A solid electrolyte and electrochromic device for color-white conversion

By optimizing the composition and structure of solid electrolytes, the visible light reflectivity and contrast of electrochromic devices are improved, the problem of low contrast in the prior art is solved, and the color state conversion effect with high contrast is achieved.

CN114815427BActive Publication Date: 2024-11-19江苏慧智新材料科技有限公司
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202210521263.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-05-13
Publication Date
2024-11-19
Estimated Expiration
2042-05-13

AI Technical Summary

Technical Problem

The contrast between the color loss and chromatic states of existing electrochromic devices is low, making it difficult to effectively resolve color state conversion in applications with high contrast requirements.

Method used

The solid electrolyte composed of polymer substrate and ionic liquid is used to optimize the composition of polymer substrate and the mass ratio of ionic liquid, combined with white inorganic fillers, improve the visible light reflectivity and contrast of the solid electrolyte, and achieve color through the laminated structure design. White conversion.

Benefits of technology

The visible light reflectivity and ionic conductivity of the solid electrolyte membrane are significantly improved, and the high contrast color state conversion is achieved, making it easier for the human eye to distinguish the color loss and color state of the device.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114815427B_ABST
    Figure CN114815427B_ABST
Patent Text Reader

Abstract

The present invention discloses a solid electrolyte, comprising a polymer substrate and an ionic liquid. The main components of the polymer substrate are polyvinylidene fluoride, or polyvinylidene fluoride and polymethyl methacrylate; the mass percentage of polyvinylidene fluoride in the substrate is greater than 60%. The solid electrolyte membrane prepared by the solid electrolyte of the present invention has both excellent visible light reflectivity and ionic conductivity. When a voltage is applied to an electrochromic device comprising the solid electrolyte membrane, when the color-changing layer is colored, the color of the color-changing layer of the device is displayed. When the color-changing layer loses color to a transparent state, the device displays the white color of the electrolyte; the color change contrast between the above-discolored state and the colored state is high, and the human eye can more easily distinguish the color state conversion. The present invention also discloses an electrochromic device based on a solid electrolyte for colored white conversion.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of solid electrolytes, and in particular to a solid electrolyte and a colored-white conversion electrochromic device. Background Art

[0002] Electrochromism refers to the phenomenon that the optical properties of a material (reflectivity, transmittance, absorption rate, etc.) undergo stable and reversible color changes under the action of an external electric field, which is manifested in appearance as reversible changes in color and transparency. Electrochromism has broad application prospects in the fields of displays, intelligent temperature control, sun visors, etc. As an important component of electrochromic devices, electrolytes have always been a difficult point in the application of electrochromic devices. There are solid electrolytes including gel electrolytes and solid electrolytes.

[0003] The electrochromic device in the prior art is transparent in the fading state and black, blue, red, etc. in the colored state. The contrast between the fading state and the colored state is low, and it is not suitable for color-changing devices with high contrast requirements and where the human eye can more easily distinguish color state transitions. Summary of the invention

[0004] One of the purposes of the present invention is to overcome the defects existing in the prior art and provide a solid electrolyte. By optimizing the composition of the polymer substrate, the visible light reflectance and contrast of the solid electrolyte used in the electrochromic device are improved, making it easier for the human eye to distinguish between the decolorized state and the colored state.

[0005] In order to achieve the above-mentioned purpose, the technical solution of the present invention is: a solid electrolyte, including a polymer substrate and an ionic liquid, wherein the main components of the polymer substrate are polyvinylidene fluoride, or polyvinylidene fluoride and polymethyl methacrylate; the mass percentage of polyvinylidene fluoride in the substrate is greater than 60%.

[0006] The preferred technical solution is that the mass ratio of the polymer substrate to the ionic liquid is 1:(1.3-1.8). Based on the preferred range of the above mass ratio, if the ratio is too small, the electrolyte ion conductivity will be too low due to the low content of the ionic liquid; if the ratio is too large, the film forming property will be poor, the film surface will be uneven, and even holes will appear on the film surface due to the low content of the polymer.

