Cutting Tools

By using specific proportions of cemented carbides such as WC and Ni in cutting tools and shooting peening on the surface, combined with the introduction of γ' phase, the wear resistance and cracking problems of cutting tools are solved, and the traditional ones are achieved Competing performance of Co-containing cemented carbide and the effect of reducing Co content.

CN114845828BActive Publication Date: 2024-11-01SANDVIK COROMANT
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202080088682.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-12-17
Publication Date
2024-11-01
Estimated Expiration
2040-12-17

AI Technical Summary

Technical Problem

Existing cutting tools have wear resistance and cracking problems in metal cutting applications, and the use of traditional Co-containing carbides has high material costs and environmental impacts, which are difficult to replace.

Method used

Carbide matrix is ​​used, which contains 80-93% WC, 3-13% Ni, Co/Ni<0.33, Fe/Ni<0.25, Cr/Ni<0.25 and 0.02

Benefits of technology

It significantly improves the wear resistance and crack resistance of cutting tools, extends the tool life, reduces the Co content, achieves performance that competes with traditional Co-containing carbides, and simplifies the manufacturing process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114845828B_ABST
    Figure CN114845828B_ABST
Patent Text Reader

Abstract

The present invention relates to a cutting tool comprising a cemented carbide substrate, wherein the cemented carbide is composed of hard components in a metal binder. The hard components comprise WC, and the WC content in the cemented carbide is 80 wt% to 93 wt%. The cemented carbide comprises Ni and Al, and has a Ni content of 3 wt% to 13 wt% and a weight ratio of Co / Ni < 0.33 and a weight ratio of Fe / Ni < 0.25 and a weight ratio of Cr / Ni < 0.25 and a weight ratio of 0.02 < Al / (Ni + Co + Fe) < 0.1. The crack resistance W is defined as the ratio of the load applied on a Vickers hardness indentation to the total crack length of the cracks formed at the corners of the Vickers hardness indentation. The product of the hardness H(rake face) at the rake face and the crack resistance W(rake face) at the rake face is H(rake face)*W(rake face) > 5000 HV100*N / μm.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a cutting tool of cemented carbide, wherein the cemented carbide comprises a metal binder and a hard component containing WC. The surface area of ​​the cutting tool has a higher crack resistance than the body area of ​​the cutting tool. Background Art

[0002] Cutting tools for metal cutting applications generally comprise a matrix of cemented carbide. Cemented carbide is a material that exhibits both high hardness and high toughness and has been successful for decades in performance in cutting applications. In order to further improve the performance of cutting tools, it is known to coat the tool with a wear-resistant coating. It is also known to process cutting tools in a process called post-processing, which includes steps such as wet blasting, dry blasting, brushing of cutting edges and / or polishing. These post-processing processes generally change the surface roughness of cutting tools and / or the residual stress in the surface area of ​​cutting tools.

[0003] Wang et al., “Effect of shot peening on the residual stresses and microstructure of tungsten cemented carbide”, Materials and Design 95, 2016, pp. 159-164, describes the effect of shot peening of cemented carbide. It shows that compressive residual stresses are induced in the surface layer, both in Co and WC.

[0004] There is a continuous need to improve the life and performance of cutting tools to save manufacturing time and reduce the risk of failure due to cutting tool breakage. There is also a need to reduce the amount of Co in cemented carbides and find alternative cemented carbides that can compete with traditional Co-containing cemented carbides in terms of metal cutting performance. Summary of the invention

[0005] The object of the present invention is to provide a cutting tool with improved wear resistance in metal cutting applications, and the object of the present invention is also to provide a method for manufacturing the cutting tool. Another object of the present invention is to provide a cutting tool with high resistance to chipping of the coating at the cutting edge. Another object is to provide a turning tool with increased resistance to chipping of the cutting edge and / or breakage of the cutting tool.

[0006] At least one of these objects is achieved by a cutting tool according to item 1 and a method according to item 14. Preferred embodiments are listed in the dependent claims.

