A method for preparing nanoscale titanium dioxide with controllable particle size
By using ammonium carbonate or ammonium bicarbonate as a control agent in the preparation of nanoscale titanium dioxide, combined with low-temperature hydrolysis and a two-step heat treatment process, the problems of complex processes and difficult particle size control in the existing technology are solved, and efficient and simple nanoscale production is achieved. The preparation of high-grade titanium dioxide powder promotes the high-quality development of electronic components.
Patent Information
- Application Number
- CN202210440450.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-04-25
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2042-04-25
AI Technical Summary
Existing methods for preparing nanoscale titanium dioxide have complex processes, introduced impurities that are difficult to remove, high costs, and low yields, making it difficult to achieve industrial large-scale production, and the particle size is difficult to control and adjust at the nanoscale.
Using ammonium carbonate or ammonium bicarbonate as a process control agent, uniformly dispersed, high-purity nanoscale titanium dioxide powder is prepared through low-temperature hydrolysis and a two-step heat treatment process. Metatitanic acid precursor is first generated, and then converted into rutile type through high-temperature heat treatment. Nanoscale titanium dioxide, adjust hydrolysis temperature and heat treatment conditions to control particle size.
It achieves the industrialized and stable preparation of nanoscale titanium dioxide powder with controllable particle size, high purity and uniform dispersion, simplifies the process, improves efficiency and yield, and is suitable for the development of high-quality electronic components.
Abstract
Description
Technical Field
[0001] The invention belongs to the field of inorganic non-metallic materials and new chemical materials, and specifically relates to a method for preparing nano-scale titanium dioxide with controllable particle size. Background Art
[0002] Electronic components are the cornerstone of the development of the information technology industry (smart terminals, 5G, industrial Internet, data centers), and are also the key to ensuring the security and stability of the industrial chain and supply chain. At present, my country's electronic components industry has problems such as being large but not strong, which restricts the development of the information technology industry. One of the key factors is that the high-quality basic raw materials required for electronic components are heavily dependent on imports.
[0003] As the basic material and key core material in the field of electronic components, high-quality, nano-scale, rutile-type electronic titanium dioxide ceramic powders are heavily dependent on imports, and a serious technical blockade has been imposed on my country. The chip multilayer ceramic capacitors (MLCCs) and PTC thermistors required in different fields such as electronic products, communication base stations, and new energy vehicles have significant differences in the particle size, morphology, crystal form, and specific surface area of nano-scale electronic titanium dioxide ceramic powders.
[0004] At present, the main methods for preparing nano-scale titanium dioxide include: liquid phase methods such as sol-gel method, hydrothermal reaction method, chemical precipitation method, alcohol salt hydrolysis method, and gas phase methods such as gas phase hydrolysis method and gas phase oxidation method. These methods are usually only applicable to the preparation of small samples of nano-scale titanium dioxide in the laboratory, and there are problems such as complex process, difficult to remove impurities, high cost, high equipment requirements, or low yield, which makes it difficult to carry out industrial large-scale production. Therefore, inventing a preparation technology for nano-titanium dioxide that is suitable for industrial production and has a controllable and adjustable particle size at the nanoscale is of great significance for promoting the high-quality development of basic electronic components in my country. Summary of the invention
[0005] The present invention aims to provide a method for preparing nano-scale titanium dioxide with controllable particle size, which has simple process, high efficiency and yield, good repeatability, and high purity, uniform dispersion and no agglomeration of the prepared titanium dioxide powder. The particle size is controllable and adjustable at the nanometer scale, and is suitable for the industrialized stable preparation of nano-scale high-purity titanium dioxide.
