Lithium-sulfur battery positive electrode material and preparation method thereof, lithium-sulfur battery positive electrode, lithium-sulfur battery

By preparing the hot melt composite of zinc cobaltate nano-thin cage material and elemental sulfur in lithium sulfur batteries, the problems of volume expansion and contraction of electrodes and polysulfide shuttle effects of lithium sulfur batteries are solved, and the specific capacity and cycle stability of the battery are improved , realizes efficient utilization of electrode materials.

CN114864902BActive Publication Date: 2024-11-12JIMEI UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210584106.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-05-27
Publication Date
2024-11-12
Estimated Expiration
2042-05-27

AI Technical Summary

Technical Problem

Lithium sulfur batteries have low utilization rate and poor circulation stability due to the volume expansion and contraction of the electrodes and the polysulfide shuttle effect, which limits their development and application.

Method used

Trivalent cobalt and divalent zinc metal compounds are mixed with organic solvents, adjusted pH value and carried out reflux heating and pyrolysis reactions to prepare zinc cobaltate nano-thin cage material, and heat-treated with elemental sulfur to form the positive electrode material of lithium sulfur battery , the conductivity and cyclic stability of the electrode are improved by its adsorption and catalytic action.

Benefits of technology

Effectively adsorb polysulfides, reduce the distance between the electrode and the current collector, improve ion and electron transmission efficiency, enhance the specific capacity and cycling stability of lithium-sulfur batteries, reduce useless space, and is suitable for large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114864902B_ABST
    Figure CN114864902B_ABST
Patent Text Reader

Abstract

The present invention discloses a method for preparing a positive electrode material for a lithium-sulfur battery, comprising the following steps: mixing a trivalent cobalt metal compound, a divalent zinc metal compound and an organic solvent to obtain a mixed solution. Adjusting the pH value of the mixed solution to 13-14 to obtain a raw material solution. The raw material solution is subjected to reflux heating treatment, and after sufficient reaction, solid-liquid separation is performed and the solid is retained to obtain a precursor. The precursor is subjected to a pyrolysis reaction to obtain a zinc cobaltate nano-thin cage material. The zinc cobaltate nano-thin cage material is mixed with elemental sulfur, and then heat-treated, and after sufficient reaction, a lithium-sulfur battery positive electrode material is obtained. The lithium-sulfur battery positive electrode material prepared by this method is used for lithium-sulfur batteries, and has high specific capacity and cycle stability while having a high sulfur loading. Accordingly, the present invention also provides a lithium-sulfur battery positive electrode material, a lithium-sulfur battery positive electrode and a lithium-sulfur battery prepared by the above-mentioned method for preparing a lithium-sulfur battery positive electrode material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of energy material preparation, and in particular to a lithium-sulfur battery positive electrode material and a preparation method thereof, a lithium-sulfur battery positive electrode, and a lithium-sulfur battery. Background Art

[0002] With the development of economy and science and technology, the energy structure of mankind is constantly changing towards clean and sustainable directions. At present, lithium-ion batteries with high energy density and long cycle stability have become the main power source for consumer electronic products and play an important role. However, with the development of high-energy mobile devices, lithium-ion batteries can no longer meet the current market demand. Compared with traditional lithium-ion batteries, lithium-sulfur batteries are considered to be one of the most promising new energy storage systems due to their ultra-high theoretical specific capacity (1675mAh / g) and theoretical energy density (2600Wh / kg), abundant sulfur reserves and low prices. They can be applied to portable electronic products, power vehicles and large-scale energy storage. However, lithium-sulfur batteries still have many problems and challenges, such as the extremely low electronic and ionic conductivity of the reactant single substance S8 and the final reduction products Li2S2 and Li2S of the battery system, the volume expansion and contraction of the electrode during charging and discharging, and the shuttle effect of polysulfides. The above defects lead to low utilization of active materials in lithium-sulfur batteries and poor battery cycle stability, which restricts the development and application of lithium-sulfur batteries.