[0007] The present invention relates to a cutting tool comprising a cemented carbide substrate, wherein the cemented carbide consists of hard constituents in a metallic binder, the hard constituents comprising WC, and the WC content in the cemented carbide being 80 wt% to 93 wt%, wherein the cemented carbide comprises Ni and Al, the cemented carbide having a Ni content of 3 wt% to 13 wt% and a weight ratio of Co / Ni < 0.33 and a weight ratio of Fe / Ni < 0.25 and a weight ratio of Cr / Ni < 0.25 and a weight ratio of 0.02 < Al / (Ni + Co + Fe) < 0.1, and wherein the cutting tool comprises a rake face, a flank face and a cutting edge therebetween, wherein the crack resistance W is defined as

[0008]

[0009] where P is the load of the Vickers hardness indentation 100 * 9.81 N, and ā is the average crack length [μm] of each crack formed at the corners of the Vickers hardness indentation, and wherein the product of the hardness H(rake face) at the rake face and the crack resistance at the rake face is H(rake face) * W(rake face) > 5000 HV100 * N / μm, preferably > 10000 HV100 * N / μm, more preferably > 15000 HV100 * N / μm.

[0010] Generally for most technical composites, such as cemented carbide materials, an increase in toughness is associated with a decrease in hardness. One way to represent the combination of toughness and resistance to plastic deformation (i.e., hardness) for cutting tool applications is by multiplying the hardness H by the crack resistance W, i.e., H * W. The higher H * W, the greater both the crack formation resistance and the resistance to plastic deformation of the cutting tool. It has unexpectedly been found that the method of the present invention enables a combination of very high crack resistance with a maintained or increased hardness. These properties are advantageous for metal cutting tools as they contribute to increasing the wear resistance of the tool.

[0011] In one embodiment of the present invention, the cemented carbide comprises x wt% Ni, y wt% Fe and z wt% Co, and wherein 5 < x + y + z < 10. Cemented carbides within this binder content range have a good combination of toughness and resistance to plastic deformation suitable for cutting tool applications. Depending on the metal cutting application, the amount of binder can be optimized by those skilled in the art.

[0012] In one embodiment of the present invention, the metal binder comprises a γ' phase. The space group of the γ' phase is preferably Pm-3m and preferably has an L12 crystal structure. To overcome the high creep rate of pure Ni, the target addition amount of Al is set to precipitate the γ' phase. This has been shown to enhance the combination of toughness and resistance to plastic deformation. Dislocations in the disordered metal binder will be pinned on the intermetallic γ' phase due to the difference in the length of the Burgers vector. The γ' phase has a cubic structure. The γ' phase or γ' grains or γ' precipitates can be seen in the SEM micrograph.

[0013] In one embodiment of the present invention, the average grain size of the γ' phase is 10 nm to 1000 nm in diameter, preferably 15 nm to 600 nm. The grain size is measured using the mean linear intercept method in an image of the cross-section of the matrix. The grain size of the γ' phase has been selected such that the dislocation pinning effect will strengthen the material. The optimum point between the generation and annihilation of defects is obtained within this range. To benefit from this effect, a person skilled in the art can optimize the size of the phase. The size of the γ' phase can be adjusted in a variety of alternative ways, such as adding Cr which reduces the size. The size also depends on the cooling of the cemented carbide after sintering. Very fast cooling may result in a very small γ' phase. The size of the γ' phase is saturated, so too long a cooling time does not change the size.

[0014] In one embodiment of the present invention, the metal binder in the cemented carbide comprises 10 vol% to 75 vol% of the γ' phase, preferably 15 vol% to 35 vol%, more preferably. The amount or fraction of the γ' phase can be adjusted by changing the Al / (Ni + Co + Fe) ratio, in a way that a higher ratio results in a higher amount or fraction of the γ' phase.

[0015] In one embodiment of the present invention, the γ' phase comprises Ni3Al. Preferably, the γ' comprises Ni3Al having solubility for elements such as Cr, Co, Fe, Ta, Ti, Hf, W, Mo, V, Mn, Si, Cu. Additional elements can be used to customize the size, morphology and properties of the γ' phase. The influence of each element can be evaluated by a person skilled in the art and optimized for a specific application.

[0016] In one embodiment of the present invention, the hardness of the rake face of the cutting tool is H(rake face) and the hardness of the body region of the cutting tool is H(body), where 0.90 < H(rake face) / H(body) < 1.10. High crack resistance on the surface can be achieved by reducing the hardness, but this will reduce the resistance to plastic deformation, which will be negative for the cutting tool life. Advantageously, the body and the rake face of the cutting tool have highly consistent hardness.

