Method for manufacturing bottom cell of TOPCon perovskite laminated cell
Through double-sided secondary velvet making and PECVD growth mask oxide layer, combined with laser cutting surface alumina passivation, the problems of cutting surface defects and single-sided doping of bottom battery are solved, and the overall efficiency and optical absorption of stacked batteries are improved. Effect.
Patent Information
- Application Number
- CN202411115533.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-14
- Publication Date
- 2024-11-29
AI Technical Summary
During the production of crystalline silicon TOPCon/perovskite stacked batteries, laser cutting causes cutting defects in the cutting surface of the bottom battery, which is low in efficiency. In addition, conventional bottom battery is only doped with one-sided Poly silicon, which is not fully passivated, affecting the stacking Layer battery efficiency.
The passivation process of double-sided secondary velvet making and polysilicon dielectric layer is adopted to add PECVD growth mask oxide layer to form microsuede, and an alumina passivation layer is prepared on the laser cutting surface to ensure the optical absorption and passivation effect of the bottom battery. .
The overall efficiency of the stacked battery is improved, boron and phosphorus co-doping is prevented, the impact of high temperature on the silicon wafer is reduced, and the passivation effect of the cutting surface of the bottom battery is improved, and the efficiency of the stacked battery is increased by more than 1%.
Smart Images

Figure CN119050198A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of solar cells, and in particular relates to a method for manufacturing a TOPCon perovskite stacked cell bottom cell. Background Art
[0002] TOPCon (Tunnel Oxide Passivated Contact) is a tunnel oxide passivated contact. At present, the production process of crystalline silicon TOPCon / perovskite two-terminal stacked cells is mainly small-area stacked cells in the laboratory (within 5cm*5cm), and industrial production has not yet been formed. Crystalline silicon TOPCon / perovskite stacked cells mainly consist of bottom cells, connecting layers, and perovskite top cells. During the production process, the bottom cell is usually made of a large-area crystalline silicon cell. After completion, it is cut into a small-area bottom cell by a laser cutting machine, and then produced by matching the connecting layer and the top cell. Stacked cells. In the process of making the bottom cell, there are cutting defects on the cutting surface of the bottom cell due to laser cutting, resulting in low efficiency of the bottom cell, affecting the efficiency of the stacked cell, and conventional bottom cells are only passivated on one side of the Poly silicon doping, which is not conducive to the overall passivation effect of the bottom cell. Summary of the invention
[0003] In the process of making batteries, a micro-suede surface is formed on the bottom battery and double-sided Poly silicon is doped. In order to avoid the formation of boron-phosphorus co-doping in the secondary Poly doping process of the bottom battery, a separate PECVD method is added to the process flow to grow the mask oxide layer. The overall production of the bottom battery takes into account the optical absorption effect, the upper and lower polycrystalline passivation contact effect, and the reduction of the polycrystalline silicon parasitic absorption on the upper surface of the bottom battery. The micro-suede surface can ensure a good connection effect with the top battery TCO and optical absorption effect. After laser cutting, the passivation of the cut surface is increased. Through the above operations, the passivation function of the bottom battery as a whole and the cut surface is increased, further improving the efficiency of the stacked battery.
[0004] In a first aspect of the present invention, a method for manufacturing a TOPCon perovskite tandem battery bottom cell is provided, comprising the following steps:
[0005] Clean the original silicon wafer and perform double-sided texturing to form a silicon wafer layer;
[0006] Growing a tunnel oxide layer and a first polysilicon dielectric layer in sequence on both sides of the silicon wafer layer;
[0007] Boron-doping the first polysilicon dielectric layer to prepare a P-poly doped layer;
[0008] On the borosilicate glass layer formed outside the P-poly doped layer on the lower surface of the silicon wafer layer, an oxidation mask layer is grown using PECVD alone;
[0009] Go to wrap plating;
[0010] The upper surface of the silicon wafer layer is subjected to alkaline polishing and micro-texturing to remove the P-poly doped layer and the tunneling oxide layer on the upper surface and side of the silicon wafer layer;
[0011] Depositing a tunnel oxide layer and a second polysilicon dielectric layer in sequence on both sides of the micro-textured silicon wafer layer;
[0012] Phosphorus doping is performed on the second polysilicon dielectric layer on the upper surface of the silicon wafer layer to prepare an N-poly layer;
[0013] Secondary de-plating;
[0014] An aluminum oxide dielectric layer and a silicon nitride dielectric layer are sequentially prepared on the P-poly layer on the lower surface of the silicon wafer layer;
[0015] Laser cutting of silicon wafers and generation of an aluminum oxide passivation layer on the laser cut surface of the silicon wafers;
[0016] A metal electrode is prepared on the silicon nitride dielectric layer on the lower surface of the silicon wafer layer.