[0003] Adding sulfur skeleton materials to the positive electrode of lithium-sulfur batteries can effectively improve the conductivity of the electrode, inhibit the shuttling effect of polysulfides, and catalyze sulfur conversion reactions. Currently, a lot of work is centered around this issue. The use of hollow materials is one of the main solutions. The surface of the hollow material can effectively adsorb polysulfides, and the hollow space inside can inhibit the volume expansion effect of the battery, thereby improving the cycle stability of the battery. However, the interior of the hollow material has a large number of hollow structures that cannot store sulfur, resulting in a large amount of waste of battery space. At a high sulfur loading, the electrode thickness is too large, resulting in the electrode being too far away from the current collector, limiting the transmission of ions and electrons on the electrode. If the thickness is forcibly reduced by increasing pressure, the internal pores of the electrode will be blocked, and the electrolyte will not be able to infiltrate the pores, affecting battery performance.

[0004] How to make lithium-sulfur batteries with hollow structure sulfur skeleton materials have higher specific capacity and cycle stability is a research hotspot in this field. Summary of the invention

[0005] The technical problem to be solved by the embodiments of the present invention is how to make a lithium-sulfur battery with a hollow structure sulfur skeleton material have a higher specific capacity and cycle stability.

[0006] In order to solve the above technical problems, the present invention provides a method for preparing a positive electrode material for a lithium-sulfur battery, comprising the following steps:

[0007] The trivalent cobalt metal compound, the divalent zinc metal compound and the organic solvent are mixed to obtain a mixed solution.

[0008] The pH value of the mixed solution was adjusted to 13-14 to obtain a raw material solution.

[0009] The raw material solution is subjected to reflux heating treatment, and after sufficient reaction, solid-liquid separation is performed and the solid is retained to obtain a precursor.

[0010] The precursor is subjected to a pyrolysis reaction to obtain a zinc cobaltate nano-thin cage material.

[0011] The zinc cobalt oxide nano-thin cage material is mixed with elemental sulfur, then heat treated, and after sufficient reaction, the positive electrode material of the lithium-sulfur battery is obtained.

[0012] In a feasible implementation, the mass ratio of the trivalent cobalt metal compound, the divalent zinc metal compound and the organic solvent is (3-8):(3-8):(500-2000).

[0013] In a feasible implementation, the mass ratio of zinc cobaltate nano-thin cage material to elemental sulfur is (10-40):(60-90).

[0014] In a feasible implementation, the temperature of the reflow heating treatment is 120°C-200°C.

[0015] In a feasible implementation, the temperature of the pyrolysis reaction is 500°C-950°C, the heating rate of the pyrolysis reaction is 1°C / min-5°C / min, and the pyrolysis time of the pyrolysis reaction is 2h-12h.

[0016] In a feasible implementation, in the operation of uniformly mixing the zinc cobalt oxide nano-thin cage material and elemental sulfur and then performing heat treatment, the heat treatment temperature is 140° C.-180° C., and the heat treatment time is 4 h-6 h.

[0017] In a feasible implementation, the trivalent cobalt metal compound is selected from at least one of cobalt acetylacetonate, cobalt acetate, cobalt nitrate and cobalt carbonate.

[0018] In a feasible implementation, the divalent zinc metal compound is selected from at least one of zinc acetylacetonate, zinc acetate, zinc nitrate and zinc carbonate. In a feasible implementation, the organic solvent is selected from at least one of ethanol, acetone, ethylene glycol and glycerol.

[0019] In a feasible implementation, an alkaline solution is used to adjust the pH value of the mixed solution, and the alkaline solution is selected from at least one of aqueous ammonia, sodium hydroxide solution and potassium hydroxide solution.

[0020] In a feasible implementation, the pyrolysis reaction is carried out in an air atmosphere or an oxygen atmosphere.

