A low-temperature hydrogen plasma assisted annealing method for improving the performance of passivation contact structure and TOPCon solar cell
The low-temperature hydrogen plasma-assisted annealing method solves the problem of performance attenuation of the passivated contact structure after high-temperature sintering, significantly improves the efficiency and passivation performance of TOPCon solar cells, reduces energy consumption, and the equipment is compatible with existing production lines.
Patent Information
- Application Number
- CN202210297222.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-03-24
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2042-03-24
AI Technical Summary
The passivation performance of the existing passivated contact structure is seriously attenuated after high-temperature sintering, and it is difficult to effectively repair grain boundary defects and impurities through existing low-temperature annealing technology, resulting in a decrease in the efficiency of TOPCon solar cells.
The low-temperature hydrogen plasma-assisted annealing method is used to anneal the silicon wafer with a passivated contact structure using hydrogen or a mixed gas containing hydrogen. By introducing hydrogen plasma, the grain boundary defects are repaired after high-temperature sintering, and the defects at the interface and grain boundaries are reduced. Carrier recombination.
The performance of the passivated contact structure is significantly improved, the photoelectric conversion efficiency of the solar cell is improved, and energy consumption is reduced. The equipment is compatible with existing production lines, easy to process in batches, and has low operating costs.
Smart Images

Figure CN114823969B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a low-temperature hydrogen plasma assisted annealing method for improving the performance of a passivation contact structure and a TOPCon solar cell. Background Art
[0002] At present, crystalline silicon (c-Si)-based solar cells have a market share of over 95% in commercial solar cells. To further improve the competitiveness of photovoltaics with traditional energy sources, the conversion efficiency (PCE) of c-Si solar cells must be continuously improved. In this context, solar cell production technology has gradually transitioned from traditional aluminum back surface field (Al-BSF) cells to passivated emitter and back cell (PERC) technology, among which the efficiency of currently produced PERC cells has exceeded 23%. However, PERC cells have local metal silicon contacts, which increases the process complexity and the high degree of recombination at the contact, so that the efficiency of PERC cells has reached a bottleneck and it is difficult to improve it further.
[0003] In order to improve the efficiency of solar cells, the concept of passivation contacts was developed to minimize the recombination losses in the contact area. It is generally believed in the industry that the next generation of crystalline silicon solar cells that will replace PERC cell technology will be solar cells based on advanced passivation contact technology. In general, passivation contact technology can be divided into 2 different types: silicon heterojunction technology (SHJ) and polycrystalline silicon-based passivation contacts. Polycrystalline silicon-based passivation contacts consist of an ultra-thin tunneling silicon oxide layer and a doped polysilicon layer, sometimes also referred to as TOPCon. Silicon heterojunction (SHJ) contacts, consisting of an intrinsic and doped hydrogenated amorphous silicon (a-Si:H) stack, provide excellent surface passivation and have achieved a world record efficiency of 26.7%. However, SHJ technology is only applicable to low-temperature technology (<250℃), has a relatively narrow process window and requires expensive deposition systems. In addition, using traditional double-sided contact design, SHJ cells are affected by parasitic absorption of a-Si:H, which limits the short-circuit current density J sc . In contrast, the ultra-thin tunneling silicon oxide layer / doped polysilicon passivation contact shows very good high temperature resistance and also has very high efficiency potential, which is comparable to SHJ technology. Currently, by adopting a full-area polysilicon back contact, its cell efficiency has reached 25.8%. At the same time, this contact can be compatible with current solar cell production lines as a hole-selective passivation back contact, replacing the PERC type contact structure.
[0004] At present, in the field of tunneling oxide passivation contact (TOPCon) solar cells, whether it is low pressure chemical vapor deposition (LPCVD) technology or plasma enhanced chemical vapor deposition (PECVD) technology, when preparing ultra-thin tunneling silicon oxide + doped polysilicon passivation contact, the formed SiO2 / poly-Si(n+) / SiNx:H double-sided passivation contact structure will show serious attenuation of passivation performance after high temperature sintering, and the minority carrier lifetime and implicit open circuit voltage (iV oc ) have all dropped severely, and the saturation current density (J0) has increased significantly. The passivation performance of the battery is closely related to the battery conversion efficiency, which will also cause a decrease in the efficiency of the TOPCon battery. In the prior art, the efficiency improvement of the passivation contact structure in the n-type battery generally adopts the same production equipment as the p-type PERC battery, that is, after printing and sintering, a light recovery furnace is used for annealing, that is, high-intensity LED lights and heating equipment are used to achieve annealing efficiency improvement. This is because p-type batteries generally have a light-induced degradation effect (LID), so light needs to be used for recovery, but there is no light-induced degradation in n-type batteries, so light has limited efficiency improvement for n-type batteries. If a light recovery furnace is used to anneal the n-type battery, it is easy to consume a lot of energy to provide high light intensity, increase operating costs, and this method has limited improvement in passivation performance. In addition, as shown in Table 1, the existing low-temperature annealing technology for ultra-thin tunneling silicon oxide layer and doped polysilicon passivation contact structure can only repair the crystal defects generated after high-temperature sintering. At the same time, it is difficult to overcome the defect that the interface state defect density and the defects in the grain boundary increase and the H passivation effect decreases due to the large amount of overflow of H atoms in polysilicon and anti-reflection passivation film during high-temperature sintering. Therefore, it is still difficult to effectively improve the passivation performance and electrical performance of the battery by only performing low-temperature annealing after high-temperature sintering. Therefore, how to obtain an annealing method that can not only repair grain boundary defects and impurities, but also reduce carrier recombination at the interface and grain boundary is of great significance for improving the passivation performance and electrical performance of the battery.
