A high-activity molded black paste and its preparation method and application
By using highly active formulas and specific processes in the molded black slurry, the blackness and mechanical strength of the molded products are improved, the problem of insufficient carbon black content in the existing technology is solved, and efficient production of molded products is achieved.
Patent Information
- Application Number
- CN202110563058.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-05-24
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2041-05-24
AI Technical Summary
The effective content of carbon black in the existing molded black slurry is not high, resulting in insufficient blackness and mechanical strength of the molded products. Increasing the amount of carbon black will lead to rising costs and a sharp increase in viscosity, affecting the appearance quality and reactivity of the product.
It adopts a highly active molded black paste formula, containing 65 to 80% styrene-free unsaturated resin, 5 to 15% high molecular weight copolymer alkylammonium salt additives and 20 to 30% carbon black. Through specific The mixing and grinding process controls the carbon black particle size to 20-30nm to ensure a high-content and high-viscosity black slurry.
It significantly improves the blackness and brightness of molded products, reduces the agglomeration of carbon black particles and the sharp rise in viscosity, maintains good mechanical strength and appearance quality at high content, and reduces production costs.
Smart Images

Figure BDA0003079795160000111 
Figure BDA0003079795160000121
Abstract
Description
Technical Field
[0001] The invention belongs to the field of molding, and in particular relates to a high-activity molding black slurry and a preparation method and application thereof. Background Art
[0002] The compression molding process uses the characteristics of each stage in the resin curing reaction to achieve product molding, that is, the molding material plasticizes, flows and fills the mold cavity, and the resin solidifies. In the process of the molding material filling the mold cavity, not only the resin flows, but also the reinforcing material flows with it. Therefore, the molding pressure of the compression molding process is higher than other process methods, which belongs to high-pressure molding. There are a considerable number of black products among the molded products, and such products require high brightness and high blackness. Molded black slurry is one of the key raw materials for producing such black and bright molded parts.
[0003] At present, the molded black slurry on the market generally has three problems: low effective content, great influence on the reaction activity of the molded system, and great influence on thickening. In order to have sufficient blackness and hiding power, black molded parts must contain a certain amount of carbon black. In order to achieve blackness and hiding power, the amount of molded black slurry with low effective content must be increased, resulting in the increase of other unnecessary components in the system, resulting in increased product costs and decreased mechanical properties. The brightness of molded parts is closely related to the reaction activity and thickening of the system. The base resin, additives, and carbon black powder in the molded black slurry have a very obvious effect on reaction and thickening.
[0004] Therefore, the present invention applies to study a high-content and high-activity black paste, which can effectively reduce the adverse effects of the black paste on molded products, improve the overall performance of the black paste, improve the appearance quality of the molded products, and simultaneously reduce production costs. Summary of the invention
[0005] 1. Problem to be solved
[0006] In view of the problems in the prior art such as low effective content of carbon black, low activity, and low appearance quality and mechanical strength of the prepared molded products, the present invention provides a high-activity molding black slurry with high effective content, good appearance quality of molded products, high mechanical strength, and a preparation method and application thereof.
[0007] 2. Technical solution
[0008] The first aspect of the present invention provides a high-activity molding black paste, the raw materials of which include the following parts by weight: 65 to 80 parts of base resin, 5 to 15 parts of auxiliary agent, and 20 to 30 parts of carbon black.
[0009] As a preferred solution, the base resin is an unsaturated resin that does not contain styrene.
[0010] As a preferred solution, the raw materials of the base resin include the following parts by weight: 20 to 30 parts of alcohol ether, 10 to 20 parts of dibasic acid, 15 to 25 parts of unsaturated acid anhydride, and 20 to 24 parts of diol.
[0011] As a preferred solution, the weight ratio of the unsaturated acid anhydride to the diol is 3-5:4-5.
[0012] As a preferred solution, the viscosity of the base resin is 600-800 mPa·s.
[0013] As a preferred solution, the auxiliary agent is at least one of the high molecular weight copolymer alkyl ammonium salts.
[0014] As a preferred solution, the weight ratio of the auxiliary agent to carbon black is 1-3:4-6.
[0015] As a preferred solution, the particle size of the carbon black is 20 to 30 nm.