[0021] The implementation of the present invention has the following beneficial effects:

[0022] The positive electrode material of the lithium-sulfur battery prepared by the method can effectively adsorb polysulfides, catalyze sulfur conversion reactions, have a certain hollow structure, and the hollow structure occupies a very low space, which can reduce the distance between the positive electrode material of the lithium-sulfur battery and the current collector, improve the transmission efficiency of ions and electrons on the electrode, and at the same time reduce useless space on the basis of inhibiting the battery volume expansion of the lithium-sulfur battery, thereby improving the specific capacity and cycle stability of the lithium-sulfur battery.

[0023] The present invention adopts a non-template method to prepare a precursor, and then obtains a zinc cobalt oxide nano-thin cage material through a pyrolysis reaction, and then obtains a lithium-sulfur battery positive electrode material provided by the present invention through a hot melt composite with elemental sulfur. The method of the present invention is simple to operate, has a low temperature, simple post-processing, simple equipment requirements, moderate cost, and is suitable for large-scale production.

[0024] Correspondingly, the present invention also provides a lithium-sulfur battery positive electrode material, which is prepared by the above-mentioned preparation method of the lithium-sulfur battery positive electrode material.

[0025] The above-mentioned lithium-sulfur battery positive electrode material is used in lithium-sulfur batteries and has high specific capacity and cycle stability.

[0026] The cobalt zinc nanocage material has a good adsorption effect on polysulfides, which can effectively increase the sulfur loading of the positive electrode material of lithium-sulfur batteries and effectively inhibit the shuttle effect. At the same time, the cobalt zinc nanocage material has a good catalytic effect on the electrochemical conversion reaction of sulfur, which can effectively improve the utilization rate of active sulfur in lithium-sulfur batteries.

[0027] Correspondingly, the present invention also provides a lithium-sulfur battery positive electrode, and the material for preparing the lithium-sulfur battery positive electrode includes the above-mentioned lithium-sulfur battery positive electrode material.

[0028] The lithium-sulfur battery positive electrode is used in lithium-sulfur batteries and has high specific capacity and cycle stability.

[0029] Correspondingly, the present invention also provides a lithium-sulfur battery, which includes the above-mentioned lithium-sulfur battery positive electrode.

[0030] The above-mentioned lithium-sulfur battery has high specific capacity and cycle stability.

[0031] When the prepared lithium-sulfur battery has a 2When the sulfur loading is 2.5%, the capacity of the lithium-sulfur battery still remains at a high level of 700mAh / g after 1000 cycles at a high current density of 2C, and the specific capacity decay rate is only 0.016% per cycle.

[0032] Furthermore, the lithium-sulfur battery provided by the present invention can maintain a high specific capacity and cycle stability at a high sulfur loading. 2 When the sulfur loading is 100%, the lithium-sulfur battery can still release a specific capacity of more than 1000 mAh / g after 50 cycles, which is equivalent to a 10 mAh / cm 2 High area specific capacity. High specific capacity and low capacity decay rate. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 is a scanning electron microscope image of the zinc cobaltate nano-thin cage material prepared in Example 1;

[0034] Figure 2 The scanning electron microscope image and EDS scanning data of the zinc cobalt oxide nano-thin cage material prepared in Example 1;

[0035] Figure 3 is the X-ray diffraction pattern of the zinc cobaltate nano-thin cage material prepared in Example 1;

[0036] Figure 4 This is a battery cycle test diagram of the lithium-sulfur battery prepared in Example 1;

[0037] Figure 5 1 is a battery cycle test diagram of the lithium-sulfur battery prepared in Example 2 and the lithium-sulfur battery prepared in Comparative Example 1;

[0038] Figure 6 This is a battery cycle test diagram of the lithium-sulfur battery prepared in Example 3. DETAILED DESCRIPTION

[0039] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific embodiments of the present invention are described in detail below in conjunction with the accompanying drawings. In the following description, many specific details are set forth to facilitate a full understanding of the present invention. However, the present invention can be implemented in many other ways different from those described herein, and those skilled in the art can make similar improvements without violating the connotation of the present invention, so the present invention is not limited by the specific embodiments disclosed below.