[0017] Furthermore, the tunneling oxide layer is silicon oxide with a thickness of 1.2-2.0 nm, for example, 1.3 nm, 1.4 nm, 1.5 nm, 1.6 nm, 1.7 nm, 1.8 nm or 1.9 nm; the thickness of the first polysilicon dielectric layer is 100-150 nm, for example, 110 nm, 120 nm, 130 nm, 140 nm or 150 nm.
[0018] Furthermore, the first polysilicon dielectric layer is doped with boron to prepare a P-poly doped layer, and the borosilicate glass layer on the surface of the P-poly doped layer has a thickness of 30-100nm, for example, 40nm, 50nm, 60nm, 70nm, 80nm, 90nm or 100nm.
[0019] Furthermore, the oxidation mask layer is silicon oxide or silicon oxynitride, and has a thickness of 30 nm-100 nm, for example, 40 nm, 50 nm, 60 nm, 70 nm, 80 nm, 90 nm or 100 nm.
[0020] Furthermore, the de-plating includes: using 10%-30% HF solution to etch the borosilicate glass layer plated around the silicon wafer layer, the P-poly doped layer on the upper surface of the silicon wafer layer, and the mask oxide layer around the silicon wafer layer, and the etching time is 50-300s.
[0021] Furthermore, the thickness of the micro-texture surface formed by the micro-texturing is 0.1-0.5 μm, preferably 0.1-0.3 μm.
[0022] Furthermore, the thickness of the second polysilicon dielectric layer and the N-poly layer formed on the second polysilicon dielectric layer is 20-40 nm, for example, 20 nm, 25 nm, 30 nm, 35 nm or 40 nm.
[0023] Further, the secondary de-plating comprises the following steps:
[0024] Removing the phosphosilicate glass layer on the lower surface and side of the silicon wafer layer;
[0025] Remove the N-poly layer on the lower surface and side periphery of the silicon wafer layer;
[0026] The tunneling oxide layer and the mask oxide layer on the lower surface of the silicon wafer layer, the phosphosilicate glass layer on the upper surface of the silicon wafer layer, and the tunneling oxide layer around the side of the silicon wafer layer are removed.
[0027] Furthermore, the thickness of the aluminum oxide dielectric layer is 2-5nm, for example, 2nm, 2.5nm, 3nm, 3.5nm, 4nm, 4.5nm or 5nm; the thickness of the silicon nitride dielectric layer is 60nm-120nm, for example, 60nm, 70nm, 80nm, 90nm, 100nm, 110nm or 120nm.
[0028] The second aspect of the present invention provides a TOPCon perovskite stacked battery bottom cell prepared by the above method, the structure of the bottom cell includes an N-poly layer, a tunneling oxide layer, a silicon wafer layer, a tunneling oxide layer, a P-poly doped layer, an aluminum oxide dielectric layer, a silicon nitride dielectric layer and a metal electrode arranged in sequence.
[0029] The third aspect of the present invention provides a TOPCon perovskite stacked cell, comprising the above-mentioned bottom cell.
[0030] Compared with the prior art, the present invention has the following beneficial effects:
[0031] (1) The bottom cell is made by using a double-sided secondary texturing and a double-sided secondary preparation of a polysilicon dielectric layer passivation process. First, a P-poly layer is prepared on the lower surface of the texturing surface of the silicon wafer layer. Then, a second micro-texturing is performed on the lower surface of the silicon wafer layer to remove the wrap-around plating produced by the preparation of the P-poly layer, and to prevent the residual wrap-around layer and boron-phosphorus doping when the N-poly layer is prepared on the lower surface of the silicon wafer layer. The two-time texturing can produce velvet surfaces of different sizes on the upper and lower sides of the bottom cell, fully considering the matching of the upper surface morphology of the bottom cell with the top cell and the matching of the interconnection layer, and increasing the optical absorption effect of the bottom cell.