[0005] Table 1 Data changes of minority carrier lifetime and iVoc before and after sintering of N-type TOPCon battery with double-sided symmetric structure
[0006] Summary of the invention
[0007] The technical problem to be solved by the present invention is to overcome the deficiencies of the prior art and provide a low-temperature hydrogen plasma assisted annealing method and a TOPCon solar cell for improving the performance of a passivation contact structure.
[0008] In order to solve the above technical problems, the technical solution adopted by the present invention is:
[0009] A low-temperature hydrogen plasma assisted annealing method for improving the performance of a passivation contact structure uses hydrogen or a mixed gas containing hydrogen as a process gas to anneal a silicon wafer prepared with the passivation contact structure.
[0010] The above-mentioned low-temperature hydrogen plasma assisted annealing method for improving the performance of the passivation contact structure is further improved, in which when the process gas used in the annealing process is hydrogen, the flow rate of hydrogen is 500sccm to 2000sccm;
[0011] Alternatively, during the annealing process, when the process gas used is a mixed gas containing hydrogen, the process gas is a mixed gas of hydrogen and argon; in the mixed gas of hydrogen and argon, the flow rate of the hydrogen is 500sccm to 2000sccm, and the flow rate of the argon is 500sccm to 2000sccm.
[0012] The above-mentioned low-temperature hydrogen plasma assisted annealing method for improving the performance of the passivation contact structure is further improved in that the temperature of the annealing treatment is 300° C. to 500° C.; and the time of the annealing treatment is 10 min to 60 min.
[0013] The above-mentioned low-temperature hydrogen plasma assisted annealing method for improving the performance of the passivation contact structure is further improved by using a tubular PECVD device to anneal the silicon wafer prepared with the passivation contact structure; during the annealing process, the process parameters of the tubular PECVD device are: the plasma power frequency is 40kHz, the power is 1000W~5000W, and the RF on-off ratio is 1:10~1:30.
[0014] The above-mentioned low-temperature hydrogen plasma assisted annealing method for improving the performance of the passivation contact structure is further improved, wherein the silicon wafer prepared with the passivation contact structure is prepared by the following method:
[0015] (1) Cleaning and texturing of silicon wafers;
[0016] (2) sequentially preparing an ultra-thin tunneling oxide layer and an intrinsic amorphous silicon layer on the surface of a silicon wafer;
[0017] (3) phosphorus-doping the intrinsic amorphous silicon layer to prepare a phosphorus-doped polycrystalline silicon layer;
[0018] (4) preparing an anti-reflection passivation film on both sides of a silicon wafer having an ultra-thin tunneling oxide layer and a phosphorus-doped polysilicon layer;
[0019] (5) The silicon wafer prepared with the anti-reflection passivation film is subjected to high-temperature rapid sintering to obtain a silicon wafer prepared with a passivation contact structure.
[0020] The above-mentioned low-temperature hydrogen plasma assisted annealing method for improving the performance of the passivation contact structure is further improved by using low-pressure chemical vapor deposition technology to sequentially prepare an ultra-thin tunneling oxide layer and an intrinsic amorphous silicon layer; when the ultra-thin tunneling oxide layer is prepared by low-pressure chemical vapor deposition technology, the preparation process conditions are: temperature of 500°C to 700°C, process gas is O2, flow rate is 5000sccm to 10000sccm, process pressure is 20Pa to 200Pa, and process time is 10min to 60min; when the intrinsic amorphous silicon layer is prepared by low-pressure chemical vapor deposition technology, the preparation process conditions are: temperature of 500°C to 700°C, process gas is SiH4, flow rate is 500sccm to 2000sccm, process pressure is 20Pa to 100Pa, and process time is 10min to 30min.
[0021] The above-mentioned low-temperature hydrogen plasma assisted annealing method for improving the performance of the passivation contact structure is further improved by using plasma enhanced chemical vapor deposition technology to sequentially prepare an ultra-thin tunneling oxide layer and an intrinsic amorphous silicon layer; when the ultra-thin tunneling oxide layer is prepared by plasma enhanced chemical vapor deposition technology, the preparation process conditions are: power supply frequency is 40kHz~300kHz, process temperature is 300℃~600℃, process time is 10s~100s, process pressure is 50Pa~300Pa, process gas is a mixed gas of N2O and Ar, the volume ratio of N2O and Ar in the mixed gas of N2O and Ar is 1~5:1~10, the process power is 1000~10000W, and the RF on-off ratio is 1: 10~1:30; when the intrinsic amorphous silicon layer is prepared by plasma enhanced chemical vapor deposition technology, the preparation process conditions are: power frequency is 40kHz~300kHz, process temperature is 300℃~600℃, process time is 100s~1000s, process pressure is 100Pa~300Pa, process gas is a mixed gas of SiH4 and Ar or a mixed gas of SiH4 and H2, the volume ratio of SiH4 and Ar in the mixed gas of SiH4 and Ar is 1:1~1:10, the volume ratio of SiH4 and H2 in the mixed gas of SiH4 and H2 is 1:1~1:10, the process power is 5000~10000W, and the RF on-off ratio is 1:10~1:30.
[0022] The above-mentioned low-temperature hydrogen plasma assisted annealing method for improving the performance of the passivation contact structure is further improved, wherein the thickness of the ultra-thin tunneling oxide layer is 1nm to 3nm; the ultra-thin tunneling oxide layer is SiO2; and the thickness of the intrinsic amorphous silicon layer is 50nm to 200nm.
