution risk.
Smart Images

Figure CN114773796B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a polyester film, a method for preparing the same, and a method for recycling a polyethylene terephthalate container using the same. Specifically, the present invention relates to a polyester film having excellent seaming properties and recyclability due to controllable crystallinity, a method for preparing the same, and a method for recycling a polyethylene terephthalate (PET) container having the polyester film. Background Art
[0002] In recent years, as containers for beverages or foods are manufactured in various forms, or there is an increase in the use of complete packaging in order to attract consumer attention, heat shrink labels and packaging materials have attracted attention. Such heat shrink labels or packaging materials utilize the following characteristics of polymer films: once the polymer film is oriented by stretching it, the polymer film tends to shrink to the shape before it is stretched at a certain temperature or higher. In a typical process of heat shrink labels or packaging, the heat shrink film is cut, printed with a desired design, rolled up, bonded at both ends with an adhesive solvent, wrapped loosely around the container, and then shrunk when heat is applied thereto.
[0003] The film used in the above-mentioned heat shrinking process is required to have not only basic properties such as heat resistance, chemical resistance, weather resistance, and printability, but also container sealing, heat shrinkage uniformity, running characteristics in the longitudinal direction, and crack resistance. Generally, polyvinyl chloride film, polystyrene film, polypropylene film, etc. have been used in the heat shrinking process. In recent years, polyester film having properties such as high heat resistance and weather resistance, convenience of incineration, and excellent printability has been widely used.
[0004] However, since conventional polyester films have a fast shrinkage speed and high shrinkage stress, there have been defects caused by uneven shrinkage or distortion of plastic containers. Therefore, Korean Laid-open Patent Publication No. 2002-0062838 discloses a technology in which 5 wt% or more of a polyester elastomer is added to a heat-shrinkable polyester film to suppress the occurrence of wrinkles, shrinkage stains, distortion, etc. when the film is used for complete packaging of plastic bottles.
[0005] Therefore, a polyester film having a lower crystallinity prepared by blending a soft component with a polyester resin is used in a heat shrink process. In addition, a polyester film having thermal properties such as shrinkage rate and shrinkage stress with respect to temperature, chemical resistance suitable for a seaming process, and recently recyclability due to the waste plastic problem has been developed.
[0006] In addition, as concerns about environmental issues have increased in recent years, the recycling of products manufactured using thermoplastic polymers has become important. In particular, polyethylene terephthalate (PET) resins, which have excellent properties in terms of heat resistance, processability, transparency, and non-toxicity, have been widely used to produce various products such as films, fibers, bottles, containers, etc., and efforts have been continued to increase their recycling rates.
[0007] [Prior art literature]
[0008] [Patent Document]
[0009] (Patent Document 1) Korean Laid-open Patent Publication No. 2002-0062838. Summary of the invention
[0010] Technical issues
[0011] Therefore, the embodiments are intended to provide a polyester film having excellent seam characteristics and excellent recyclability by virtue of controllable crystallinity (whereby uneven agglomeration rarely occurs even after heat treatment for a long period of time in its recycling method), a method for preparing the polyester film, and a method for recycling a polyethylene terephthalate container using the polyester film.
[0012] Solution to the problem
[0013] According to an embodiment, there is provided a polyester film comprising a copolyester resin in which a diol is copolymerized with a dicarboxylic acid and optionally comprising a homopolyethylene terephthalate (HOMO-PET) resin, wherein the melting enthalpy (ΔHm) as measured by differential scanning calorimetry is 9 J / g or more, and the blocking rate is 10% or less.
[0014] According to another embodiment, a method for preparing a polyester film is provided, which includes preparing a copolyester resin in which a diol and a dicarboxylic acid are copolymerized; optionally adding a homopolyethylene terephthalate (HOMO-PET) resin to the copolyester resin, and then melt-extrude the resin at a temperature of 250° C. to 300° C. to prepare an unstretched sheet; and stretching the unstretched sheet and then heat-setting it at a temperature of 70° C. to 100° C. to prepare a polyester film, wherein the melting enthalpy (ΔHm) of the polyester film is 9 J / g or more as measured by differential scanning calorimetry, and the blocking rate of the polyester film is 10% or less.
[0015] According to yet another embodiment, a method for recycling a polyethylene terephthalate container is provided, which includes providing a polyethylene terephthalate (PET) container having a polyester film; crushing the polyethylene terephthalate (PET) container having the polyester film to obtain flakes; and heat-treating the flakes to produce recycled polyester chips, wherein the agglomeration rate of the flakes is 10% or less, and the flakes include first flakes obtained by crushing the polyethylene terephthalate (PET) container and second flakes obtained by crushing the polyester film.
[0016] Beneficial effects of the present invention
[0017] In the polyester film according to the embodiment, the melting enthalpy (ΔHm) as measured by differential scanning calorimetry satisfies 9 J / g or more, thereby being able to easily control its crystallinity, resulting in improved thermal and chemical properties. Therefore, the polyester film according to the embodiment not only has excellent shrinkage relative to temperature, but also has excellent solvent adhesive strength even when applied to gravure printing, UV curing printing, and variable sleeve offset printing (VSOP), making it suitable for heat shrinking processes and seaming processes.
[0018] Alternatively, the polyester film according to the embodiment satisfies a melting point (Tm) of 190° C. to 230° C. when measured by differential scanning calorimetry and a peel strength of 150 gf / 3 cm or more, thereby being able to easily control its crystallinity, resulting in improved thermal and chemical properties. Therefore, the polyester film according to the embodiment not only has an excellent shrinkage rate relative to temperature, but also has excellent solvent adhesive strength even when applied to gravure printing, UV curing printing, and variable sleeve offset printing (VSOP), making it suitable for heat shrinking processes and seaming processes.
[0019] In addition, since the occurrence of agglomeration is suppressed during the heat treatment process for a long period of time, the polyester film has a low defect rate during the recycling process. Therefore, the quality, yield, and productivity of recycled polyester chips produced by the recycling method of the polyethylene terephthalate container using the polyester film can be improved.
[0020] In addition, the method for regenerating the polyethylene terephthalate container according to this embodiment does not require a separation step of separating the container and the membrane. Therefore, it is economical because time and cost are saved. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 Shown is a polyester film applied to a product before and after heat shrinking the polyester film.
[0022] Figure 2 A method for measuring the caking of polyethylene terephthalate containers with polyester film is shown.
[0023] Figure 3 A method for measuring the peel strength of a polyester film is shown.
[0024] Figure 4 A method for measuring the heat shrinkage of polyester films is shown.
[0025] Figure 5 Differential Scanning Calorimetry (DSC) curves of the polyester films of Examples 1-3 are shown.
[0026] [Explanation of Reference Numerals]
[0027] d: diameter of the hole
[0028] x1: The first size before shrinking
[0029] x1: The first size after shrinking
[0030] y: Second dimension
[0031] w: Length to the bonding part
[0032] TL: Trend Line
[0033] T1: Melting start temperature
[0034] T2: Melting completion temperature
[0035] 1: Products with tags
[0036] 6: Crusher
[0037] 7: Compression weights
[0038] 8: Screen
[0039] 10a: Second sheet
[0040] 10b: Agglomerated mixed flakes
[0041] 11: Label (before shrinking)
[0042] 11a: Label after shrinking
[0043] 20: Products
[0044] 20a: First sheet
[0045] 100: (first) polyester film (before shrinkage)
[0046] 100a: Polyester film after shrinkage
[0047] 110: Bonding part
[0048] 120: Pressure plate
[0049] 130: Heavy Objects
[0050] 200: Second polyester film
[0051] 300: Sample A
[0052] Best Mode for Carrying Out the Invention
[0053] Hereinafter, the present invention will be described in detail with reference to embodiments. The embodiments are not limited to those described below. Instead, they can be modified into various forms as long as the gist of the present invention is not changed.
[0054] Throughout the specification, when a part is referred to as “comprising” an element, it should be understood that other elements may be included rather than excluded unless specifically stated otherwise.
[0055] Unless otherwise indicated, all numbers and expressions relating to amounts of ingredients, reaction conditions, and so forth used herein are to be understood as modified by the term "about."