[0007] The preferred technical solution is that the ionic liquid is an ionic liquid with non-volatility, high thermal stability and high ionic conductivity, and is selected from at least one of 1-butyl-3-methylbis(trifluoromethanesulfonyl)imide, 1-ethyl-3-methylbis(trifluoromethanesulfonyl)imide, 1-butyl-3-methyltetrafluoroborate, 1-butyl-1-methylpyrrolidinebis(trifluoromethanesulfonyl)imide, 1-ethyl-3-methyltetrafluoroborate and 1-butyl-3-methyltetrafluoroborate.

[0008] The preferred technical solution is that the average molecular weight of polyvinylidene fluoride is 300,000 to 400,000; and / or the average molecular weight of polymethyl methacrylate is 1.9 million to 2.1 million. Further, the average molecular weight of polyvinylidene fluoride is 300,000 to 350,000; the average molecular weight of polymethyl methacrylate is 1.95 million to 2.05 million. The higher the molecular weight of PVDF, the higher the strength of the film, and the higher the crystallinity, therefore, the stronger the visible light reflectivity; too high or too low molecular weight is not conducive to the formation of the film.

[0009] The preferred technical solution is that the mass percentage of polyvinylidene fluoride in the substrate is 70% to 95%, further 80% to 93%, and more preferably 86% to 92%. The preferred solid electrolyte with a mass percentage of polyvinylidene fluoride has both excellent visible light reflectivity and ionic conductivity.

[0010] The preferred technical solution is that the solid electrolyte also includes a white inorganic filler, and the mass percentage of the white inorganic filler in the solid electrolyte is 5% to 15%, further 8% to 13%, and further 9% to 11%; specifically, 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, and 15% points can be selected. The more white inorganic filler content, the higher the visible light reflectivity of the electrolyte membrane. However, if the filler content is too high, uneven dispersion may occur; affecting the uniformity of the electrolyte membrane. The inorganic filler content has a great influence on the ionic conductivity of the electrolyte. Within an appropriate range, the more inorganic fillers are added, the greater the ionic conductivity of the solid electrolyte. However, when this range is exceeded, as the content of the inorganic filler increases, the ionic conductivity will decrease instead. The reason is that the addition of an appropriate amount of inorganic filler will reduce the crystallinity of the polymer, and ions can be transmitted through two channels, the inorganic filler and the interface between the polymer and the inorganic filler, thereby improving the ionic conductivity. However, too much filler will reduce the ionic conductivity of the system, possibly by destroying the polymer matrix structure and thus the ion transport channel.

[0011] The preferred technical solution is that the white inorganic filler is titanium dioxide, and the particle size of the white inorganic filler is 30 to 40 nm. Adding titanium dioxide to the solid polymer electrolyte can significantly improve the mechanical strength of the electrolyte, reduce the crystallinity of the polymer matrix to a certain extent, and improve the ionic conductivity of the electrolyte.

[0012] The second object of the present invention is to provide an electrochromic device for colored white conversion, comprising a transparent conductive electrode layer, an electroactive material layer, a white electrolyte layer, an electrochromic layer, and a transparent conductive electrode layer stacked in sequence, wherein the white electrolyte layer is prepared by coating and drying the electrolyte mother solution of the above-mentioned solid electrolyte and solution.

[0013] The preferred technical solution is that the thickness of the white electrolyte layer is 180-230 μm. The thicker the solid electrolyte, the higher its visible light reflectivity. The preferred thickness of the white electrolyte layer has excellent light reflectivity, film toughness and tensile strength.

