Dinuclear cyclopentadienyl group IV metal catalyst for polymerization of styrene and its derivatives, preparation method, composition and application thereof
By developing dinuclear Group IV metal catalysts and using semi-sandwich Group IV metal trialkyl compounds bridged by single atoms or ethylene groups, the problem of insufficient application of Group IV metal catalysts in the existing technology has been solved, and a wide temperature range has been achieved. It can efficiently catalyze the polymerization of styrene to prepare ultra-high molecular weight syndiotactic polystyrene, which is suitable for industrial production.
Patent Information
- Application Number
- CN202210628814.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-06-06
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2042-06-06
AI Technical Summary
There is a lack of Group IV metal catalysts suitable for industrial applications in the existing technology, which are used to catalyze the syndiotactic stereoselective polymerization of styrene and its derivatives, and the metal cost of dinuclear cenyl rare earth catalysts is high, which limits its industrial promotion.
A dinuclear Group IV metal catalyst using single-atom or ethylene-bridged semi-sandwich Group IV metal trialkyl compounds was developed to catalyze the polymerization of styrene and its derivatives to prepare ultra-high molecular weight syndiotactic compounds. Stereopolystyrene. This catalyst optimizes the structure of the catalyst through a specific combination of ligands and bridging groups to achieve a bimetallic synergistic effect.
The catalytic effect is significantly improved in a wide temperature range, and ultra-high molecular weight syndiotactic polystyrene is produced. The preparation method is mild and efficient, and is suitable for industrial production.
Smart Images

Figure CN114874258B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of metallocene catalysts, and in particular relates to a binuclear metallocene group IV metal catalyst for polymerization of styrene and its derivatives, a preparation method, a composition and an application thereof. Background Art
[0002] According to the different stereoregular structures, polystyrene can be divided into three types: atactic polystyrene, isotactic polystyrene and syndiotactic polystyrene (sPS). Among them, syndiotactic polystyrene is used as engineering plastics due to its high melting point (Tm = 270°C), high crystallization rate, high elastic modulus, and excellent heat resistance and chemical resistance. Syndiotactic polystyrene was first prepared by Ishihara of Idemitsu Chemical in Japan, using a transition metal titanium catalyst system Cp'TiX3 / MAO (Cp' = cyclopentadiene and its derivatives, X = alkyl or halogen, MAO = methylaluminoxane) to catalyze the syndiotactic stereoselective polymerization of styrene (Macromolecules 1986, 19, 2464). Chien and Rausch et al. used IndTiCl3 as a catalyst to catalyze the syndiotactic polymerization of styrene. Compared with CpTiCl3, IndTiCl3 has higher polymerization activity and a higher proportion of sPS in the polymer (Macromolecules 1993, 26, 5822). In addition, they used Cp′Ti(OiPr)3 to catalyze the syndiotactic polymerization of styrene and found that the catalyst structure had an important influence on the polymerization activity, sPS content and sPS molecular weight (Organometallics 1993, 12, 3075).
[0003] In order to study the influence of binuclear synergistic effect on the selective polymerization behavior of styrene syndiotactic stereoselective polymerization. Some monotantalum catalysts connected with rigid skeletons or long-chain bridging groups have been synthesized (Organometallics 2005, 24, 3618; J.Organomet.Chem.2006, 691, 5000). However, the distance between the two metal centers of these binuclear cyclopentadienyl group-four metal complexes is too far, or due to the limitation of the rigid skeleton, the two active centers cannot coordinate the distance between each other according to the polymerization process to achieve the best synergistic effect. The patent application with publication number CN113307896 reports that the binuclear cyclopentadienyl rare earth catalyst system can catalyze the selective polymerization of styrene syndiotactic stereoselective under the action of a cocatalyst to prepare high molecular weight syndiotactic polystyrene. However, the metal of the binuclear cyclopentadienyl catalyst is a rare earth metal element, and its price is much higher than that of the group-four metal elements, which greatly limits its industrial promotion and application. Therefore, it is very necessary to explore a new catalyst system suitable for industrial application.