[0056] Throughout this specification, the terms first, second, etc. are used to describe various components. However, the components should not be limited by these terms. These terms are only used to distinguish one component from another.
[0057] Since heat shrink labels or packaging materials composed of polyester films are difficult to recycle despite their excellent thermal characteristics and chemical resistance, most of them are disposed of after use. This is because, when the polyester film is introduced into the current recycling method (i.e., the regeneration method), the polyester film causes various process defects during the heat treatment at high temperature for a long period of time. Therefore, although additional methods can be performed to improve recyclability, there is a problem of increased process costs.
[0058] In addition, a method of adjusting the composition of the polyester film can be used to improve recyclability. In this case, when the polyester film is applied to gravure printing, UV curing printing, and variable sleeve offset printing (VSOP), the solvent bonding strength is low due to its high crystallinity, making it unsuitable for heat shrinking process and seaming process.
[0059] However, since the polyester film according to the embodiment has excellent thermal characteristics and chemical resistance, it is suitable for heat shrinking processes and seaming processes, whereby it can be easily applied as various types of heat shrink labels and packaging materials and has excellent recyclability when its use is completed.
[0060] In addition, the polyethylene terephthalate (PET) containers recovered from consumers have labels indicating product information. Typically, once they have been washed and broken, they are then subjected to liquid specific gravity separation, dehydration, drying, and / or wind specific gravity separation in order to remove a large amount of film contained in the broken product, and then subjected to additional steps such as granulation to obtain recycled polyester chips. However, even after the above process, it is difficult to completely remove the film used as a label for polyethylene terephthalate (PET) containers. There is a problem of coloring the recycled polyester chips due to the ink contained in the film. In addition, there has been a problem that the recycled polyester chips are unevenly agglomerated during the regeneration process, especially the heat treatment process, due to the thermal characteristics of the film.
[0061] Therefore, in order to easily perform specific gravity separation, a method of using a film made of a low specific gravity polymer such as polystyrene, polyethylene, polypropylene, etc. as a label has been proposed. However, in the specific gravity separation method, since the ink layer cannot effectively achieve its low specific gravity, this still makes it difficult to completely separate and remove the film, and the problem of residual ink coloring the recycled polyester chips cannot be solved.
[0062] The polyester film according to the embodiment is excellent in shrinkage characteristics by means of controllable crystallinity and seam characteristics in various printing methods, and has excellent recyclability, whereby agglomeration rarely occurs even if it is heat-treated for a long period of time in a regeneration method. Therefore, the quality, yield, and productivity of recycled polyester chips produced by a regeneration method of a polyethylene terephthalate (PET) container including the polyester film can be improved. In addition, the polyester film according to the embodiment can be advantageously applied as a heat shrink label or packaging material to containers of various types of products including beverages and foods.
[0063] Polyester film
[0064] According to an embodiment, a polyester film is provided, which includes a copolyester resin in which a diol is copolymerized with a dicarboxylic acid and optionally includes a homopolyethylene terephthalate (HOMO-PET) resin, wherein the melting enthalpy (ΔHm) as measured by differential scanning calorimetry is 9 J / g or more, and the blocking rate is 10% or less.
[0065] According to another embodiment, a polyester film is provided, which includes a copolyester resin in which a diol and a dicarboxylic acid are copolymerized and optionally includes a homopolyethylene terephthalate (HOMO-PET) resin, wherein the melting point (Tm) as measured by differential scanning calorimetry is 190° C. to 230° C., the blocking rate is 10% or less, and the peel strength is 150 gf / 3 cm or more.
[0066] The polyester film according to the embodiment has a melting enthalpy (ΔHm) of 9 J / g or more as measured by differential scanning calorimetry. For example, the melting enthalpy (ΔHm) of the polyester film as measured by differential scanning calorimetry may be 9 J / g or more, 10 J / g or more, 12 J / g or more, or 15 J / g or more, 9 J / g to 33 J / g, 9 J / g to 30 J / g, 9 J / g to 28 J / g, 10 J / g to 33 J / g, 10 J / g to 30 J / g, 10 J / g to 28 J / g, 12 J / g to 33 J / g, 12 J / g to 30 J / g, 12 J / g to 28 J / g, 15 J / g to 33 J / g, 15 J / g to 30 J / g, or 15 J / g to 28 J / g.
[0067] Since the melting enthalpy of the polyester film is adjusted within the above range, the crystallinity of the polyester film can be effectively controlled, whereby seam characteristics such as solvent bonding strength are excellent, and the blocking rate is very low in a recycling method of the film or a polyethylene terephthalate (PET) container including the film, whereby environmental pollution can be prevented while improving recyclability.
[0068] Specifically, if the melting enthalpy of the polyester film is less than the above range, the thermal characteristics are poor, thereby increasing the agglomeration rate in the regeneration method for recycling. In addition, if the melting enthalpy of the polyester film exceeds the above range, the agglomeration rate may be reduced, but the peel strength may be deteriorated, so that it may be difficult to use as a heat shrink film.
[0069] The differential scanning calorimeter (DSC) may specifically be a modulated differential scanning calorimeter (modulated DSC or MDSC), more specifically a temperature-modulated differential scanning calorimeter (TMDSC).
[0070] Specifically, the melting enthalpy can be measured by scanning at a heating rate of 10°C / min using a differential scanning calorimeter (DSC) mode. More specifically, the melting enthalpy can be measured by scanning at a heating rate of 10°C / min using a differential scanning calorimeter (DSC) mode. st scan) or a second scan (2 nd In this specification, the melting enthalpy is measured by the first scan of the polyester film.
[0071] The glass transition temperature (Tg), crystallization temperature (Tc), and melting point (Tm) can be measured from the heat flow curve obtained by scanning.
[0072] Specifically, in the heat flow curve obtained by scanning, the first endothermic temperature is the glass transition temperature (Tg), the exothermic temperature measured after the glass transition temperature (Tg) is the crystallization temperature (Tc), and the endothermic temperature measured after the crystallization temperature (Tc) is the melting point (Tm).
[0073] Here, the integral value at the melting point (Tm) is calculated as the melting enthalpy. Specifically, the melting enthalpy is the energy in the interval where endothermic absorption occurs in the heat flow curve of differential scanning calorimetry. The trend line from the melting start temperature to the melting completion temperature is set as the baseline, and the integral value of the peak along the baseline is converted and calculated.
[0074] Figure 5 The differential scanning calorimetry (DSC) curves of the polyester films of Examples 1-3 are shown. Figure 5 , the first endothermic temperature of 73.34°C is the glass transition temperature, the exothermic temperature of 100.59°C measured after the glass transition temperature is the crystallization temperature, and the endothermic temperature of 201.99°C measured after the crystallization temperature is the melting point (Tm). Here, the integrated value of 25.94 J / g at the melting point (Tm) is calculated as the melting enthalpy. More specifically, the trend line (TL) from the melting start temperature (T1) to the melting completion temperature (T2) is set as the baseline, and the integrated value of the peak along the baseline is calculated as the melting enthalpy.
[0075] The polyester film may have a melting point (Tm) of 190° C. to 230° C. as measured by differential scanning calorimetry. For example, the film may have a melting point of 193° C. to 230° C., 195° C. to 228° C., or 195° C. to 225° C. as measured by differential scanning calorimetry.
[0076] Since the melting point of the polyester film is adjusted within the above range, the polyester film is effectively controlled in crystallinity, thereby having excellent seam characteristics such as solvent bonding strength. In addition, since the agglomeration rate is very low in the recycling method of the film or the polyethylene terephthalate (PET) container including the film, it is possible to prevent environmental pollution while improving recyclability.
[0077] Specifically, if the melting point of the polyester film exceeds the above range, the adhesive strength of the solvent to the polyester film is reduced, making it difficult to use in the seaming process. If the melting temperature is lower than the above range, the blocking rate may increase.
[0078] The polyester film may have a glass transition temperature (Tg) of 60°C or more as measured by differential scanning calorimetry. For example, the film may have a glass transition temperature (Tg) of 60°C or more, 65°C or more, 70°C or more, 60°C to 85°C, 60°C to 80°C, or 60°C to 78°C as measured by differential scanning calorimetry.
