Dielectric ceramic composition and multilayer ceramic capacitor including the same
By using barium titanate-based dielectric ceramic composition in a multi-layer ceramic capacitor and adding an appropriate amount of zinc oxide to control its content, the effective capacity change rate and reliability of the dielectric layer under high frequency and low electric field is solved, and the problem of the dielectric layer is realized Improved temperature stability and high-frequency performance of dielectric materials.
Patent Information
- Application Number
- CN202210398373.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-06-17
- Filing Date
- 2020-04-03
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2040-04-03
AI Technical Summary
Under the demands of miniaturization and high capacity, the reliability and temperature stability of the dielectric layer are difficult to ensure, especially under high frequency and low electric fields, the effective capacity change rate is large and sensitive to temperature changes.
Using a barium titanate (BaTiO3)-based dielectric ceramic composition, an appropriate amount of zinc oxide (ZnO) is added as a sub-component, and its content is controlled from 0.1 mol% to 0.4 mol% to inhibit the growth of dielectric grains and reduce the effective capacity. rate of change and increase reliability.
The effective capacity change rate and reliability are reduced under the DC electric field, the temperature stability and high-frequency performance of the dielectric material are improved, and the reliability problem of the dielectric layer under the film composition is avoided.
Smart Images

Figure CN114823138B_ABST
Abstract
Description
[0001] This application is a divisional application of the invention patent application with the application date of April 3, 2020 and application number 202010259098.8 and the invention name “Dielectric ceramic composition and multilayer ceramic capacitor including the same”. Technical Field
[0002] The present disclosure relates to a dielectric ceramic composition capable of improving reliability and a multilayer ceramic capacitor including the same. Background Art
[0003] Generally, electronic components using ceramic materials, such as capacitors, inductors, piezoelectric elements, varistors, thermistors, etc., include a ceramic body formed using the ceramic material, an internal electrode formed in the ceramic body, and an external electrode disposed on a surface of the ceramic body to be connected to the internal electrode.
[0004] In recent years, due to the trend of miniaturization and multifunctionalization of electronic products, chip components have tended to be miniaturized and realized as highly functional. Therefore, multilayer ceramic capacitors are required to be high-capacity products with small size and high capacity.
[0005] As a method for achieving both miniaturization and high capacity of multilayer ceramic capacitors, the thickness of dielectric layers and electrode layers in multilayer ceramic capacitors is reduced to allow a greater number of layers to be stacked. In this regard, the thickness of the dielectric layer is currently at a level of about 0.6 μm and is continuously being developed toward a thinner level.
[0006] In this case, regarding the dielectric material, ensuring the reliability of the dielectric layer may be important.
[0007] In addition, applying a large electric field per unit thickness to a dielectric layer with a thin film has the problem of being sensitive to temperature changes, and it is difficult to achieve effective capacitance and temperature characteristics under actual use conditions.
[0008] Therefore, in order to solve such a problem, it is necessary to develop a dielectric material whose dielectric constant changes little due to an external direct current (DC) electric field and temperature changes. Summary of the invention
[0009] An aspect of the present disclosure is to provide a dielectric ceramic composition capable of improving reliability and a multilayer ceramic capacitor including the same.
[0010] According to one aspect of the present disclosure, a dielectric ceramic composition includes a barium titanate (BaTiO3)-based matrix material main component and a subcomponent, wherein the subcomponent includes zinc oxide (ZnO) as a first subcomponent, and based on 100 mol% of the matrix material main component, the content of ZnO is greater than or equal to 0.1 mol% and less than 0.4 mol%.
[0011] According to another aspect of the present disclosure, a multilayer ceramic capacitor includes: a ceramic body including a dielectric layer and a first inner electrode and a second inner electrode, the first inner electrode and the second inner electrode being arranged opposite to each other with the dielectric layer interposed therebetween; and a first outer electrode and a second outer electrode arranged on the outside of the ceramic body, the first outer electrode being electrically connected to the first inner electrode, and the second outer electrode being electrically connected to the second inner electrode, the dielectric layer including dielectric grains containing a dielectric ceramic composition, the dielectric ceramic composition including a BaTiO3-based matrix material main component (matrix material main component) and a subcomponent, the subcomponent including zinc oxide (ZnO) as a first subcomponent, and the content of ZnO is greater than or equal to 0.1 mol % and less than 0.4 mol % relative to 100 mol % of the matrix material main component.
[0012] Other features and aspects will be apparent from the following detailed description, drawings, and claims. BRIEF DESCRIPTION OF THE DRAWINGS
[0013] The above and other aspects, features and advantages of the present disclosure will be more clearly understood through the following detailed description in conjunction with the accompanying drawings, in which:
[0014] Figure 1 is a schematic perspective view showing a multilayer ceramic capacitor according to an embodiment;
[0015] Figure 2 It is along Figure 1 A cross-sectional view taken along line I-I';
[0016] Figure 3 is a graph showing dielectric grain sizes according to examples of experimental examples and comparative examples; and
[0017] Figure 4A and Figure 4B It is a graph of the results of strict reliability evaluation based on the test example and the comparative example. DETAILED DESCRIPTION
[0018] Hereinafter, embodiments of the present disclosure will be described as follows with reference to the accompanying drawings.
