Method for welding particle foams by means of porous sleeves

Through thin-walled porous shell filling and steam welding technology, the problems of characteristic differences and high production costs in molded products are solved, multi-region characteristic control and surface treatment are simplified, and the performance and economy of molded products are improved.

CN114829471BActive Publication Date: 2024-10-15BASF SE
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202080087607.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-12-17
Filing Date
2020-12-17
Publication Date
2024-10-15
Estimated Expiration
2040-12-17

AI Technical Summary

Technical Problem

The existing technology is difficult to achieve controlled characteristic differences in molded products, and the production cost is high, the surface treatment does not meet the technical requirements, and multiple molds and complex molding machines complicate production.

Method used

Molded articles are prepared by filling expanded granular materials with thin-walled, breathable porous shells and steam welding them. The shells can form an inseparable bond with the granules or be removed after welding. Multi-region is achieved by positioning the granules of different materials and colors. Feature control.

Benefits of technology

It saves process steps, enables new material combinations, and reduces production costs. The surface of the molded product does not require additional treatment, and it has the ability to control multi-regional characteristics.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to a method for producing a molded body (FK), comprising: providing a thin-walled, air-permeable cover; filling the cover with foamed particles consisting of a polymer (P1); and welding the foamed particles, thereby obtaining a molded body (FK). The invention further relates to a molded body obtainable or obtained according to this method and to the use of a molded body obtainable or obtained according to the method according to the invention or of a molded body according to the invention as a sole, a part of a sole, a mattress, a seat cushion, a padding, a handle, a protective film, as a component for the interior and exterior area of ​​a motor vehicle, as a gymnastics mat, a body protector, a lining element in automobile construction, a silencer, a shock absorber, a cushioning pad, a bicycle saddle, a toy, a tire or a part of a tire or the surface of an athletic track, a surface of a gymnasium or a pavement, a sandwich element or a cushioning layer or a cushioning core in packaging.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The present invention relates to a process for producing a molded article (M), which comprises providing a thin-walled, air-permeable shell, filling the shell with a foamed granular material consisting of a polymer (P1), and fusing the foamed granular material to obtain the molded article (M). Furthermore, the present invention also relates to a molded article obtainable by or by this process, and to the use of the molded article obtainable by or by the process of the present invention as a sole, a part of a sole, a mattress, a seat cushion, a padding, a handle, a protective film, as a component for the interior and exterior of a car, as a gymnastic mat, a body protector, a decorative element in a car structure, a sound insulator, a shock absorber, a cushioning pad, a bicycle saddle, a toy, a tire or a part of a tire or a covering for a track surface, a covering for a gymnasium or a sidewalk, a sandwich element or a cushioning layer or a cushioning core in packaging.

[0002] Moldings made from granular forms (e.g. EPS, EPP and ETPU) and methods for their preparation are well known. Such moldings usually consist of one type of granules; the moldings thereof have essentially uniform properties, but there may be process-related unexpected property variations in the moldings, for example due to excessive compression at the constriction.

[0003] Also known are moldings made from mixtures of foam particles, for example gray and white EPS (known as Dalmatian foam). Here, the particles are randomly distributed in the molding, resulting in a uniform combination of properties and appearance.

[0004] However, in many higher quality applications, it is required that the moldings have different properties in different segments (in a controlled manner). This is usually solved by separately preparing molding segments made of different types of granules and then combining them by gluing, welding or form-fitting to give the molding.

[0005] It is also known that molded articles in which segments with different properties are required are produced using, for example, a mold with slides that allow filling of different cavities in the mold, pulling out separate slides, and subsequent welding. For example, JP355228A2 and JP03097529 describe a method using multiple cavities.

[0006] MX 2006-GT0017 describes the preforming of expandable EPS particles in a prefoamer and the subsequent welding of two preformed segments in a mold.

[0007] It is also possible to use special methods (eg the slot method) in which the segments can be compressed differently. However, the density of the molding can thus only be adjusted within a narrow range. For example, it is not possible to create various colors in this way.

[0008] Due to the incorporation or use of a slide mold, such molded parts have clearly defined characteristic areas, but this is disadvantageous in many applications, such as in the case of shoe soles. In addition, the production costs are high, since multiple molds are required or complex slide molds and correspondingly complex and expensive molding machines must be used.

[0009] Moldings made from welded particle foams often also have the disadvantage that the surface of the molding does not meet the technical requirements or customer demands. Due to the manufacturing process, the surface and structure correspond to the foam particles before welding. If a surface different from that created in the welding operation is required, complex modification methods are required. For example: painting visible parts, coating with reactive systems or dissolved elastomers, or introducing the molding into a shell that has to be produced additionally.

[0010] The object of the present invention is to introduce expanded particles having different properties in a controlled manner into a primary molding, to hold the primary molding in place or to position it directly by introducing it into a mold in a controlled manner and then to produce a molding therefrom.

[0011] According to the invention, this object is achieved by a method for producing a molded article (M), comprising the following steps

[0012] (i) providing a thin-walled, air-permeable shell;

[0013] (ii) filling the shell with a foamed granular material made of polymer (P1);

[0014] (iii) The expanded granular materials are welded to obtain a molded article (M).