[0004] So far, there is no conclusive literature reporting on single-atom or ethylene-bridged cyclopentadienyl Group IV metal alkyl compounds (the dinuclear cyclopentadienyl Group IV metal alkyl compounds referred to herein refer to semi-sandwich Group IV metal trialkyl (amine) compounds bridged by single-atom or ethylene groups) and their application in the syndiotactic stereoselective polymerization of styrene monomers. Summary of the invention
[0005] In view of this, the present invention aims to solve the technical problems in the prior art and provide a dinuclear cyclopentadienyl Group IV metal catalyst for the polymerization of styrene and its derivatives, and its preparation method, composition and application. The catalyst is a dinuclear cyclopentadienyl Group IV metal complex bridged by a single atom group or ethylene, which can be used to catalyze the polymerization of styrene and its derivative monomers to prepare ultra-high molecular weight syndiotactic polystyrene and its derivatives.
[0006] In order to solve the above technical problems, the technical solutions of the present invention are as follows:
[0007] The present invention provides a binuclear cyclopentadienyl group IV metal catalyst for polymerization of styrene and its derivatives, having a structure shown in formula I:
[0008]
[0009] Among them, Cp 1 and Cp 2 independently selected from a substituted or unsubstituted cyclopentadienyl group, a substituted or unsubstituted indene group, or a substituted or unsubstituted fluorene group;
[0010] U is a single atom bridging group or ethylene;
[0011] X 1 , X 2 and X 3 independently selected from an alkyl group having 1 to 16 carbon atoms, a silyl group having 4 to 16 carbon atoms, an amine group having 2 to 16 carbon atoms, a silylamine group having 4 to 20 carbon atoms, an arylamine group having 6 to 20 carbon atoms, or a benzyl group having 7 to 20 carbon atoms;
[0012] M is selected from titanium, zirconium or hafnium.
[0013] In the above technical solution, the Cp 1 and Cp 2The fluorenyl, 2,7-di-tert-butylfluorenyl, benzofluorenyl, bisbenzofluorenyl, cycloalkane-substituted fluorenyl, indenyl, 4,7-dimethylindenyl, 2-methylindenyl, cyclopentadienyl, tetramethylcyclopentadienyl, 1-tert-butyl-2-trimethylsilylcyclopentadienyl, 1,3-bis(trimethylsilyl)cyclopentadienyl, methylcyclopentadienyl, tert-butylcyclopentadienyl, trimethylsilyl cyclopentadienyl, 1,2-dimethylcyclopentadienyl, 1,3-dimethylcyclopentadienyl, 1,2-diethylcyclopentadienyl, ethylcyclopentadienyl, n-butylcyclopentadienyl, n-octylcyclopentadienyl, tetrahydroindenyl, propylcyclopentadienyl, octahydrofluorenyl, phenylcyclopentadienyl, 1,2-diphenylcyclopentadienyl, cyclohexylcyclopentadienyl or 2,2′-biphenylcyclopentadienyl.
[0014] In the above technical solution, the single atom bridging group is preferably CH2CH2 2- 、CH2 2- 、CMe2 2- 、SiMe2 2- 、SiHMe 2- 、SiH2 2- 、SiPhMe 2- 、PMe 2- , BMe 2- or SnMe2 2- .
[0015] In the above technical solution, the binuclear cyclopentadienyl group IV metal catalyst is preferably selected from one of the following structures:
[0016]
[0017]
[0018] The present invention also provides a method for preparing a binuclear cyclopentadienyl group IV metal catalyst for polymerization of styrene and its derivatives, comprising the following steps:
[0019] Step 1: Under anhydrous and oxygen-free conditions, 1 -U-Cp 2 The ligand is dissolved in an organic solvent to obtain a ligand solution;
[0020] Step 2, reacting the ligand solution with twice the molar amount of an alkali metal reagent to obtain an alkali metal salt of the ligand;
[0021] Step 3: The alkali metal salt of the ligand and twice the molar amount of (A)M(X 1 X 2 X 3 ) to obtain a binuclear cyclopentadienyl Group IV metal catalyst having a structure shown in Formula I;
[0022] The (A)M(X 1 X 2 X 3 ) wherein A is selected from halogen, BH4 – 、[(C6H5)4B] – or [(C6F5)4B] – , M, X 1 , X 2 and X 3 , and the Cp 1 -U-Cp 2 Cp 1 , Cp 2 and U are consistent with the above definitions and will not be repeated here.