[0032] (2) The preparation of the bottom cell adds a separate mask oxide layer process step. The mask oxide layer is grown separately on the borosilicate glass layer on the bottom surface, which can prevent the phosphorus doping that is plated to the bottom surface during the N-poly doping process from passing through the polysilicon layer and tunneling the oxide layer to be doped into the P-poly doping layer on the bottom surface of the bottom cell, resulting in phosphorus and boron co-doping on the bottom surface of the bottom cell, reducing the impact on the performance of the bottom cell. The temperature of the mask oxide layer growth process using PECVD is lower than that of the conventional boron doping process, which reduces the impact of the high temperature process on the silicon wafer substrate and has a fast growth rate.
[0033] (3) Preparation of bottom cell An aluminum oxide passivation layer is prepared on the cut surface of the silicon wafer, which increases the passivation effect on the laser cut surface, reduces the impact of laser cutting on the quality of the bottom cell cut surface, and further improves the passivation effect of the bottom cell cut surface. The efficiency of the stacked cell prepared by this method is increased by more than 1% compared with the conventional method.
[0034] Other features and advantages of the present invention will be described in the following description, and partly become obvious from the description, or be understood by implementing the present invention. The purpose and other advantages of the present invention can be realized and obtained by the structures pointed out in the description and the drawings. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] FIG1 is a method for preparing a TOPCon perovskite tandem battery bottom cell according to an embodiment of the present invention; Figure 1A is a schematic diagram of steps S1-S5 of Examples, Figure 1B This is a schematic diagram of steps S6-S9. Figure 1C It is a schematic diagram of steps S10-S14;
[0036] Figure 2 It is the TOPCon perovskite tandem cell of the present invention;
[0037] Figure 3 It is a conventional TOPCon perovskite tandem cell. DETAILED DESCRIPTION
[0038] In order to make the purpose, technical scheme and advantages of the present invention clearer, the implementation scheme of the present application will be described in detail below in conjunction with specific examples. The technical terms and scientific terms used in the present invention have the meanings generally understood by ordinary technicians in the technical field to which the present invention belongs, without other definitions. Without departing from the concept of the present invention, those skilled in the art may make various improvements and changes to the specific implementation methods of the present invention specification, which all belong to the protection scope of the present invention.
[0039] The TOPCon perovskite stacked cell structure prepared by the present invention can be found in Figure 2, a method for manufacturing a TOPCon perovskite tandem battery bottom cell, see FIG1 , comprising the following steps:
[0040] S1, cleaning the original silicon wafer, and performing double-sided texturing to form a silicon wafer layer;
[0041] Using N-type single crystal silicon as the silicon substrate, using deionized water and liquid sodium hydroxide solution to prepare a NaOH solution with a mass concentration of 0.5%-2.0%, the silicon substrate is initially polished for 20s-100s, and each time it enters the NaOH solution tank, it enters the water tank for water washing.
[0042] Then, deionized water and liquid sodium hydroxide solution are used to prepare a NaOH solution with a mass concentration of 1.5%-2.5%, and a texturing additive solution is added. The temperature of the tank solution is controlled at 80-85°C, and the etching time is controlled at 450s-600s. The silicon wafer is anisotropically etched to form a pyramid velvet surface. The size of the pyramid is controlled at 1.5-2.5μm, and the integrated color reflection rate is controlled in the range of 8%-20%. The integrated reflectivity is a parameter that characterizes the light limiting property of the surface of the silicon wafer after texturing. The lower the optical light limiting property is, the better.
[0043] S2, sequentially growing a tunnel oxide layer and a first polysilicon dielectric layer i-poly on both sides of the silicon wafer layer;
[0044] Adopt LPCVD (Low Pressure Chemical Vapor Deposition), low pressure chemical vapor deposition method, pressure 50-500Torr, use high temperature LPCVD vacuum equipment, through oxygen and silane gas source, chemical reaction is carried out at high temperature environment 800-1000°C, and a tunneling oxide layer with a thickness of 1.2-2.0nm and a first polysilicon dielectric layer i-poly with a thickness of 100-150nm are grown on both sides of the silicon wafer layer in sequence; the tunneling oxide layer is silicon oxide SiO2;
[0045] In the actual production process, this method adopts a single-insertion method to place the semi-finished product on a horizontal quartz boat fixture. Since the LPCVD deposited film has no directionality, and the cell stands on the quartz boat during the processing, the tunnel oxide layer and the polysilicon dielectric layer will also adhere to the side and front of the cell, forming a wrap, that is, the "wrap-around plating" phenomenon (such as Figure 1A As shown in the figure, the redundant tunnel oxide layer and polysilicon dielectric layer must be removed, so a “de-plating” process needs to be introduced later.