[0023] The above-mentioned low-temperature hydrogen plasma assisted annealing method for improving the performance of the passivation contact structure is further improved by using low-pressure diffusion technology to dope the intrinsic amorphous silicon layer with phosphorus, and the doping process conditions are: diffusion temperature 700°C~800°C, diffusion pressure 100mbar~300mbar, diffusion small nitrogen flow 500sccm~2000sccm, diffusion large nitrogen flow 1000sccm~5000sccm, diffusion oxygen 500sccm~2000sccm, diffusion time 10min~30min; advancement temperature 850°C~900°C, large nitrogen flow 2000sccm~5000sccm, oxygen flow 500sccm~2000sccm, advancement time 20min~40min.
[0024] The above-mentioned low-temperature hydrogen plasma assisted annealing method for improving the performance of the passivation contact structure is further improved by using plasma enhanced chemical vapor deposition technology to dope the intrinsic amorphous silicon layer with phosphorus. The doping process conditions are: the power frequency is 40kHz~300kHz, the process temperature is 300℃~600℃, the process time is 100s~1000s, the process pressure is 100Pa~300Pa, the process gas is a mixed gas of SiH4, Ar and PH3 or a mixed gas of SiH4, H2 and PH3, the volume ratio of SiH4, Ar and PH3 in the mixed gas of SiH4, Ar and PH3 is 1:1:1~1:10:1, the volume ratio of SiH4, H2 and PH3 in the mixed gas of SiH4, H2 and PH3 is 1:1:1~1:10:1, the process power is 5000W~10000W, and the RF on-off ratio is 1:10~1:30.
[0025] The above-mentioned low-temperature hydrogen plasma assisted annealing method for improving the performance of the passivation contact structure is further improved. When the intrinsic amorphous silicon layer is phosphorus-doped using plasma enhanced chemical vapor deposition technology, it also includes high-temperature annealing treatment of the silicon wafer prepared with an ultra-thin tunneling oxide layer and a phosphorus-doped polysilicon layer; the temperature of the high-temperature annealing treatment is 700°C to 1000°C; the time of the high-temperature annealing treatment is 30min to 60min.
[0026] The above-mentioned low-temperature hydrogen plasma assisted annealing method for improving the performance of the passivation contact structure is further improved. In step (1), the silicon wafer is an N-type silicon wafer; the resistivity of the silicon wafer is 1Ωcm~3Ωcm; before the silicon wafer is cleaned, the silicon wafer is also pre-cleaned; the solution used in the pre-cleaning process is a potassium hydroxide aqueous solution; the concentration of the potassium hydroxide aqueous solution is 10wt%~20wt%; the temperature of the solution in the pre-cleaning process is 8005℃; the treatment time of the solution in the pre-cleaning process is 300050s.
[0027] The above-mentioned low-temperature hydrogen plasma assisted annealing method for improving the performance of the passivation contact structure is further improved. In step (3), a tubular PECVD device is used to prepare an anti-reflection passivation film; the anti-reflection passivation film is a SiNx:H film.
[0028] The above-mentioned low-temperature hydrogen plasma assisted annealing method for improving the performance of the passivation contact structure is further improved. In step (4), the temperature of the high-temperature rapid sintering is 700°C to 900°C; and the time of the high-temperature rapid sintering is 5 to 30 seconds.
[0029] As a general technical concept, the present invention also provides a TOPCon solar cell, which is prepared by the above-mentioned low-temperature hydrogen plasma assisted annealing method for improving the performance of the passivation contact structure.
[0030] The above-mentioned TOPCon solar cell is further improved, wherein the TOPCon solar cell includes a silicon substrate, and the front side of the silicon substrate is provided with a front aluminum oxide layer and a front anti-reflection passivation layer in sequence from the inside to the outside; the back side of the substrate is provided with an ultra-thin tunneling oxide layer, a phosphorus-doped polysilicon layer, and a back anti-reflection passivation layer in sequence from the inside to the outside.
[0031] Compared with the prior art, the advantages of the present invention are:
[0032] In view of the defects of the passivation performance improvement effect of the passivation contact structure and the battery electrical performance improvement effect in the existing annealing process, the present invention proposes a low-temperature hydrogen plasma assisted annealing method for improving the performance of the passivation contact structure, using hydrogen or a mixed gas containing hydrogen as a process gas, annealing a silicon wafer prepared with a passivation contact structure, and after high-temperature sintering, annealing under hydrogen plasma, which can not only repair grain boundary defects and impurities by low-temperature annealing, but also saturate the dangling bonds at the film interface and the crystal internal grain boundary by introducing H plasma, reduce the carrier recombination at the interface and the grain boundary, thereby achieving a good passivation effect, which is beneficial to improve the photoelectric conversion efficiency of solar cells. In addition, the present invention does not require lighting conditions, which can reduce energy consumption, and the equipment used for low-temperature H plasma assisted annealing of the present invention is a conventional industrial tubular PECVD equipment, which is compatible with existing production lines. The low-temperature hydrogen plasma assisted annealing method for improving the performance of the passivation contact structure of the present invention has the advantages of easy batch processing and low operating cost. It can be widely used to improve the passivation performance of back-side passivation contact structures, ultra-thin tunneling oxide layers and doped polysilicon layer double-sided passivation contact structures, and the passivation performance is greatly improved, which is of great significance for improving the production capacity of TOPCon solar cells. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] In order to make the purpose, technical solution and advantages of the embodiments of the present invention more clear, the technical solution in the embodiments of the present invention will be clearly and completely described below in conjunction with the accompanying drawings in the embodiments of the present invention.