[0006] A method for preparing nano-sized titanium dioxide with controllable particle size is provided, and the specific steps are as follows:
[0007] (1) Preparation of a metatitanic acid precursor: titanium tetrachloride is added dropwise into deionized water, and then a process control agent is added, stirred, heated for hydrolysis, filtered, and vacuum dried to obtain a metatitanic acid precursor; wherein the control agent is ammonium carbonate or ammonium bicarbonate, and the hydrolysis temperature is 65 to 95°C;
[0008] (2) Preparation of nano-scale titanium dioxide powder: The metatitanate precursor obtained in step (1) is subjected to two-step heat treatment in an air atmosphere, and then naturally cooled to room temperature to obtain nano-scale titanium dioxide powder; wherein the two-step heat treatment process is as follows: the first step heat treatment temperature is 350-400°C, and the time is 0.5-3h; the second step heat treatment temperature is 440-480°C, and the reaction time is 0.5-3h.
[0009] In the above scheme, in step (1), titanium tetrachloride is added to deionized water to obtain a titanium tetrachloride aqueous solution with a concentration of 0.5 to 1 mol / L.
[0010] In the above scheme, in step (1), the molar ratio of titanium tetrachloride to the process control agent is 1:1-4.
[0011] In the above scheme, in step (1), the hydrolysis time is 0.5 to 3 hours.
[0012] In the above scheme, in step (1), the drying temperature is 105-115° C. and the drying time is 12-24 hours.
[0013] The present invention provides a method for preparing nano-scale titanium dioxide with controllable particle size. Ammonium carbonate or ammonium bicarbonate is used as a process control agent to control low-temperature (65-95°C) hydrolysis, and a two-step heat treatment process is used to obtain uniformly dispersed, controllable particle size, and nano-scale titanium dioxide. The mechanism is as follows: First, when preparing a metatitanic acid precursor, adding ammonium carbonate or ammonium bicarbonate process control agents and coordinating low-temperature hydrolysis can effectively control the hydrolysis kinetics: on the one hand, carbonate or bicarbonate ions can promote the nucleation of metatitanic acid, inhibit its grain growth, reduce the size of metatitanic acid, and prevent metatitanic acid from agglomerating, and a uniformly dispersed, nano-scale metatitanic acid precursor can be obtained during low-temperature hydrolysis; on the other hand, ammonium ions can effectively promote the hydrolysis reaction and improve the reaction efficiency. The generated ammonium chloride is easy to remove during subsequent heat treatment, and has no obvious effect on the product quality and purity. Subsequently, by controlling the temperature and time of the two-step high-temperature heat treatment, a uniformly dispersed, high-purity, and fully rutile nano-scale titanium dioxide powder can be obtained. In the first step of heat treatment, metatitanic acid reacts to generate anatase-type titanium dioxide, and ammonium carbonate or ammonium bicarbonate and by-products produced when preparing a metatitanic acid precursor can be removed; in the second step of heat treatment, anatase-type titanium dioxide can be completely converted into rutile-type nano-scale titanium dioxide, and the particle size can be controlled and adjusted at the nanoscale by adjusting the hydrolysis temperature, heat treatment temperature and time.
[0014] The beneficial effects of the present invention are:
[0015] 1. The present invention provides a method for preparing nano-sized titanium dioxide with controllable particle size. Ammonium carbonate or ammonium bicarbonate is used as a process control agent, titanium tetrachloride is controlled to be added dropwise into deionized water and hydrolyzed at a low temperature (65-95° C.), and a two-step heat treatment process of the obtained metatitanic acid precursor is carried out at the same time, so that a nano-sized titanium dioxide powder with uniform dispersion, no agglomeration, high purity and full rutile crystal form can be obtained, and its particle size is controllable and adjustable at the nanometer scale.
[0016] 2. The preparation process of the present invention is simple, with high efficiency and yield and good repeatability. It is suitable for the industrial and stable preparation of nano-scale high-purity titanium dioxide, and is conducive to promoting the high-quality development of basic electronic components. DETAILED DESCRIPTION
[0017] In order to better understand the present invention, the content of the present invention is further explained below in conjunction with the embodiments, but the content of the present invention is not limited to the following embodiments.
[0018] Example 1
[0019] A method for preparing nano-sized titanium dioxide with controllable particle size is provided, and the specific steps are as follows:
[0020] (1) Preparation of titanate precursor: 0.5 mol titanium tetrachloride was added dropwise into 1 L of deionized water, and then 2 mol ammonium carbonate was added. The mixture was stirred and heated to 65° C. for hydrolysis reaction for 0.5 h. The mixture was filtered and vacuum dried at 105° C. for 24 h to obtain a titanate precursor.