[0014] The advantages and beneficial effects of the present invention are:

[0015] The solid electrolyte membrane prepared by the solid electrolyte of the present invention has both excellent visible light reflectivity and ionic conductivity; when voltage is applied to an electrochromic device including the solid electrolyte membrane, the color-changing layer is colored, and the device displays the color of the color-changing layer; when the color-changing layer loses color to a transparent state, the device displays the white color of the electrolyte;

[0016] The color change contrast between the decolorized state and the colored state is high, and the human eye can more easily distinguish the color state transition. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 This is an optical photograph of the electrolyte of Example 1 of the present invention;

[0018] Figure 2 is a graph showing changes in visible light reflectivity of the solid electrolyte membranes of Examples 1-5;

[0019] Figure 3 Graph showing ionic conductivity of the solid electrolyte membrane of Examples 1-5;

[0020] Figure 4 These are optical photographs of the blue electrochromic device in Example 1 in the colored and decolored states;

[0021] Figure 5 This is a comparison chart of the reflectivity of the blue device in Example 1 in the colored state and the decolorized state. DETAILED DESCRIPTION

[0022] The specific implementation of the present invention is further described below in conjunction with the examples. The following examples are only used to more clearly illustrate the technical solutions of the present invention, and cannot be used to limit the protection scope of the present invention.

[0023] Preparation method of solid electrolyte mother solution in embodiment:

[0024] The polymer matrix, ionic liquid (and white inorganic filler) are configured in proportion, and the above components are introduced into a mixed organic solvent of acetone and DMF. After sealing, the mixture is heated to 60°C, kept warm and stirred for several hours at a stirring speed of 500 r / min. When the polymer matrix is ​​dissolved in the mixed organic solvent, a solid electrolyte mother solution is obtained.

[0025] Example Preparation method of colored white conversion electrochromic device:

[0026] S1: spraying the electroactive material evenly onto the surface of the transparent conductive substrate using a spray gun and drying;

[0027] S2: coating the surface of the electroactive material layer obtained in S1 with a solid electrolyte by scraping, and obtaining a white solid electrolyte layer adhered to the transparent conductive substrate after the mother liquid is dried;

[0028] S3: The electrochromic material solution is evenly sprayed on the conductive surface of another transparent conductive substrate. After drying, the electrochromic layer is bonded to the solid electrolyte in S2, and then sealed around with glue to obtain an electrochromic device that converts from colored to white.

[0029] In the embodiment, the electroactive material may be any known electroactive material such as an electrochromic material, a conductive polymer material, an electrode modification material, etc. The white electrolyte layer has excellent light reflectivity, so the electrochromic material on one side or both sides of the thickness direction of the white electrolyte layer can show its corresponding colored state and decolorized state, and the color states of the electrochromic material layers on both sides have little mutual influence.

[0030] Examples 1-5

[0031] The solid electrolytes of Examples 1-5 are composed of a polymer substrate (polyvinylidene fluoride PVDF and polymethyl methacrylate PMMA), an ionic liquid and titanium dioxide. The solid electrolyte and the solid electrolyte mother solution are configured according to the following table:

[0032]

[0033] The ionic liquids in the above table are all 1-butyl-3-methylbis(trifluoromethanesulfonyl)imide salt; the average molecular weight of polyvinylidene fluoride (PVDF) is 300,000; the average molecular weight of polymethyl methacrylate (PMMA) is 2 million; and the particle size of titanium dioxide is 30 nm.

[0034] Performance testing of solid electrolyte membrane:

[0035] 1. Use UV-visible spectrophotometer to detect the visible light reflectance of solid electrolyte membrane;

[0036] 2. The electrochemical workstation tests the ionic conductivity of the solid electrolyte membrane.

[0037] The above performance test results of Examples 1-5 are shown in the following table:

[0038] Example 1 Example 2 Example 3 Example 4 Example 5 Visible light reflectance / % 70% 75% 80% 90% 93% Ionic conductivity / S / cm <![CDATA[1.6*10 -5 ]]> <![CDATA[8*10 -6 ]]> <![CDATA[6*10 -6 ]]> <![CDATA[5*10 -6 ]]> <![CDATA[3.5*10 -6 ]]>

[0039] PVDF is a semi-crystalline polymer with high visible light reflectivity. The ionic conductivity of crystalline polymers is low. Adding PMMA to PVDF can reduce its crystallinity and improve its ionic conductivity. As the crystallinity decreases, the visible light reflectivity of the polymer will also decrease. In comparison, Example 4 in the above table is more preferred, with a visible light reflectivity of 90% and an ionic conductivity of 5*10 -6 Compared with Example 3, the ionic conductivity is reduced by a small margin, but the visible light reflectance is increased by 10%, while in Example 5, the visible light reflectance is only increased by 3% compared with Example 4, which is a small change, but the ionic conductivity is reduced by a large margin, which has a more adverse effect on the color change performance.