[0015] Compared to the methods known to date, which involve multi-part production, welding and the use of inserts, the method according to the invention makes it possible to save process steps and to produce new material combinations that were not achievable to date.

[0016] In the context of the present invention, a thin-walled, air-permeable shell is used. In the context of the present invention, the shell is preferably porous. In the context of the present invention, the shell is preferably configured so that it has a shape that simulates the desired shape of the molded article (M). In the context of the present invention, the shell can be configured in such a way that it is part of the molded article (M). In an alternative embodiment, the shell can be configured so that it is removed from the molded article (M) after step (iii).

[0017] It has been found that foam parts can be produced by introducing expanded foam particles into a steam-permeable shell, positioning them and fusing them to the shell in a steam fusion of the particles; depending on the type of shell used, the shell thus forms an inseparable bond with the particles or can be removed from the molded article after step (iii). By means of the properties of the shell, the properties of the molded article can also be varied according to the invention.

[0018] The method of the present invention comprises steps (i) to (iii). First, in step (i), a shell made of a porous material is provided. In step (ii), the shell is filled with a foamed granular material made of a polymer (P1). In step (iii), the foamed granular material is welded to obtain a molded article (M).

[0019] In the context of the present invention, the method may comprise further steps, such as a shaping step or introducing the shell into a suitable mould.

[0020] According to the invention, the shell may consist of a material which forms a bond with the molded article during the welding in step (iii). However, in the context of the present invention, the shell may also consist of a material which does not form any bond with the expanded granular material and is removed from the molded article after step (iii).

[0021] The shell can be composed of, for example, plastic, metal, ceramic, cellulose, glass or similar materials. The shell can be, for example, a film, a braid, a knitted fabric, a nonwoven fabric or a mesh.

[0022] According to the invention, the shell consists of a porous material. According to the invention, preferably the steam permeability of the shell is sufficient to ensure a good weld.

[0023] In another embodiment, the present invention therefore also relates to a process for producing a molded article as described above, wherein the shell is a film, a braid, a knit, a mesh or a perforated metal.

[0024] It is particularly preferred to configure the shell, for example, in a porous, woven, perforated or film-like manner, so that during welding with steam, the medium can easily access the particles, thus leading to welding within a short time.

[0025] According to the invention, preferably, the shell consists of a flexible porous material. In another embodiment, the invention therefore also relates to a method for preparing a molded article as described above, wherein the shell consists of a flexible porous material.

[0026] For example, the shell may be a hose, a sheath, a shell, a prefabricated hose, a bonded article, or the like.

[0027] If the shell is welded to the expanded granular material during the production of the molded article, it is preferred according to the invention that the shell consists of the same material as the particles of the expanded granular material. According to the invention, the method can also be carried out with different materials, preferably the materials have little difference in melting temperature and the polymers are compatible with each other.

[0028] In step (ii), the shell is filled with the foamed granular material. According to the invention, this forms an initial molding. According to the invention, the shape of the initial molding can be defined by the shape of the shell. However, the shape of the initial molding can also be determined by the mold before welding.

[0029] In this case, the initial molding is introduced into a mold and welded in step (iii). In the context of the present invention, the particles of the foamed granular material are welded here and the molded article (M) is obtained. In the context of the present invention, the shell can be welded to the particles of the foamed granular material. In the context of the present invention, the shell can also be configured so that it does not weld to the foamed granular material under the conditions of step (iii), so that the shell can be removed from the molded article after step (iii).

[0030] According to the invention, the shape of the molded article can be preformed by the shape of the shell.In the context of the present invention, a mold can also be used to define the shape of the molded article (M).

[0031] The initial molding can be produced in the molding machine itself or in a chamber upstream of the mold, or the initial molding is produced in a separate step.The chamber or container used in the molding machine is, for example, a steel cylinder.

[0032] According to the invention, the shell can be welded before welding in step (iii). In this case, the pre-initial molding is preferably closed and then transferred to the mold. This can be achieved by pneumatic, hydraulic, automatic or other mechanical means.

[0033] According to the invention, the welding in step (iii) can be carried out by methods known per se to those skilled in the art. In the context of the present invention, a suitable example is welding with water vapor (e.g. steam). In another embodiment, the present invention therefore also relates to a method for preparing a molded article as described above, wherein the welding is carried out by steam welding.

[0034] Suitable conditions and equipment for steam welding are known per se to the person skilled in the art. In steam welding, welding is achieved by contact with steam. Suitable welding parameters are known per se to the person skilled in the art. According to the invention, the welding parameters are matched, for example, to the size of the molded article and to the polymer (P1). Suitable steam contact times are, for example, 1 to 120 seconds per steam contact step. Suitable steam temperatures are, for example, 100 to 160° C.

[0035] In a further embodiment, the present invention therefore also relates to a process for producing a moulded article as described above, wherein the shell is closed after the filling in step (ii).

[0036] In one embodiment of the invention, the porous shell consists of the same polymer as the particle foam.