[0046] S3, boron-doping the first polysilicon dielectric layer to prepare a P-poly doped layer;
[0047] Boron tribromide or boron trichloride diffusion source is used, and the high-temperature doping advancement temperature is controlled at 900-1050°C. Considering that too long high-temperature doping time may easily lead to poor polysilicon passivation effect, the boron doping high-temperature advancement time is controlled within 50-100 minutes. After doping boron element on the first polysilicon dielectric layer, a P-poly doping layer is formed. The doping process will eventually form a borosilicate glass layer (BSG) covering the surface of the P-poly doping layer, and the thickness is controlled in the range of 30-100nm.
[0048] A P-poly doped layer is grown on the velvet structure. Considering the optical absorption effect of the lower surface of the bottom battery on the long-wave band, the optical absorption effect of the P-poly doped layer on the long-wave band is increased, thereby increasing the generation of photogenerated carriers in the long-wave band of the bottom battery.
[0049] S4, growing an oxidation mask layer separately on the borosilicate glass layer (BSG) formed outside the P-poly doped layer on the lower surface of the silicon wafer layer;
[0050] Plasma enhanced chemical vapor deposition (PECVD) is used to introduce silane and nitrous oxide at a temperature range of 400-500°C, respectively, to grow a mask oxide layer of silicon oxide or silicon oxynitride with a thickness of 30nm-100nm on the P-poly doping layer, and the deposition time is 50-300S. This step can prevent the phosphorus doping that is plated to the lower surface during the N-poly doping process from passing through the polysilicon layer and tunneling the oxide layer to be doped into the P-poly doping layer on the lower surface of the bottom cell, resulting in phosphorus-boron co-doping on the lower surface of the bottom cell, reducing the impact on the performance of the bottom cell.
[0051] S5, de-plating: De-plating around the silicon wafer layer, the borosilicate glass layer (BSG) on the P-poly doped layer on the upper surface of the silicon wafer layer, and the mask oxide layer around the silicon wafer layer during the etching preparation process.
[0052] Use chain etching equipment with 10%-30% HF solution, and the etching time is 50-300s to remove the borosilicate glass layer (BSG) plated around the silicon wafer layer, the P-poly doped layer on the upper surface of the silicon wafer layer, and the mask oxide layer around the silicon wafer layer during the preparation process.
[0053] S6, performing alkali polishing and micro-texturing on the upper surface of the silicon wafer layer to remove the P-poly doped layer and the SiO2 tunneling oxide layer on the upper surface and side of the silicon wafer layer;
[0054] Use 1%-5% mass concentration of NaOH solution with alkaline polishing additive solution, control the temperature at 60℃-80℃, and control the etching time at 240s-500s to remove the P-poly doped layer and SiO2 tunneling oxide layer on the upper surface and side surfaces and form a 0.1-0.5μm micro-suede surface on the upper surface.
[0055] The size of the velvet is controlled at 0.1-0.5μm, fully considering the optical light limiting effect of the bottom cell and the contact effect with the top cell connection layer. Too large a velvet surface will cause uneven growth of the dielectric layer during the deposition of the TCO contact layer and other dielectric layers of the top cell, resulting in poor contact transmission effect between the bottom cell and the top cell connection layer.
[0056] The purpose of micro-texturing in this step is mainly to take into account the connection effect between the bottom cell and the top cell and the optical absorption effect of the bottom cell, to prepare for the subsequent phosphorus doping to prepare the N-poly layer, and to remove the P-poly doping layer on the upper surface to prevent boron and phosphorus co-doping, thereby improving the overall performance of the stacked cell.
[0057] S7, sequentially depositing a SiO2 tunneling oxide layer and a second polysilicon dielectric layer on both sides of the micro-textured silicon wafer layer;
[0058] Using high-temperature LPCVD vacuum equipment, a chemical reaction is carried out in a high-temperature environment through oxygen and silane gas sources to prepare a 1.2-2.0nm tunneling oxide layer and a 20-40nm second polysilicon dielectric layer on both sides of the micro-textured silicon wafer layer; in the actual production process, this method uses a single-insertion or double-insertion method to place the semi-finished product on a horizontal quartz boat fixture.
[0059] A polysilicon layer that is too thick will cause serious optical parasitic absorption problems, while a polysilicon layer that is too thin will have poor passivation effect. The thickness of the second polysilicon dielectric layer is controlled in the range of 20-40nm, which can fully consider the optical absorption effect of the bottom cell, the passivation effect of the N-poly layer on the upper surface of the bottom cell, and the contact passivation and transmission effects with the top cell connection layer.