[0016] The second aspect of the present invention provides a method for preparing the above-mentioned high-activity molded black paste, which comprises the following steps: (1) adding a base resin and an additive into a reaction container, and stirring at a speed of 500 to 800 rpm for 10 to 15 minutes; (2) reducing the speed to 100 to 200 rpm and slowly adding a formulated amount of carbon black in batches. After the feeding is completed, increasing the speed to 500 to 800 rpm and stirring for 30 to 60 minutes; (3) after the stirring is completed, putting the color paste into a three-roll grinder and grinding it for 3 to 5 times to obtain the color paste.
[0017] The third aspect of the present invention provides an application of the above-mentioned high-activity molding black paste, including the application of the high-activity molding black paste in the preparation of black molded products.
[0018] 3. Beneficial effects
[0019] Compared with the prior art, the present invention has the following beneficial effects:
[0020] 1. The present invention applies the use of specific carbon black to add to the preparation process of black paste. Through the effective absorption and light scattering of visible light by carbon black particles, the covering degree of carbon black in the black paste product is effectively improved, thereby significantly improving the blackness and brightness of the molded product.
[0021] 2. The present invention adopts high molecular weight copolymer alkyl ammonium salt to add to the black paste, which solves the agglomeration and reduced covering degree caused by the addition of a large amount of carbon black particles, and at the same time greatly reduces the sharp increase in the viscosity of the color paste caused by the addition of a large amount of carbon black, so that the black paste still has good blackness and mechanical strength of the mold product when it has a high content.
[0022] 3. The present invention uses a self-made styrene-free unsaturated resin as the base resin and limits the viscosity of the base resin, thereby further increasing the content of carbon black. The effective content of the black paste reaches up to 30wt%, and the viscosity of the black paste can be controlled within the range of 6000 to 8000mPa·s, which has good applicability to the SMC process. DETAILED DESCRIPTION
[0023] The content of the present invention can be more easily understood by selecting the following detailed description of the preferred implementation method of the present invention and the embodiments included. Unless otherwise specified, all technical and scientific terms used herein have the same meanings as those of ordinary skill in the art to which the present invention belongs. When there is a conflict, the definition in this specification shall prevail.
[0024] As used herein, the term "prepared from" is synonymous with "comprising." As used herein, the terms "comprising," "including," "having," "containing," or any other variation thereof, are intended to cover a non-exclusive inclusion. For example, a composition, process, method, article, or apparatus that comprises the listed elements is not necessarily limited to only those elements but may include other elements not expressly listed or inherent to such composition, process, method, article, or apparatus.
[0025] When amount, concentration or other value or parameter is expressed as range, preferred range or a series of upper preferred value and lower preferred value limit range, this should be understood as specifically disclosing all ranges formed by any pairing of any range upper limit or preferred value and any range lower limit or preferred value, regardless of whether the range is disclosed separately. For example, when disclosing range "1 to 5", described range should be interpreted as including range "1 to 4", "1 to 3", "1 to 2", "1 to 2 and 4 to 5", "1 to 3 and 5" etc. When numerical range is described in this article, unless otherwise stated, the range is intended to include its end value and all integers and fractions within the range.
[0026] Approximate terms in the specification and claims are used to modify quantities, indicating that the present invention is not limited to the specific quantity, but also includes acceptable and modified parts close to the quantity without causing changes in the relevant basic functions. Accordingly, the use of "about", "approximately", etc. to modify a numerical value means that the present invention is not limited to the exact numerical value. In some examples, the approximate terms may correspond to the accuracy of the instrument for measuring the numerical value. In the specification and claims of this application, range limitations can be combined and / or interchanged, and if not otherwise stated, these ranges include all subranges contained therein.
[0027] In addition, the indefinite articles "a" and "an" before the elements or components of the present invention have no restrictions on the quantity requirements (i.e. the number of occurrences) of the elements or components. Therefore, "a" or "an" should be interpreted as including one or at least one, and the elements or components in the singular form also include the plural form, unless the number is obviously intended to be in the singular form.
[0028] The first aspect of the present invention provides a high-activity molding black paste, the raw materials of which include the following parts by weight: 65 to 80 parts of base resin, 5 to 15 parts of auxiliary agent, and 20 to 30 parts of carbon black.
[0029] In some preferred embodiments, the base resin is an unsaturated resin that does not contain styrene.