[0023] The present invention also provides a binuclear cyclopentadienyl Group IV metal catalyst composition for catalyzing the polymerization of styrene and its derivatives, comprising the binuclear cyclopentadienyl Group IV metal catalyst, an organic boron salt and a main group metal alkyl reagent described in the present invention; the molar ratio of the binuclear cyclopentadienyl Group IV metal catalyst, the organic boron salt and the main group metal alkyl reagent is 1:(0-4):(0-4000).
[0024] In the above technical solution, the organic boron salt is preferably selected from [B(C6F5)4] – Negative ion organic boron salt, containing [1,4-(C6F5)3BC6F4B(C6F5)3] 2– One or more of anion organic boron salts, B(C6F5)3 and 1,4-(C6F5)2BC6F4B(C6F5)2; the main group metal alkyl reagent is selected from one or more of aluminoxane, alkyl aluminum, alkyl zinc and alkyl magnesium reagents.
[0025] The present invention also provides a method for catalyzing the polymerization of styrene and its derivatives, comprising the following steps:
[0026] Under anhydrous and oxygen-free conditions, styrene monomers or styrene derivative monomers are subjected to homopolymerization or copolymerization reaction under the catalysis of the binuclear cyclopentadienyl group IV metal catalyst composition of the present invention.
[0027] In the above technical solution, the styrene monomer is preferably one or more of styrene, p-methylstyrene and p-tert-butylstyrene; the styrene derivative monomer is preferably a styrene derivative containing a long-chain alkane of 2 to 25 carbon atoms at the para position of styrene.
[0028] In the above technical solution, preferably, the temperature of the homopolymerization or copolymerization reaction is 0 to 180° C., and the time is 1 min to 100 h.
[0029] The beneficial effects of the present invention are:
[0030] The present invention provides a dinuclear cyclopentadienyl Group IV metal catalyst for the polymerization of styrene and its derivatives, which has a structure of Formula I. Compared with the corresponding mononuclear cyclopentadienyl Group IV metal catalyst or the cyclopentadienyl dinuclear rare earth catalyst bridged by long chain groups and rigid groups, the dinuclear cyclopentadienyl Group IV metal catalyst of the present invention exhibits a significant bimetallic synergistic effect in the process of catalyzing olefin polymerization, and can produce ultra-high molecular weight syndiotactic polystyrene under a very wide temperature range.
[0031] The invention provides a method for preparing a binuclear cyclopentadienyl group IV metal catalyst for polymerization of styrene and its derivatives. The method has mild reaction conditions and high efficiency and is suitable for industrial production.
[0032] The invention provides a binuclear cyclopentadienyl group IV metal catalyst composition catalytic system, which can be used for catalyzing olefin polymerization to obtain ultra-high molecular weight syndiotactic polystyrene. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] The present invention is further described in detail below in conjunction with the accompanying drawings and specific embodiments.
[0034] Figure 1 is the DSC curve of the polystyrene sample obtained in Polymerization Example 7;
[0035] Figure 2 Carbon NMR spectrum of the polystyrene sample obtained in Polymerization Example 7;
[0036] Figure 3 H NMR spectrum of the poly(p-methylstyrene) sample obtained in Polymerization Example 8. DETAILED DESCRIPTION
[0037] The present invention provides a binuclear cyclopentadienyl group IV metal catalyst for polymerization of styrene and its derivatives, having a structure of formula I:
[0038]
[0039] The Cp 1 and Cp 2 independently selected from a substituted or unsubstituted cyclopentadienyl group, a substituted or unsubstituted indene group, or a substituted or unsubstituted fluorene group;
[0040] The U is a single atom bridging group or an ethylene group;
[0041] The X 1 , X 2 and X 3independently selected from an alkyl group having 1 to 16 carbon atoms, a silyl group having 4 to 16 carbon atoms, an amine group having 2 to 16 carbon atoms, a silylamine group having 4 to 20 carbon atoms, an arylamine group having 6 to 20 carbon atoms, or a benzyl group having 7 to 20 carbon atoms;
[0042] The M is selected from titanium, zirconium or hafnium.