[0019] However, the present disclosure may be embodied in many different forms and should not be construed as limited to the specific embodiments set forth herein. Rather, these embodiments are provided so that this disclosure will be thorough and complete, and will fully convey the scope of the present disclosure to those skilled in the art.
[0020] Throughout this specification, it will be understood that when an element such as a layer, region, or wafer (substrate) is referred to as being "located on," "connected to," or "bonded to" another element, the element may be directly "located on," "connected to," or "bonded to" another element, or there may be other elements in between. In contrast, when an element is referred to as being "directly located on," "directly connected to," or "directly bonded to" another element, there may be no intervening elements or layers. The same reference numerals always represent the same elements. As used herein, the term "and / or" includes any and all combinations of one or more of the associated listed items.
[0021] It will be clear that although the terms "first", "second", and "third" etc. may be used herein to describe various members, components, regions, layers, and / or portions, these members, components, regions, layers, and / or portions should not be limited by these terms. These terms are only used to distinguish one member, component, region, layer, or portion from another member, component, region, layer, or portion. Thus, the first member, first component, first region, first layer, or first portion discussed below may be referred to as a second member, second component, second region, second layer, or second portion without departing from the teachings of the exemplary embodiments.
[0022] For ease of description, spatially relative terms such as "above," "above," "below," and "below" may be used herein to describe the relationship of one element to another element shown in the drawings. It will be understood that the spatially relative terms are intended to include different orientations of the device in use or operation in addition to the orientation depicted in the drawings. For example, if the device in the drawings is turned over, an element described as being "above" or "above" other elements or features would subsequently be positioned "below" or "below" the other elements or features. Thus, the term "above" may include both above and below orientations depending on the particular orientation of the drawing. The device may be otherwise positioned (rotated 90 degrees or in other orientations), and the spatially relative descriptors used herein may be interpreted accordingly.
[0023] The terms used herein describe only specific embodiments, and the present disclosure is not limited thereto. Unless the context clearly indicates otherwise, as used herein, the singular form is also intended to include the plural form. It will be further understood that when the terms "comprise" and / or "include" are used in the specification, the stated features, quantities, steps, operations, components, elements and / or their groups are listed, but the presence or addition of one or more other features, quantities, steps, operations, components, elements and / or their groups is not excluded.
[0024] Hereinafter, embodiments of the present disclosure will be described with reference to schematic diagrams showing embodiments of the present disclosure. In the accompanying drawings, for example, changes in the shapes shown may be expected due to manufacturing techniques and / or tolerances. Therefore, the embodiments of the present disclosure should not be interpreted as being limited to the specific shapes of the regions shown herein, for example, and should be interpreted as including shape changes caused by manufacturing. The following embodiments may also be composed of one or a combination thereof.
[0025] The contents of the present disclosure described below may have various configurations, and only required configurations are proposed here, but the present disclosure is not limited thereto.
[0026] Figure 1 is a schematic perspective view showing a multilayer ceramic capacitor according to an embodiment.
[0027] Figure 2 It is along Figure 1 A cross-sectional view taken along line I-I'.
[0028] Reference Figure 1 and Figure 2 According to the embodiment, the multilayer ceramic capacitor 100 includes: a ceramic body 110, including a dielectric layer 111 and a first internal electrode 121 and a second internal electrode 122 which are arranged opposite to each other, and the dielectric layer 111 is interposed between the first internal electrode 121 and the second internal electrode 122; and a first external electrode 131 and a second external electrode 132 which are arranged outside the ceramic body 110, the first external electrode 131 is electrically connected to the first internal electrode 121, and the second external electrode 132 is electrically connected to the second internal electrode 122.
[0029] In the multilayer ceramic capacitor 100 according to the embodiment, the “length direction” is defined as Figure 1 The “L” direction in FIG. 1 is defined as the “width direction”, the “W” direction is defined as the “thickness direction”, and the “T” direction is defined as the “thickness direction”. Here, the “thickness direction” may be used to mean the same as the direction along which the dielectric layers are stacked, i.e., the “stacking direction”.
[0030] The form of the ceramic body 110 is not particularly limited, but the ceramic body may have a hexahedral form as shown in the drawings.
[0031] One end of each of the plurality of internal electrodes 121 and 122 formed inside the ceramic body 110 is exposed to one end of the ceramic body 110 or the other end of the ceramic body 110 opposite to the one end of the ceramic body 110 .
[0032] The internal electrodes 121 and 122 may be provided as a pair of internal electrodes including a first internal electrode 121 and a second internal electrode 122 having different polarities.