[0040] Examples 6-7 and Comparative Example 1

[0041] The solid electrolyte group composition and electrolyte mother solution composition of Examples 6-7 and Comparative Example 1 are configured according to the following table:

[0042]

[0043] In the above table, “—” means that the solid electrolyte raw material does not contain titanium dioxide.

[0044] The performance test results of the solid electrolyte membrane of Examples 6-7 are shown in the following table:

[0045] Example 6 Example 7 Comparative Example 1 Visible light reflectance / % 34% 75% 50% Ionic conductivity / S / cm <![CDATA[7.7*10 -6 ]]> <![CDATA[2.6*10 -5 ]]> <![CDATA[1.2*10 -5 ]]>

[0046] Comparison of the titanium dioxide content in the solid electrolyte compositions formed in Examples 4, 6 and 7 shows that the addition of titanium dioxide can significantly improve the visible light reflectance based on a PVDF to PMMA mass ratio of 9:1, while in Comparative Example 1, the PVDF to PMMA mass ratio is 5:5, and the addition of titanium dioxide has little effect on improving the visible light reflectance.

[0047] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the technical principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A solid electrolyte comprising a polymer substrate and an ionic liquid, characterized in that: The main components of the polymer substrate are polyvinylidene fluoride, or polyvinylidene fluoride and polymethyl methacrylate; the mass percentage of polyvinylidene fluoride in the substrate is 70% to 95%; the solid electrolyte also includes a white inorganic filler, and the mass percentage of the white inorganic filler in the solid electrolyte is 5% to 15%.

2. The solid electrolyte according to claim 1, characterized in that The mass ratio of the polymer substrate to the ionic liquid is 1:(1.3-1.8).

3. The solid electrolyte according to claim 1, characterized in that The ionic liquid is at least one selected from 1-butyl-3-methylbis(trifluoromethanesulfonyl)imide, 1-ethyl-3-methylbis(trifluoromethanesulfonyl)imide, 1-butyl-3-methyltetrafluoroborate, 1-butyl-1-methylpyrrolidinebis(trifluoromethanesulfonyl)imide, 1-ethyl-3-methyltetrafluoroborate, and 1-butyl-3-methyltetrafluoroborate.

4. The solid electrolyte according to claim 1, characterized in that The average molecular weight of polyvinylidene fluoride is 300,000 to 400,000; and / or the average molecular weight of the polymethyl methacrylate is 1.9 million to 2.1 million.

5. The solid electrolyte according to claim 1, characterized in that The white inorganic filler is titanium dioxide, and the particle size of the white inorganic filler is 30 to 40 nm.

6. A colored white conversion electrochromic device, comprising a transparent conductive electrode layer, an electroactive material layer, a white electrolyte layer, an electrochromic layer, and a transparent conductive electrode layer stacked in sequence, characterized in that: The white electrolyte layer is prepared by coating and drying the solid electrolyte according to any one of claims 1 to 5 and the electrolyte mother solution of the solution.

7. The electrochromic device for color white conversion according to claim 6, characterized in that: The thickness of the white electrolyte layer is 180-230 μm.

Citation Information

Patent Citations

  • Electrochromic display element

    CN102243407A

  • Electro-chromic display element, display apparatus, and driving method

    CN103562787A

  • Electrochromic display element and display device

    CN104049432A

  • Composite solid-state electrolyte, preparation method thereof and lithium secondary solid-state battery containing composite solid-state electrolyte

    CN110931852A

  • Composite solid-state electrolyte, solid-state battery and preparation method of solid-state battery

    CN111244537A