[0040] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.

[0041] A method for preparing a positive electrode material for a lithium-sulfur battery comprises the following steps:

[0042] The trivalent cobalt metal compound, the divalent zinc metal compound and the organic solvent are uniformly mixed to obtain a mixed solution.

[0043] The pH value of the mixed solution was adjusted to 13-14 to obtain a raw material solution.

[0044] The raw material solution is subjected to reflux heating treatment, and after sufficient reaction, solid-liquid separation is performed and the solid is retained to obtain a precursor.

[0045] The precursor is subjected to a pyrolysis reaction to obtain a zinc cobaltate nano-thin cage material.

[0046] The zinc cobalt oxide nano-thin cage material is evenly mixed with elemental sulfur, and then heat treated to obtain the lithium-sulfur battery positive electrode material after full reaction.

[0047] The positive electrode material of the lithium-sulfur battery prepared by the method can effectively adsorb polysulfides, catalyze sulfur conversion reactions, have a certain hollow structure, and the hollow structure occupies a very low space, which can reduce the distance between the positive electrode material of the lithium-sulfur battery and the current collector, improve the transmission efficiency of ions and electrons on the electrode, and at the same time reduce useless space on the basis of inhibiting the battery volume expansion of the lithium-sulfur battery, thereby improving the specific capacity and cycle stability of the lithium-sulfur battery.

[0048] Furthermore, the hollow structure of the lithium-sulfur battery positive electrode material prepared by this method is only one-fifth of the traditional hollow material, which can greatly improve the transmission capacity of ions and electrons on the electrode.

[0049] In a feasible implementation, the mass ratio of the trivalent cobalt metal compound, the divalent zinc metal compound and the organic solvent is (3-8):(3-8):(500-2000).

[0050] In a feasible implementation, the mass ratio of zinc cobaltate nano-thin cage material to elemental sulfur is (10-40):(60-90).

[0051] In a feasible implementation, the temperature of the reflow heating treatment is 120°C-200°C.

[0052] In a feasible implementation, the temperature of the pyrolysis reaction is 500°C-950°C, the heating rate of the pyrolysis reaction is 1°C / min-5°C / min, and the pyrolysis time of the pyrolysis reaction is 2h-12h.

[0053] In a feasible implementation, in the operation of uniformly mixing the zinc cobalt oxide nano-thin cage material and elemental sulfur and then performing heat treatment, the heat treatment temperature is 140° C.-180° C., and the heat treatment time is 4 h-6 h.

[0054] In a feasible implementation, the trivalent cobalt metal compound is selected from at least one of cobalt acetylacetonate, cobalt acetate, cobalt nitrate and cobalt carbonate.

[0055] In a feasible implementation, the divalent zinc metal compound is selected from at least one of zinc acetylacetonate, zinc acetate, zinc nitrate and zinc carbonate.

[0056] Zinc cobaltate prepared from trivalent cobalt metal compounds and divalent zinc metal compounds can not only adsorb polysulfides, but also has good electrical conductivity and electrocatalytic properties, and can effectively improve the utilization rate of active sulfur in lithium-sulfur batteries.

[0057] In a feasible implementation, the organic solvent is selected from at least one of ethanol, acetone, ethylene glycol and glycerol.

[0058] In a feasible implementation, an alkaline solution is used to adjust the pH value of the mixed solution, and the alkaline solution is selected from at least one of aqueous ammonia, sodium hydroxide solution and potassium hydroxide solution.

[0059] In a feasible implementation, the pyrolysis reaction is carried out in an air atmosphere or an oxygen atmosphere.

[0060] The present invention adopts a non-template method to prepare a precursor, and then obtains a zinc cobalt oxide nano-thin cage material through a pyrolysis reaction, and then obtains a lithium-sulfur battery positive electrode material provided by the present invention through a hot melt composite with elemental sulfur. The operation is simple and easy to mass produce.