[0017] In one embodiment of the present invention, the crack resistance W measured on the rake face of the cutting tool is W(rake face), the W measured on the flank face of the cutting tool is W(flank face), and wherein W(rake face) / W(flank face) > 5, preferably > 8, more preferably > 10. Cracks formed during metal cutting usually originate from the front side of the cutting tool. Therefore, good crack resistance on the rake face is advantageous for metal cutting applications. Additionally, if only the rake face is shot-peened, the manufacturing process of the cutting tool will be relatively simple, and the importance of the flank face is slightly lower.

[0018] In one embodiment of the present invention, the crack resistance W measured on the rake face of the cutting tool is W(rake face), and the W measured on the body region of the cutting tool is W(body), and wherein W(rake face) / W(body) > 5, preferably > 8, more preferably > 10. Cracks formed during metal cutting usually originate from the rake face of the cutting tool. Therefore, good crack resistance on the rake face is advantageous for metal cutting applications. Cracks usually appear in the surface of the cutting tool rather than in the body. Therefore, high crack resistance in the surface region is advantageous.

[0019] In one embodiment of the present invention, the compressive residual stress measured in the surface region on the rake face of the cutting tool > 1500 MPa, preferably > 2000 MPa, more preferably > 2200 MPa, where the stress measurement is carried out using the X-ray diffraction and sin 2 ψ method with the (2 1 1) reflection of WC. Compressive residual stress inhibits the formation of cracks. Therefore, increasing the compressive residual stress on the rake face will extend the tool life of the cutting tool in metal cutting applications.

[0020] In one embodiment of the present invention, the cemented carbide contains 8 wt% to 12 wt% of Ni content and a weight ratio of Co / Ni < 0.05 and a weight ratio of Fe / Ni < 0.05 and a weight ratio of Cr / Ni < 0.02 and a weight ratio of 0.04 < Al / (Ni + Co + Fe) < 0.07. These compositions are suitable for metal cutting applications that require a combination of high toughness and appropriate hardness.

[0021] In one embodiment, the weight ratio of Fe / Ni < 0.02.

[0022] In one embodiment of the present invention, the cemented carbide contains 8 wt% to 12 wt% of Ni content and a weight ratio of Co / Ni < 0.05 and a weight ratio of Fe / Ni < 0.05 and a weight ratio of Cr / Ni < 0.08 and a weight ratio of 0.04 < Al / (Ni + Co + Fe) < 0.07. These compositions are suitable for applications that require a combination of high toughness and appropriate hardness.

[0023] In one embodiment of the present invention, the average grain size of WC in the cemented carbide is 0.2 μm to 10 μm, preferably 0.3 μm to 5 μm, and more preferably 0.5 μm to 2 μm. The WC grain size in this range is optimal for cemented carbides targeted for metal cutting inserts. The grain size is measured using the mean linear intercept method in an image of the cross-section of the substrate. According to the metal cutting application, those skilled in the art can optimize the WC grain size.

[0024] In one embodiment of the present invention, the cemented carbide contains one or more of Ti, Nb, Ta, Mo, W, Re, Ru. These elements can be used for further solid solution or particle strengthening.

[0025] The present invention relates to a method of treating a cutting tool comprising a cemented carbide substrate, wherein the cemented carbide is composed of hard components in a metal binder, the hard components contain WC, and the WC content in the cemented carbide is 80 wt% to 93 wt%, wherein the cemented carbide contains Ni and Al, the cemented carbide has a Ni content of 3 wt% to 13 wt% and a weight ratio of Co / Ni < 0.33 and a weight ratio of Fe / Ni < 0.25 and a weight ratio of Cr / Ni < 0.25 and a weight ratio of 0.02 < Al / (Ni + Co + Fe) < 0.1, wherein the cutting tool (1) comprises a rake face (2), a flank face (3) and a cutting edge therebetween, and wherein at least the rake face (2) is subjected to shot peening, and the method comprises the step of shot peening the rake face of the cutting tool. The shot peening increases the crack resistance of the surface while maintaining the hardness, thereby improving the combination of hardness and crack resistance.