[0033] One end of the first internal electrode 121 is exposed to one end of the ceramic body, and one end of the second internal electrode 122 is exposed to the other end of the ceramic body opposite to the one end of the ceramic body.
[0034] The first and second external electrodes 131 and 132 are formed on one end of the ceramic body 110 and the other end of the ceramic body 110 opposite to the one end of the ceramic body 110 to be electrically connected to the internal electrodes.
[0035] Here, there is no particular limitation on the material forming the first and second internal electrodes 121 and 122. For example, the first and second internal electrodes 121 and 122 may be formed using a conductive paste including at least one element selected from the group consisting of silver (Ag), lead (Pb), platinum (Pt), nickel (Ni), and copper (Cu).
[0036] The first and second external electrodes 131 and 132 may be electrically connected to the first and second internal electrodes 121 and 122 , respectively, to form capacitance, and the second external electrode 132 may be connected to a potential different from that of the first external electrode 131 .
[0037] The conductive material included in the first and second external electrodes 131 and 132 is not particularly limited, and may include nickel (Ni), copper (Cu), or an alloy thereof.
[0038] The thickness of the first and second external electrodes 131 and 132 may be appropriately determined depending on their intended applications, etc., and is not particularly limited, but may be 10 μm to 50 μm as an example.
[0039] According to an embodiment, the raw material of the dielectric layer 111 is not particularly limited as long as sufficient capacitance can be obtained therewith. For example, the raw material of the dielectric layer 111 may be barium titanate (BaTiO 3 ) powder.
[0040] According to the purpose of the present disclosure, the material of the dielectric layer 111 may be prepared by adding various additives, organic solvents, plasticizers, binders, dispersants, etc. to powders such as barium titanate (BaTiO 3 ) powders.
[0041] The dielectric layer 111 is sintered, so the boundaries between adjacent dielectric layers may be integrated and may not be easily recognized.
[0042] The first and second internal electrodes 121 and 122 may be formed on the dielectric layer 111 , and the internal electrodes 121 and 122 may be formed in the ceramic body through sintering with the dielectric layer interposed therebetween.
[0043] The thickness of the dielectric layer 111 can be arbitrarily changed according to the capacitance design of the capacitor. In an embodiment, the thickness of the dielectric layer after sintering can be preferably 0.4 μm or less per layer.
[0044] In addition, the thickness of each of the first and second internal electrodes 121 and 122 after sintering may preferably be 0.4 μm or less per layer.
[0045] According to an embodiment of the present disclosure, the dielectric layer 111 includes dielectric grains including a dielectric ceramic composition, and the dielectric ceramic composition includes a BaTiO3-based matrix material main component (matrix material main component) and a subcomponent, the subcomponent includes zinc oxide (ZnO) as a first subcomponent, and relative to 100 mol% of the matrix material main component, the content of zinc oxide (ZnO) in the dielectric ceramic composition satisfies greater than or equal to 0.1 mol% and less than 0.4 mol%.
[0046] Generally, it is necessary to suppress the grain growth of dielectric materials accompanying sintering in order to reduce the effective capacity change rate and ensure temperature stability under high frequency and low electric field environments.
[0047] In order to suppress the grain growth of the ceramic material, the drag effect caused by grain boundary segregation is used. When the drag effect occurs, the mobility of the dielectric grains at the boundary is reduced to suppress the grain growth. Therefore, in the embodiment, zinc oxide (ZnO) as an additive capable of causing the drag effect is added to suppress the grain growth, but the content of ZnO is controlled. As a result, a reduction in the effective capacity change rate under a direct current (DC) electric field and an improvement in reliability can be achieved.
[0048] Generally, the size of zinc (Zn) ions is relatively small, and thus the Zn ions are suitable for substitution at the B site in a perovskite structure such as ABO 3 .
[0049] However, the valence of Zn is lower than that of titanium (Ti), so it is difficult for Zn to actually dissolve.
[0050] Zn ions have a valence of +2, and in terms of low valence, preferably replace a barium (Ba) site (i.e., an A site in a perovskite structure such as ABO3) having a valence of +2. In this case, due to the large size mismatch with Ba having a large ion size, the solid solubility limit is very low.
[0051] Therefore, when zinc oxide (ZnO) is added, most of ZnO does not dissolve in the lattice but segregates in the grain boundaries as ZnO. ZnO segregated in the grain boundaries as described above causes a drag effect that interferes with the movement of the grain boundaries during grain growth, thus inhibiting the grain growth of the ceramic material.
[0052] When the grain growth of the ceramic material is suppressed, the width of the domain wall in the dielectric grains is reduced, and thus the mobility of the domain wall is increased under high frequency and low electric field.
[0053] In this regard, the DC effective capacity under high frequency and low electric field DC can be increased. In addition, as the domain size decreases, the room temperature nominal capacity decreases. In addition, as the proportion of the shell part of the core-shell structured dielectric grains decreases, the temperature stability can be improved.