[0030] In some preferred embodiments, the raw materials of the base resin include the following parts by weight: 20 to 30 parts of alcohol ether, 10 to 20 parts of dibasic acid, 15 to 25 parts of unsaturated acid anhydride, and 20 to 24 parts of diol.
[0031] In some preferred embodiments, the preparation method of the matrix resin comprises the following steps: (1) weighing alcohol ether, dibasic acid, unsaturated acid anhydride and diol into a reaction kettle; (2) rapidly heating to 90°C under nitrogen protection, rapidly heating to 150°C after heat release, and then heating to 210°C at a rate of 2°C per 10 minutes; (3) after heating, continue to introduce nitrogen, stir the reaction until the acid value is less than 10, and then cool down and stop.
[0032] In some preferred embodiments, the weight ratio of the unsaturated acid anhydride to the diol is 3-5:4-5.
[0033] The applicant uses an unsaturated resin that does not contain styrene to effectively control the viscosity of the color paste product within the range of 6000 to 8000 mPa·s, thereby effectively ensuring the good SMC thickening applicability of the color paste product. The applicant speculates that when an unsaturated resin that does not contain styrene is used, and the weight ratio of unsaturated anhydride to diol is 3 to 5:4 to 5, the diol can be inserted and added into the polyester chain segment formed with the unsaturated anhydride, effectively improving the steric hindrance of the polyester main chain, thereby effectively reducing the reactivity of the unsaturated anhydride in the polyester chain, avoiding excessive cross-linking after the addition of alcohol ether due to the high reactivity of both, and no styrene is added during the preparation of the unsaturated resin, controlling the overall cross-linking degree of the unsaturated resin, and controlling the viscosity of the synthesized unsaturated resin within the applicable range, thereby ensuring that when the carbon black content is at most 30wt%, the viscosity of the high-activity molded black paste is maintained within the range of 6000 to 8000 mPa·s, retaining good SMC thickening applicability.
[0034] In some preferred embodiments, the viscosity of the base resin is 600-800 mPa·s.
[0035] In some preferred embodiments, the alcohol ether is at least one of propylene glycol butyl ether and ethylene glycol butyl ether.
[0036] In some preferred embodiments, the dibasic acid is at least one of isophthalic acid, succinic acid, glutaric acid, adipic acid, and sebacic acid.
[0037] In some preferred embodiments, the unsaturated acid anhydride is at least one of maleic anhydride and fumaric anhydride.
[0038] In some preferred embodiments, the diol is at least one of pentanediol, butanediol, and propylene glycol.
[0039] In some preferred embodiments, the auxiliary agent is at least one of high molecular weight copolymer alkyl ammonium salts.
[0040] In some preferred embodiments, the auxiliary agent is a high molecular weight copolymer alkyl ammonium salt product of model Byk9076 produced and sold by BYK.
[0041] In some preferred embodiments, the weight ratio of the auxiliary agent to carbon black is 1-3:4-6.
[0042] As the carbon black content increases further, carbon black is prone to agglomeration, and as the carbon black content increases, the pores between the carbon black particles also increase further, which will greatly affect the covering degree of carbon black in the resin and cause the viscosity of the product to rise sharply. The applicant has found that when a high molecular weight copolymer alkyl ammonium salt is used as an auxiliary agent, the blackness of the color paste can be effectively improved, and the effect of the increase in carbon black content on the viscosity can be reduced. The applicant of the present invention speculates that: when a high molecular weight copolymer alkyl ammonium salt is used as an auxiliary agent, and the weight ratio to carbon black is 1 to 3: 4 to 6, the fine side chains in the high molecular weight copolymer alkyl ammonium salt can be effectively inserted into the structural pores of carbon black, enhancing the wetting effect of carbon black particles in the matrix resin and reducing the agglomeration of carbon black ions; on the other hand, the lipophilic groups on the high molecular weight copolymer alkyl ammonium salt can effectively improve the fluidity of the carbon black particles infiltrated on the high molecular weight copolymer alkyl ammonium salt in the matrix resin, thereby reducing the shear stress of the color paste product and reducing the effect of carbon black particles on the viscosity of the product.
[0043] In some preferred embodiments, the particle size of the carbon black is 20 to 30 nm.