[0037] In the context of the present invention, the thickness of the shell can vary within a wide range, provided that the particles of the foamed granular material can be welded. For example, the thickness of the shell is 1 to 5000 μm, more preferably 2 to 1000 μm, more preferably 5 to 500 μm, further preferably 10 to 250 μm, and particularly preferably 20 to 100 μm.

[0038] In an alternative embodiment of the invention, the shell consists of a material different from the particle foam or a polymer which does not bond to the polymer of the particle foam even at high temperatures.

[0039] The shell of the initial molding, for example after welding, can be removed from the molding and, depending on their design, can be reused or discarded in the case of single use. In this context, reusable, stable shells are preferred. In another embodiment, the present invention therefore also relates to a method for producing a molding as described above, wherein the shell is removed from the molding after welding.

[0040] According to the invention, the shell can also have a preformed shape corresponding to the shape of the desired molding. However, the shape of the molding can also be produced by the mold, and the initial molding serves only as a carrier, which primarily prevents mixing of different particles. Advantageously, the initial molding can fix the particles.

[0041] In another embodiment, the present invention therefore also relates to a process for producing a moulded article as described above, wherein the shell consists of a material which can be welded to the foamed particulate material.

[0042] In another embodiment, the porous shell is composed of the same polymer as the expanded granular material. This also ensures that the shell has good weldability to the expanded granular material.

[0043] Suitable polymers (P1) are known per se to the person skilled in the art. In the context of the present invention, thermoplastic elastomers are particularly suitable, for example thermoplastic polyurethanes, thermoplastic polyetheramides, polyetheresters, polyesteresters, thermoplastic olefin-based elastomers, crosslinked thermoplastic olefin-based elastomers or thermoplastic vulcanizates, or thermoplastic styrene-butadiene block copolymers. Suitable examples are polystyrene or derivatives thereof, polypropylene, polyethylene, ethylene propylene diene monomer rubber (EPDM), ethylene-vinyl acetate (EVA), ethylene-vinyl acetate copolymers, thermoplastic polyurethanes, polyamides, polyesters, polyvinylidene fluoride, polyetheramides, polyethylene terephthalate or polybutylene terephthalate, or mixtures and blends of said polymers. In another embodiment, the present invention therefore also relates to a process for preparing a molded article as described above, wherein polymer (P1) is selected from polystyrene, polypropylene, thermoplastic polyurethane, polyamide, polyester, polyvinylidene fluoride, polyetheramide, polyethylene terephthalate or polybutylene terephthalate, or mixtures and blends of said polymers.

[0044] Expanded granular materials consisting of said polymers are also known per se to the person skilled in the art.In another embodiment, the invention therefore also relates to a process for producing a molded article as described above, wherein the average diameter of the particles of the expanded granular material is in the range from 0.5 to 20 mm.

[0045] According to the present invention, two or more different foamed granular materials can also be used. In this article, first, the foamed granular material can be composed of different materials in each case, provided that the particles of the foamed granular material used are weldable. The color or size of the particles can also be different. The molded article prepared in this way has, for example, regions with different properties (such as mechanical properties, color, particle shape, density, etc.). This is achieved in the following manner, that is, according to the required properties of the molded article, the individual particles with different properties are positioned in the initial molded article or mold, and then, for example, they are firmly combined with each other by welding. In principle, expanded particles can be used according to the present invention. However, a mixture of expanded particles and expandable particles can also be used basically.

[0046] In another embodiment, the present invention therefore also relates to a method for preparing a molded article as described above, wherein at least one other expanded granular material is used. The polymer used as polymer (P1) is suitable in principle. In the context of the present invention, thermoplastic elastomers are particularly suitable, such as thermoplastic polyurethanes, thermoplastic polyetheramides, polyetheresters, polyesteresters, thermoplastic olefin-based elastomers, crosslinked thermoplastic olefin-based elastomers or thermoplastic vulcanizates, or thermoplastic styrene-butadiene block copolymers. For example, polystyrene or its derivatives, polypropylene, polyethylene, ethylene propylene diene rubber (EPDM), ethylene-vinyl acetate (EVA), ethylene-vinyl acetate copolymers, thermoplastic polyurethanes, polyamides, polyesters, polyvinylidene fluoride, polyetheramides, polyethylene terephthalate or polybutylene terephthalate, or mixtures and blends of the polymers can be used. The different properties of the particles used can, for example, be selected from the type of polymer used, such as EPS; EPP, E-TPU, E-PVDF, E-PEBA, E-PA, E-PBT E-PET; E-PES; E-PPSU, E-PSU, E-PEI; molecular weight, additives, color, density, size, shape, mechanical properties, such as elastic modulus, compression strength, insulation properties, resilience, lambda value, fire resistance or electrical properties.

[0047] In a further embodiment, the present invention therefore also relates to a process for producing a moulded article as described above, wherein at least two different expanded granular materials of different colours are used.

[0048] In another embodiment, the present invention also relates to a method for producing a molded article as described above, wherein at least two different expanded granular materials having different particles are used.

[0049] In this context, different particles can be introduced into the shell in a suitable manner to control the properties or regions of the resulting molded article. For example, the surface of the resulting molded article can also be structured. In another embodiment, the invention also relates to a method for preparing a molded article as described above, wherein at least two different expanded granular materials of different colors are used, which are arranged in the shell so that the graphic elements are visible after welding.