[0034] Figure 1 This is a process flow chart of low-temperature hydrogen plasma assisted annealing for improving the performance of the passivation contact structure in Example 1 of the present invention.
[0035] Figure 2 Schematic diagram of the double-sided passivation contact structure in Example 1 of the present invention.
[0036] Figure 3 Schematic diagram of the structure of the TOPCon solar cell in Example 1 of the present invention.
[0037] Figure 4 This is a process flow chart of low-temperature hydrogen plasma assisted annealing for improving the performance of the passivation contact structure in Example 2 of the present invention.
[0038] Legend:
[0039] 1. N-type silicon substrate; 2. Front aluminum oxide layer; 3. Front anti-reflection passivation layer; 4. Ultra-thin tunneling oxide layer; 5. Phosphorus-doped polysilicon layer; 6. Back anti-reflection passivation layer; 7. Electrode. DETAILED DESCRIPTION
[0040] The present invention is further described below in conjunction with the accompanying drawings and specific preferred embodiments, but the protection scope of the present invention is not limited thereby.
[0041] In the following examples, unless otherwise specified, the raw materials and instruments used are commercially available, the processes used are conventional processes, and the equipment used are conventional equipment.
[0042] Embodiment 1:
[0043] A low-temperature hydrogen plasma assisted annealing method for improving the performance of a passivation contact structure, specifically using hydrogen as a process gas to anneal a silicon wafer prepared with a passivation contact structure, the process flow chart is as follows Figure 1 As shown, the following steps are included:
[0044] (1) An N-type silicon wafer with a resistivity of 1 Ωcm and a size of 158.75 mm*158.75 mm was placed in a slot machine for pre-cleaning and damage layer removal. The solution was a potassium hydroxide aqueous solution with a potassium hydroxide concentration of 10% wt. The treatment time was 300 s and the treatment temperature was 80°C. After treatment, it was rinsed with deionized water and dried.
[0045] (2) Clean, texture and dry the silicon wafer.
[0046] (3) The cleaned and textured silicon wafer is placed in a tubular LPCVD furnace, and a 1.5nm ultra-thin tunneling oxide layer and a 150nm intrinsic amorphous silicon layer are sequentially deposited on the front and back sides of the silicon wafer, wherein the deposition process of the ultra-thin tunneling oxide layer is as follows: process temperature 600°C, process time 30min, process pressure 200Pa, process gas O2, O2 flow rate 8000sccm. The deposition process conditions of the intrinsic amorphous silicon layer are as follows: process temperature 600°C, process time 30min, process pressure 26Pa, process gas SiH4, segmented gas intake, flow ratio 250sccm:350sccm.
[0047] (4) The intrinsic amorphous silicon layer is doped with phosphorus using low-pressure diffusion technology, and the silicon wafer is transferred to a phosphorus diffusion furnace for phosphorus diffusion doping to obtain a phosphorus-doped polycrystalline silicon layer. The doping process is as follows: diffusion temperature 780°C, diffusion pressure 150 mbar, diffusion small nitrogen flow 800 sccm, diffusion large nitrogen flow 2000 sccm, diffusion oxygen 800 sccm, diffusion time 15 min; push temperature 890°C, large nitrogen flow 3000 sccm, oxygen flow 800 sccm, push time 30 min.
[0048] (5) After phosphorus diffusion doping is completed, an anti-reflection passivation film is prepared, specifically, the silicon wafer is transferred to a tubular PECVD furnace for double-sided SiNx:H deposition. After the anti-reflection passivation film is prepared, a minority carrier lifetime test is performed.
[0049] (6) After testing the minority carrier lifetime, the silicon wafer is placed in a chain high-temperature sintering furnace for high-temperature rapid sintering, with a peak temperature of 800°C and a time of 5 seconds. The minority carrier lifetime after sintering is then tested. After high-temperature rapid sintering, SiO2+poly-Si(n + ) Double-sided passivated contact structure, such as Figure 2 shown.
[0050] (7) The sintered silicon wafer is placed in a tubular PECVD furnace for low-temperature hydrogen plasma assisted annealing. The annealing temperature is 400°C, the annealing time is 20 min, the plasma power frequency is 40 kHz, the power is 2000 W, the RF on-off ratio is 1:30, the process gas is H2, and the H2 flow rate is 2000 sccm, thereby completing the treatment of the passivated contact structure.
[0051] The surface passivation effect of the samples before sintering, after sintering and after low-temperature hydrogen plasma annealing was tested using Sinton WCT-120. The test results are shown in Table 2.
[0052] Table 2 Changes in minority carrier lifetime, iVoc, J0 and iFF of the N-type TOPCon cell with double-sided symmetric structure prepared by LPCVD before and after sintering and after low-temperature hydrogen plasma annealing
[0053]
[0054]
[0055] It can be seen from Table 2 that the average implicit open circuit voltage iVoc of the sample before sintering is 735mV, the iVoc distribution is 728~739mV, and the corresponding minority carrier lifetime is 4829 microseconds. After the sample is sintered, the minority carrier lifetime and iVoc decrease significantly. However, after low-temperature hydrogen plasma annealing, the minority carrier lifetime and iVoc increase significantly, indicating that the passivation effect is significantly improved.