[0054] According to the embodiment, the dielectric ceramic composition includes a BaTiO3-based matrix material main component (matrix material main component) and a subcomponent, the subcomponent includes ZnO as a first subcomponent, and based on 100 mol% of the matrix material main component, the content of ZnO satisfies greater than or equal to 0.1 mol% and less than 0.4 mol%, so that grain growth suppression and low-temperature densification can be achieved. Therefore, under a DC electric field, the effective capacity change rate can be reduced and reliability can be improved.
[0055] If the content of ZnO in the dielectric ceramic composition is less than 0.1 mol % relative to 100 mol % of the main component of the matrix material, the content of ZnO is low, and thus the grain growth suppressing effect is extremely low.
[0056] In addition, if the content of ZnO in the dielectric ceramic composition is 0.4 mol% or more relative to 100 mol% of the main component of the matrix material, a large amount of ZnO having semiconductor characteristics segregates in the dielectric grain boundaries, so the resistance of the grain boundaries decreases and reliability may be reduced.
[0057] If the ZnO content in the dielectric ceramic composition satisfies 0.1 mol% or more and less than 0.4 mol% relative to 100 mol% of the main component of the matrix material, densification of the dielectric material occurs at a sintering temperature 20°C lower than that of the same model, and a significant grain growth suppression effect is confirmed.
[0058] In addition, according to an embodiment, the subcomponent includes magnesium (Mg) as a second subcomponent, and the total content of zinc oxide (ZnO) and magnesium (Mg) may be less than 0.8 mol % with respect to 100 mol % of the main component of the base material.
[0059] When the total content of zinc oxide (ZnO) and magnesium (Mg) in the dielectric ceramic composition increases, it is advantageous in terms of reliability improvement. However, in a certain amount or more, semiconductor characteristics are provided, thereby deteriorating the characteristics of the insulator and deteriorating the sintering properties. Therefore, it is preferred that the total content of zinc oxide (ZnO) and magnesium (Mg) in the dielectric ceramic composition is less than 0.8 mol% relative to 100 mol% of the main component of the base material.
[0060] That is, if the total content of zinc oxide (ZnO) and magnesium (Mg) in the dielectric ceramic composition is greater than or equal to 0.8 mol% based on 100 mol% of the main component of the base material, the sintering performance may be insufficient due to the excessive content. Therefore, there may be problems such as capacity uncertainty, reduced breakdown voltage (BDV), etc. in terms of reliability.
[0061] The multilayer ceramic capacitor 100 according to the embodiment is an ultra-small high-capacity product as described above. Here, the thickness of the dielectric layer 111 is 0.4 μm or less, and the thickness of each of the first and second internal electrodes 121 and 122 is 0.4 μm or less, but the embodiment is not limited thereto.
[0062] Furthermore, the size of the multilayer ceramic capacitor 100 may be 1005 (length×width, 1.0 mm×0.5 mm) or less.
[0063] That is, since the multilayer ceramic capacitor 100 according to the embodiment is an ultra-small high-capacity product, each of the dielectric layer 111 and the first and second internal electrodes 121 and 122 is composed of a thin film, and the thickness of the thin film is reduced compared to the product according to the related art. In the case of a product of a multilayer ceramic capacitor to which a dielectric layer and internal electrodes composed of thin films are applied as described above, research on reduction of effective capacity change rate under a DC electric field and improvement of reliability is a very important issue.
[0064] That is, compared with the dielectric layer and the inner electrode included in the multilayer ceramic capacitor according to the embodiment, in the case of the multilayer ceramic capacitor according to the prior art, a relatively large thickness is provided. Therefore, even when the composition of the dielectric ceramic is the same as that of the dielectric ceramic according to the prior art, there is no problem with reliability.
[0065] However, in the case of a product in which the dielectric layer and the internal electrodes are composed of thin films as in the embodiment, there may be problems with the effective capacity change rate and reliability of the multilayer ceramic capacitor under a DC electric field. For this reason, it is necessary to control the dielectric ceramic composition.
[0066] That is, in the embodiment, the content of ZnO in the dielectric ceramic composition is controlled to satisfy 0.1 mol% or more and less than 0.4 mol% relative to 100 mol% of the main component of the base material. In detail, the total content of zinc oxide (ZnO) and magnesium (Mg) in the dielectric ceramic composition is controlled to be less than 0.8 mol% relative to 100 mol% of the main component of the base material. Therefore, in the case of a thin film having a dielectric layer 111 with a thickness of 0.4 μm or less, grain growth suppression and low-temperature densification can be achieved. Therefore, under a DC electric field, the effective capacity change rate can be reduced and reliability can be improved.
[0067] Here, the film does not mean that the thickness of the dielectric layer 111 and the thickness of each of the first inner electrode 121 and the second inner electrode 122 are 0.4 μm or less, but can be understood to include the concept of a dielectric layer and an inner electrode having a reduced thickness compared to products according to the prior art.