[0026] In one embodiment of the present invention, the shot peening is carried out at a temperature of 100 °C to 600 °C, preferably 200 °C to 550 °C, and more preferably 300 °C to 500 °C. In one embodiment, the shot peening of the present invention is carried out at an elevated temperature, and this temperature is herein defined as the temperature at which the material (part of the cutting tool) being shot peened is during the shot peening process. A variety of methods can be used to generate the elevated temperature of the cutting tool part, such as induction heating, resistance heating, preheating on a hot surface / furnace, laser heating, etc. Alternatively, the cutting tool can be heated in a separate step before the shot peening step.

[0027] The temperature is appropriately measured on the substrate by any suitable method for measuring temperature. Preferably, an infrared temperature measuring device is used.

[0028] The portion of the substrate subjected to shot peening is at said temperature.It has been unexpectedly found that treating a cutting tool with shot peening while the cutting tool is heated increases its resistance to cracking in the surface region, which is an important property for increasing the life of a cutting tool.

[0029] In one embodiment of the invention, at least a portion of the cutting edge has an edge rounding (ER) between 10 μm and 50 μm, preferably between 20 μm and 40 μm. It has surprisingly been found that cutting tools manufactured according to the method of the invention perform well when the cutting tool has such an ER. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 is a schematic diagram of a cutting tool insert 1, which is provided with a rake face 2, a flank face 3 and a cutting edge disposed therebetween.

[0031] Figure 2 is a schematic diagram of a cross section of a cutting edge, in which the cutting edge bluntness ER is shown, and the width A of the cutting edge is also schematically shown.

[0032] Figures 3-4 is a SEM micrograph of a cross section of a cemented carbide of the cutting tool invention 1. The γ' phase is shown as gray squares in the binder phase.

[0033] Figures 5-6 is a SEM micrograph of a cross section of a cemented carbide of cutting tool invention 2. The γ' phase is shown as gray squares in the binder phase.

[0034] Figure 7 yes Figure 5 but with the γ′ phase marked in black.

[0035] Figure 8 yes Figure 6 but with the γ′ phase marked in black.

[0036] definition

[0037] "Cemented carbide" is a material comprising a hard component distributed in a continuous metal binder or forming a skeleton embedded in a continuous metal binder. The hard component mainly comprises WC. This material has the characteristics of combining high hardness from the hard component and high toughness from the metal binder, and is suitable as a matrix material for metal cutting tools.

[0038] The "composition" or "content" of cemented carbide herein means the average composition or average content in the cemented carbide matrix. For example, a gradient in a surface region of, for example, 15 μm to 30 μm from the substrate surface toward the body with a locally higher metal binder content does not change the average composition of the cemented carbide matrix of the cutting tool, because the size of the cutting tool is at least several millimeters.

[0039] The "metal binder" of cemented carbide may contain elements that dissolve in the metal binder during sintering, such as W and C from WC. Other elements may also dissolve in the binder, depending on what type of hard constituents are present.

[0040] "Cutting tool" in this context means a cutting tool used for metal cutting applications, such as an insert, end mill or drill. The application area may be turning, milling or drilling.

[0041] "ER" is a value of the cutting edge rounding intended to indicate the sharpness of a cutting edge. A larger ER value represents a rougher shaped cutting edge, while a smaller ER value represents a sharp cutting edge.

[0042] ER is defined in this paper as the value calculated according to:

[0043] - Placing the cutting tool with its support surface or a corresponding surface of said cutting tool on a flat surface.

[0044] - aligning a first face perpendicular to the flat surface in contact with the cutting edge to be measured along one side of the cutting tool, for example along the flank face 3 of the cutting tool 1,

[0045] - aligning a second face parallel to the flat surface and intersecting the first face at an intersection point, the second face being in contact with the cutting edge to be measured at the contact point, for example aligning the second face along the rake face 2 of the cutting tool 1 .

[0046] The value "ER" is equal to the distance between the intersection point between the first face and the second face and the contact point between the first face and the cutting tool close to the cutting edge, see Figure 2 .

[0047] "Shot blasting" means herein a process using abrasive particles in which material is removed from the treated surface, usually by abrasive wear. Shot blasting is well known in the cutting tool art and is, for example, known to introduce residual stresses in coatings on cutting tools.

[0048] "Shot peening" herein means that the surface of a cutting tool is bombarded with a medium containing particles such as beads, which are non-abrasive and generally have a rounded shape. The medium may be beads of a hard material such as oxide, steel or cemented carbide.

[0049] The term "body" herein means the innermost part (center) of the cutting tool.