[0061] Correspondingly, the present invention also provides a lithium-sulfur battery positive electrode material, which is prepared by the above-mentioned preparation method of the lithium-sulfur battery positive electrode material.

[0062] The hollow structure of the positive electrode material of the lithium-sulfur battery inhibits the volume expansion of the positive electrode of the lithium-sulfur battery, improves the utilization rate of the active materials of the lithium-sulfur battery, and thus improves the specific capacity and cycle stability of the lithium-sulfur battery.

[0063] Furthermore, compared with the traditional hollow structure positive electrode material, since the lithium-sulfur battery positive electrode material provided by the present invention has fewer hollow structures and smaller volume, it can provide a higher sulfur loading while shortening the distance between the lithium-sulfur battery positive electrode material and the current collector on the lithium-sulfur battery, thereby bringing the active material sulfur closer to the current collector and improving the transmission efficiency of ions and electrons on the electrode.

[0064] Correspondingly, the present invention also provides a lithium-sulfur battery positive electrode, and the material for preparing the lithium-sulfur battery positive electrode includes the above-mentioned lithium-sulfur battery positive electrode material.

[0065] The lithium-sulfur battery positive electrode is used in a lithium-sulfur battery, which has a higher specific capacity and cycle stability.

[0066] Correspondingly, the present invention also provides a lithium-sulfur battery, which includes the above-mentioned lithium-sulfur battery positive electrode. The lithium-sulfur battery has high specific capacity and cycle stability.

[0067] With reference to the above implementation contents, in order to make the technical solution of the present invention more specific, clear and easy to understand, the technical solution of the present invention is now exemplified. However, it should be noted that the contents to be protected by the present invention are not limited to the following Examples 1 to 5.

[0068] Example 1

[0069] 0.514 g of zinc acetylacetonate, 0.706 g of cobalt acetylacetonate and 100 mL of ethylene glycol were mixed to obtain a mixed solution, and aqueous ammonia was added to the mixed solution to adjust the pH value to 13 to obtain a raw material solution.

[0070] The raw material solution was heated to 170° C., condensed and refluxed for 3 h, and then cooled to room temperature. The solid product was separated by centrifugation, washed with ethanol and deionized water, and vacuum dried at 80° C. overnight to obtain a precursor.

[0071] Air atmosphere was introduced to carry out pyrolysis reaction of the precursor, the heating rate of the pyrolysis reaction was 5°C / min, the temperature of the pyrolysis reaction was 800°C, and the pyrolysis reaction time was 6h, thereby obtaining zinc cobaltate nano-thin cage material.

[0072] 0.5 g of the prepared zinc cobalt oxide nano-thin cage material and 1.5 g of sublimated sulfur powder were mixed and heat treated at 155° C. for 6 h to obtain a lithium-sulfur battery positive electrode material.

[0073] The lithium-sulfur battery positive electrode material, the conductive agent Sup P and the binder LA123 were mixed in a mass ratio of 7:2:1 to obtain a slurry.

[0074] Use a coating machine to coat at 1.5 mg / cm 2 The slurry was coated on aluminum foil with a sulfur areal loading of , and after drying, a lithium-sulfur battery positive electrode with a diameter of 14 mm was obtained.

[0075] The lithium-sulfur battery positive electrode, lithium-sulfur battery negative electrode (metal lithium sheet with a diameter of 14.5 mm), separator and electrolyte (1 mol / L LITFSI + 1% LiNO3 dissolved in DOL + DME with a volume ratio of 1:1) were assembled into a 2025-type button-type lithium-sulfur battery in an argon-filled glove box.

[0076] The prepared lithium-sulfur battery was left to stand for 6 hours before testing.

[0077] Example 2

[0078] The difference between this embodiment and embodiment 1 is that the sulfur loading of the prepared lithium-sulfur battery positive electrode is 6 mg / cm 2 .

[0079] Example 3

[0080] The difference between this embodiment and embodiment 1 is that the sulfur loading of the prepared lithium-sulfur battery positive electrode is 10 mg / cm 2 .