[0068] Hereinafter, each component of the dielectric ceramic composition according to the embodiment will be described in more detail.
[0069] a) Main component of the matrix material
[0070] The dielectric ceramic composition according to the embodiment may include a main component of the matrix material represented by BaTiO3.
[0071] According to an embodiment of the present disclosure, the main component of the matrix material includes one or more selected from the group consisting of BaTiO3, (Ba 1-x Ca x )(Ti 1-y Ca y )O3 (where x is 0 ≤ x ≤ 0.3 and y is 0 ≤ y ≤ 0.1), (Ba 1-x Ca x )(Ti 1-y Zr y )O3 (where x is 0 ≤ x ≤ 0.3 and y is 0 ≤ y ≤ 0.5), and Ba(Ti 1-y Zr y )O3 (where 0 < y ≤ 0.5), but is not limited thereto.
[0072] The room-temperature dielectric constant of the dielectric ceramic composition according to the embodiment may be 2000 or greater.
[0073] The main component of the matrix material is not particularly limited, but the average particle size of the main component of the matrix material in powder form may be greater than or equal to 40 nm and less than or equal to 200 nm.
[0074] b) First sub-component
[0075] According to an embodiment of the present disclosure, the dielectric ceramic composition may include one or more oxides containing at least one element selected from the group consisting of manganese (Mn), vanadium (V), chromium (Cr), iron (Fe), nickel (Ni), cobalt (Co), copper (Cu), and zinc (Zn) and / or one or more carbonates containing at least one element selected from the group consisting of Mn, V, Cr, Fe, Ni, Co, Cu, and Zn as the first sub-component.
[0076] As the first subcomponent, the total amount of oxides of at least one element selected from the group consisting of Mn, V, Cr, Fe, Ni, Co, Cu, and Zn and / or carbonates containing at least one element selected from the group consisting of Mn, V, Cr, Fe, Ni, Co, Cu, and Zn contained in the dielectric ceramic composition may be greater than or equal to 0.1 mol % and less than or equal to 2.0 mol % relative to 100 mol % of the main component of the base material. The total amount of the first subcomponent in the dielectric ceramic composition of the present disclosure may be the total amount of the first subcomponent in the dielectric layer 111.
[0077] The first subcomponent can be used to reduce the sintering temperature of a multilayer ceramic capacitor to which the dielectric ceramic composition is applied, and to improve high-temperature withstand voltage characteristics.
[0078] The content of the first subcomponent and the contents of the second to fourth subcomponents refer to inclusion amounts relative to 100 mol % of the base material powder, and specifically, may be defined as mol % of metal ions included in each subcomponent.
[0079] If the content of the first subcomponent in the dielectric ceramic composition is less than 0.1 mol %, the sintering temperature increases, and the high-temperature withstand voltage characteristics are positively degraded.
[0080] If the content of the first subcomponent exceeds 2.0 mol %, high temperature withstand voltage characteristics and room temperature resistivity may decrease.
[0081] In detail, the dielectric ceramic composition according to the embodiment may include the first subcomponent having a content of 0.1 mol% or more and 2.0 mol% or less relative to 100 mol% of the main component of the matrix material. In this regard, low temperature sintering can be performed and a high degree of high temperature withstand voltage characteristics can be obtained.
[0082] c) Second subcomponent
[0083] According to embodiments, the dielectric ceramic composition may include a second subcomponent that is an oxide and / or a carbonate including a fixed-valence acceptor element of magnesium (Mg).
[0084] The fixed valence acceptor element Mg may be included in the dielectric ceramic composition as a second subcomponent in an amount of 0.2 mol % or more and 0.7 mol % or less with respect to 100 mol % of the main component of the base material.
[0085] The second subcomponent is a fixed valence acceptor element and a compound including the fixed valence acceptor element, and serves as an acceptor for reducing electron concentration. The fixed valence acceptor element Mg (second subcomponent) is included in the dielectric ceramic composition in an amount of 0.2 mol% or more and 0.7 mol% or less relative to 100 mol% of the main component of the base material, so the reliability improvement effect due to the n-type can be significantly improved. The total amount of the second subcomponent disclosed in the present invention can be the total amount of the second subcomponent included in the dielectric layer 111.
[0086] If the content of the second subcomponent in the dielectric ceramic composition exceeds 0.7 mol% relative to 100 mol% of the matrix material main component, the dielectric constant decreases and the dielectric breakdown voltage (BDV) decreases. Therefore, an excessive amount of the second subcomponent is not preferred.
[0087] d) The third subcomponent
[0088] According to an embodiment of the present disclosure, the dielectric ceramic composition may include one or more oxides including at least one of silicon (Si) and aluminum (Al) or a glass compound including Si as a third subcomponent.
[0089] The dielectric ceramic composition may further include greater than 0.001 mol % and less than or equal to 0.5 mol % of a third subcomponent including one or more oxides including at least one of Si and Al or a glass compound including Si, relative to 100 mol % of the base material main component.