[0079] In addition, the crystallization temperature of the polyester film is not measured or is 70°C to 130°C as measured by differential scanning calorimetry. For example, the crystallization temperature (Tc) of the film is not measured or may be 80°C to 130°C, 85°C to 125°C, 90°C to 125°C, 96°C to 125°C, or 98°C to 120°C as measured by differential scanning calorimetry. Since the crystallization temperature of the polyester film is adjusted within the above range, the crystallinity of the polyester film can be effectively controlled, thereby making the agglomeration rate very low in the recycling method of the film or the polyethylene terephthalate (PET) container including the film. Therefore, environmental pollution can be prevented while improving recyclability.
[0080] The crystallization heat of the film as measured at the crystallization temperature (Tc) can be 0.01J / g to 50J / g. For example, the crystallization heat can be calculated as the integral value at the crystallization temperature (Tc). The crystallization heat of the film can be 0.01J / g to 40J / g, 0.05J / g to 30J / g, 0.1J / g to 20J / g, 0.1J / g to 10J / g, 0.2J / g to 10J / g, 0.3J / g to 10J / g or 0.5J / g to 9J / g as measured at the crystallization temperature (Tc). Since the crystallization heat of the polyester film meets the above range, it is possible to effectively control the crystallinity of the polyester film, thereby the agglomeration rate is very low in the film or the regeneration method of the polyethylene terephthalate (PET) container comprising the film. Therefore, it is possible to prevent environmental pollution while improving recyclability.
[0081] In addition, the polyester film has a blocking rate of 10% or less. For example, when a sheet obtained by crushing a polyethylene terephthalate (PET) container having a polyester film is subjected to a pressure of 8.7 kPa and heat-treated at 210° C. for 90 minutes, the blocking rate may be 9% or less, 8.5% or less, 8% or less, 6% or less, 5% or less, 4% or less, preferably 3% or less, 2% or less, 1.5% or less, 1% or less, 0.8% or less, 0.5% or less.
[0082] Agglomeration refers to aggregates that may be formed in the regeneration process. The size of the aggregates may be, for example, at least three times the size of the flake particles before heat treatment. Agglomeration rate refers to the fraction of aggregates based on the total weight of the initial mixed flakes (i.e., flakes before heat treatment). It can be calculated by the following equation 1.
[0083] [Equation 1]
[0084]
[0085] Specifically, in the regeneration method of the polyethylene terephthalate (PET) container in which the film is provided as a label, the thin slice obtained by breaking it is passed through a screen, and then subjected to a heat treatment process. In this case, when the broken thin slice agglomerates, aggregates can be formed, which are called agglomerates. The aggregates are filtered through a screen again, and the weight is measured. The weight ratio of the aggregates based on the total weight of the thin slice before the heat treatment is calculated as the agglomeration rate. Therefore, the higher the value of the agglomeration rate, the lower the recyclability.
[0086] Since the polyester film according to the embodiment is effectively controlled in crystallinity, there is no wrinkle or distortion of the polyethylene terephthalate (PET) container when applied as a label for the polyethylene terephthalate (PET) container. In addition, even if the flakes broken together with the polyethylene terephthalate container at the end of use are heat-treated during the regeneration method, the agglomeration rate is very low. Therefore, it is possible to improve recyclability, and improve the quality, yield, and productivity of recycled polyester chips produced by recycling.
[0087] If the flakes are melted to form agglomerates in the recycling process, various problems may arise. Therefore, the Association of Plastic Recyclers (APR) is preparing a procedure (APR PET-S-08) for evaluating the agglomeration rate. Specifically, 3 parts by weight of polyester film and 97 parts by weight of polyethylene terephthalate containers are respectively crushed to a particle diameter of 9.5 mm or less, and heat-treated at a temperature of 210°C and a pressure of 8.7 kPa for 90 minutes (i.e., a load of 2.5 kgf is applied to a cylinder with a diameter of 6 cm). The agglomeration rate may refer to the ratio of agglomerates that cannot pass through a sieve with an aperture of 11.2 mm (or a 0.625" sieve).
[0088] In addition, the polyester film according to the embodiment may have excellent solvent adhesive strength, that is, seam properties.
[0089] Specifically, the polyester film according to the embodiment may have a peel strength of 150 gf / 3cm or more. For example, the peel strength may be 150 gf / 3cm or more, 180 gf / 3cm or more, 200 gf / 3cm or more, 230 gf / 3cm or more, 250 gf / 3cm or more, 300 gf / 3cm or more, or 330 gf / 3cm or more, 150 gf / 3cm to 3,000 gf / 3cm, 180 gf / 3cm to 2,800 gf / 3cm, 200 gf / 3cm or more, gf / 3cm to 2,500 gf / 3cm, 250 gf / 3cm to 2,000 gf / 3cm, 300 gf / 3cm to 3,000 gf / 3cm, 300 gf / 3cm to 2,500 gf / 3cm, 300 gf / 3cm to 2,000 gf / 3cm, 330 gf / 3cm to 1,500 gf / 3cm, or 330 gf / 3cm to 1,300 gf / 3cm. Since the peel strength is adjusted within the above range, the polyester film has excellent seam characteristics such as solvent adhesive strength and is suitable for seam processes.
[0090] The peel strength can be measured using two sheets of polyester film (i.e., a first polyester film and a second polyester film). Specifically, 1,3-dioxolane is applied to one side of a first polyester film in the form of a tape having a width of 2 mm and a length of 30 mm to form an adhesive portion, and a second polyester film is laminated on the first polyester film on which the adhesive portion has been formed. In this case, the second polyester film is laminated immediately while applying 1,3-dioxolane. A pressure of 160 Pa is applied to the adhesive portion for 1 hour for aging, and then the maximum force when the first and second polyester films are peeled off at a speed of 300 mm / min and an angle of 180° is measured as the peel strength.
[0091] In addition, in the polyester film according to the embodiment, the shrinkage rate in the main shrinkage direction relative to the temperature can be adjusted within a specific range. Specifically, the polyester film according to the embodiment may be a heat shrinkable film. For example, when the shrinkage rate of the polyester film in the main shrinkage direction when heat-treated at a temperature of X°C for 10 seconds is defined as T X When T 70 , T 80 , T 90 , and T 100 The range can be adjusted. X The heat treatment may specifically refer to immersing the polyester film in hot water at X° C. for 10 seconds.
[0092] Specifically, when heat-treated at 70° C. for 10 seconds, the film may have a heat shrinkage rate (T 70 ). For example, T 70It may be 0.1% to 50%, 0.5% to 48%, 0.5% to 46%, 2% to 46%, or 3.5% to 45.5%.
[0093] In this specification, the first direction may be a transverse direction (TD) or a longitudinal direction (MD), and the second direction perpendicular to the first direction may be a longitudinal direction (MD) or a transverse direction (TD). Specifically, the first direction may be a transverse direction (TD) as a main shrinkage direction, and the second direction may be a longitudinal direction (MD).
[0094] In addition, when heat-treated at a temperature of 80° C. for 10 seconds, the film may have a heat shrinkage rate (T 80 ). For example, T 80 It can be 23% or more, 25% or more, 40% or more, 45% or more, 50% or more, or 55% or more, 20% to 85%, 23% to 80%, 25% to 75%, 40% to 85%, 45% to 80%, 50% to 78%, or 55% to 75%.
[0095] When heat-treated at 90° C. for 10 seconds, the film may have a heat shrinkage rate (T 90 ). For example, T 90 It may be 50% or greater, 60% or greater, or 70% or greater, 40% to 85%, 50% to 80%, 60% to 78%, or 70% to 80%.
[0096] In addition, when heat-treated at a temperature of 100° C. for 10 seconds, the film may have a heat shrinkage rate (T 100 ). For example, T 100 It may be 45% to 80%, 50% to 80%, 65% to 80%, 70% to 80%, 70% to 78%, or 73% to 78%. Since the heat shrinkage rate in the first direction satisfies the above range when heat-treated at 80° C. for 10 seconds, a labeling process in which the film surrounds at least a portion of a container is facilitated. Specifically, when the film is applied as a label for a polyethylene terephthalate (PET) container, there is no wrinkle or distortion of the polyethylene terephthalate container.