[0060] S8, phosphorus-doping the second polysilicon dielectric layer on the upper surface of the silicon slice layer to prepare an N-poly layer;
[0061] Using high-temperature doping equipment, phosphorus oxychloride, oxygen, and nitrogen gas sources are introduced to carry out chemical reactions in a high-temperature environment of 500-650°C to form a 20-40nm N-poly layer. The doping process will eventually form a phosphosilicate glass layer (PSG layer) covering the surface of the N-poly layer. The PSG layer is between 20-100nm.
[0062] Secondary de-winding plating S9-S11:
[0063] S9, removing the phosphosilicate glass layer PSG layer on the lower surface and side of the silicon wafer layer: removing the phosphosilicate glass layer (PSG layer) that is plated around the lower surface and side periphery during the process of preparing the N-poly layer by phosphorus doping on the upper surface;
[0064] Using chain horizontal etching equipment, first use 0.5%-5% mass concentration HF solution, the HF solution temperature is controlled at 8-25°C, the etching time is within 30S-200S, and the PSG layer plated around the lower surface and the PSG layer around the side of the silicon wafer layer are removed.
[0065] S10, removing the N-poly layer on the lower surface and the side periphery of the silicon wafer layer;
[0066] A NaOH solution with a mass concentration of 0.5% to 5% and a de-wrapping additive solution with a mass concentration of 0.5% to 5% are used to etch the N-poly layer on the lower surface and the side periphery.
[0067] S11, removing the tunneling oxide layer and the mask oxide layer on the lower surface of the silicon wafer layer, the phosphosilicate glass layer on the upper surface of the silicon wafer layer, and the tunneling oxide layer around the side of the silicon wafer layer;
[0068] Using HF solution with a concentration of 3%-20%, immerse the silicon wafer layer in a solution tank device, and the corrosion time is within the range of 200-500S.
[0069] S12, sequentially preparing an aluminum oxide dielectric layer Al2O3 and a silicon nitride dielectric layer (Si3N4) on the P-poly layer on the lower surface of the silicon wafer layer;
[0070] Through high temperature vacuum ALD equipment (atomic layer deposition), TMA gas source is introduced at a temperature of 100-300°C to grow an aluminum oxide dielectric layer Al2O3 with a thickness of 2.0-5.0nm;
[0071] Through high-temperature vacuum PECVD equipment, silane and ammonia gas sources are introduced to grow a silicon nitride dielectric layer of about 60nm-120nm on the aluminum oxide dielectric layer at 450-600°C.
[0072] S13, laser cutting the silicon wafer, and generating a 2.0-10.0 nm aluminum oxide passivation layer on the laser cut surface of the silicon wafer;
[0073] Use laser to cut silicon wafers of appropriate size, with the cutting surface perpendicular to the textured surface / P-poly layer / N-poly layer of the silicon wafer;
[0074] Laser parameters: power 100-200w, frequency 300-500, speed 5000-40000mm / s, silicon wafer cutting.
[0075] ALD is used to generate an aluminum oxide passivation layer on the laser-cut surface of the silicon wafer;
[0076] Use plate or tube ALD equipment with fixtures to passivate the laser cut surface to increase the passivation performance of the laser cut surface; Alumina growth is achieved by introducing TMA (trimethylaluminum) and water into the chamber of the plate or tube ALD equipment, and growing in a reaction temperature environment of 100-300°C. The thickness of the alumina growth is controlled within 2.0-10nm.
[0077] S14. Preparation of metal electrodes
[0078] A metal electrode is prepared on the silicon nitride dielectric layer on the lower surface of the silicon wafer layer. The metal electrode includes any one of an Ag electrode, an Au electrode, and a Cu electrode.
[0079] At this point, the preparation of TOPCon perovskite bottom cell is completed.
[0080] S15, sequentially preparing a connection layer, a perovskite top cell, and an electrode layer of the top cell on the perovskite bottom cell;
[0081] The connecting layer is a commonly used transparent conductive layer TCO material, the perovskite top cell is a PIN structure, and the top cell electrode layer is any one of an Ag electrode, an Au electrode, and a Cu electrode.
[0082] At this point, the preparation of TOPCon perovskite stacked cells is completed. The structure is shown in Figure 2 .