[0050] Preferably, about 10-300 g / m 2 The shell material is introduced into the outer layer of the molded article.

[0051] If a colored shell material is selected for the particles, color effects can be achieved that do not require painting. Transparent shell materials protect the interior of the molding from damage and contamination, but show the structure and color of the original particles.

[0052] Positioning can be achieved by preparing an initial molding in which the particles are fixed according to the desired arrangement, then introducing the initial molding into the mold and welding the particles. The particles can also be positioned directly in the mold in the desired arrangement. In other technical fields, for example in the processing of fluids or solids (e.g. bulk materials, gravel, slurries), or in ceramic processing and powder metallurgy, simulation of the movement of individual particles is very common in order to be able to predict the density distribution in the molding.

[0053] The filling of the initial molding is done, for example, by manual introduction or by layering, pushing, squeezing, robot positioning, spinning or suction. It is important that the particles are positioned in such a way that they then take up the desired position in the molding and also maintain this position during the welding process. This can be simulated in advance, for example, by means of the above-mentioned FEM simulation and designed accordingly. Suitable methods are known per se to the person skilled in the art.

[0054] In another embodiment, the present invention therefore also relates to a process for producing a moulded article as described above, wherein the shell is filled by layering, pushing, extruding, robotic positioning, spinning or suction.

[0055] The initial molding may contain only foam particles, but other substances may also be placed, such as inserts, fixing elements, struts, reinforcing elements, metal plates, meshes, grids, electrical or electronic components, hollow bodies, foams, pastes, adhesives, lubricants, processing aids, PU reaction systems within the initial molding. Therefore, in the context of the present invention, inserts made of substances that are compatible with the particle foam or incompatible substances can be introduced into the initial molding. In this way, the properties of the finished molding can be further changed. Such inserts are preferably used for parts that are subjected to high mechanical stresses, such as the soles of sports shoes, in order to achieve the above-mentioned dynamic properties of the soles. As a prior art, in this case, the reinforcing element or the torsion bar is incorporated into the sole at a later stage.

[0056] In this way, inserts such as sensors, cables, electrical components etc. can also be easily positioned within the welded moulding.

[0057] In a further embodiment, the present invention therefore also relates to a process for producing a moulded article as described above, wherein further elements are introduced into the shell during the filling in step (ii).

[0058] In another embodiment, the present invention therefore also relates to a process for producing a molded article as described above, wherein the further elements are selected from inserts, fixing elements, struts, reinforcing elements, metal sheets, meshes, grids, electrical or electronic components, hollow bodies, foams, pastes, adhesives, lubricants and processing aids.

[0059] According to the invention, the particles can be positioned within the shell. It is advantageous to position the individual particles intentionally and reproducibly. For this purpose, the particles are introduced into the mold, for example by spraying, so that they stay exactly at the desired position. This can be achieved by means of a pneumatic nozzle, which can also be moved directionally, or by designing the mold so that, for example, a robot arm performs the positioning.

[0060] If the introduction into the mold is achieved by a flow of air or fluid, or if the particles are dropped, the flight path can be determined by the properties of the particles themselves, for example by their weight, shape, surface properties, etc. In this context, computer simulations can also be used as an aid to pre-calculate the flight path.

[0061] The particles can also be drawn into the desired location by suction through openings in the die.

[0062] Positioning can be accomplished using auxiliary materials such as adhesives, etc. This also applies to the filling / preparation of the initial molded product. This is called discrete element method (DEM). Suitable simulation methods for positioning particles are known to those skilled in the art per se. For example, there are known methods for simulating the behavior of particles in fluids. These can be described by a combination of the above-mentioned DEM method and CFD method.

[0063] In another aspect, the present invention also relates to a moulded article obtainable by or by a process as described above.

[0064] The moldings of the invention may, for example, have a plurality of regions, for example at least two regions with different properties. The position of the regions relative to one another and their position within the molding may vary within wide ranges.

[0065] Preferably, it is a feature of the mouldings of the invention that the transitions in properties between regions can also be fluid or dynamic, if desired, and not just abrupt, as is the case with parts of mouldings formed from separately connected parts.

[0066] The molded articles of the invention may have one or more such regions having different properties.

[0067] The moldings according to the invention can also consist only partially of the above-mentioned properties and can be bonded by other molding concepts (eg adhesive bonding). Special methods can also be used in combination, such as slot molds and / or slide molds.

[0068] If the shell is fused to the particles, the molded article has an additional outer layer which can have a crucial influence on the properties of the molded article.

[0069] These properties can be, for example, color, tactile properties, hydrophobicity / hydrophilicity, compression strength, elongation at break, elasticity, resilience, shear strength, conductivity. Depending on the thickness of the shell used and the corresponding volume and thickness of the inner layer, these properties can be adjusted individually.