[0081] Example 4

[0082] 0.549 g of zinc nitrate, 0.725 g of cobalt nitrate and 150 mL of ethylene glycol were mixed to obtain a mixed solution, and sodium hydroxide was added to the mixed solution to adjust the pH value to 14 to obtain a raw material solution.

[0083] The raw material solution was heated to 180° C., condensed and refluxed for 4 h, and then cooled to room temperature. The solid product was separated by centrifugation, washed with ethanol and deionized water, and vacuum dried at 80° C. overnight to obtain a precursor.

[0084] Air atmosphere was introduced to carry out pyrolysis reaction of the precursor, the heating rate of the pyrolysis reaction was 5°C / min, the temperature of the pyrolysis reaction was 700°C, and the pyrolysis reaction time was 6h, thereby obtaining zinc cobaltate nano-thin cage material.

[0085] 0.5 g of the prepared zinc cobalt oxide nano-thin cage material and 1.5 g of sublimated sulfur powder were mixed and heated at 155° C. for 6 h to obtain a lithium-sulfur battery positive electrode material.

[0086] The lithium-sulfur battery positive electrode material, the conductive agent Sup P and the binder LA123 were mixed in a mass ratio of 7:2:1 to obtain a slurry.

[0087] Use a coating machine to coat at 8mg / cm 2 The slurry was coated on aluminum foil with a sulfur areal loading of , and after drying, a lithium-sulfur battery positive electrode with a diameter of 14 mm was obtained.

[0088] The lithium-sulfur battery positive electrode, lithium-sulfur battery negative electrode (metal lithium sheet with a diameter of 14.5 mm), separator and electrolyte (1 mol / L LITFSI + 1% LiNO3 dissolved in DOL + DME with a volume ratio of 1:1) were assembled into a 2025-type button-type lithium-sulfur battery in an argon-filled glove box.

[0089] The prepared lithium-sulfur battery was left to stand for 6 hours before testing.

[0090] Example 5

[0091] 0.514 g of zinc acetylacetonate, 0.706 g of cobalt acetylacetonate and 100 mL of glycerol were mixed to obtain a mixed solution, and potassium hydroxide was added to the mixed solution to adjust the pH value to 14 to obtain a raw material solution.

[0092] The raw material solution was heated to 190° C., condensed and refluxed for 3 h, and then cooled to room temperature. The solid product was separated by centrifugation, washed with ethanol and deionized water, and vacuum dried at 80° C. overnight to obtain a precursor.

[0093] Air atmosphere was introduced to carry out pyrolysis reaction of the precursor, the heating rate of the pyrolysis reaction was 5°C / min, the temperature of the pyrolysis reaction was 700°C, and the pyrolysis reaction time was 6h, thereby obtaining zinc cobaltate nano-thin cage material.

[0094] 0.5 g of the prepared zinc cobalt oxide nano-thin cage material and 1.5 g of sublimated sulfur powder were mixed and heated at 155° C. for 6 h to obtain a lithium-sulfur battery positive electrode material.

[0095] The lithium-sulfur battery positive electrode material, the conductive agent Sup P and the binder LA123 were mixed in a mass ratio of 7:2:1 to obtain a slurry.

[0096] Use a coating machine to coat at 8mg / cm 2 The slurry was coated on aluminum foil with a sulfur areal loading of , and after drying, a lithium-sulfur battery positive electrode with a diameter of 14 mm was obtained.

[0097] The lithium-sulfur battery positive electrode, lithium-sulfur battery negative electrode (metal lithium sheet with a diameter of 14.5 mm), separator and electrolyte (1 mol / L LITFSI + 1% LiNO3 dissolved in DOL + DME with a volume ratio of 1:1) were assembled into a 2025-type button-type lithium-sulfur battery in an argon-filled glove box.

[0098] The prepared lithium-sulfur battery was left to stand for 6 hours before testing.

[0099] Comparative Example 1

[0100] Sup PS, a conductive agent, and a binder LA123 were mixed in a mass ratio of 7:2:1 to obtain a slurry.