[0083] Embodiment 1:
[0084] S1, cleaning the original silicon wafer, and performing double-sided texturing to form a silicon wafer layer;
[0085] See also Figure 1A , using N-type single crystal silicon as the silicon substrate, using deionized water and liquid sodium hydroxide solution to prepare a 1% mass concentration NaOH solution, the silicon substrate was initially polished for 70s, and each time it entered the NaOH solution tank, it would enter the water tank for water washing.
[0086] Deionized water and liquid sodium hydroxide solution are then used to prepare a NaOH solution with a mass concentration of 2%, and a texturing additive solution is added. The temperature of the tank solution is controlled at 82°C, and the corrosion time is controlled at 500s. The silicon wafer is anisotropically etched to form a pyramid velvet surface. The size of the pyramid is controlled at 1.5μm, and the integrated inversion rate is controlled within 10%.
[0087] S2, sequentially growing a tunnel oxide layer and a first polysilicon dielectric layer on both sides of the silicon wafer layer;
[0088] See also Figure 1AUsing high-temperature LPCVD vacuum equipment, oxygen and silane gas sources are used to carry out chemical reactions at a temperature of 900°C and a pressure of 150Torr to sequentially grow a 1.5nm thick SIO2 tunneling oxide layer and a 120nm thick first polysilicon dielectric layer i-poly on both sides of the silicon wafer layer.
[0089] S3, boron-doping the first polysilicon dielectric layer to prepare a P-poly doped layer;
[0090] See also Figure 1A , using boron tribromide diffusion source, the high-temperature doping advancement temperature is controlled at 950°C, the boron doping high-temperature advancement time is controlled at 60 minutes, and a P-poly doped layer is formed after doping boron element on the first polysilicon dielectric layer. The doping process will eventually form a borosilicate glass layer (BSG) covering the surface of the P-poly doped layer with a thickness controlled at 50nm.
[0091] S4, separately growing an oxidation mask layer on the borosilicate glass layer (BSG) covering the surface of the P-poly doped layer on the lower surface of the silicon wafer layer;
[0092] See also Figure 1A , plasma enhanced chemical vapor deposition (PECVD) was used to control the temperature at 450°C and the deposition time for 100s to grow a 50nm thick silicon oxide mask oxide layer on the P-poly doped layer.
[0093] S5, de-plating: De-plating around the silicon wafer layer, the borosilicate glass layer (BSG) on the P-poly doped layer on the upper surface of the silicon wafer layer, and the mask oxide layer around the silicon wafer layer during the etching preparation process.
[0094] See also Figure 1A , using chain etching equipment, with 20% HF solution, the etching time is 200s, to remove the borosilicate glass layer (BSG) plated around the silicon wafer layer during the preparation process, the P-poly doped layer on the upper surface of the silicon wafer layer, and the mask oxide layer around the silicon wafer layer.
[0095] S6, performing alkali polishing and micro-texturing on the upper surface of the silicon wafer layer to remove the P-poly doped layer and the SiO2 tunneling oxide layer on the upper surface and side of the silicon wafer layer;
[0096] See also Figure 1B , using a 3% mass concentration NaOH solution with an alkaline polishing additive solution, the temperature was controlled at 70°C, the etching time was controlled at 360s, the P-poly doped layer and the SiO2 tunneling oxide layer on the upper surface and the side were removed, and a 0.5μm micro-texture surface was formed on the upper surface.
[0097] S7, sequentially depositing a SiO2 tunneling oxide layer and a second polysilicon dielectric layer on both sides of the micro-textured silicon wafer layer;
[0098] See also Figure 1B Using high-temperature LPCVD vacuum equipment, a chemical reaction is carried out in a high-temperature environment through oxygen and silane gas sources to prepare a 2.0nm tunneling oxide layer and a 30nm second polysilicon dielectric layer on both sides of the micro-textured silicon wafer layer; in the actual production process, this method uses a double-insertion method to place the semi-finished product on a horizontal quartz boat fixture.
[0099] S8, phosphorus-doping the second polysilicon dielectric layer on the upper surface of the silicon slice layer to prepare an N-poly layer;
[0100] See also Figure 1B Using high-temperature doping equipment, phosphorus oxychloride, oxygen, and nitrogen gas sources are introduced to carry out chemical reactions at a high temperature of 600°C to form a 30nm N-poly layer. The doping process will eventually form a phosphosilicate glass layer (PSG layer) covering the surface of the N-poly layer. The thickness of the PSG layer is no more than 100nm.