[0097] Meanwhile, in the polyester film according to the embodiment, the shrinkage rate with respect to temperature in the first direction and the second direction perpendicular to the first direction can be adjusted within a specific range. For example, when the shrinkage rate of the polyester film in the second direction is defined as T when heat-treated at a temperature of X°C for 10 seconds, X ', T 70 '、T 75 '、T 80 '、T90 ', and T 100 The range of ' can be adjusted within a specific range. X The heat treatment may refer to immersing the polyester film in hot water at X°C for 10 seconds.
[0098] Polyester film T 70 '、T 75 '、T 80 '、T 90 ', and T 100 ' can be independently -10% to 10%. For example, the T of a polyester film 70 '、T 75 '、T 80 '、T 90 ', and T 100 ' can each be -10% or more, -8% or more, -6% or more, -4% or more, -2% or more, 0% or more, and 10% or less, 8% or less, 6% or less, 4% or less, or 2% or less.
[0099] Specifically, when heat-treated at a temperature of 100° C. for 10 seconds, the film may have a heat shrinkage rate (T 100 '). For example, T 100 ' can be 7% or less or 6% or less, -16% to 7%, -10% to 7%, -7% to 7%, -5% to 7%, 0% to 7%, 0.5% to 7%, or 2% to 6%.
[0100] In addition, the polyester film can have a light transmittance of 90% or more at a wavelength of 550nm. Specifically, before and after immersion in a sodium hydroxide (NaOH) aqueous solution having a concentration of 1% at 85°C, the light transmittance of the film measured at a wavelength of 550nm can be 90.5% or more, 91% or more, 92% or more, or 93% or more, respectively.
[0101] The light transmittance change of the polyester film before and after immersion in a sodium hydroxide (NaOH) aqueous solution having a concentration of 1% at 85° C. may be 0.7% or less. For example, the light transmittance change of the film before and after immersion may be 0.6% or less or 0.5% or less.
[0102] The light transmittance change refers to the absolute value of the difference between the light transmittance of the film measured at a wavelength of 550 nm before immersion and the light transmittance of the film measured at a wavelength of 550 nm after immersion.
[0103] In addition, before and after the membrane is immersed in a sodium hydroxide (NaOH) aqueous solution having a concentration of 1% at 85° C., the change in Col-L (ΔL) may be 0.7 or less, the change in Col-a (Δa) may be 0.5 or less, and the change in Col-b (Δb) may be 0.5 or less. For example, before and after the immersion, the change in Col-L (ΔL) may be 0.65 or less, 0.6 or less, 0.55 or less, or 0.5 or less, the change in Col-a (Δa) may be 0.3 or less, 0.1 or less, 0.08 or less, 0.06 or less, or 0.05 or less, and the change in Col-b (Δb) may be 0.3 or less, 0.1 or less, 0.08 or less, or 0.07 or less.
[0104] The change in Col-L (ΔL) refers to the absolute value of the difference between the Col-L value before immersion and the Col-L value after immersion, the change in Col-a (Δa) refers to the absolute value of the difference between the Col-a value before immersion and the Col-a value after immersion, and the change in Col-b (Δb) refers to the absolute value of the difference between the Col-b value before immersion and the Col-b value after immersion.
[0105] Col-L, Col-a, and Col-b are color coordinates established by the Commission International d'Eclairage (CIE), where color is represented by L (brightness), a (green to red complementary color), and b (yellow to blue complementary color). They can be measured using UltraScan PRO (manufacturer: Hunterlab), but are not limited thereto.
[0106] The polyester film according to the embodiment includes a copolyester resin. Specifically, the copolyester resin may be a copolyester resin in which two or three or more diols and dicarboxylic acids are polymerized. More specifically, it may be a copolymerized polyethylene terephthalate (Co-PET) resin.
[0107] Specifically, the diol may include at least one selected from the group consisting of ethylene glycol, diethylene glycol, neopentyl glycol, unsubstituted or alkyl-substituted propylene glycol, unsubstituted or alkyl-substituted butanediol, unsubstituted or alkyl-substituted pentanediol, unsubstituted or alkyl-substituted hexanediol, unsubstituted or alkyl-substituted octanediol, and combinations thereof.
[0108] For example, the diol may include at least one selected from the group consisting of ethylene glycol, diethylene glycol, neopentyl glycol, 1,3-propylene glycol, 1,2-octanediol, 1,3-octanediol, 2,3-butanediol, 1,3-butanediol, 1,4-butanediol, 1,5-pentanediol, 2-butyl-2-ethyl-1,3-propylene glycol, 2,2-diethyl-1,5-pentanediol, 2,4-diethyl-1,5-pentanediol, 3-methyl-1,5-pentanediol, and 1,1-dimethyl-1,5-pentanediol.
[0109] The dicarboxylic acid may include an aromatic dicarboxylic acid, an aliphatic dicarboxylic acid, an alicyclic dicarboxylic acid, or an ester thereof.
[0110] For example, the dicarboxylic acid can be terephthalic acid, dimethyl terephthalic acid, isophthalic acid, naphthalene dicarboxylic acid, phthalic acid, adipic acid, azelaic acid, sebacic acid, decanedicarboxylic acid, esters thereof, or combinations thereof. Specifically, the dicarboxylic acid can include at least one selected from the group consisting of terephthalic acid, dimethyl terephthalate, naphthalene dicarboxylic acid, and phthalic acid.
[0111] According to an embodiment, the copolyester resin may be a copolyester resin in which two or three or more diols are polymerized with an aromatic dicarboxylic acid. Specifically, the copolyester resin may be a copolyester resin in which a diol including ethylene glycol and at least one comonomer is polymerized with an aromatic dicarboxylic acid.
[0112] The diol may include ethylene glycol and at least one comonomer selected from the group consisting of neopentyl glycol and diethylene glycol. In addition, the polyester film may include ethylene glycol and at least one comonomer selected from the group consisting of neopentyl glycol and diethylene glycol.
[0113] Specifically, the polyester film can include ethylene glycol in an amount of 50 mol % to 90 mol %. For example, the polyester film can include ethylene glycol in an amount of 60 mol % to 90 mol %, 65 mol % to 88 mol %, 68 mol % to 85 mol %, or 70 mol % to 83 mol %.
[0114] In addition, the polyester film may contain at least one comonomer selected from the group consisting of neopentyl glycol and diethylene glycol in an amount of 10 mol% or more. For example, the polyester film may contain at least one comonomer selected from the group consisting of neopentyl glycol and diethylene glycol in an amount of 10 mol% or more, 13 mol% or more, or 15 mol% or more, 10 mol% to 30 mol%, 10 mol% to 29 mol%, 10 mol% to 28 mol%, 15 mol% to 30 mol%, 15 mol% to 29 mol%, or 15 mol% to 28 mol%. Since the content of the comonomer satisfies the above range, the crystallinity can be more effectively controlled while the heat shrinkage in the main shrinkage direction is excellent.
[0115] In addition, if the content of the comonomer is less than the above range, the heat shrinkage characteristics of the polyester film may deteriorate. Specifically, the heat shrinkage rate of the polyester film in the main shrinkage direction may be insufficient at a specific temperature, and the heat shrinkage rate of the polyester film in a direction perpendicular to the main shrinkage direction may be too large at a specific temperature.
[0116] Specifically, the polyester film may include diethylene glycol as a comonomer. For example, the content of diethylene glycol may be 1 mol % to 10 mol %, 1 mol % to 8 mol %, 3 mol % to 6 mol %, 3.5 mol % to 5.5 mol %, or 3.8 mol % to 5.2 mol %.
[0117] In addition, the polyester film may include neopentyl glycol as a comonomer. For example, the content of neopentyl glycol may be 5 mol % to 35 mol %, 7 mol % to 33 mol %, 10 mol % to 30 mol %, 13 mol % to 28 mol %, or 15 mol % to 25 mol %.
[0118] Since the content of neopentyl glycol satisfies the above range, when the polyester film is heat-shrunk, the heat shrinkage rate in the first direction or in the second direction perpendicular to the first direction is easily adjusted, so that when the film is applied to a container, wrinkles or distortion can be more effectively prevented.