[0056] After low-temperature hydrogen plasma assisted annealing, the silicon wafer is further made into TOPCon solar cells, such as Figure 3 As shown, the prepared TOPCon solar cell includes a silicon N-type substrate 1, and the front side of the N-type silicon substrate 1 is provided with a front aluminum oxide layer 2 and a front anti-reflection passivation layer 3 in sequence from the inside to the outside; the back side of the N-type substrate 1 is provided with an ultra-thin tunneling oxide layer 4, a phosphorus-doped polysilicon layer 5, and a back anti-reflection passivation layer 6 in sequence from the inside to the outside. In the above-mentioned TOPCon solar cell, the N-type silicon substrate 1 is an N-type silicon wafer, the front aluminum oxide layer 2 is an Al2O3 film, the front anti-reflection passivation layer 3 is a SiNx:H film, the ultra-thin tunneling oxide layer 4 is a SiO2 film, the phosphorus-doped polysilicon layer 5 is poly-Si(n+), and the back anti-reflection passivation layer 6 is a SiNx:H film. Electrodes are also provided on the front and back sides of the TOPCon solar cell, and the electrodes are Ag electrodes.
[0057] Example 2
[0058] A low-temperature hydrogen plasma assisted annealing method for improving the performance of a passivation contact structure, specifically using hydrogen as a process gas to anneal a silicon wafer prepared with a passivation contact structure, the process flow chart is as follows Figure 4 As shown, the following steps are included:
[0059] (1) An N-type silicon wafer with a resistivity of 1 Ωcm and a size of 158.75 mm*158.75 mm was placed in a slot machine for pre-cleaning and damage layer removal. The solution was a potassium hydroxide aqueous solution with a potassium hydroxide concentration of 10% wt. The treatment time was 300 s and the treatment temperature was 80°C. After treatment, it was rinsed with deionized water and dried.
[0060] (2) Clean, texture and dry the silicon wafer.
[0061] (3) The cleaned and textured silicon wafer is placed in a tubular PECVD furnace, and an ultra-thin tunneling silicon oxide layer and a phosphorus-doped amorphous silicon layer are sequentially deposited on the front and back sides of the silicon wafer.
[0062] A 1.5 nm ultra-thin tunneling silicon oxide layer was prepared. The deposition process was: power frequency was 150 kHz, process temperature was 480 °C, process time was 20 s, process pressure was 120 Pa, process gases were N2O and Ar, N2O / Ar=2000 sccm:2000 sccm, process power was 8000 W, and RF on-off ratio was 1:20.
[0063] The doped amorphous silicon is multi-layer gradient doped, and the deposition is mainly divided into two steps. The first step is to deposit a 70nm intrinsic amorphous silicon layer. The process conditions are as follows: the power frequency is 40kHz, the process temperature is 480℃, the process time is 600s, the process pressure is 200Pa, the process gas is SiH4 and Ar, SiH4 / Ar=1000sccm:4000sccm, the process power is 8000W, and the RF on-off ratio is 1:20. The second step is to deposit an 80nm doped amorphous silicon layer. The process conditions are as follows: the power frequency is 40kHz, the process temperature is 480℃, the process time is 600s, the process pressure is 200Pa, the process gas is SiH4, Ar and PH3, SiH4 / Ar / PH3=1000sccm:4000sccm:800sccm, the process power is 8000W, and the RF on-off ratio is 1:20.
[0064] After the single-side preparation is completed, the silicon wafer is turned over and the above operation is repeated to make an ultra-thin tunneling silicon oxide layer and a phosphorus-doped amorphous silicon layer on the other side.
[0065] (4) The prepared double-sided ultra-thin tunneling silicon oxide layer + a-Si:H(n+) structure silicon wafer is placed in an annealing furnace and subjected to high-temperature annealing treatment in a nitrogen atmosphere at a temperature of 850°C, a N2 flow rate of 5000sccm, and an annealing time of 60min.
[0066] (5) After annealing, an anti-reflection passivation film is prepared, specifically, the silicon wafer is transferred to a tubular PECVD furnace for double-sided SiNx:H deposition. After the anti-reflection passivation film is prepared, a minority carrier lifetime test is performed.
[0067] (6) After testing the minority carrier lifetime, the silicon wafer is placed in a chain high-temperature sintering furnace for rapid high-temperature annealing treatment, with a peak temperature of 800°C and a time of 5 seconds. The minority carrier lifetime after sintering is then tested. After high-temperature rapid sintering treatment, SiO2+poly-Si(n + ) Double-sided passivated contact structure, such as Figure 2 shown.
[0068] (7) The sintered silicon wafer is placed in a tubular PECVD furnace for low-temperature hydrogen plasma assisted annealing. The annealing temperature is 400°C, the annealing time is 20 min, the plasma power frequency is 40 kHz, the power is 2000 W, the RF on-off ratio is 1:30, the process gas is H2, and the H2 flow rate is 2000 sccm.
[0069] The surface passivation effect of the samples before sintering, after sintering and after low-temperature hydrogen plasma annealing was tested using Sinton WCT-120. The test results are shown in Table 3.
[0070] Table 3 Data changes of minority carrier lifetime, iVoc, J0 and iFF of N-type TOPCon cells with double-sided symmetric structure prepared by PECVD before and after sintering and after low-temperature H plasma annealing
[0071]
[0072]
[0073] As shown in Table 3, the average implicit open circuit voltage iVoc of the sample before sintering is 724mV, and the iVoc distribution is 721-726mV, corresponding to the minority carrier lifetime of 2986 microseconds. After the sample is sintered, the minority carrier lifetime and iVoc decrease significantly. However, after low-temperature H plasma annealing, the minority carrier lifetime and iVoc increase significantly, indicating that the passivation effect is significantly improved.