[0050] The term "surface area" is used herein to refer to the exterior of a substrate that is affected by the shot peening process disclosed herein.

[0051] Other embodiments of the present invention

[0052] In one embodiment of the present invention, the shot peening is performed with ceramic beads, preferably with beads comprising ZrO2, SiO2 and Al2O3.

[0053] In one embodiment of the present invention, the shot peening is performed with beads having a diameter of about 50 μm to 200 μm. If the beads are too large, the risk of damaging the cutting edge increases. If the beads are too small, the energy and impact transferred from the medium to the substrate are less noticeable. The impact or energy from the beads during shot peening should not be too high, as this will increase the risk of damaging the surface and cutting edge of the cutting tool. The impact or energy from the beads should not be too low either, as that would not achieve the technical effect. If the beads are too large, the risk of damaging the cutting edge increases. If the beads are too small, the energy and impact transferred from the medium to the substrate are less noticeable. The appropriate size of the beads is related to the material of the beads and is selected by a person skilled in the art.

[0054] In one embodiment of the invention, the cemented carbide further comprises a cubic phase, sometimes referred to as a γ phase, which is a solid solution of cubic carbides and / or carbonitrides of one or more elements selected from Ti, Ta, Nb, Hf, Zr, V and Cr. The amount of the cubic phase (in area %) is suitably 2% to 25%, preferably between 3% and 15%. This can be measured in different ways, but one method is to perform image analysis on an optical microscope image or a scanning electron microscope (SEM) micrograph of a cross section of the substrate to calculate the average fraction of the γ phase.

[0055] In one embodiment of the present invention, the cemented carbide comprises a cubic phase and a surface zone rich in a cubic phase and rich in a binder phase. The thickness of the surface zone is suitably 2 μm to 100 μm, preferably 3 μm to 70 μm, and more preferably 8 μm to 35 μm. The thickness is determined by measuring on a SEM or LOM image of a cross section of the substrate. These measurements should be made in a moderately flat area on the substrate surface, i.e., not close to a cutting edge, at least 0.3 mm from a cutting edge or a tip, in order to obtain a true value. The boundary between the surface zone and the body is determined by the absence / presence of a cubic phase, which is usually quite obvious when observing a cross section of the substrate in an SEM or LOM image. The thickness is determined by the distance between the surface and the boundary between the surface zone and the body. Rich in binder means in this article that the binder phase content in the surface zone is suitably 1.05 to 1.65 times, preferably 1.1 to 1.5 times, of the binder phase content in the body. The binder phase content in the surface zone is suitably measured at half the depth of the total thickness / depth of the surface zone. All measurements made on the bulk should be made at an area not too close to the surface area. This means in this context that any measurement of the microstructure of the bulk should be made at a depth of at least 200 μm from the surface.

[0056] A surface region depleted of cubic phase means herein that the surface region contains no or very few (ie, less than 0.5 area %) cubic phase particles.

[0057] In one embodiment of the present invention, the cutting tool is provided with a coating, which may be a coloring layer or a wear-resistant coating.

[0058] In one embodiment of the present invention, the thickness of the coating is 2 μm to 20 μm, preferably 5 μm to 10 μm.

[0059] In one embodiment of the present invention, the coating is a CVD coating or a PVD coating, preferably the coating comprises one or more layers selected from TiN, TiCN, TiC, TiAlN, Al2O3 and ZrCN. The coating is preferably a CVD coating comprising a TiCN layer and an Al2O3 layer.

[0060] In one embodiment of the present invention, the cemented carbide substrate is provided with a wear resistant PVD coating, suitably a nitride, oxide, carbide or mixture thereof of one or more elements selected from Al, Si and elements of Groups 4, 5 and 6 of the periodic table.

[0061] In one embodiment of the invention, the cutting tool comprises a rake face, a flank face and a cutting edge therebetween, and wherein the shot peening is performed at least on the rake face. Shot peening of the rake face is advantageous because during the cutting operation, the working material strikes the cutting tool at the rake face, so that during the shot peening, the mechanism affecting the substrate is applied at the relevant area or volume of the substrate. Applying shot peening at the rake face is further advantageous because for many cutting tool geometries this means treating multiple cutting edges simultaneously.