[0119] In addition, the polyester film may include both diethylene glycol and neopentyl glycol as comonomers. When the polyester film includes diethylene glycol and neopentyl glycol as comonomers, the molar ratio of neopentyl glycol to diethylene glycol may be 1:3 to 6, 1:3 to 5, or 1:3 to 4.
[0120] In addition, in addition to the diol component, the polyester film may further include a monohydric alcohol. For example, the monohydric alcohol may be methanol, ethanol, isopropanol, allyl alcohol, or benzyl alcohol. For example, the polyester film may further include a monohydric alcohol in an amount of 10 mol % to 30 mol %, 13 mol % to 25 mol %, or 15 mol % to 22 mol %, but is not limited thereto.
[0121] The dicarboxylic acid may include an aromatic dicarboxylic acid. For example, the polyester film may include terephthalic acid or dimethyl terephthalic acid in an amount of 80 mol % or more, 90 mol % or more, 95 mol % or more, 99 mol % or more, or 100 mol %.
[0122] The copolyester resin can be obtained by transesterification of a diol with a dicarboxylic acid, followed by polymerization thereof.
[0123] Specifically, at least one catalyst selected from manganese acetate, calcium acetate, and zinc acetate can be used as a catalyst for the transesterification reaction. The content of the catalyst can be 0.02 to 0.2 parts by weight, 0.02 to 0.1 parts by weight, or 0.05 to 0.1 parts by weight based on the total weight of the dicarboxylic acid.
[0124] In addition, upon completion of the transesterification reaction, at least one additive selected from the group consisting of silica, potassium, and magnesium; a stabilizer such as trimethyl phosphate; a polymerization catalyst such as antimony trioxide and tetrabutyl titanate; and the like may be selectively added.
[0125] The polyester film according to the embodiment optionally includes a homopolymer polyethylene terephthalate (HOMO-PET) resin. Since the polyester film further includes the homopolymer polyethylene terephthalate resin, the thermal characteristics of the film can be further improved.
[0126] Homopolymer polyethylene terephthalate (HOMO-PET) resin refers to a resin containing a polyethylene terephthalate structure in which terephthalic acid (TPA) or dimethyl terephthalic acid (DMT) is polymerized with ethylene glycol (EG) in an amount of 90 wt % or more, 95 wt % or more, 97 wt % or more, or 98 wt % or more.
[0127] For example, homopolymer polyethylene terephthalate (HOMO-PET) resin may be a resin that has been recycled.
[0128] Specifically, homopolymer polyethylene terephthalate (HOMO-PET) resin can be obtained by recycling a container to which a polyester film, specifically a polyester heat shrink film, has been attached. Alternatively, homopolymer polyethylene terephthalate (HOMO-PET) resin can be obtained by recycling the polyester film and polyester fiber together. The container can have a form that can hold or package a product. For example, it can be a polyester bottle, a polyester tray, a polyester bag, a polyester sheet, a polyester heat molded product, or a polyester packaging material.
[0129] The polyester film may include a homopolymer polyethylene terephthalate (HOMO-PET) resin in an amount of 0.5 wt % to 37 wt %. For example, based on the total weight of the copolyester resin and the homopolymer polyethylene terephthalate (HOMO-PET) resin, the content of the homopolymer polyethylene terephthalate (HOMO-PET) resin may be 0.5 wt % to 37 wt %, 1 wt % to 37 wt %, 2 wt % to 37 wt %, 2 wt % to 35 wt %, 2 wt % to 30 wt %, 2 wt % to 27 wt %, 2 wt % to 25 wt %, 2 wt % to 20 wt %, 3 wt % to 37 wt %, 3 wt % to 35 wt %, 3 wt % to 30 wt %, or 3 wt % to 25 wt %.
[0130] Since the content of the homopolymer polyethylene terephthalate (HOMO-PET) resin satisfies the above range, the crystallinity of the polyester film can be effectively controlled, whereby seam characteristics such as solvent adhesion strength are excellent, and the blocking rate is very low in the recycling method of the film or the polyethylene terephthalate (PET) container including the film. Therefore, environmental pollution can be prevented while improving recyclability.
[0131] Specifically, if the content of the homopolymer polyethylene terephthalate resin exceeds the above range, thermal characteristics may be improved, resulting in an increase in the effect of preventing a blocking phenomenon, while joint characteristics may be deteriorated.
[0132] The polyester film may have a thickness of 10 to 100 μm. For example, the polyester film may have a thickness of 20 to 80 μm, 30 to 70 μm, 35 to 65 μm, 35 to 55 μm, 40 to 60 μm, or 35 to 45 μm.
[0133] Method for preparing polyester film
[0134] According to another embodiment, there is provided a method for preparing a polyester film, comprising preparing a copolyester resin in which a diol is copolymerized with a dicarboxylic acid; optionally adding a homopolyethylene terephthalate (HOMO-PET) resin to the copolyester resin and then melt-extruding at a temperature of 250° C. to 300° C. to prepare an unstretched sheet; and stretching the unstretched sheet and then heat-setting it at a temperature of 70° C. to 100° C. to prepare a polyester film, wherein a melting enthalpy (ΔHm) of the polyester film as measured by differential scanning calorimetry is 9 J / g or more, and a blocking rate of the polyester film is 10% or less.
[0135] According to yet another embodiment, there is provided a method for preparing a polyester film, comprising preparing a copolyester resin in which a diol is copolymerized with a dicarboxylic acid; optionally adding a homopolyethylene terephthalate (HOMO-PET) resin to the copolyester resin and then melt-extruding at a temperature of 250° C. to 300° C. to prepare an unstretched sheet; and stretching the unstretched sheet and then heat-setting it at a temperature of 70° C. to 100° C. to prepare a polyester film, wherein the polyester film has a melting point (Tm) of 190° C. to 230° C. as measured by differential scanning calorimetry, a blocking rate of 10% or less, and a peel strength of 150 gf / 3 cm or more.
[0136] The composition and process conditions are adjusted so that the polyester film finally produced by the above method satisfies the characteristics (melting enthalpy, melting point, shrinkage characteristics, etc.) as discussed above. Specifically, in order to make the final polyester film satisfy the characteristics as discussed above, the composition of the copolyester resin is adjusted, the extrusion temperature, the casting temperature, the preheating temperature during stretching, the stretching ratio in each direction, the stretching temperature, the stretching speed, etc. are adjusted, or heat treatment and relaxation are performed after stretching, and the heat treatment temperature and the relaxation rate are adjusted at the same time.
[0137] In the following, each step will be described in more detail.
[0138] First, a copolymer polyester resin is prepared. The details of the copolymer polyester resin are as described above.
[0139] Specifically, the polymerization of the copolyester resin may be performed by a conventional transesterification reaction and polycondensation reaction. In this case, the diol and dicarboxylic acid components used and their contents are as exemplified above.
[0140] Thereafter, a homopolyethylene terephthalate (HOMO-PET) resin is optionally added to the copolyester resin, which is melt-extruded at a temperature of 250° C. to 300° C. to prepare an unstretched sheet.
[0141] Specifically, the copolyester resin or the copolyester resin to which the homopolyethylene terephthalate (HOMO-PET) resin has been added is melt-extruded through a T-die at a temperature of 250° C. to 300° C. or 260° C. to 300° C., and then cooled to prepare an unstretched sheet. The details of the homopolyethylene terephthalate (HOMO-PET) resin are as described above.
[0142] The unstretched sheet is passed through the chamber to be preheated while being conveyed at a speed of 10 to 110 m / min, 25 to 90 m / min, 40 to 80 m / min, or 50 to 60 m / min.
[0143] Preheating may be performed at 100 to 120° C. for 0.01 to 1 minute. For example, the preheating temperature may be 100 to 120° C. or 100 to 117° C., and the preheating time may be 0.05 to 0.5 minutes or 0.05 to 0.2 minutes.
[0144] Thereafter, the preheated unstretched sheet is stretched at a temperature of 70 to 95° C. For example, the stretching may be performed at 70 to 95° C., 75 to 95° C., or 80 to 90° C.
[0145] Specifically, the stretching may be uniaxial stretching or biaxial stretching. More specifically, the stretching may be uniaxial stretching performed in the transverse direction (TD), or biaxial stretching performed in the longitudinal direction (MD) and then in the transverse direction (TD).