[0101] Use a coating machine to coat at 6mg / cm 2 The slurry was coated on aluminum foil with a sulfur areal loading of 14 mm to produce a lithium-sulfur battery positive electrode with a diameter of 14 mm.

[0102] The lithium-sulfur battery positive electrode, lithium-sulfur battery negative electrode (metal lithium sheet with a diameter of 14.5 mm), separator and electrolyte (1 mol / L LITFSI + 1% LiNO3 dissolved in DOL + DME with a volume ratio of 1:1) were assembled into a 2025-type button-type lithium-sulfur battery in an argon-filled glove box.

[0103] The prepared lithium-sulfur battery was left to stand for 6 hours before testing.

[0104] Performance Test:

[0105] Morphological characterization of zinc cobalt oxide nano-thin cage materials:

[0106] The zinc cobalt oxide nano-thin cage material prepared in Example 1 was scanned by electron microscope, and the results were as follows: Figure 1 As shown;

[0107] The zinc cobalt oxide nano-thin cage material prepared in Example 1 was subjected to energy spectrum line scanning analysis to obtain electron microscope level EDS line scanning data. The results are as follows: Figure 2 As shown;

[0108] The zinc cobalt oxide nano-thin cage material prepared in Example 1 was subjected to X-ray diffraction to obtain a diffraction pattern. The results are as follows: Figure 3 As shown;

[0109] Specific capacity and cycle stability of lithium-sulfur batteries:

[0110] The lithium-sulfur battery prepared in Example 1 was subjected to a battery cycle test at a current density of 2C. The results are as follows: Figure 4 As shown;

[0111] The lithium-sulfur batteries prepared in Example 2 and Comparative Example 1 were subjected to battery cycle tests at a current density of 1C. The results are as follows: Figure 5 As shown;

[0112] The lithium-sulfur battery prepared in Example 3 was subjected to a battery cycle test at a current density of 0.1C. The results are as follows: Figure 6 shown.

[0113] The battery cycle test of Example 4 and Example 5 was performed, and the results are shown in Table 1.

[0114] Table 1 Specific capacity of lithium-sulfur batteries obtained in Example 4 and Example 5 after attenuation

[0115]

[0116] from Figure 1 and Figure 2 It can be seen from a that the zinc cobaltate nano-thin cage material prepared in Example 1 has a thick sheet structure with a size of 1 micron and a thickness of about 300 nanometers.

[0117] Figure 2 b and Figure 2 c is the EDS scanning data of cobalt and zinc elements in the zinc cobaltate nano-thin cage material prepared in Example 1, indicating that the zinc and cobalt content on both sides of the zinc cobaltate nano-thin cage material is higher than that in the middle, indicating that there is a hollow structure in the middle of the zinc cobaltate nano-thin cage material prepared in Example 1.

[0118] Figure 3 This is the X-ray diffraction pattern of the zinc cobaltate nano-thin cage material prepared in Example 1. The diffraction peak is consistent with the X-ray diffraction pattern of zinc cobaltate.

[0119] from Figure 4 It can be seen that the initial specific capacity of the lithium-sulfur battery prepared in Example 1 is greater than 800 mAh / g, and the capacity remains at a high level of 700 mAh / g after 1000 cycles at a high current density of 2C, and the capacity decay rate is only 0.016% per cycle. This shows that the lithium-sulfur battery positive electrode material prepared in the present invention has high battery cycle stability.

[0120] It can be seen from Table 1 that Example 4 and Example 5 can still achieve a high specific capacity of 600 mAh / g after 500 cycles at a high current density of 1 C, indicating that the lithium-sulfur battery positive electrode material prepared in the present invention has high battery cycle stability.

[0121] from Figure 5 It can be seen that the initial specific capacity and the specific capacity after 50 cycles of the lithium-sulfur battery prepared in Example 2 are much greater than the initial specific capacity and the specific capacity after 50 cycles of the lithium-sulfur battery prepared in Comparative Example 1, indicating that the lithium-sulfur battery positive electrode material prepared in the present invention has a higher specific capacity than the traditional Sup PS material at the same sulfur loading.