[0062] In one embodiment of the invention, the shot peening is performed on a heated cutting tool, the method comprising a step prior to the shot peening in which the cutting tool is heated.

[0063] In one embodiment of the present invention, the method further comprises the step of shot blasting at least a portion of the cutting tool. Preferably, the portion comprises at least a portion of the cutting edge or an area close to the cutting edge.

[0064] In one embodiment of the present invention, the shot blasting step is performed after shot peening. The heat during shot peening may reduce some of the positive effects of shot peening, such as inducing residual stress in the coating, so by choosing to perform shot peening before shot peening, the positive effects of both can be maintained.

[0065] In one embodiment of the invention, the shot blasting and the shot peening are performed on the same part of the cutting tool. This is advantageous, for example, during large-scale manufacturing, since the cutting tool is loaded more efficiently.

[0066] In one embodiment of the present invention, the shot peening is performed in a shot direction perpendicular to the surface of the cutting tool. Vertical shot peening is advantageous because the depth of the impacted substrate is maximum when the heated shot peening is in this direction.

[0067] In one embodiment of the present invention, the cutting tool 1 is an insert, preferably a milling insert.

[0068] The shot peening process according to the invention may also be combined with other process steps known in the art for manufacturing cutting tools, such as brushing, polishing, wet blasting, dry blasting, etc. Example

[0069] Exemplary embodiments of the present invention will now be disclosed in more detail and compared with reference embodiments. Cutting tools (inserts) were prepared and analyzed.

[0070] Sample preparation

[0071] Cutting tools of cemented carbide are prepared by forming a matrix from the raw materials according to Table 1. Prealloyed NiAl powder consisting of 93.9 wt. % Ni and 5.3 wt. % Al is used. The average particle size (FSSS) of WC is 5.5 μm to 6.3 μm. The amount of each raw material is based on the total dry powder weight. The matrix is ​​manufactured according to conventional methods, including mixing, grinding, spray drying, pressing and sintering. Grinding is carried out in a grinder with a Co-containing grinding body, leaving Co in the powder and resulting in a Co content of about 0.02 wt. % Co in the sintered cemented carbide. Cutting tools of blade type CNMG120408-PM are formed.

[0072] The size of the γ' phase precipitates was measured in the SEM micrographs by the average linear intercept method. The average size of the γ' phase precipitates in Invention 1 was 150 nm, and the average size of the γ' phase precipitates in Invention 2 was 75 nm. The measurement of the size of each γ' phase was performed using the equivalent circle method. The volume fraction of the γ' phase was analyzed in the SEM micrographs. For Invention 1, the volume fraction in the metal binder was 23% by volume, and all phases larger than 30 nm were counted, see Figure 7 For Invention 2, the volume fraction in the metal binder is 17 volume %, and all phases larger than 30 nm are counted, see Figure 8 .

[0073] Table 1. Raw material composition (wt % of total dry powder weight)

[0074]

[0075] After sintering, both types of cutting tools were shot peened at 500°C to form Inventions 1-2.

[0076] The shot peening was carried out in an AUER Manual Blasting Cabinet ST 700PS. The blasting medium used was a spherical ceramic bead with an average diameter of about 100 μm. B120. The grain size of the ceramic beads is 63μm to 125μm. The composition of the ceramic beads is 60% to 70% ZrO2, 28% to 33% SiO2 and <10% Al2O3. The gun pressure is set to 5 bar, the working time is set to 20 seconds, the nozzle diameter is 8mm, and the projection distance is 100mm. The shot peening is applied perpendicular to the rake face of the cutting tool. In the case of heated shot peening, the cutting tool is heated with an induction coil heater before shot peening, and the temperature of the cutting tool is measured with a temperature sensor. The induction heater is a Rimac induction heater, 1.5kW.

[0077] After these post-treatments, the cutting edge of the cutting tool was about ER 40 μm.

[0078] Vickers measurement

[0079] Vickers indentations are formed on the rake face of the cutting tool and on the cross section of the cutting tool. Vickers indentations may also be formed on the flank face.

[0080] The rake face of the sample was lightly polished to obtain a suitable surface for crack length measurement. The sample was polished on paper using 0.25 μm diamond paste and hand polished, or polished on a 20 mm diameter felt wheel using 0.25 μm diamond paste using a Gatan Inc. Dimple Grinder Model 656 at medium speed and 35 g load. Polishing was performed until the surface exposed sufficient polished area for subsequent crack length measurement.