[0044] In some preferred embodiments, the specific surface area of the carbon black is 80 to 90 m 2 / g.
[0045] The applicant has found that when adding particles with a diameter of 20 to 30 nm and a specific surface area of 80 to 90 m 2 / g of carbon black can significantly improve the blackness of the color paste product and the mechanical strength of the molded product after curing. The applicant speculates that: when the particle size of carbon black is 20-30nm, and the specific surface area is 80-90m2 / g, the same amount of carbon black added has more structural pores. In addition, the low-dimensional structure of carbon black can effectively enhance the absorption wavelength range of carbon black for visible light in the color paste product, enhance the light absorption performance, and improve the scattering performance of visible light, thereby significantly improving the covering degree of carbon black in the color paste product; when the particle size of carbon black is less than 20nm, as the pores between the carbon black particles themselves and the particles increase significantly, the pores The large amount of air in the air gap is difficult to be completely discharged quickly and effectively, and requires a stronger wetting effect, which greatly affects the dispersion of carbon black in the color paste product, and the covering degree is reduced accordingly. When the particle size is greater than 30nm, the blackness of the product will be reduced; and when the particle size of carbon black is 20-30nm, the active surface and active atomic center of carbon black can form a filamentous structure with the matrix resin molecular chain. When impacted or subjected to external force, the generated microscopic cracks can be converted into a silver streak state, delaying the rupture of the cured material, thereby significantly improving the mechanical strength of the molded product.
[0046] In some preferred embodiments, the content of carbon black is 20-30 wt %.
[0047] In some preferred embodiments, the carbon black is a carbon black product of model Cabot E4115 produced and sold by Cabot Corporation.
[0048] In some preferred embodiments, the viscosity of the high-activity molding black slurry is 6000-8000 mPa·s.
[0049] In some preferred embodiments, the thixotropy of the high-activity molding black paste is 1.1 to 1.4.
[0050] In some preferred embodiments, the fineness of the high-activity molded black slurry is 5 to 15 microns.
[0051] The second aspect of the present invention provides a method for preparing the above-mentioned high-activity molded black paste, which comprises the following steps: (1) adding a base resin and an additive into a reaction container, and stirring at a speed of 500 to 800 rpm for 10 to 15 minutes; (2) reducing the speed to 100 to 200 rpm and slowly adding a formulated amount of carbon black in batches. After the feeding is completed, increasing the speed to 500 to 800 rpm and stirring for 30 to 60 minutes; (3) after the stirring is completed, putting the color paste into a three-roll grinder and grinding it for 3 to 5 times to obtain the color paste.
[0052] The third aspect of the present invention provides an application of the above-mentioned high-activity molding black paste, including the application of the high-activity molding black paste in the preparation of black molded products.
[0053] Example
[0054] The technical solution of the present invention is described in detail below by way of examples, but the protection scope of the present invention is not limited to all the examples described. Unless otherwise specified, the raw materials of the present invention are all commercially available.
[0055] Example 1
[0056] Embodiment 1 provides a high-activity molding black paste in the first aspect, the raw materials comprising the following parts by weight: 70 parts of unsaturated resin without styrene, 10 parts of high molecular weight copolymer alkyl ammonium salt, and 25 parts of carbon black.
[0057] In this embodiment, the raw materials of the unsaturated resin not containing styrene include the following parts by weight: 25 parts of propylene glycol butyl ether, 15 parts of adipic acid, 20 parts of maleic anhydride, and 22 parts of propylene glycol.
[0058] In this embodiment, the unsaturated resin not containing styrene is homemade, and the steps include the following: (1) weighing propylene glycol butyl ether, adipic acid, maleic anhydride, and propylene glycol into a reaction kettle; (2) rapidly heating to 90°C under nitrogen protection, rapidly heating to 150°C after heat release, and then heating to 210°C at a rate of 2°C per 10 minutes; (3) after heating, continue to introduce nitrogen, stir the reaction until the acid value is less than 10, and then cool down and stop.
[0059] In this embodiment, the viscosity of the matrix resin is 700 mPa·s.
[0060] In this embodiment, the high molecular weight copolymer alkyl ammonium salt is a high molecular weight copolymer alkyl ammonium salt product of model Byk9076 produced and sold by BYK.
[0061] In this embodiment, the particle size of the carbon black is 25 nm.