[0101] S9, removing the phosphosilicate glass layer PSG layer on the lower surface and side of the silicon wafer layer: removing the phosphosilicate glass layer (PSG layer) that is plated around the lower surface and side periphery during the process of preparing the N-poly layer by phosphorus doping on the upper surface;
[0102] See also Figure 1B Using a chain horizontal etching device, first use a 2.5% mass concentration HF solution, the HF solution temperature is controlled at 20°C, the etching time is within 100S, and the PSG layer plated around the lower surface and the PSG layer around the side of the silicon wafer layer are removed.
[0103] S10, removing the N-poly layer on the lower surface and the side periphery of the silicon wafer layer;
[0104] See also Figure 1C , using a 35% mass concentration NaOH solution and a 3.5% mass concentration de-wrapping additive solution to etch the N-poly layer on the lower surface and the side periphery.
[0105] S11, removing the SiO2 tunneling oxide layer and the silicon oxide mask oxide layer on the lower surface of the silicon wafer layer, the PSG layer on the upper surface of the silicon wafer layer, and the SiO2 tunneling oxide layer around the side of the silicon wafer layer;
[0106] See also Figure 1C , using a 12% HF solution, immerse the silicon wafer layer in a solution tank device, and the corrosion time is within 300S.
[0107] S12, sequentially preparing an aluminum oxide dielectric layer Al2O3 and a silicon nitride dielectric layer (Si3N4) on the P-poly layer on the lower surface of the silicon wafer layer;
[0108] See also Figure 1C , through high temperature vacuum ALD equipment (atomic layer deposition), TMA gas source is introduced to grow an aluminum oxide dielectric layer Al2O3 with a thickness of 3.0nm;
[0109] A silane and ammonia gas source is introduced through a high-temperature vacuum PECVD device to grow an 80nm silicon nitride dielectric layer on the aluminum oxide dielectric layer.
[0110] S13, laser cutting the silicon wafer, and forming an aluminum oxide passivation layer on the laser cut surface of the silicon wafer;
[0111] Use laser to cut 1.0*2.0cm silicon wafer, with the cutting surface perpendicular to the textured surface / P-poly layer / N-poly layer of the silicon wafer;
[0112] Laser parameters: power 100w, frequency 300H, speed 10000mm / s, for cutting silicon wafers.
[0113] ALD was used to generate a 3.0nm thick aluminum oxide passivation layer on the laser-cut surface of the silicon wafer;
[0114] Use plate or tube ALD equipment with fixtures to passivate the laser cut surface to increase the passivation performance of the laser cut surface; Alumina growth is achieved by introducing TMA (trimethylaluminum) and water into the chamber of the plate or tube ALD equipment, and growing in a reaction temperature environment of 220°C. The growth thickness of alumina is controlled at 6nm.
[0115] S14. Preparation of metal electrodes
[0116] See also Figure 1C , a metal electrode Cu electrode is prepared on the silicon nitride dielectric layer on the lower surface of the silicon wafer layer.
[0117] At this point, the preparation of the TOPCon perovskite bottom cell is completed.
[0118] S15, sequentially preparing a connection layer, a perovskite top cell, and an electrode layer of the top cell on the perovskite bottom cell;
[0119] The connecting layer is made of the commonly used transparent conductive layer TCO material, the perovskite top cell is a PIN structure, and the top cell electrode layer uses a Cu electrode.
[0120] At this point, the preparation of TOPCon perovskite stacked cells is completed. The structure is shown in Figure 2 The battery was tested with a voltage of 1.65V and a current of 14.5A.
[0121] The comparative example is a conventional TOPCon perovskite stacked cell, the structure of which is shown in Figure 3 , which is different from the embodiment of the present invention in that:
[0122] 1. The comparative example does not have steps S4 and S13.
[0123] 2. In step S6, no micro-texture preparation is performed, and only the upper surface of the bottom battery is polished or conventionally suede-prepared.
[0124] 3. In step S7, the thickness of the i-poly in the comparative example is generally in the range of 60-150 nm, and is 140 nm in the comparative example.
[0125] The comparative battery test voltage is 1.50V and the current is 13.7A.
[0126] The above shows that the present invention can improve the overall efficiency of the stacked cell by increasing the optical absorption effect of the bottom cell by adding a PECVD method to grow a mask silicon oxide layer and a micro-suede surface on the upper surface of the bottom cell, and adding an aluminum oxide dielectric layer passivation on the laser cut surface of the bottom cell.