[0021] (2) Preparation of nano-scale titanium dioxide powder: The metatitanate precursor obtained in step (1) is placed in a muffle furnace with air atmosphere, heat treated at 350°C for 0.5 h, then heated to 440°C for 0.5 h, and then naturally cooled to room temperature. The precursor is completely converted into pure white nano-scale titanium dioxide.
[0022] The average particle size of the titanium dioxide product obtained was measured by scanning electron microscopy, transmission electron microscopy and laser particle size analyzer to be 5 nm, and it was evenly dispersed without obvious agglomeration; the crystal form of the titanium dioxide product was measured by X-ray diffractometer to be rutile; the purity of the titanium dioxide product was measured by inductively coupled plasma atomic emission spectrometer to be greater than 99.9%.
[0023] Example 2
[0024] A method for preparing nano-sized titanium dioxide with controllable particle size is provided, and the specific steps are as follows:
[0025] (1) Preparation of titanate precursor: 1 mol of titanium tetrachloride was added dropwise into 1 L of deionized water, and then 1 mol of ammonium bicarbonate was added. The mixture was stirred and heated to 95° C. for hydrolysis reaction for 3 h, filtered, and vacuum dried at 115° C. for 12 h to obtain a titanate precursor.
[0026] (2) Preparation of nano-scale titanium dioxide powder: The metatitanate precursor obtained in step (1) is placed in a muffle furnace with air atmosphere, heat treated at 400°C for 3 hours, then heated to 480°C for 3 hours, and then naturally cooled to room temperature. The precursor is completely converted into pure white nano-scale titanium dioxide.
[0027] The average particle size of the titanium dioxide product obtained was measured by scanning electron microscopy, transmission electron microscopy and laser particle size analyzer to be 94 nm, and it was evenly dispersed without obvious agglomeration; the crystal form of the titanium dioxide product was measured by X-ray diffractometer to be rutile; the purity of the titanium dioxide product was measured by inductively coupled plasma atomic emission spectrometer to be greater than 99.9%.
[0028] Example 3
[0029] A method for preparing nano-sized titanium dioxide with controllable particle size is provided, and the specific steps are as follows:
[0030] (1) Preparation of titanate precursor: 1 mol of titanium tetrachloride was added dropwise into 1 L of deionized water, and then 1 mol of ammonium carbonate was added. The mixture was stirred and heated to 95° C. for hydrolysis reaction for 0.5 h. The mixture was filtered and vacuum dried at 115° C. for 24 h to obtain a titanate precursor.
[0031] (2) Preparation of nano-scale titanium dioxide powder: The metatitanate precursor obtained in step (1) is placed in a muffle furnace with air atmosphere, heat treated at 400°C for 0.5 h, then heated to 480°C for 0.5 h, and then naturally cooled to room temperature. The precursor is completely converted into pure white nano-scale titanium dioxide.
[0032] The average particle size of the titanium dioxide product obtained was measured by scanning electron microscopy, transmission electron microscopy and laser particle size analyzer to be 58 nm, and it was evenly dispersed without obvious agglomeration; the crystal form of the titanium dioxide product was measured by X-ray diffractometer to be rutile; the purity of the titanium dioxide product was measured by inductively coupled plasma atomic emission spectrometer to be greater than 99.9%.
[0033] Example 4
[0034] A method for preparing nano-sized titanium dioxide with controllable particle size is provided, and the specific steps are as follows:
[0035] (1) Preparation of titanate precursor: 0.5 mol titanium tetrachloride was added dropwise into 1 L of deionized water, and then 1 mol ammonium bicarbonate was added. The mixture was stirred and heated to 65° C. for hydrolysis reaction for 3 h, filtered, and vacuum dried at 105° C. for 12 h to obtain a titanate precursor.