[0062] In this embodiment, the specific surface area of the carbon black is 85m 2 / g.
[0063] In this embodiment, the carbon black is a carbon black product of model Cabot E4115 produced and sold by Cabot Corporation.
[0064] Example 2
[0065] The specific implementation of this embodiment is the same as that of Embodiment 1, except that the particle size of the carbon black is 30 nm.
[0066] Example 3
[0067] The specific implementation of this embodiment is the same as that of Embodiment 1, except that: the amount of the high molecular weight copolymer alkyl ammonium salt is 15 parts.
[0068] Comparative Example 1
[0069] The specific implementation of this comparative example is the same as that of Example 1, except that the particle size of the carbon black is 50 nm.
[0070] Comparative Example 2
[0071] The specific implementation of this comparative example is the same as that of Example 1, except that the particle size of the carbon black is 15 nm.
[0072] Comparative Example 3
[0073] The specific implementation of this comparative example is the same as that of Example 1, except that: the amount of the high molecular weight copolymer alkyl ammonium salt is 2 parts.
[0074] Comparative Example 4
[0075] The specific implementation of this comparative example is the same as that of Example 1, except that: the amount of the high molecular weight copolymer alkyl ammonium salt is 25 parts.
[0076] Comparative Example 5
[0077] The specific implementation of this comparative example is the same as that of Example 1, except that: the amount of maleic anhydride is 10 parts.
[0078] Comparative Example 6
[0079] The specific implementation manner of this comparative example is the same as that of Example 1, except that: the amount of propylene glycol is 30 parts.
[0080] Performance Evaluation
[0081] 1. Filler paste thickening data: The same amount of low shrinkage resin, solid filler, black paste (prepared in different embodiments and comparative examples) and magnesium oxide powder were added to the same unsaturated polyester resin for molding, and the mixture was stirred continuously. Samples were taken after stirring for 5 minutes, 30 minutes, 24 hours, 48 hours and 72 hours, and the viscosity of the samples was tested by Brookfield viscometer; E represents complete curing; the blank sample is the unsaturated polyester resin without the addition of black paste; 5 samples were tested for each embodiment and comparative example, and the average value of the measured values was recorded in Table 1.
[0082] 2. 130°C reaction activity data: 1 wt% of curing agent was added to the same unsaturated polyester resin for molding, and the black paste prepared in all the embodiments and comparative examples was added and stirred evenly. After stirring evenly, the resin was tested for gel time, curing time and exothermic peak performance with reference to GB / T 24148.6-2009. The blank sample was the unsaturated polyester resin without the black paste. Five samples were tested for each embodiment and comparative example, and the average value of the measured values was recorded in Table 2.
[0083] 3. Black slurry viscosity: The viscosity of the black slurry prepared in each embodiment and comparative example was tested using a viscosity meter. Five samples were tested for each embodiment and comparative example, and the average value of the measured values was recorded in Table 3.
[0084] Table 1