[0074] After low-temperature hydrogen plasma assisted annealing, the silicon wafer is further made into TOPCon solar cells, such as Figure 3 As shown, the prepared TOPCon solar cell includes a silicon N-type substrate 1, and the front side of the N-type silicon substrate 1 is provided with a front aluminum oxide layer 2 and a front anti-reflection passivation layer 3 in sequence from the inside to the outside; the back side of the N-type substrate 1 is provided with an ultra-thin tunneling oxide layer 4, a phosphorus-doped polysilicon layer 5, and a back anti-reflection passivation layer 6 in sequence from the inside to the outside. In the above-mentioned TOPCon solar cell, the N-type silicon substrate 1 is an N-type silicon wafer, the front aluminum oxide layer 2 is an Al2O3 film, the front anti-reflection passivation layer 3 is a SiNx:H film, the ultra-thin tunneling oxide layer 4 is a SiO2 film, the phosphorus-doped polysilicon layer 5 is poly-Si(n+), and the back anti-reflection passivation layer 6 is a SiNx:H film. Electrodes 7 are also provided on the front and back sides of the TOPCon solar cell, and the electrodes are Ag electrodes.
[0075] Comparative Example
[0076] A low-temperature annealing method for a passivated contact structure, wherein a silicon wafer having a passivated contact structure is annealed in a hydrogen-free atmosphere, and comprises the following steps:
[0077] (1) An N-type silicon wafer with a resistivity of 1 Ωcm and a size of 158.75 mm*158.75 mm was placed in a slot machine for pre-cleaning and damage layer removal. The solution was a potassium hydroxide aqueous solution with a potassium hydroxide concentration of 10% wt. The treatment time was 300 s and the treatment temperature was 80°C. After treatment, it was rinsed with deionized water and dried.
[0078] (2) Clean, texture and dry the silicon wafer.
[0079] (3) The cleaned and textured silicon wafer is placed in a tubular PECVD furnace, and an ultra-thin tunneling silicon oxide layer and a phosphorus-doped amorphous silicon layer are sequentially deposited on the front and back sides of the silicon wafer.
[0080] The deposition process of the ultra-thin tunneling silicon oxide layer is: power frequency is 150kHz, process temperature is 480℃, process time is 20s, process pressure is 120Pa, process gases are N2O and Ar, N2O / Ar=2000sccm:2000sccm, process power is 8000W, and RF on-off ratio is 1:20.
[0081] Doped amorphous silicon is multi-layer gradient doping, and the deposition is mainly divided into two steps. The first step is to deposit the intrinsic amorphous silicon layer. The process conditions are as follows: the power frequency is 40kHz, the process temperature is 480℃, the process time is 600s, the process pressure is 200Pa, the process gas is SiH4 and Ar, SiH4 / Ar=1000sccm:4000sccm, the process power is 8000W, and the RF on-off ratio is 1:20. The second step is the deposition of doped amorphous silicon. The process conditions are as follows: the power frequency is 40kHz, the process temperature is 480℃, the process time is 600s, the process pressure is 200Pa, the process gas is SiH4, Ar and PH3, SiH4 / Ar / PH3=1000sccm:4000sccm:800sccm, the process power is 8000W, and the RF on-off ratio is 1:20.
[0082] After the single-side preparation is completed, the silicon wafer is turned over and the above operation is repeated to make an ultra-thin tunneling silicon oxide layer and a phosphorus-doped amorphous silicon layer on the other side.
[0083] (4) The prepared double-sided ultra-thin tunneling silicon oxide layer + a-Si:H(n+) structure silicon wafer is placed in an annealing furnace for N2 annealing. The annealing temperature is 850°C, the N2 flow rate is 5000sccm, and the annealing time is 60min.
[0084] (5) After annealing, the silicon wafer is transferred to a tubular PECVD furnace for double-sided SiNx:H deposition and minority carrier lifetime testing.
[0085] (6) After testing the minority carrier lifetime, the steel is placed in a chain high-temperature sintering furnace for rapid high-temperature annealing treatment at a peak temperature of 800°C for 5 seconds, and then the minority carrier lifetime after sintering is tested.
[0086] (7) The sintered silicon wafer is placed in an annealing furnace for low-temperature annealing. The annealing temperature is 400°C, the annealing time is 20 minutes, the process gas is N2, and the N2 flow rate is 2000sccm.
[0087] The surface passivation effect of the samples before sintering, after sintering and after low temperature annealing was tested by Sinton WCT-120. The test results are shown in Table 4.
[0088] Table 4 Data changes of minority carrier lifetime, iVoc, J0 and iFF of N-type TOPCon cells with double-sided symmetric structure prepared by PECVD before and after sintering and low-temperature annealing
[0089]
[0090]
[0091] As shown in Table 4, the average implicit open circuit voltage iVoc≈719mV before sintering, iVoc distribution is 716~722mV, and the corresponding minority carrier lifetime is 2333 microseconds. After sintering, the minority carrier lifetime and iVoc decreased significantly, and the minority carrier lifetime and iVoc were 1473 microseconds and 707mV respectively. However, after low-temperature annealing, the minority carrier lifetime and iVoc increased slightly, and the minority carrier lifetime increased to 1541 microseconds, and iVoc increased to 709mV, indicating that the passivation effect is not as obvious as that of low-temperature H plasma annealing.