[0090] The content of the third subcomponent may be the content of the element Si and the element Al included in the dielectric ceramic composition as the third subcomponent relative to 100 mol % of the main component of the base material, regardless of the addition form (such as glass, oxide) in which the element Si and the element Al are included. The content of the third subcomponent of the present disclosure may be the content of the third subcomponent included in the dielectric layer 111.
[0091] The third subcomponent can be used to reduce the sintering temperature of a multilayer ceramic capacitor to which the dielectric ceramic composition is applied, and to improve high-temperature withstand voltage characteristics.
[0092] If the content of the third subcomponent in the dielectric ceramic composition exceeds 0.5 mol% relative to 100 mol% of the main component of the matrix material, sintering properties and densification may be reduced and a secondary phase may be generated. Therefore, an excessive amount of the third subcomponent is not preferred.
[0093] In detail, according to an embodiment of the present disclosure, the dielectric ceramic composition includes Al in an amount of 0.5 mol % or less. Therefore, when Al acts as an acceptor, electron concentration is surely reduced, and thus reliability can be improved.
[0094] e) The fourth component
[0095] According to an embodiment of the present disclosure, the dielectric ceramic composition may include a fourth subcomponent of 0.001 mol% or more and 4.0 mol% or less relative to 100 mol% of the main component of the base material, and the fourth subcomponent includes one or more oxides containing at least one element selected from the group consisting of dysprosium (Dy), yttrium (Y), holmium (Ho), erbium (Er), cerium (Ce), neodymium (Nd), promethium (Pm), europium (Eu), gadolinium (Gd), thulium (Tm), ytterbium (Yb), lutetium (Lu), lanthanum (La), and samarium (Sm) and / or one or more carbonates containing at least one element selected from the group consisting of Dy, Y, Ho, Er, Ce, Nd, Pm, Eu, Gd, Tm, Yb, Lu, La, and Sm. The content of the fourth subcomponent of the present disclosure may be the content of the fourth subcomponent included in the dielectric layer 111.
[0096] In the embodiment, the fourth subcomponent is used to prevent a decrease in reliability of a multilayer ceramic capacitor to which the dielectric ceramic composition is applied.
[0097] If the content of the fourth subcomponent in the dielectric ceramic composition exceeds 4.0 mol %, reliability may be reduced, the dielectric constant of the dielectric ceramic composition may be reduced, and high-temperature withstand voltage characteristics may be deteriorated.
[0098] In detail, according to an embodiment of the present disclosure, lanthanum (La) of the fourth subcomponent may be disposed at grain boundaries of dielectric grains.
[0099] In addition, when a rare earth element having an ionic radius larger than that of dysprosium (Dy), for example, lanthanum (La), is used, the site of barium (Ba) can be more effectively substituted. In this regard, the oxygen vacancy defect concentration can be more effectively reduced.
[0100] Therefore, lanthanum (La) may be further included as a fourth subcomponent in order to ensure insulation resistance while significantly reducing the oxygen vacancy defect concentration to improve reliability.
[0101] Here, if the content of lanthanum (La) in the dielectric ceramic composition is too much, the insulation resistance will be rapidly reduced due to the excessive semiconductor characteristics. In this regard, the content of La in the dielectric ceramic composition is preferably greater than or equal to 0.233 mol% and less than or equal to 0.699 mol% relative to 100 mol% of the main component of the matrix material.
[0102] If the content of lanthanum (La) in the dielectric ceramic composition is less than 0.233 mol%, the dielectric constant may not be improved. If the content of La in the dielectric ceramic composition exceeds 0.699 mol%, the insulation resistance may be reduced or the dielectric loss (ie, dissipation factor (DF)) may be reduced.
[0103] Hereinafter, the present disclosure will be described in more detail with reference to examples and comparative examples. However, the examples and comparative examples are provided to help a specific understanding of the present disclosure, and the scope of the embodiments according to the present disclosure is not limited thereto.
[0104] (Example)
[0105] In the example, additives (such as Dy, Al, Mg, Zn, etc.), a binder, and an organic solvent (e.g., ethanol) are added to a dielectric material powder (matrix material main component) including a barium titanate (BaTiO3)-based matrix material main component in powder form, and wet mixed to prepare a dielectric slurry. Then, the dielectric slurry is applied to a carrier film to be dried, thereby providing a ceramic green sheet. Through the above process, a dielectric layer can be formed.
[0106] In this case, the particle size of the additives of all elements is 40% or less relative to the particle size of barium titanate added as a main component of the base material, and the additives of all elements are monodispersed and added.
[0107] In the embodiment, the content of ZnO in the dielectric slurry (i.e., the total content of ZnO in the dielectric composition) is greater than or equal to 0.1 mol% and less than 0.4 mol% relative to 100 mol% of the main component of the matrix material. In detail, in Examples 1 and 2, the total content of zinc oxide (ZnO) and magnesium (Mg) is less than 0.8 mol% relative to 100 mol% of the main component of the matrix material.