[0070] The molded articles of the invention can be used in various ways. In another aspect, the invention also relates to the use of the molded articles obtainable by or by the process of the invention as soles, parts of soles, mattresses, seat cushions, padding, handles, protective films, as components for automotive interiors and exteriors, as gymnastic mats, body protectors, decorative elements in automotive construction, sound insulators, shock absorbers, cushioning pads, bicycle saddles, toys, tires or parts of tires or coverings for athletic surfaces, coverings for gymnasiums or coverings for sidewalks, for example in the form of floor tiles, sandwich elements or as cushioning layers or cushioning cores in packaging.

[0071] Further embodiments of the invention can be found in the claims and the examples. It is to be understood that the features of the subject matter / method or use of the invention described above and explained below can be used not only in the combination specified in each case, but also in other combinations without departing from the scope of the invention. Thus, for example, combinations of preferred features with particularly preferred features, or combinations of features not further characterized with particularly preferred features, etc. are also implicitly included, even if this combination is not explicitly mentioned.

[0072] Exemplary embodiments of the present invention are described in detail below, but are not intended to limit the present invention. In particular, the present invention also includes those embodiments resulting from dependent references and combinations thereof described in detail below. More particularly, it should be noted that in the case of referring to the scope of the embodiment, for example in the case of the expression "according to any one of embodiments 1 to 4", it is intended to explicitly disclose each embodiment within the scope. Those skilled in the art will consider this phrase to be synonymous with the phrase "any one of embodiments 1, 2, 3 and 4". It is expressly pointed out that the following embodiments do not constitute claims, but are structural parts of the description related to the general and preferred aspects of the present invention.

[0073] 1. A method for preparing a molded article (M), comprising the following steps

[0074] (i) providing a thin-walled, air-permeable shell;

[0075] (ii) filling the shell with a foamed granular material made of polymer (P1);

[0076] (iii) The expanded granular materials are welded to obtain a molded article (M).

[0077] 2. The method according to embodiment 1, wherein the welding is performed by steam welding.

[0078] 3. The method according to any one of embodiments 1 and 2, wherein the shell is porous.

[0079] 4. The method according to any one of embodiments 1 to 3, wherein the shell is a film, a braid, a knitted fabric, a mesh or a perforated metal.

[0080] 5. The method according to any one of embodiments 1 to 4, wherein the shell is composed of a flexible porous material.

[0081] 6. The method according to any one of embodiments 1 to 5, wherein the shell is closed after the filling in step (ii).

[0082] 7. The method according to any one of embodiments 1 to 6, wherein the shell consists of a material that can be welded to the foamed granular material.

[0083] 8. The method according to any one of embodiments 1 to 6, wherein the shell is removed from the molded article after welding.

[0084] 9. The method according to any one of embodiments 1 to 8, wherein polymer (P1) is selected from polystyrene, polypropylene, polyethylene, ethylene propylene diene monomer (EPDM), ethylene vinyl acetate (EVA), ethylene vinyl acetate copolymers, thermoplastic polyurethanes, polyamides, polyesters, polyvinylidene fluoride, polyetheramides, polyethylene terephthalate, polybutylene terephthalate, and mixtures and blends of said polymers.

[0085] 10. The process according to any one of embodiments 1 to 9, wherein at least one additional expanded granular material is used.

[0086] 11. The method according to any one of embodiments 1 to 10, wherein at least two different expanded granular materials of different colors are used.

[0087] 12. The method according to any one of embodiments 1 to 11, wherein at least two different expanded granular materials with different particles are used.

[0088] 13. The method according to any one of embodiments 1 to 12, wherein at least two different expanded granular materials of different colors are used, which are arranged in the shell in such a way that the graphic element is visible after welding.

[0089] 14. The method according to any one of embodiments 1 to 13, wherein the shell is filled by layering, pushing, extruding, robotic positioning, spinning or suction.

[0090] 15. The method according to any one of embodiments 1 to 14, wherein the particles are positioned in the shell in a controlled manner.

[0091] 16. The method according to any one of embodiments 1 to 15, wherein the controlled introduction of the particles into the shell is accomplished using computer simulation.

[0092] 17. The method according to any one of embodiments 1 to 16, wherein during the filling in step (ii), further elements are introduced into the shell.

[0093] 18. The method according to embodiment 17, wherein the further element is selected from inserts, fixing elements, struts, reinforcing elements, metal plates, meshes, grids, electrical or electronic components, hollow bodies, foams, pastes, adhesives, lubricants and processing aids.

[0094] 19. The method according to any one of embodiments 1 to 18, wherein the particles of the expanded granular material have an average diameter of 0.5 to 20 mm.

[0095] 20. A moulded article obtainable by or by the process according to any one of embodiments 1 to 19.

[0096] 21. A molded article (M) obtainable by or by a process comprising the following steps:

[0097] (i) providing a thin-walled, air-permeable shell;

[0098] (ii) filling the shell with a foamed granular material made of polymer (P1);

[0099] (iii) The expanded granular materials are welded to obtain a molded article (M).

[0100] 22. The molded article according to embodiment 21, wherein the welding is performed by steam welding.

[0101] 23. The molded article according to any one of embodiments 21 and 22, wherein the shell is porous.

[0102] 24. The molded article according to any one of embodiments 21 to 23, wherein the shell is a film, a braid, a knitted fabric, a mesh or a perforated metal.