[0081] Bulk samples were prepared by cutting the insert perpendicular to the rake face using a diamond wheel, followed by polishing using 9 μm diamonds dispersed in oil on paper and then polishing using 1 μm diamonds dispersed in oil.

[0082] The Vickers hardness of the polished samples was measured using a programmable hardness tester KB30S from KB Prüftechnik. The measurements were calibrated against HV100 using a test block issued by the Euro Products Calibration Laboratory, UK. The Vickers hardness was measured according to ISO EN6507.

[0083] Vickers hardness measurements are made by programming the hardness tester to make an indentation at a specific location. The indentation is then made using a specified load. At least two parallel HV100 indentations are made, at least 1.5 mm apart from each other, and the results given are average values.

[0084] The crack length at each corner of the Vickers indentation was analyzed and measured with a camera and computer in an Olympus BX51M optical microscope. The specimen and camera were oriented so that the diagonal lines of the Vickers indentation were horizontal and vertical on the computer screen. A magnification of at least 100 times was used. If it was difficult to find the tip of the crack, a higher magnification was applied to locate the tip of the crack before measurement. The two diagonals of each indentation were measured, and the crack was measured as the projection from the corresponding indentation corner to the crack tip on the extended diagonal line of the indentation.

[0085] The hardness, crack length and crack resistance are presented in Table 2.

[0086] Table 2. Summary of hardness, crack length and crack resistance

[0087]

[0088] In the two inventive examples, the crack resistance of the body is 2.08 for Inventive 1 and 1.36 for Inventive 2. Thus, W(rake face) / W(body) of the two inventive examples is 15.2 for Inventive 1 and 10.4 for Inventive 2.

[0089] Residual stress measurement

[0090] Using X-ray diffraction, the so-called sin 2 The ψ method determines the residual stress in the above samples. In this method, the change in the lattice spacing d (and therefore the strain) is measured as a function of the sample tilt angle ψ. The residual stress is given by the strain vs. sin 2 The linear slope of the ψ curve is obtained. The residual stress is converted from the strain value by using the X-ray elastic constants.

[0091] XRD measurements were performed on a Bruker Discover D8 diffractometer with Davinci design equipped with a 1 μS microfocus source (CuK α radiation, ), -500 area detector and 1 / 4 Eulerian bracket. The (2 1 1) reflection of WC located at 117.32° 2θ was used for strain measurement. Residual stress measurements were performed in 1 to 4 angular directions, 0°, 90°, 180°, 270°, and for each Direction, 10 equally spaced ψ angles (0° to 50°) were measured for 400 seconds. A collimator with a diameter of 1.0 mm was used in all measurements.

[0092] The resulting residual stress was obtained from the strain data using the X-ray elastic constants of the WC Bragg peak (2 1 1). The X-ray elastic constants were calculated from Poisson's ratio v = 0.191 and Young's modulus = 717.360 GPa.

[0093] Mount the sample to the sample holder using tape.

[0094] The XRD data were analyzed using the software DIFFRAC EVA (Bruker) and High Score Plus (Malvern Panalytical). In the residual stress analysis the software LEPTOS 7 (Bruker) was used.

[0095] The residual stresses are presented in Table 3.

[0096] Table 3. Summary of residual stress results

[0097] Cutting Tools Shot peening Surface residual stress [MPa] Invention 1 500℃ -2276 Reference 1 none -311 Invention 2 500℃ -2275 Reference 2 none -506

[0098] Although the present invention has been described in conjunction with various exemplary embodiments, it should be understood that the present invention is not limited to the disclosed exemplary embodiments; on the contrary, it is intended to cover various modifications and equivalent arrangements within the appended claims. In addition, it should be recognized that any disclosed form or embodiment of the present invention may be combined with any other disclosed or described or suggested form or embodiment as a general matter of design choice. Therefore, the present invention is limited only as indicated by the scope of the appended claims.