[0092] From Tables 2-4, it can be seen that by comparing the comparative example and Example 1 with Example 2, it can be found that SiO2+poly-Si(n +)+SiNx:H double-sided passivation contact structure will show a significant decrease in minority carrier lifetime and iVoc after sintering, but after low-temperature hydrogen plasma annealing, the minority carrier lifetime and iVoc will show a significant recovery or even improvement, while the minority carrier lifetime and iVoc of the battery that has only undergone low-temperature annealing have not been significantly restored. This is because only low-temperature annealing has certain benefits for crystal defect repair and passivation, but H atoms in polycrystalline silicon and anti-reflection passivation film will overflow in large quantities due to high-temperature sintering, resulting in an increase in interface state defect density and defects within grain boundaries, resulting in a decrease in H passivation effect. It can be seen that the simple low-temperature annealing method has a limited effect on the improvement of passivation performance, and further improves the efficiency of TOPCon solar cells. Completely different from this, in the present invention, after low-temperature hydrogen plasma annealing, because hydrogen plasma can saturate the defects and dangling bonds in polycrystalline silicon and anti-reflection passivation film, the defect state density in polycrystalline silicon and anti-reflection passivation film is reduced, thereby improving its passivation effect.
[0093] In addition, after being treated by the annealing methods of the comparative example, embodiment 1, and embodiment 2, the conversion efficiency of the TOPCon solar cell further prepared is shown in Table 5.
[0094] Table 5 Comparison of electrical parameters of TOPCon cells prepared under different annealing processes
[0095] Number of batteries Efficiency before annealing Efficiency after annealing Efficiency changes Example 1 50 22.95 23.28 0.33% Example 2 50 22.87 23.25 0.38% Comparative Example 50 22.84 22.98 0.14% Comparative Example (No Annealing) 50 22.85 22.85 0%
[0096] It can be seen from Table 5 that the low-temperature hydrogen plasma annealing treatment used in the present invention can significantly improve the conversion efficiency of TOPCon solar cells, wherein conventional low-temperature annealing can obtain an average efficiency improvement of 0.14%, while low-temperature hydrogen plasma annealing can obtain an efficiency improvement of more than 0.3%.
[0097] The above embodiments are only preferred implementations of the present invention, and the protection scope of the present invention is not limited to the above embodiments. All technical solutions under the concept of the present invention belong to the protection scope of the present invention. It should be pointed out that for ordinary technicians in this technical field, improvements and modifications without departing from the principle of the present invention should also be regarded as the protection scope of the present invention.
Claims
1. A low temperature hydrogen plasma assisted annealing method for improving the performance of a passivation contact structure, characterized in that: Using hydrogen or a mixed gas containing hydrogen as a process gas, a low-temperature hydrogen plasma-assisted annealing treatment is performed on a silicon wafer prepared with a passivation contact structure; the temperature of the low-temperature hydrogen plasma-assisted annealing treatment is 300°C to 500°C; The silicon wafer with the passivation contact structure is prepared by the following method: (1) Cleaning and texturing of silicon wafers; (2) Sequentially preparing an ultra-thin tunneling oxide layer and an intrinsic amorphous silicon layer on the surface of a silicon wafer; (3) doping the intrinsic amorphous silicon layer with phosphorus to prepare a phosphorus-doped polycrystalline silicon layer; (4) preparing an anti-reflection passivation film on both sides of a silicon wafer having an ultra-thin tunneling oxide layer and a phosphorus-doped polysilicon layer; the anti-reflection passivation film is a SiNx:H thin film; (5) The silicon wafer prepared with the anti-reflection passivation film is subjected to high-temperature rapid sintering to obtain a silicon wafer prepared with a passivation contact structure.
2. The low temperature hydrogen plasma assisted annealing method for improving the performance of the passivation contact structure according to claim 1, characterized in that: During the low-temperature hydrogen plasma assisted annealing treatment, when the process gas used is hydrogen, the flow rate of hydrogen is 500 sccm to 2000 sccm; Or, during the low-temperature hydrogen plasma assisted annealing process, when the process gas used is a mixed gas containing hydrogen, the process gas is a mixed gas of hydrogen and argon; in the mixed gas of hydrogen and argon, the flow rate of the hydrogen is 500 sccm to 2000 sccm, and the flow rate of the argon is 500 sccm to 2000 sccm.
3. The low temperature hydrogen plasma assisted annealing method for improving the performance of the passivation contact structure according to claim 2, characterized in that: The low temperature hydrogen plasma assisted annealing treatment lasts for 10 min to 60 min.
4. The low temperature hydrogen plasma assisted annealing method for improving the performance of the passivation contact structure according to claim 3, characterized in that: A tubular PECVD device is used to perform low-temperature hydrogen plasma-assisted annealing treatment on a silicon wafer prepared with a passivated contact structure; during the low-temperature hydrogen plasma-assisted annealing treatment process, the process parameters of the tubular PECVD device are: a plasma power supply frequency of 40kHz, a power of 1000W to 5000W, and a radio frequency on-off ratio of 1:10 to 1:
30.