[0103] 25. The molded article according to any one of embodiments 21 to 24, wherein the shell consists of a flexible porous material.

[0104] 26. The molded article according to any one of embodiments 21 to 25, wherein the shell is closed after the filling in step (ii).

[0105] 27. The molded article according to any one of embodiments 21 to 26, wherein the shell consists of a material that can be welded to the expanded particulate material.

[0106] 28. The molded article according to any one of embodiments 21 to 26, wherein the shell is removed from the molded article after welding.

[0107] 29. The molded article according to any one of embodiments 21 to 28, wherein polymer (P1) is selected from polystyrene, polypropylene, polyethylene, ethylene propylene diene monomer (EPDM), ethylene vinyl acetate (EVA), ethylene vinyl acetate copolymers, thermoplastic polyurethanes, polyamides, polyesters, polyvinylidene fluoride, polyetheramides, polyethylene terephthalate, polybutylene terephthalate, and mixtures and blends thereof.

[0108] 30. The molded article according to any one of embodiments 21 to 29, wherein at least one additional expanded granular material is used.

[0109] 31. The molded article according to any one of embodiments 21 to 30, wherein at least two different expanded granular materials of different colors are used.

[0110] 32. The molded article according to any one of embodiments 21 to 31, wherein at least two different expanded granular materials with different particles are used.

[0111] 33. The molded article according to any one of embodiments 21 to 32, wherein at least two different expanded granular materials of different colors are used, which are arranged in the shell in such a way that the graphic element is visible after welding.

[0112] 34. The molded article according to any one of embodiments 21 to 33, wherein the shell is filled by layering, pushing, extruding, robotic positioning, spinning or suction.

[0113] 35. The molded article according to any one of embodiments 21 to 34, wherein the particles are positioned in the shell in a controlled manner.

[0114] 36. The molded article according to any one of embodiments 21 to 35, wherein the controlled introduction of the particles into the shell is accomplished using computer simulation.

[0115] 37. The molded article according to any one of embodiments 21 to 36, wherein during the filling of step (ii), further elements are introduced into the shell.

[0116] 38. The molded article according to embodiment 37, wherein the further elements are selected from inserts, fixing elements, struts, reinforcing elements, metal sheets, meshes, grids, electrical or electronic components, hollow bodies, foams, pastes, adhesives, lubricants and processing aids.

[0117] 39. The molded article according to any one of embodiments 21 to 38, wherein the particles of the expanded granular material have an average diameter of 0.5 to 20 mm.

[0118] 40. Use of a molded article obtainable by or by a process according to any one of embodiments 1 to 19 or a molded article according to any one of embodiments 20 to 39 as a sole, part of a sole, a mattress, a seat cushion, a liner, a handle, a protective film, as a component for automotive interiors and exteriors, as a gymnastic mat, a body protector, a decorative element in automotive construction, a sound insulator, a vibration damper, a cushioning pad, a bicycle saddle, a toy, a tire or part of a tire or a covering for athletic surfaces, a covering for gymnasiums or sidewalks, a sandwich element or a cushioning layer or a cushioning core in packaging.

[0119] 41. A method for producing a sole, a part of a sole, a mattress, a seat cushion, a liner, a handle, a protective film, a component for the interior and exterior of an automobile, a gymnastics mat, a body protector, a decorative element in an automobile structure, a sound insulator, a vibration damper, a cushioning pad, a bicycle saddle, a toy, a tire or a part of a tire or a covering for a track surface, a covering for a gymnasium or a sidewalk, a sandwich element or a cushioning layer or a cushioning core in packaging, wherein a molded article obtainable by or by a method according to any one of embodiments 1 to 19 or a molded article according to any one of embodiments 20 to 39 is used.

[0120] The following examples serve to illustrate the invention but in no way limit the subject matter of the invention. Example

[0121] 1. Example 1

[0122] Different colors (white and red) of E-TPU 1180G2 particles were layered into 25g / m 2 The tube is sealed under slight pretension. The tube is placed in a perforated, steam-permeable mold in an unsecured manner. This mold is placed in a sheet mold and welded with steam in an Erlenbach molding machine as follows:

[0123] Steam temperature: 105℃

[0124] Horizontal steam 1: 2 seconds 0.5 bar

[0125] Horizontal steam 2: 2 seconds 0.5 bar

[0126] Autoclave, mobile side: 2 seconds at 1.6 bar

[0127] Autoclave, fixed side: 2 seconds at 1.6 bar

[0128] Result: loosely welded molding, density about 150 g / l, no noticeable movement of the particles, TPU nonwoven barely noticeable (melted), particle structure not very distinct.

[0129] 2. Example 2

[0130] E-TPU 1180G2 particles were introduced into the 150g / m 2 The hose is sealed under slight pretension. The hose is placed in a perforated, steam-permeable mold in an unsecured manner. The mold is placed in a sheet mold and welded with steam in an Erlenbach molding machine as follows:

[0131] Steam temperature: 110℃

[0132] Horizontal steam 1: 2 seconds 0.8 bar

[0133] Horizontal steam 2: 2 seconds 0.8 bar

[0134] Autoclave, mobile side: 2 seconds at 1.6 bar

[0135] Autoclave, fixed side: 2 seconds at 1.6 bar

[0136] Result: Loosely welded molding, density of about 150 g / l, no noticeable particle migration, TPU nonwoven still visible. The particle structure is not very obvious. The tensile strength of the molding is 20% higher than that of the molding without shell.