Claims

1. A cutting tool comprising a cemented carbide substrate, wherein the cemented carbide consists of hard components in a metal binder, the hard components comprising WC, and the WC content in the cemented carbide is 80 wt% to 93 wt%, wherein the cemented carbide comprises Ni and Al, the cemented carbide has a Ni content of 3 wt% to 13 wt% and a weight ratio of Co / Ni < 0.33 and a weight ratio of Fe / Ni < 0.25 and a weight ratio of Cr / Ni < 0.25 and a weight ratio of 0.02 < Al / (Ni + Co + Fe) < 0.1, and wherein the cutting tool (1) comprises a rake face (2), a flank face (3) and a cutting edge therebetween, wherein the fracture resistance W is defined as Where P is the load of the Vickers hardness indentation, 100*9.81 N, and ā is the average crack length of each crack formed at the corner of the Vickers hardness indentation, in μm, and wherein the hardness H at the rake face 前刀面 and the crack resistance W at the front cutting edge 前刀面 The product of is H 前刀面 *W 前刀面 >5000HV100*N / μm.

2. The cutting tool according to claim 1, wherein the cemented carbide comprises x wt% Ni, y wt% Fe and z wt% Co, and wherein 5 < x + y + z < 10.

3. The cutting tool according to claim 1 or 2, wherein the metal binder comprises a γ' phase.

4. The cutting tool according to claim 3, wherein the average grain size of the γ' phase is 10 nm to 1000 nm in diameter.

5. The cutting tool according to claim 3, wherein the γ' phase comprises Ni3Al.

6. The cutting tool according to claim 1 or 2, wherein the hardness of the rake face of the cutting tool is H 前刀面 And the hardness of the body area of ​​the cutting tool is H 本体 , and 0.90 <H 前刀面 / H 本体 <1.

10.

7. The cutting tool according to claim 1 or 2, wherein the crack resistance W measured on the rake face of the cutting tool is W 前刀面 , W measured on the back face of the cutting tool is W 后刀面 , where W 前刀面 / W 后刀面 >5.

8. The cutting tool according to claim 1 or 2, wherein the crack resistance W measured on the rake face of the cutting tool is W 前刀面 , and W measured on the body area of ​​the cutting tool is W 本体 , where W 前刀面 / W 本体 >5.

9. The cutting tool according to claim 1 or 2, wherein the compressive residual stress measured in the surface area on the rake face of the cutting tool is >1500 MPa, wherein the stress measurement is performed using X-ray diffraction and sin 2 The ψ method is performed using the (2 11) reflection of WC.

10. The cutting tool according to claim 1 or 2, wherein the cemented carbide comprises a Ni content of 8 wt% to 12 wt% and a weight ratio of Co / Ni < 0.05 and a weight ratio of Fe / Ni < 0.05 and a weight ratio of Cr / Ni < 0.02 and a weight ratio of 0.04 < Al / (Ni + Co + Fe) < 0.

07.

11. The cutting tool according to claim 1 or 2, wherein the cemented carbide comprises a Ni content of 8 wt% to 12 wt% and a weight ratio of Co / Ni < 0.05 and a weight ratio of Fe / Ni < 0.05 and a weight ratio of Cr / Ni < 0.08 and a weight ratio of 0.04 < Al / (Ni + Co + Fe) < 0.

07.

12. The cutting tool according to claim 1 or 2, wherein the average grain size of WC in the cemented carbide is 0.2 μm to 10 μm.

13. The cutting tool according to claim 1 or 2, wherein the cemented carbide comprises one or more of Ti, Nb, Ta, Mo, W, Re, Ru.

14. The cutting tool according to claim 1 or 2, wherein the cutting edge radius ER of at least a part of the cutting edge is between 10 μm and 50 μm.

15. A method of treating a cutting tool according to claim 1, the cutting tool comprising a cemented carbide substrate, wherein the cemented carbide consists of hard constituents in a metal binder, the hard constituents comprising WC, and the WC content in the cemented carbide being 80 wt% to 93 wt%, wherein the cemented carbide comprises Ni and Al, the cemented carbide having a Ni content of 3 wt% to 13 wt% and a weight ratio of Co / Ni < 0.33 and a weight ratio of Fe / Ni < 0.25 and a weight ratio of Cr / Ni < 0.25 and a weight ratio of 0.02 < Al / (Ni + Co + Fe) < 0.1, wherein the cutting tool (1) comprises a rake face (2), a flank face (3) and a cutting edge therebetween, the method comprising the step of shot peening the rake face of the cutting tool, wherein at least the rake face (2) is shot peened, and wherein the shot peening is carried out at a temperature of 100°C to 600°C.