5. The low temperature hydrogen plasma assisted annealing method for improving the performance of the passivation contact structure according to claim 1, characterized in that: The ultra-thin tunneling oxide layer and the intrinsic amorphous silicon layer are prepared in sequence by low-pressure chemical vapor deposition technology; when the ultra-thin tunneling oxide layer is prepared by low-pressure chemical vapor deposition technology, the preparation process conditions are: temperature of 500°C to 700°C, process gas of O2, flow rate of 5000 sccm to 10000 sccm, process pressure of 20 Pa to 200 Pa, and process time of 10 min to 60 min; the intrinsic amorphous silicon layer is prepared by low-pressure chemical vapor deposition technology, and the preparation process conditions are: temperature of 500°C to 700°C, process gas of SiH4, flow rate of 500 sccm to 2000 sccm, process pressure of 20 Pa to 100 Pa, and process time of 10 min to 30 min; Or, an ultra-thin tunneling oxide layer and an intrinsic amorphous silicon layer are prepared in sequence by plasma enhanced chemical vapor deposition technology; when the ultra-thin tunneling oxide layer is prepared by plasma enhanced chemical vapor deposition technology, the preparation process conditions are: a power frequency of 40 kHz to 300 kHz, a process temperature of 300°C to 600°C, a process time of 10s to 100s, a process pressure of 50 Pa to 300 Pa, and a process gas of a mixed gas of N2O and Ar, wherein the volume ratio of N2O to Ar in the mixed gas of N2O and Ar is 1 to 5: 1 to 10, the process power is 1000 to 10000 W, and the radio frequency on-off ratio is 1:10 to 1:30; when the intrinsic amorphous silicon layer is prepared by plasma enhanced chemical vapor deposition technology, the preparation process conditions are: a power frequency of 40 kHz to 300 kHz, a process temperature of 300°C to 600°C, a process time of 100s to 1000s, and a process pressure of 100 Pa~300Pa, the process gas is a mixed gas of SiH4 and Ar or a mixed gas of SiH4 and H2, the volume ratio of SiH4 to Ar in the mixed gas of SiH4 and Ar is 1:1~1:10, the volume ratio of SiH4 to H2 in the mixed gas of SiH4 and H2 is 1:1~1:10, the process power is 5000~10000W, and the RF on-off ratio is 1:10~1:30; The thickness of the ultra-thin tunneling oxide layer is 1 nm to 3 nm; the ultra-thin tunneling oxide layer is SiO2; and the thickness of the intrinsic amorphous silicon layer is 50 nm to 200 nm.
6. The low temperature hydrogen plasma assisted annealing method for improving the performance of the passivation contact structure according to claim 5, characterized in that: The intrinsic amorphous silicon layer is doped with phosphorus using low-pressure diffusion technology. The doping process conditions are as follows: diffusion temperature 700℃~800℃, diffusion pressure 100 mbar~300mbar, diffusion small nitrogen flow 500 sccm~2000sccm, diffusion large nitrogen flow 1000 sccm~5000sccm, diffusion oxygen 500 sccm~2000sccm, diffusion time 10 min~30min; push temperature 850℃~900℃, large nitrogen flow 2000 sccm~5000sccm, oxygen flow 500 sccm~2000sccm, push time 20 min~40min; Or, the intrinsic amorphous silicon layer is doped with phosphorus using plasma enhanced chemical vapor deposition technology, and the doping process conditions are: power frequency is 40 kHz to 300 kHz, process temperature is 300°C to 600°C, process time is 100s to 1000s, process pressure is 100 Pa to 300Pa, process gas is a mixed gas of SiH4, Ar and PH3 or a mixed gas of SiH4, H2 and PH3, the volume ratio of SiH4, Ar and PH3 in the mixed gas of SiH4, Ar and PH3 is 1:1:1 to 1:10:1, the volume ratio of SiH4, H2 and PH3 in the mixed gas of SiH4, H2 and PH3 is 1:1:1 to 1:10:1, the process power is 5000W to 10000W, and the RF on-off ratio is 1:10 to 1:30; When the intrinsic amorphous silicon layer is phosphorus-doped by plasma enhanced chemical vapor deposition technology, the method also includes high-temperature annealing of the silicon wafer prepared with an ultra-thin tunneling oxide layer and a phosphorus-doped polysilicon layer; the temperature of the high-temperature annealing is 700°C to 1000°C; the time of the high-temperature annealing is 30 min to 60 min.
7. The low temperature hydrogen plasma assisted annealing method for improving the performance of the passivation contact structure according to claim 6, characterized in that: (1), the silicon wafer is an N-type silicon wafer; the resistivity of the silicon wafer is 1Ωcm to 3Ωcm; before the silicon wafer is cleaned, the silicon wafer is pre-cleaned; the solution used in the pre-cleaning process is a potassium hydroxide aqueous solution; the concentration of the potassium hydroxide aqueous solution is 10 wt% to 20 wt%; the temperature of the solution in the pre-cleaning process is 80±5°C; the treatment time of the solution in the pre-cleaning process is 300±50 s; (3) In this method, a tubular PECVD device is used to prepare an anti-reflection passivation film; In (4), the temperature of the high-temperature rapid sintering is 700° C. to 900° C.; and the time of the high-temperature rapid sintering is 5 to 30 seconds.
8. A TOPCon solar cell, characterized in that: The TOPCon solar cell is prepared by the low-temperature hydrogen plasma assisted annealing method for improving the performance of the passivation contact structure as described in any one of claims 1 to 7.
9. The TOPCon solar cell according to claim 8, characterized in that: The TOPCon solar cell comprises a silicon substrate, wherein the front side of the silicon substrate is provided with a front aluminum oxide layer and a front anti-reflection passivation layer in sequence from the inside to the outside; the back side of the silicon substrate is provided with an ultra-thin tunneling oxide layer, a phosphorus-doped polysilicon layer, and a back anti-reflection passivation layer in sequence from the inside to the outside.