[0137] 3. Example 3

[0138] Expanded particles of Ecoflex (a biodegradable polyester from BASF SE) were introduced into a 30 g / m 2 The Ecoflex nonwoven hose is sealed under slight pretension. The hose is placed in a perforated, steam-permeable mold in an unsecured manner. This mold is placed in a sheet mold and welded with steam in an Erlenbach forming machine as follows:

[0139] Steam temperature: 105℃

[0140] Horizontal steam 1: 2 seconds 0.5 bar

[0141] Horizontal steam 2: 2 seconds 0.5 bar

[0142] Autoclave, mobile side: 2 seconds at 1.6 bar

[0143] Autoclave, fixed side: 2 seconds at 1.6 bar

[0144] Result: loosely welded moulding, density about 150 g / l, no noticeable movement of the particles, nonwoven barely noticeable (melted), particle structure not very distinct.

[0145] 4. Example 4

[0146] E-TPU 1180G2 particles were introduced into the 25g / m 2 The tube is sealed under slight pretension. The tube is placed in a perforated, steam-permeable mold in an unsecured manner. This mold is placed in a sheet mold and welded with steam in an Erlenbach molding machine as follows:

[0147] Steam temperature: 105℃

[0148] Horizontal steam 1: 2 seconds 0.5 bar

[0149] Horizontal steam 2: 2 seconds 0.5 bar

[0150] Autoclave, mobile side: 2 seconds at 1.6 bar

[0151] Autoclave, fixed side: 2 seconds at 1.6 bar

[0152] Result: loosely welded moulding, density about 150 g / l, TPU nonwoven structure barely noticeable (melted), moulding red on the outside.

[0153] 5. Example 5

[0154] E-TPU Infinergy granules of different colors (white and red) were introduced manually in two layers into a hose (40 mm in diameter, 150 mm in length, made of 15-denier nylon braid). The hose was sealed under slight pretension. Subsequently, the hose was introduced into a steam-permeable metal mold with dimensions of 200×200×60 mm. The mold was positioned in a disc-shaped tool with a diameter of 300 mm and a thickness of 90 mm.

[0155] The pieces are welded in an Erlenbach EHV-C 520 / 420 forming machine.

[0156] Steam temperature: 105℃

[0157] Horizontal steam 1: 2 seconds 0.5 bar

[0158] Horizontal steam 2: 2 seconds 0.5 bar

[0159] Autoclave, mobile side: 2 seconds at 1.6 bar

[0160] Autoclave, fixed side: 2 seconds at 1.6 bar

[0161] Result: loosely welded molding with a density of 150 g / l, no significant displacement of particles, and the nylon hose can be easily separated from the molding after the welding operation.

[0162] 6. Example 6

[0163] E-TPU Infinergy granules of different colors (white and red) were manually introduced in layers into multiple hoses made of 15-denier nylon braid. The hoses were sealed under slight pretension and then introduced into a steam-permeable metal mold with dimensions of 200×200×60 mm. The mold was positioned in a disc-shaped tool with a diameter of 300 mm and a thickness of 90 mm and welded in an Erlenbach EHV-C 520 / 420 molding machine.

[0164] Steam temperature: 105℃

[0165] Horizontal steam 1: 2 seconds 0.5 bar

[0166] Horizontal steam 2: 2 seconds 0.5 bar

[0167] Autoclave, mobile side: 2 seconds at 1.6 bar

[0168] Autoclave, fixed side: 2 seconds at 1.6 bar

[0169] Result: loosely welded molding, density 150 g / l, no noticeable movement of the hoses or pellets relative to each other, the nylon hoses can be separated from each other, the molding can be easily removed from the hoses.

[0170] 7. Example 7

[0171] E-TPU Infinergy granules of different colors (white and red) were introduced manually in two layers into a hose (40 mm in diameter, 150 mm in length, made of 15-denier nylon braid). The hose was sealed under slight pretension. Subsequently, the hose was introduced into a steam-permeable metal mold with dimensions of 200×200×60 mm. The mold was positioned in a disc-shaped tool with a diameter of 300 mm and a thickness of 90 mm.

[0172] The pieces are welded in an Erlenbach EHV-C 520 / 420 forming machine.

[0173] Steam temperature: 115℃

[0174] Horizontal steam 1: 2 seconds 0.5 bar

[0175] Horizontal steam 2: 2 seconds 0.5 bar

[0176] Autoclave, mobile side: 2 seconds at 1.6 bar

[0177] Autoclave, fixed side: 2 seconds at 1.6 bar

[0178] Result: Loosely welded molding with a density of 300 g / l, no voids under pressure, no obvious displacement of particles, and the nylon hose can be easily separated from the molding after the welding operation.