[0036] (2) Preparation of nano-scale titanium dioxide powder: The metatitanate precursor obtained in step (1) is placed in a muffle furnace with air atmosphere, heat treated at 350°C for 3 hours, then heated to 440°C for 3 hours, and then naturally cooled to room temperature. The precursor is completely converted into pure white nano-scale titanium dioxide.
[0037] The average particle size of the titanium dioxide product obtained was measured by scanning electron microscopy, transmission electron microscopy and laser particle size analyzer to be 23 nm, and it was evenly dispersed without obvious agglomeration; the crystal form of the titanium dioxide product was measured by X-ray diffractometer to be rutile; the purity of the titanium dioxide product was measured by inductively coupled plasma atomic emission spectrometer to be greater than 99.9%.
[0038] Example 5
[0039] A method for preparing nano-sized titanium dioxide with controllable particle size is provided, and the specific steps are as follows:
[0040] (1) Preparation of titanate precursor: 0.6 mol titanium tetrachloride was added dropwise into 1 L of deionized water, and then 0.8 mol ammonium bicarbonate was added. The mixture was stirred and heated to 70° C. for hydrolysis reaction for 2.5 h. The mixture was filtered and vacuum dried at 105° C. for 18 h to obtain a titanate precursor.
[0041] (2) Preparation of nano-scale titanium dioxide powder: The metatitanate precursor obtained in step (1) is placed in a muffle furnace with air atmosphere, heat treated at 350°C for 2 hours, then heated to 440°C for 1 hour, and then naturally cooled to room temperature. The precursor is completely converted into pure white nano-scale titanium dioxide.
[0042] The average particle size of the titanium dioxide product obtained was measured by scanning electron microscopy, transmission electron microscopy and laser particle size analyzer to be 12 nm, and it was evenly dispersed without obvious agglomeration; the crystal form of the titanium dioxide product was measured by X-ray diffractometer to be rutile; the purity of the titanium dioxide product was measured by inductively coupled plasma atomic emission spectrometer to be greater than 99.9%.
[0043] Example 6
[0044] A method for preparing nano-sized titanium dioxide with controllable particle size is provided, and the specific steps are as follows:
[0045] (1) Preparation of titanate precursor: 0.7 mol titanium tetrachloride was added dropwise into 1 L of deionized water, and then 1 mol ammonium bicarbonate was added. The mixture was stirred and heated to 75° C. for hydrolysis reaction for 2 h, filtered, and vacuum dried at 110° C. for 12 h to obtain a titanate precursor.
[0046] (2) Preparation of nano-scale titanium dioxide powder: The metatitanate precursor obtained in step (1) is placed in a muffle furnace with air atmosphere, heat treated at 360°C for 1 h, then heated to 480°C for 2 h, and then naturally cooled to room temperature. The precursor is completely converted into pure white nano-scale titanium dioxide.
[0047] The average particle size of the titanium dioxide product obtained was measured by scanning electron microscopy, transmission electron microscopy and laser particle size analyzer to be 76 nm, and it was evenly dispersed without obvious agglomeration; the crystal form of the titanium dioxide product was measured by X-ray diffractometer to be rutile; the purity of the titanium dioxide product was measured by inductively coupled plasma atomic emission spectrometer to be greater than 99.9%.
[0048] Example 7
[0049] A method for preparing nano-sized titanium dioxide with controllable particle size is provided, and the specific steps are as follows:
[0050] (1) Preparation of titanate precursor: 0.8 mol titanium tetrachloride was added dropwise into 1 L of deionized water, and then 1.6 mol ammonium carbonate was added. The mixture was stirred and heated to 80° C. for hydrolysis reaction for 1.5 h. The mixture was filtered and vacuum dried at 110° C. for 18 h to obtain a titanate precursor.
[0051] (2) Preparation of nano-scale titanium dioxide powder: The metatitanate precursor obtained in step (1) is placed in a muffle furnace with air atmosphere, heat treated at 370°C for 2 h, then heated to 470°C for 2.5 h, and then naturally cooled to room temperature. The precursor is completely converted into pure white nano-scale titanium dioxide.