[0127] Finally, it should be noted that the above is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, it is still possible for those skilled in the art to modify the technical solutions described in the aforementioned embodiments or to make equivalent substitutions for some of the technical features therein. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for manufacturing a TOPCon perovskite tandem battery bottom cell, characterized in that: The following steps are involved: Clean the original silicon wafer and perform double-sided texturing to form a silicon wafer layer; Growing a tunnel oxide layer and a first polysilicon dielectric layer in sequence on both sides of the silicon wafer layer; Boron-doping the first polysilicon dielectric layer to prepare a P-poly doped layer; On the borosilicate glass layer formed outside the P-poly doped layer on the lower surface of the silicon wafer layer, an oxidation mask layer is grown using PECVD alone; Go to wrap plating; The upper surface of the silicon wafer layer is subjected to alkaline polishing and micro-texturing to remove the P-poly doped layer and the tunneling oxide layer on the upper surface and side of the silicon wafer layer; Depositing a tunnel oxide layer and a second polysilicon dielectric layer in sequence on both sides of the micro-textured silicon wafer layer; Phosphorus doping is performed on the second polysilicon dielectric layer on the upper surface of the silicon wafer layer to prepare an N-poly layer; Secondary de-plating; An aluminum oxide dielectric layer and a silicon nitride dielectric layer are sequentially prepared on the P-poly layer on the lower surface of the silicon wafer layer; Laser cutting of silicon wafers and generation of an aluminum oxide passivation layer on the laser cut surface of the silicon wafers; A metal electrode is prepared on the silicon nitride dielectric layer on the lower surface of the silicon wafer layer.
2. The bottom cell manufacturing method according to claim 1, characterized in that: The tunneling oxide layer is silicon oxide with a thickness of 1.2-2.0 nm; the first polysilicon dielectric layer has a thickness of 100-150 nm.
3. The bottom cell manufacturing method according to claim 1, characterized in that: The first polysilicon dielectric layer is doped with boron to prepare a P-poly doped layer, and the thickness of the borosilicate glass layer on the surface of the P-poly doped layer is 30-100 nm.
4. The bottom cell manufacturing method according to claim 1, characterized in that: The oxidation mask layer is silicon oxide or silicon oxynitride, and has a thickness of 30nm-100nm.
5. The bottom cell manufacturing method according to claim 1, characterized in that: The de-plating includes: using 10%-30% HF solution to etch the borosilicate glass layer on the P-poly doped layer on the upper surface of the silicon layer and the mask oxide layer around the silicon layer, and the etching time is 50-300s.
6. The bottom cell manufacturing method according to claim 1, characterized in that: The thickness of the micro-texture surface formed by the micro-texturing is 0.1-0.5 μm.
7. The bottom cell manufacturing method according to claim 1, characterized in that: The thickness of the second polysilicon dielectric layer and the N-poly layer prepared on the second polysilicon dielectric layer is 20-40 nm.
8. The bottom cell manufacturing method according to claim 1, characterized in that: The secondary de-plating comprises the following steps: Removing the phosphosilicate glass layer on the lower surface and side of the silicon wafer layer; Remove the N-poly layer on the lower surface and side periphery of the silicon wafer layer; The tunneling oxide layer and the mask oxide layer on the lower surface of the silicon wafer layer, the phosphosilicate glass layer on the upper surface of the silicon wafer layer, and the tunneling oxide layer around the side of the silicon wafer layer are removed.
9. The bottom cell manufacturing method according to claim 1, characterized in that: The thickness of the aluminum oxide dielectric layer is 2-5 nm; the thickness of the silicon nitride dielectric layer is 60 nm-120 nm.
10. A TOPCon perovskite tandem battery bottom cell, characterized in that: The bottom cell manufacturing method according to any one of claims 1 to 9 is used to manufacture the bottom cell, wherein the structure of the bottom cell comprises an N-poly layer, a tunneling oxide layer, a silicon wafer layer, a tunneling oxide layer, a P-poly doped layer, an aluminum oxide dielectric layer, a silicon nitride dielectric layer and a metal electrode arranged in sequence.
11. A TOPCon perovskite tandem cell, characterized in that: Comprising the bottom battery as claimed in claim 10.
Citation Information
Cited By
Perovskite / TOPCon laminated cell and bottom cell and preparation method thereof
CN119894147A
Photoelectric conversion element
JP2026144316A