[0179] 8. Example 8

[0180] Infinergy E-TPU 1180G2 pellets of different colors (white and red) were added to a perforated, steam-permeable metal mold of dimensions 200 x 200 x 60 mm. The pellets were positioned so that there was a clear separation of the red and white pellet layers in the vertical direction in the 2 parts of the mold.

[0181] The mold was positioned in a disc-shaped tool with a diameter of 300 mm and a thickness of 90 mm and welded in an Erlenbach EHV-C 520 / 420 molding machine.

[0182] Steam temperature: 105℃

[0183] Horizontal steam 1: 2 seconds 0.5 bar

[0184] Horizontal steam 2: 2 seconds 0.5 bar

[0185] Autoclave, mobile side: 2 seconds at 1.6 bar

[0186] Autoclave, fixed side: 2 seconds at 1.6 bar

[0187] Result: loosely welded molding with a density of 150 g / l, no significant displacement of the particles, the molding can be easily removed from the metal mold after the welding operation.

[0188] 9. Example 9 (Comparative Example):

[0189] Infinergy E-TPU 1180G2 pellets were added to a steam-impermeable polyethylene film of 200×200×60 mm in size. The inlet for introducing the pellets was welded to make the entire film steam-impermeable. The added pellets were placed in a 200 mm×20

[0190] mm square moulds and contacted with steam to fuse them.

[0191] The welding was carried out in a forming machine from Kurtz ersa GmbH (Energy Foamer K68).

[0192] Steam temperature: 150℃

[0193] Horizontal steam 1: 40 sec 1.3 bar

[0194] Horizontal steam 2: 20 seconds 1.1 bar

[0195] Autoclave, mobile side: 10 sec 0.8 bar

[0196] Autoclave, fixed side: 10 sec 1.3 bar

[0197] Results: Compared to Examples 1 to 8, an increased energy supply (partly longer steam times and higher steam pressures) was used here, which additionally promoted welding. Nevertheless, the particles were not welded in the steam-tight polyethylene film, but remained loose in the film.

[0198] References:

[0199] JP355228A2

[0200] JP03097529

[0201] MX 2006-GT0017

Claims

1. A method for preparing a molded article (M), comprising the following steps (i) providing a thin-walled, gas-permeable shell, wherein the shell has a thickness of 1 to 5000 μm; (ii) filling the shell with a foamed granular material made of polymer (P1); (iii) welding the expanded granular material to obtain a molded article (M); The shell is constructed as a part of the molded article (M).

2. The method according to claim 1, wherein the welding is performed by steam welding.

3. A method according to claim 1 or 2, wherein the shell is porous.

4. The method of claim 1 or 2, wherein the shell is a film, a braid, a knitted fabric, a mesh or a perforated metal.

5. The method according to claim 1 or 2, wherein the shell consists of a flexible porous material.

6. The method according to claim 1 or 2, wherein the shell is closed after the filling in step (ii).

7. The method of claim 1 or 2, wherein the shell is composed of a material that can be welded to the expanded granular material.

8. The method according to claim 1 or 2, wherein the polymer (P1) is selected from polystyrene, polypropylene, polyethylene, ethylene propylene diene monomer (EPDM), ethylene vinyl acetate (EVA), ethylene vinyl acetate copolymers, thermoplastic polyurethanes, polyamides, polyesters, polyvinylidene fluoride, polyetheramides, polyethylene terephthalate, polybutylene terephthalate, and mixtures and blends of said polymers.

9. The method according to claim 1 or 2, wherein at least one additional expanded granular material is used.

10. The method according to claim 1 or 2, wherein at least two different expanded granular materials of different colors are used.

11. The method according to claim 1 or 2, wherein at least two different expanded granular materials having different particles are used.

12. The method according to claim 1 or 2, wherein at least two different expanded granular materials of different colors are used, which are arranged in the shell in such a way that the graphic element is visible after welding.

13. The method of claim 1 or 2, wherein the shell is filled by layering, pushing, extruding, robotic positioning, spinning or suction.

14. The method of claim 1 or 2, wherein the particles are positioned in the shell in a controlled manner.

15. The method of claim 1 or 2, wherein the controlled introduction of the particles into the shell is accomplished using computer simulation.

16. A method according to claim 1 or 2, wherein during the filling process of step (ii), further elements are introduced into the shell.

17. The method according to claim 16, wherein the further element is selected from inserts, fixing elements, struts, reinforcing elements, metal plates, meshes, grids, electrical or electronic components, hollow bodies, foams, pastes, adhesives, lubricants and processing aids.

18. The method according to claim 1 or 2, wherein the particles of the expanded granular material have an average diameter of 0.5 to 20 mm.

19. A moulded article obtainable by or by the process according to any one of claims 1 to 18.

20. Use of the molded article obtainable by or by the process according to any one of claims 1 to 18 or of the molded article according to claim 19 as a sole, part of a sole, a mattress, a seat cushion, a padding, a handle, a protective film; as a component for the interior and exterior of a car; as a gymnastic mat, a body protector, a decorative element in a car structure, a sound insulator, a shock absorber, a cushioning pad, a bicycle saddle, a toy, a tire or a part of a tire or a covering for a track surface, a covering for a gymnasium or a sidewalk, a sandwich element or a cushioning layer or a cushioning core in packaging.