[0108] In Example 1, ZnO was added to the dielectric slurry to adjust the content of ZnO to 0.1 mol % with respect to 100 mol % of the main component of the base material.
[0109] In Example 2, ZnO was added to the dielectric slurry to adjust the content of ZnO to 0.2 mol % with respect to 100 mol % of the main component of the base material.
[0110] Regarding the ceramic green sheet, a dielectric slurry is manufactured into a sheet having a thickness of several micrometers using a doctor blade method.
[0111] Then, a conductive paste for an internal electrode in which an average size of nickel particles is 0.1 μm to 0.2 μm and includes 40 parts by weight to 50 parts by weight of nickel powder relative to 100 parts by weight of the conductive paste is provided.
[0112] Conductive paste for internal electrodes is applied to the green sheets using a screen printing method to form internal electrode patterns. Then, the green sheets having the internal electrode patterns disposed therein are stacked to form a stacked body, which is then pressed and cut.
[0113] Then, the cut stacked body is heated to remove the binder, and then sintering is performed at a high temperature in a reducing atmosphere to form a ceramic body.
[0114] In the sintering process, sintering is performed at a temperature of 1100°C to 1200°C in a reducing atmosphere (0.1% H2 / 99.9% N2, H2O / H2 / N2 atmosphere) for 2 hours, and then reoxidation is performed at 1000°C in a nitrogen (N2) atmosphere for 3 hours for heat treatment.
[0115] Then, the sintered ceramic body is subjected to a termination process using copper (Cu) paste and electrode sintering to complete the external electrode.
[0116] In addition, after sintering, the dielectric layer 111 and the first and second internal electrodes 121 and 122 inside the ceramic body 110 are manufactured to have a thickness of 0.4 μm or less.
[0117] (Comparative Example 1)
[0118] In the case of Comparative Example 1, as a conventional case, ZnO was not added, and the other manufacturing processes were the same as those in the above-described examples.
[0119] (Comparative Example 2)
[0120] In the case of Comparative Example 2, ZnO was added to the dielectric slurry, the content of ZnO was adjusted to 0.4 mol % (relative to 100 mol % of the main component of the base material), and the other manufacturing processes were the same as those in the above-described embodiment.
[0121] Tests were performed on Examples 1 and 2 and Comparative Examples 1 and 2 (prototype multilayer ceramic capacitors (i.e., prototype MLCC) samples) completed as described above regarding dielectric loss (i.e., loss factor (DF)) and the effective capacity change rate at each of 1V DC and 3V DC.
[0122] Table 1 described below shows the dielectric loss (i.e., loss factor (DF)) and the effective capacity change rate at 1V DC and 3V DC of the prototype multilayer ceramic capacitor (i.e., prototype MLCC) chips according to the experimental examples (Examples 1 and 2 and Comparative Examples 1 and 2).
[0123] [Table 1]
[0124]
[0125] Referring to Table 1, as a conventional case, in the case of Comparative Example 1 in which zinc oxide (ZnO) was not added, there was a problem that the dielectric loss (ie, dissipation factor (DF)) was large, and there was a problem that the effective capacity change rate at each of 1 V DC and 3 V DC was high.
[0126] On the other hand, in Examples 1 and 2, the content of ZnO relative to 100 mol% of the main component of the base material satisfies 0.1 mol% or more and less than 0.4 mol%. In this case, it was confirmed that the dielectric loss (ie, loss factor (DF)) was reduced and the effective capacity change rate under the DC electric field was reduced.
[0127] Here, in Comparative Example 2, ZnO was added so that the content of ZnO was 0.4 mol% relative to 100 mol% of the main component of the base material. The dielectric loss (ie, dissipation factor (DF)) was reduced, and the effective capacity change rate under the DC electric field was reduced. However, the reliability degradation phenomenon was significant.
[0128] Figure 3 is a graph showing dielectric grain sizes according to the examples of the experimental examples and the comparative example.
[0129] Reference Figure 3 , as a conventional case, in the case of Comparative Example 1 in which ZnO was not added to the dielectric ceramic composition, sintering was performed at 1140° C., but the absence of a grain growth suppressing effect was confirmed.
[0130] On the other hand, in the case of Example 1, the content of ZnO in the dielectric ceramic composition was 0.1 mol% relative to 100 mol% of the main component of the base material, and sintering was performed at a sintering temperature of 1120°C, which was reduced by 20°C, and it was confirmed that densification occurred and the grain growth suppression effect was significant.
[0131] In addition, in the case of Comparative Example 2, the content of ZnO in the dielectric ceramic composition was 0.4 mol% relative to 100 mol% of the main component of the base material, and sintering was performed at a sintering temperature of 1120° C., which was lowered by 20° C., and it was confirmed that densification occurred and the grain growth suppression effect was significant. However, as will be described later, there was a problem in terms of reliability.