[0146] If the stretching is uniaxial stretching, the stretching may be performed at a stretching ratio of 3.5 to 5 times, 3.5 to 4.8 times, or 3.8 to 4.6 times in the transverse direction (TD). In addition, if the stretching is biaxial stretching, the stretching may be performed at a stretching ratio of 1.1 to 2 times or 1.1 to 1.5 times in the longitudinal direction (MD), and then at a stretching ratio of 3.5 to 5 times, 3.5 to 4.8 times, or 3.8 to 4.6 times in the transverse direction (TD).
[0147] In addition, a coating step may be further performed after stretching. Specifically, a coating step may be further performed before uniaxial stretching in the transverse direction (TD) or after stretching in the longitudinal direction and before stretching in the transverse direction. More specifically, a coating step may be further performed to form a promotion layer that can impart functions such as antistatic to the film. The coating step may be performed by spin coating or in-line coating, but is not limited thereto.
[0148] Thereafter, the stretched sheet was heat-set at a temperature of 70° C. to 100° C. to prepare a polyester film.
[0149] Heat setting may be annealing and is performed at a temperature of 70° C. to 100° C. or 70° C. to 95° C. for 0.01 minute to 1 minute or 0.05 minute to 0.5 minute.
[0150] Process for recycling polyethylene terephthalate containers
[0151] According to yet another embodiment, a method for recycling a polyethylene terephthalate container is provided, which includes providing a polyethylene terephthalate (PET) container having a polyester film; crushing the polyethylene terephthalate (PET) container having the polyester film to obtain flakes; and heat-treating the flakes to produce recycled polyester chips, wherein a blocking rate of the flakes is 10% or less, and the flakes include first flakes obtained by crushing the polyethylene terephthalate (PET) container and second flakes obtained by crushing the polyester film.
[0152] In order to recycle the polyethylene terephthalate (PET) container according to the embodiment, at least a portion of the PET container is prepared. Polyethylene terephthalate (PET) container surrounded by polyester film.
[0153] Commonly used methods include washing recycled waste products, where containers, metals, glass, and plastics can be mixed to sort polyester containers and remove the film that wraps the containers, etc., in order to improve the recyclability and quality of the containers. The removal step has been carried out by mechanically tearing or cutting the film or by additional steps such as liquid specific gravity separation, dehydration, drying, wind specific gravity separation, or granulation.
[0154] However, it is difficult to completely remove the film in the above-mentioned removal step. In particular, due to the residual ink that has been formed on the film, it is difficult to improve the quality of the recycled polyester chips produced therefrom.
[0155] In the method for recycling a polyester container according to an embodiment, recycled polyester chips can be produced without an additional step of removing a film surrounding a polyethylene terephthalate (PET) container, thereby saving costs.
[0156] In a polyethylene terephthalate (PET) container, a polyester film is provided on the outer surface of the container. Specifically, the outer surface of the polyethylene terephthalate container is covered with a polyester film, and the film can be shrunk by steam or hot air to surround at least a portion of the outer surface of the polyethylene terephthalate container. For example, the polyester film as a heat shrinkable film can be a label of the polyethylene terephthalate container, but is not limited thereto.
[0157] The details about the polyester film are as described above.
[0158] Thereafter, the polyethylene terephthalate (PET) container having the film was broken to obtain flakes.
[0159] Specifically, at least a portion of an outer surface of a polyethylene terephthalate (PET) container is surrounded by a film, and the container and the film are broken together to obtain flakes without requiring a step of separating the container and the film.
[0160] That is, the flakes include first flakes obtained by breaking a polyester container and second flakes obtained by breaking a film.
[0161] The particle size of the first flake may be 0.1 mm to 25 mm, and the particle size of the second flake may be 0.1 mm to 25 mm. For example, the particle size of the first flake may be 0.3 mm to 23 mm, 0.5 mm to 20 mm, 1 mm to 20 mm, 0.5 mm to 15 mm, 0.5 mm to 13 mm, 1 mm to 18 mm, 1 mm to 15 mm, 1 mm to 13 mm, or 2 mm to 10 mm, and the particle size of the second flake may be 0.3 mm to 23 mm, 0.5 mm to 20 mm, 1 mm to 20 mm, 0.5 mm to 15 mm, 0.5 mm to 13 mm, 1 mm to 18 mm, 1 mm to 15 mm, 1 mm to 13 mm, or 2 mm to 10 mm, but they are not limited thereto.
[0162] Thereafter, a step of washing the crushed flakes may be further performed before the heat treatment step. Specifically, the washing step may be performed at a temperature of 85°C to 90°C using a washing solution containing water and / or an aqueous solution of 1 part by weight of sodium hydroxide.
[0163] For example, the broken flakes may be washed with water for the first time, washed with a washing solution for the second time, and then washed with water for the third time. When the washing step is performed, impurities that may remain in the broken flakes can be removed, and ink components can be effectively removed. Therefore, the quality and purity of the recycled polyester chips produced thereby can be improved, thereby maximizing recyclability.
[0164] In addition, after the washing step, a step of drying the washed sheet at 60° C. to 175° C. for 10 to 90 minutes may be further performed. For example, the drying step may be performed at 65° C. to 175° C., 70° C. to 170° C., 90° C. to 165° C., 100° C. to 165° C., or 120° C. to 165° C., 140° C. to 165° C., or 150° C. to 165° C. for 10 to 85 minutes, 10 to 70 minutes, or 15 to 30 minutes.
[0165] The washing and drying steps may be repeated one to five times. For example, impurities remaining in the sheet may be effectively removed by sequentially repeating the washing and drying steps two to five times or three to five times.
[0166] Finally, the flakes are heat treated to produce recycled polyester chips.
[0167] Specifically, the flakes include a first flake obtained by crushing a polyethylene terephthalate (PET) container and a second flake obtained by crushing a polyester film.
[0168] The heat treatment may be performed at 200° C. to 220° C. for 60 to 120 minutes. For example, the heat treatment may be performed at 200° C. to 215° C. or 205° C. to 220° C. for 70 to 120 minutes or 80 to 120 minutes.
[0169] In addition, the agglomeration rate of the flakes is 10% or less. Specifically, when the flakes are subjected to a pressure of 8.7 kPa and heat-treated at a temperature of 210° C. for 90 minutes, the agglomeration rate may be 10% or less. For example, when the flakes are subjected to a pressure of 8.7 kPa and heat-treated at 210° C. for 90 minutes, the agglomeration rate may be 9% or less, 8.5% or less, 8% or less, 6% or less, 5% or less, 4% or less, preferably 3% or less, 2% or less, 1.5% or less, 1% or less, 0.8% or less, 0.5% or less.
[0170] Since the agglomeration score that may be caused by the entanglement of the first sheet and the second sheet is low, the quality of the prepared recycled polyester chips is excellent. Specifically, since the sheet includes the second sheet obtained by crushing the polyester film according to the embodiment, the formation of aggregates can be effectively reduced or prevented, thereby improving the quality of the recycled polyester chips produced thereby.
[0171] The recycled polyester chips can be obtained after the heat treatment step. Specifically, the recycled polyester chips comprising the first sheet and the second sheet can be obtained after the heat treatment step. For example, the sheets can be melt-extruded and cut to obtain the recycled polyester chips, but is not limited thereto.
[0172] Recycled polyester chips
[0173] According to yet another embodiment, a recycled polyester chip produced by a method for recycling a polyethylene terephthalate container is provided.
[0174] Specifically, the recycled polyester chip may include a first sheet including polyethylene terephthalate (PET) and a second sheet including a polyester resin.
[0175] The recycled polyester chips may have an intrinsic viscosity (IV) of 0.55 dl / g or more. For example, the recycled polyester chips may have an intrinsic viscosity (IV) of 0.58 dl / g or more, or 0.59 dl / g or more, 0.55 dl / g to 3.0 dl / g, 0.55 dl / g to 2.0 dl / g, 0.55 dl / g to 1.0 dl / g, 0.58 dl / g to 0.85 dl / g, or 0.58 dl / g to 0.7 dl / g.