[0052] The average particle size of the titanium dioxide product obtained was measured by scanning electron microscopy, transmission electron microscopy and laser particle size analyzer to be 69 nm, and it was evenly dispersed without obvious agglomeration; the crystal form of the titanium dioxide product was measured by X-ray diffractometer to be rutile; the purity of the titanium dioxide product was measured by inductively coupled plasma atomic emission spectrometer to be greater than 99.9%.
[0053] Example 8
[0054] A method for preparing nano-sized titanium dioxide with controllable particle size is provided, and the specific steps are as follows:
[0055] (1) Preparation of titanate precursor: 0.9 mol titanium tetrachloride was added dropwise into 1 L of deionized water, and then 2.7 mol ammonium carbonate was added. The mixture was stirred and heated to 85° C. for hydrolysis reaction for 1 h. The mixture was filtered and vacuum dried at 110° C. for 24 h to obtain a titanate precursor.
[0056] (2) Preparation of nano-scale titanium dioxide powder: The metatitanate precursor obtained in step (1) is placed in a muffle furnace with air atmosphere, heat treated at 380°C for 1.5 h, then heated to 460°C for 1.5 h, and then naturally cooled to room temperature. The precursor is completely converted into pure white nano-scale titanium dioxide.
[0057] The average particle size of the titanium dioxide product obtained was measured by scanning electron microscopy, transmission electron microscopy and laser particle size analyzer to be 42 nm, and it was evenly dispersed without obvious agglomeration; the crystal form of the titanium dioxide product was measured by X-ray diffractometer to be rutile; the purity of the titanium dioxide product was measured by inductively coupled plasma atomic emission spectrometer to be greater than 99.9%.
[0058] Example 9
[0059] A method for preparing nano-sized titanium dioxide with controllable particle size is provided, and the specific steps are as follows:
[0060] (1) Preparation of titanate precursor: 0.5 mol titanium tetrachloride was added dropwise into 1 L of deionized water, and then 2 mol ammonium bicarbonate was added. The mixture was stirred and heated to 90° C. for hydrolysis reaction for 0.5 h. The mixture was filtered and vacuum dried at 115° C. for 18 h to obtain a titanate precursor.
[0061] (2) Preparation of nano-scale titanium dioxide powder: The metatitanate precursor obtained in step (1) is placed in a muffle furnace with air atmosphere, heat treated at 390°C for 2.5 hours, then heated to 450°C for 1 hour, and then naturally cooled to room temperature. The precursor is completely converted into pure white nano-scale titanium dioxide.
[0062] The average particle size of the titanium dioxide product obtained was measured by scanning electron microscopy, transmission electron microscopy and laser particle size analyzer to be 37 nm, and it was evenly dispersed without obvious agglomeration; the crystal form of the titanium dioxide product was measured by X-ray diffractometer to be rutile; the purity of the titanium dioxide product was measured by inductively coupled plasma atomic emission spectrometer to be greater than 99.9%.
[0063] Obviously, the above embodiments are merely examples for clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived from this are still within the protection scope of the invention.
Claims
1. A method for preparing nano-sized titanium dioxide with controllable particle size, It is characterized in that The specific steps are as follows: (1) Preparation of metatitanic acid precursor: 0.5 mol titanium tetrachloride was added dropwise into 1 L of deionized water, and then 2 mol ammonium bicarbonate was added, stirred, heated to 90° C. for hydrolysis reaction for 0.5 h, filtered, and vacuum dried at 115° C. for 18 h to obtain a metatitanic acid precursor; (2) Preparation of nano-scale titanium dioxide powder: The metatitanate precursor obtained in step (1) was placed in a muffle furnace in an air atmosphere, heat treated at 390° C. for 2.5 h, then heated to 450° C. for 1 h, and then naturally cooled to room temperature, and the precursor was completely converted into pure white nano-scale titanium dioxide; The crystal form of the titanium dioxide product measured by an X-ray diffractometer is rutile; the purity of the titanium dioxide product measured by an inductively coupled plasma atomic emission spectrometer is greater than 99.9%.
Citation Information
Cited By
Preparation method of high-purity titanium dioxide
CN121361827A