[0132] Figure 4A and Figure 4B It is a graph of the results of strict reliability evaluation based on the test example and the comparative example.
[0133] Figure 4AThe results of Example 1 are shown, and the content of ZnO in the dielectric ceramic composition is 0.1 mol% relative to 100 mol% of the main component of the base material. In this case, it can be seen that there is no defect in the strict reliability evaluation, and therefore, the reliability is excellent.
[0134] Figure 4B The results of Comparative Example 2 are shown, and the content of ZnO in the dielectric ceramic composition is 0.4 mol% relative to 100 mol% of the main component of the base material. In this case, a large number of defects were found in a strict reliability evaluation, and thus reliability degradation was seen.
[0135] As explained above, according to the embodiments in the present disclosure, the dielectric ceramic composition used in the dielectric layer formed in the ceramic body includes zinc oxide (ZnO) as a subcomponent, and its content is controlled. Therefore, grain growth suppression and low-temperature densification can be achieved. Therefore, under a DC electric field, the effective capacity change rate can be reduced and reliability can be improved.
[0136] While exemplary embodiments have been shown and described above, it will be apparent to those skilled in the art that modifications and variations may be made without departing from the scope of the present invention as defined by the appended claims.
Claims
1. A multilayer ceramic capacitor comprising: a ceramic body including a dielectric layer and first and second internal electrodes, the first and second internal electrodes being disposed opposite to each other with the dielectric layer interposed therebetween; and a first external electrode and a second external electrode disposed on an exterior of the ceramic body, wherein the first external electrode is electrically connected to the first internal electrode and the second external electrode is electrically connected to the second internal electrode, Wherein, the dielectric layer includes dielectric grains, and the dielectric grains contain a dielectric ceramic composition. The dielectric ceramic composition comprises a main component of a barium titanate-based matrix material and a subcomponent, wherein the subcomponent comprises a first subcomponent and a second subcomponent, wherein the first subcomponent comprises ZnO, the second subcomponent comprises Mg, and ZnO is segregated at a grain boundary, and Wherein, the content of ZnO in the dielectric ceramic composition is greater than 0.1 mol % and less than 0.4 mol % relative to 100 mol % of the main component of the barium titanate-based matrix material.
2. The multilayer ceramic capacitor according to claim 1, wherein The total content of ZnO and Mg is less than 0.8 mol % relative to 100 mol % of the main component of the barium titanate-based matrix material.
3. The multilayer ceramic capacitor according to claim 1, wherein The first subcomponent also includes at least one oxide selected from the group consisting of Mn oxide, V oxide, Cr oxide, Fe oxide, Ni oxide, Co oxide and Cu oxide and / or at least one carbonate selected from the group consisting of Mn carbonate, V carbonate, Cr carbonate, Fe carbonate, Ni carbonate, Co carbonate and Cu carbonate, and the content of the first subcomponent is greater than or equal to 0.1 mol% and less than or equal to 2.0 mol% relative to 100 mol% of the main component of the barium titanate-based matrix material.
4. The multilayer ceramic capacitor according to claim 1, wherein Relative to 100 mol % of the main component of the barium titanate-based matrix material, the content of the second auxiliary component is greater than or equal to 0.2 mol % and less than or equal to 0.7 mol %, and Mg in the second auxiliary component is added in the form of oxide and / or carbonate.
5. The multilayer ceramic capacitor according to claim 1, wherein Relative to 100 mol% of the main component of the barium titanate-based matrix material, the subcomponent also includes a third subcomponent greater than or equal to 0.001 mol% and less than or equal to 0.5 mol%, and the third subcomponent includes at least one of Si oxide and Al oxide or the third subcomponent includes a glass compound containing Si.
6. The multilayer ceramic capacitor according to claim 1, wherein Relative to 100 mol % of the main component of the barium titanate-based matrix material, the subcomponent further includes a fourth subcomponent of greater than or equal to 0.001 mol % and less than or equal to 4.0 mol %, and the fourth subcomponent includes at least one oxide selected from the group consisting of Dy oxide, Y oxide, Ho oxide, Er oxide, Ce oxide, Nd oxide, Pm oxide, Eu oxide, Gd oxide, Tm oxide, Yb oxide, Lu oxide, La oxide and Sm oxide and / or at least one carbonate selected from the group consisting of Dy carbonate, Y carbonate, Ho carbonate, Er carbonate, Ce carbonate, Nd carbonate, Pm carbonate, Eu carbonate, Gd carbonate, Tm carbonate, Yb carbonate, Lu carbonate, La carbonate and Sm carbonate.
7. The multilayer ceramic capacitor according to claim 6, wherein: La is disposed at the boundaries of the dielectric grains.
8. The multilayer ceramic capacitor according to claim 1, wherein The thickness of the dielectric layer is 0.4 μm or less.
9. The multilayer ceramic capacitor according to claim 1 or 8, wherein: The thickness of the first internal electrode and the second internal electrode is 0.4 μm or less.