[0176] In addition, the recycled polyester chips may include polyethylene terephthalate in an amount of 70 to 99 wt % and copolyester resin in an amount of 1 to 30 wt % based on the total weight of the recycled polyester chips. For example, the recycled polyester chips may include polyethylene terephthalate in an amount of 80 to 99 wt %, 90 to 99 wt %, or 95 to 99 wt % and copolyester resin in an amount of 1 to 20 wt %, 1 to 10 wt %, or 1 to 5 wt % based on the total weight of the recycled polyester chips. DETAILED DESCRIPTION
[0177] Hereinafter, the present invention will be described in more detail with reference to the following examples. However, these examples are set forth to illustrate the present invention, and the scope of the present invention is not limited thereto.
[0178] [Example]
[0179] Preparation of polyester film
[0180] Example 1-1
[0181] (1) Preparation of copolyester resin
[0182] An autoclave (or first reactor) equipped with a stirrer and a distillation column was charged with 100 mol % of terephthalic acid (TPA) as dicarboxylic acid and 75.6 mol % of ethylene glycol (EG), 18.8 mol % of neopentyl glycol (NPG), and 5.6 mol % of diethylene glycol (DEG) as diols. 0.07 parts by weight of manganese acetate was added as an ester exchange catalyst per 100 parts by weight of the dicarboxylic acid, and then the mixture was heated to 220° C. and methanol produced as a by-product was removed to perform a reaction.
[0183] When the transesterification reaction is completed, 0.07 parts by weight of silicon dioxide having an average particle diameter of 0.28 μm is added per 100 parts by weight of dicarboxylic acid, and 0.4 parts by weight of trimethyl phosphate is added as a stabilizer. After 5 minutes, 0.035 parts by weight of antimony trioxide and 0.005 parts by weight of tetrabutyl titanate are added as polymerization catalysts, followed by stirring for 10 minutes. Thereafter, the reaction mixture is transferred to a second reactor equipped with a vacuum device. The pressure is gradually reduced while the temperature is raised to 285° C., and the polymerization is carried out for 210 minutes to prepare a copolyester resin.
[0184] (2) Membrane preparation
[0185] 90 parts by weight of the copolyester resin prepared in step (1) and 10 parts by weight of a homopolyethylene terephthalate (HOMO-PET) resin (CTF41, manufacturer: SKC Co., Ltd.) (i.e., 10% by weight based on a total of 100 parts by weight of the copolyester resin and the homopolyethylene terephthalate (HOMO-PET) resin) were mixed and extruded through a T-die at 280° C., which was cooled to obtain an unstretched sheet.
[0186] Thereafter, the unstretched sheet was passed through a roller while being conveyed at a speed of 55 m / min, thereby adjusting its thickness. The unstretched sheet was preheated at 105° C. for 0.1 minute while being conveyed at a speed of 55 m / min and stretched 4.15 times in the transverse direction (TD) at 83° C. Thereafter, the stretched sheet was heat-set at 75° C. for 0.1 minute to prepare a polyester film having a thickness of 40 μm.
[0187] Examples 1-2 to 1-9 and Comparative Examples 1-1 to 1-9
[0188] A polyester film was prepared in the same manner as in Example 1-1, except that the contents of dicarboxylic acid and diol, the content of homopolyethylene terephthalate, and process conditions were changed as shown in Table 1 below.
[0189] The final components of the polyester films prepared in Examples 1-1 to 1-9 and Comparative Examples 1-1 to 1-9 are shown in Table 2 below.
[0190] [Table 1]
[0191]
[0192]
[0193] [Table 2]
[0194]
[0195]
[0196] *NPG: Neopentyl Glycol
[0197] *CHDM: 1,4-cyclohexanedimethanol
[0198] *DEG: Diethylene glycol
[0199] Test Example 1-1: Melting Enthalpy (ΔHm)
[0200] 4 mg of samples of the polyester films prepared in Examples 1-1 to 1-9 and Comparative Examples 1-1 to 1-9 were scanned using a differential scanning calorimeter (Q2000, manufacturer: TA Instruments) in a differential scanning calorimeter (DSC) mode at a heating rate of 10° C. / min.
[0201] In the heat flow curve obtained by scanning, the first endothermic temperature is the glass transition temperature (Tg), the exothermic temperature measured after the glass transition temperature (Tg) is the crystallization temperature (Tc), and the endothermic temperature measured after the crystallization temperature (Tc) is the melting point (Tm). Here, the integral value at the melting point (Tm) is calculated as the melting enthalpy. Specifically, the melting enthalpy is the energy in the interval where the endothermic occurs in the heat flow curve of the differential scanning calorimeter. The trend line from the melting start temperature to the melting completion temperature is set as the baseline, and the integral value of the peak along the baseline is converted and calculated.
[0202] Figure 5 Differential Scanning Calorimetry (DSC) curves of the polyester films of Examples 1-3 are shown.
[0203] Test Example 1-2: Melting Point (Tm)
[0204] 4 mg of samples of the polyester films prepared in Examples 1-1 to 1-9 and Comparative Examples 1-1 to 1-9 were scanned using a differential scanning calorimeter (Q2000, manufacturer: TA Instruments) in a differential scanning calorimeter (DSC) mode at a heating rate of 10° C. / min.
[0205] In the heat flow curve obtained by scanning, the first endothermic temperature is the glass transition temperature (Tg), the exothermic temperature measured after the glass transition temperature (Tg) is the crystallization temperature (Tc), and the endothermic temperature measured after the crystallization temperature (Tc) is the melting point (Tm) (see Figure 5 ).
[0206] Test Example 1-3: Peel Strength
[0207] Figure 3 A method for measuring the peel strength of a polyester film is shown. That is, Figure 3 A method for testing the seam properties of polyester films such as solvent bond strength is shown.
[0208] Specifically, first, two sample sheets (ie, a first polyester film and a second polyester film) of the polyester films of Examples 1-1 to 1-9 and Comparative Examples 1-1 to 1-9 were each prepared in A4 size.
[0209] Thereafter, when 1,3-dioxolane was applied to one side of the first polyester film (100) in the form of a tape having a width of 2 mm and a length of 30 mm to form an adhesive portion (110), a second polyester film (200) was laminated on the first polyester film on which the adhesive portion had been formed (see Figure 3 (a)). Here, the adhesive portion (110) is formed at a position 6.5 cm (w) away from the upper end of the first polyester film (100). In addition, the area of the adhesive portion (110) is 60 mm 2 .
[0210] Thereafter, in order to prevent the laminated first polyester film and the second polyester film from bending, a press plate (120) was placed on the second polyester film. Thereafter, a 2 kg weight (130) was placed on the press plate (120) and aged for 1 hour (see Figure 3 (b)). Here, a weight (130) is placed at the location of the adhesive portion (110).
[0211] Thereafter, the weight (130) and the press plate (120) were removed, and the laminated first polyester film and the second polyester film were cut into a width of 3 cm and a length of 9 cm to obtain a sample A (300) (see Figure 3 (c)).
[0212] Thereafter, when the first polyester film (100) and the second polyester film (200) in the sample (300) were peeled off at a speed of 300 mm / min and an angle of 180°, the maximum force was measured as the peel strength (see Figure 3 (d)).
[0213] The test described above was performed 5 times, and the average value is shown in Table 3 below.
[0214] Test Example 1-4: Thermal Shrinkage
[0215] Figure 4 A method for measuring the thermal shrinkage of polyester films is shown. Figure 4 The polyester films (100) prepared in Examples 1-1 to 1-9 and Comparative Examples 1-1 to 1-9 were each cut to 300 mm in the direction to be measured and to 15 mm in the direction perpendicular thereto. Here, the first dimension (x1) before shrinkage was 300 mm, and the second dimension (y) was 15 mm (see Figure 4 (a)).
[0216] The cut polyester film (100) is immersed in a heated water bath, and the shrinkage dimension of the polyester film (100a) after shrinkage, that is, the first dimension (x2) after shrinkage is measured (see Figure 4(b)), and calculated according to the following Equation 2. In this test example, the heat shrinkage ratio (%) was obtained in the main shrinkage direction (TD) of the film and in the direction perpendicular thereto (MD).