[0122] from Figure 6 It can be seen that the lithium-sulfur battery prepared in Example 3 has a high sulfur loading of 10 mg / cm 2 Under this condition, the lithium-sulfur battery can still release a specific capacity of more than 1000mAh / g after 50 cycles, which is equivalent to a 10mAh / cm 2 The high area capacity density and the coulombic efficiency are maintained at about 100%. This shows that the lithium-sulfur battery prepared by the present invention can maintain a high specific capacity and cycle stability when having a high sulfur loading.

[0123] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0124] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A method for preparing a positive electrode material for a lithium-sulfur battery, characterized in that: The steps include: uniformly mixing a trivalent cobalt metal compound, a divalent zinc metal compound and an organic solvent to obtain a mixed solution; Adjusting the pH value of the mixed solution to 13-14 to obtain a raw material solution; The raw material solution is subjected to reflux heating treatment, and after sufficient reaction, solid-liquid separation is performed and solid is retained to obtain a precursor; The precursor is subjected to a pyrolysis reaction to obtain a zinc cobaltate nano-thin cage material; The zinc cobalt oxide nano-thin cage material is mixed evenly with elemental sulfur, and then subjected to heat treatment to obtain a lithium-sulfur battery positive electrode material after sufficient reaction; The mass ratio of the trivalent cobalt metal compound, the divalent zinc metal compound and the organic solvent is (3-8):(3-8):(500-2000).

2. The method for preparing a positive electrode material for a lithium-sulfur battery according to claim 1, characterized in that: The mass ratio of the zinc cobaltate nano-thin cage material to the elemental sulfur is (10-40):(60-90).

3. The method for preparing a positive electrode material for a lithium-sulfur battery according to claim 1, characterized in that: The temperature of the reflux heating treatment is 120°C-200°C.

4. The method for preparing a positive electrode material for a lithium-sulfur battery according to claim 1, characterized in that: The temperature of the pyrolysis reaction is 500° C.-950° C., the heating rate of the pyrolysis reaction is 1° C. / min-5° C. / min, and the time of the pyrolysis reaction is 2h-12h.

5. The method for preparing a positive electrode material for a lithium-sulfur battery according to claim 1, characterized in that: In the operation of uniformly mixing the zinc cobaltate nano-thin cage material and elemental sulfur and then performing heat treatment, the heat treatment temperature is 140° C.-180° C., and the heat treatment time is 4 h-6 h.

6. The method for preparing a positive electrode material for a lithium-sulfur battery according to claim 1, characterized in that: The trivalent cobalt metal compound is selected from at least one of cobalt acetylacetonate, cobalt acetate, cobalt nitrate and cobalt carbonate; and / or The divalent zinc metal compound is selected from at least one of zinc acetylacetonate, zinc acetate, zinc nitrate and zinc carbonate; and / or The organic solvent is selected from at least one of ethanol, acetone, ethylene glycol and glycerol; and / or The pH value of the mixed solution is adjusted by using an alkaline solution, wherein the alkaline solution is selected from at least one of aqueous ammonia, sodium hydroxide solution and potassium hydroxide solution; and / or The pyrolysis reaction is carried out in an air atmosphere or an oxygen atmosphere.

7. A positive electrode material for a lithium-sulfur battery, characterized in that: The positive electrode material for a lithium-sulfur battery is prepared by the method for preparing the positive electrode material for a lithium-sulfur battery according to any one of claims 1 to 6.

8. A lithium-sulfur battery positive electrode, characterized in that: The material for preparing the lithium-sulfur battery positive electrode includes the lithium-sulfur battery positive electrode material according to claim 7.

9. A lithium-sulfur battery, characterized in that: The lithium-sulfur battery comprises the lithium-sulfur battery positive electrode according to claim 8.