[0085] Example 5min 30min 1d 2d 3d 4d 5d Blank <![CDATA[2.5×10 4 ]]> <![CDATA[1.4×10 5 ]]> <![CDATA[7.1×10 7 ]]> <![CDATA[8.7×10 7 ]]> <![CDATA[1.1×10 8 ]]> E E Example 1 <![CDATA[3.1×10 5 ]]> <![CDATA[2.3×10 5 ]]> <![CDATA[4.2×10 5 ]]> <![CDATA[6.5×10 5 ]]> <![CDATA[9.5×10 5 ]]> <![CDATA[1.3×10 6 ]]> <![CDATA[1.7×10 6 <!-- 5 -->]]> Example 2 <![CDATA[4.4×10 5 ]]> <![CDATA[5.9×10 5 ]]> <![CDATA[6.3×10 5 ]]> <![CDATA[8.9×10 5 ]]> <![CDATA[1.1×10 6 ]]> <![CDATA[1.3×10 6 ]]> <![CDATA[1.6×10 6 ]]> Example 3 <![CDATA[8.9×10 4 ]]> <![CDATA[3.5×10 5 ]]> <![CDATA[4.1×10 5 ]]> <![CDATA[5.8×10 5 ]]> <![CDATA[7.9×10 5 ]]> <![CDATA[1.1×10 6 ]]> <![CDATA[1.4×10 6 ]]> Comparative Example 1 <![CDATA[9.2×10 5 ]]> <![CDATA[1.5×10 6 ]]> <![CDATA[2.1×10 6 ]]> <![CDATA[3.8×10 6 ]]> <![CDATA[4.2×10 6 ]]> E E Comparative Example 2 <![CDATA[9.1×10 5 ]]> <![CDATA[1.1×10 6 ]]> <![CDATA[1.1×10 6 ]]> <![CDATA[2.4×10 6 ]]> <![CDATA[3.8×10 6 ]]> E E Comparative Example 3 <![CDATA[9.8×10 5 ]]> <![CDATA[1.9×10 6 ]]> <![CDATA[2.7×10 6 ]]> <![CDATA[4.2×10 6 ]]> <![CDATA[5.1×10 6 ]]> E E Comparative Example 4 <![CDATA[9.8×10 5 ]]> <![CDATA[1.4×10 6 ]]> <![CDATA[1.8×10 6 ]]> <![CDATA[2.8×10 6 ]]> <![CDATA[3.9×10 6 ]]> E E Comparative Example 5 <![CDATA[8.2×10 5 ]]> <![CDATA[1.4×10 6 ]]> <![CDATA[1.9×10 6 ]]> <![CDATA[2.8×10 6 ]]> <![CDATA[3.7×10 6 ]]> E E Comparative Example 6 <![CDATA[8.6×10 5 ]]> <![CDATA[1.5×10 6 ]]> <![CDATA[2.1×10 6 ]]> <![CDATA[3.1×10 6 ]]> <![CDATA[4.1×10 6 ]]> E E
[0086] Table 2
[0087]
[0088]
[0089] Table 3
[0090] Example Viscosity mPa·s Example 1 7120 Example 2 7740 Example 3 7804 Comparative Example 1 9125 Comparative Example 2 5784 Comparative Example 3 10554 Comparative Example 4 5545 Comparative Example 5 5474 Comparative Example 6 5240
[0091] Through the examples, comparative examples and the data in Tables 1 to 3, it can be seen that the high-activity molded black paste provided by the present invention has good thickening effect and good gel curing time, and has an adapted viscosity, is suitable for promotion in the field of molded products, and has broad development prospects. Among them, Example 1 obtains the best performance index under factors such as the best raw material weight ratio and preparation process.
[0092] Finally, it is pointed out that the above-described embodiments are only preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A highly active molded black paste, characterized in that: The raw materials include the following parts by weight: 65-80 parts of base resin, 5-15 parts of auxiliary agent, and 20-30 parts of carbon black; The raw materials of the base resin include the following parts by weight: 20-30 parts of alcohol ether, 10-20 parts of dibasic acid, 15-25 parts of unsaturated acid anhydride, and 20-24 parts of diol; The base resin is an unsaturated resin that does not contain styrene; The weight ratio of the unsaturated acid anhydride to the diol is 3-5:4-5.
2. The high-activity molded black paste according to claim 1, characterized in that: The viscosity of the matrix resin is 600-800 mPa·s.
3. The high-activity molded black paste according to claim 1, characterized in that: The auxiliary agent is at least one of high molecular weight copolymer alkyl ammonium salts.
4. The high-activity molded black paste according to claim 1, characterized in that: The weight ratio of the auxiliary agent to the carbon black is 1-3:4-6.
5. The high-activity molded black paste according to claim 1, characterized in that: The particle size of the carbon black is 20 to 30 nm.
6. A method for preparing a high-activity molded black paste according to any one of claims 1 to 5, characterized in that: The method comprises the following steps: (1) adding a base resin and an additive into a reaction container, and stirring at a speed of 500 to 800 rpm for 10 to 15 minutes; (2) reducing the speed to 100 to 200 rpm, and slowly adding a formulated amount of carbon black in portions, and after the addition is completed, increasing the speed to 500 to 800 rpm and stirring for 30 to 60 minutes; (3) after the stirring is completed, putting the color paste into a three-roll grinder and grinding it for 3 to 5 times to obtain the color paste.
7. An application of the high-activity molding black paste according to any one of claims 1 to 5, characterized in that: The invention comprises the application of the high-activity molded black slurry in the preparation of black molded products.