[0217] [Equation 2]
[0218]
[0219] [Table 3]
[0220]
[0221]
[0222] [Table 4]
[0223]
[0224]
[0225] As shown in Tables 3 and 4, in the polyester films of Examples 1-1 to 1-9, the melting enthalpy, the melting point, the peel strength, and the heat shrinkage rate with respect to the temperature fall within the preferred ranges.
[0226] Specifically, since the polyester films of Examples 1-1 to 1-9 meet the preferred range of adhesive strength after the seaming process, they are suitable for use as heat shrinkable films. In addition, since the melting enthalpy, melting point, and peel strength of the polyester films of Examples 1-1 to 1-9 are adjusted to the above ranges, the agglomeration rate is very low in the recycling method of the film or the polyethylene terephthalate (PET) container containing the film. Therefore, environmental pollution can be prevented while improving recyclability.
[0227] Preparation of recycled polyester chips
[0228] Example 2-1
[0229] (1) Preparation of polyethylene terephthalate container with polyester film
[0230] Figure 1 Shown is a polyester film applied to a product before and after heat shrinking the polyester film. Figure 1 A portion of the outer surface of a polyethylene terephthalate container (PET container, 30 g) was wrapped with the polyester film prepared in Example 1-1 (see Figure 1 (a)). In this case, an acrylic adhesive was used to fix it. Thereafter, the polyester film of Example 1-1 was shrunk under hot air conditions at a temperature of 90° C. to obtain a polyethylene terephthalate container having a polyester film (see Figure 1 (b)).
[0231] (2) Method for recycling polyethylene terephthalate containers
[0232] The container with the polyester film prepared in step (1) is crushed with a crusher to obtain flakes. The flakes are first washed with water. Thereafter, the flakes are washed for a second time for 15 minutes with a washing solution (a mixture of a solution of 0.3 wt % Triton X-100 and a solution of 1.0 wt % NaOH) stirred in a bath at 88°C and 880 rpm. Thereafter, the flakes washed for the second time are washed for a third time with water at room temperature to remove the residual washing solution, and dried at 160°C for 20 minutes. Thereafter, they are heat-treated at 210°C for 90 minutes to produce recycled polyester chips.
[0233] Examples 2-2 to 2-9 and Comparative Examples 2-1 to 2-9
[0234] Recycled polyester chips were prepared in the same manner as in Example 2-1, except that the polyester films of Examples 1-2 to 1-9 and Comparative Examples 1-1 to 1-9 were each used instead of the polyester film of Example 1-1.
[0235] Test Example 2-1: Agglomeration Rate
[0236] The blocking rate (%) was measured according to the American Association of Plastics Recyclers' procedure for evaluating the blocking of polyethylene terephthalate sheets (APR PET-S-08).
[0237] Figure 2 A method for measuring the blocking of polyethylene terephthalate (PET) containers with polyester film is shown.
[0238] Specifically, a product (1) in which a polyester film as a label (11a) is provided in a polyethylene terephthalate (PET) container (20) is crushed in a crusher (6) and passed through a screen having a hole diameter of 9.5 mm (0.374" screen, not shown) to obtain a mixed sheet consisting of 97 g of a first sheet (20a) obtained by crushing polyethylene terephthalate (PET) and 3 g of a second sheet (10a) obtained by crushing a polyester film. In this case, the polyester containers of Examples 2-1 to 2-9 and Comparative Examples 2-1 to 2-9 prepared as above were used as the product (1) (see Figure 1 and 2 (a)).
[0239] Thereafter, the mixed flakes were placed on a cylinder having a diameter of 6 cm and a height of 8 cm, and a compression weight (7) of 8.7 kg was placed thereon to apply a load. Thereafter, the cylinder with the weight thereon was heat-treated in a convection oven at 210° C. for 90 minutes, and then cooled at room temperature (see Figure 2 (b)).
[0240] Thereafter, the cooled mixed flakes were placed on a second sieve (8; 0.625" sieve) having a hole diameter (d) of 11.2 mm and filtered, and the aggregated mixed flakes (10b) remaining on the second sieve (8) were collected and weighed (see Figure 2 (c)). The weight of the mixed flakes was measured and calculated according to the following equation 1.
[0241] [Equation 1]
[0242]
[0243] [Table 5]
[0244]
[0245]
[0246] As shown in Table 5, since the recycled polyester chips of Examples 2-1 to 2-9 have a very low blocking rate, they are advantageous for a recycling process at a high temperature for a long period of time, thereby improving recyclability.
[0247] Specifically, as shown in Table 3, the recycled polyester chips of Examples 2-1 to 2-9 have a low blocking rate due to the use of a polyester film that satisfies a specific range of melting enthalpy, melting point, and peel strength and has excellent mechanical properties, in particular, a polyester film containing a homopolymer polyethylene terephthalate (HOMO-PET) resin at a specific content.
[0248] On the contrary, the recycled polyester chips of Comparative Examples 2-1 to 2-4, 2-8, and 2-9 have very high blocking rates, thereby deteriorating recyclability. Meanwhile, although the recycled polyester chips of Comparative Examples 2-5 to 2-7 have low blocking rates, the thermal properties and seam properties of the polyester film are poor, as shown in Table 3, and thus are difficult to apply to various products.
Claims
1. A polyester film comprising a copolyester resin in which a diol and a dicarboxylic acid are copolymerized, and comprising a homopolyethylene terephthalate resin, wherein the melting enthalpy as measured by differential scanning calorimetry is 9 J / g or more, and the blocking rate is 10% or less; It contains the homopolyethylene terephthalate resin in an amount of 0.5 wt % to 37 wt % based on the total weight of the copolyester resin and the homopolyethylene terephthalate resin; The copolyester resin is a copolyester resin in which two or three or more diols and dicarboxylic acid are polymerized; the diol comprises ethylene glycol and at least one comonomer selected from the group consisting of neopentyl glycol and diethylene glycol; and the dicarboxylic acid comprises terephthalic acid. 2 . The polyester film according to claim 1 , which has a peel strength of 150 gf / 3 cm or more. 3 . The polyester film of claim 1 , having a melting point of 190° C. to 230° C. as measured by differential scanning calorimetry. 4 . The polyester film according to claim 1 , which has a heat shrinkage of 45% to 85% in the first direction when heat-treated at a temperature of 100° C. for 10 seconds. 5 . The polyester film according to claim 1 , which has a heat shrinkage of 7% or less in a second direction perpendicular to the first direction when heat-treated at a temperature of 100° C. for 10 seconds. 6 . The polyester film of claim 1 , wherein the diol comprises at least one comonomer selected from the group consisting of neopentyl glycol and diethylene glycol in an amount of 10 mol % or more. 7 . The polyester film of claim 1 , comprising neopentyl glycol in an amount of 5 to 35 mol % and diethylene glycol in an amount of 1 to 10 mol %.
8. A method for preparing a polyester film, comprising: preparing a copolyester resin in which a diol and a dicarboxylic acid are copolymerized; adding a homopolymer polyethylene terephthalate resin to the copolyester resin, and then melt-extruding the resin at a temperature of 250° C. to 300° C. to prepare an unstretched sheet; as well as The unstretched sheet is stretched, and then heat-set at a temperature of 70° C. to 100° C. to prepare a polyester film, wherein the melting enthalpy of the polyester film as measured by differential scanning calorimetry is 9 J / g or more, and the blocking rate of the polyester film is 10% or less; It contains the homopolyethylene terephthalate resin in an amount of 0.5 wt % to 37 wt % based on the total weight of the copolyester resin and the homopolyethylene terephthalate resin; The copolyester resin is a copolyester resin in which two or three or more diols and dicarboxylic acid are polymerized; the diol comprises ethylene glycol and at least one comonomer selected from the group consisting of neopentyl glycol and diethylene glycol; and the dicarboxylic acid comprises terephthalic acid.
9. A method for regenerating a polyethylene terephthalate container, comprising: Providing a polyethylene terephthalate container having the polyester film according to claim 1; breaking the polyethylene terephthalate container having the polyester film to obtain flakes; and heat treating the flakes to produce recycled polyester chips, wherein the blocking rate of the sheet is 10% or less, and the sheet comprises a first sheet obtained by crushing the polyethylene terephthalate container and a second sheet obtained by crushing the polyester film.