[0043] In the present invention, the Cp 1 and Cp 2 The fluorenyl, 2,7-di-tert-butylfluorenyl, benzofluorenyl, bisbenzofluorenyl, cycloalkane-substituted fluorenyl, indenyl, 4,7-dimethylindenyl, 2-methylindenyl, cyclopentadienyl, tetramethylcyclopentadienyl, 1-tert-butyl-2-trimethylsilylcyclopentadienyl, 1,3-bis(trimethylsilyl)cyclopentadienyl, methylcyclopentadienyl, tert-butylcyclopentadienyl, trimethylsilyl cyclopentadienyl, 1,2-dimethylcyclopentadienyl, 1,3-dimethylcyclopentadienyl, 1,2-diethylcyclopentadienyl, ethylcyclopentadienyl, n-butylcyclopentadienyl, n-octylcyclopentadienyl, tetrahydroindenyl, propylcyclopentadienyl, octahydrofluorenyl, phenylcyclopentadienyl, 1,2-diphenylcyclopentadienyl, cyclohexylcyclopentadienyl or 2,2′-biphenylcyclopentadienyl.
[0044] In the present invention, the X 1 , X 2 and X 3 All of them are single anion initiating groups; the X 1 , X 2 and X 3 Each is independently preferably selected from CH2SiMe3, CH3, CH2C6H5, CH2C6H4CH3, NMe2 or NEt2.
[0045] In the present invention, the bridging group U is preferably selected from CH2CH2 2- 、CH2 2- 、CMe2 2- 、SiMe2 2- 、SiHMe 2- 、SiH2 2- 、SiPhMe 2- 、PMe 2- , BMe 2- and SnMe2 2- One of them.
[0046] In the present invention, the M is preferably titanium.
[0047] In the present invention, the cyclopentadienyl ligand in the binuclear cyclopentadienyl Group IV metal catalyst is preferably selected from the following ligands:
[0048] In the present invention, the binuclear cyclopentadienyl group IV metal catalyst is preferably selected from one of the following structures:
[0049]
[0050]
[0051] The present invention also provides a method for preparing a binuclear cyclopentadienyl group IV metal catalyst for polymerization of styrene and its derivatives, comprising the following steps:
[0052] Step 1: Under anhydrous and oxygen-free conditions, 1 -U-Cp 2 The ligand is dissolved in an organic solvent to obtain a ligand solution;
[0053] Step 2, reacting the ligand solution with twice the molar amount of an alkali metal reagent to obtain an alkali metal salt of the ligand;
[0054] Step 3: The alkali metal salt of the ligand and twice the molar amount of (A)M(X 1 X 2 X 3 ) to obtain a binuclear cyclopentadienyl Group IV metal catalyst having a structure shown in Formula I;
[0055] The (A)M(X 1 X 2 X 3 ) wherein A is selected from halogen, BH4 – 、[(C6H5)4B] – or [(C6F5)4B] – etc., M, X 1 , X 2 and X 3 , and the Cp 1 -U-Cp 2 Cp 1 , Cp 2 and U are consistent with the above definitions and will not be repeated here.
[0056] The present invention also provides a binuclear cyclopentadienyl Group IV metal catalyst composition for catalyzing the polymerization of styrene and its derivatives, comprising a binuclear cyclopentadienyl Group IV metal catalyst as shown in Formula I of the present invention, an organic boron salt and a main group metal alkyl reagent; the molar ratio of the binuclear cyclopentadienyl Group IV metal catalyst, the organic boron salt and the main group metal alkyl reagent is 1:(0-4):(0-4000).
[0057] In the present invention, the organic boron salt is selected from [B(C6F5)4] –Negative ion organic boron salt, containing [1,4-(C6F5)3BC6F4B(C6F5)3] 2– One or more of anion organic boron salts, B(C6F5)3 and 1,4-(C6F5)2BC6F4B(C6F5)2;
[0058] The main group metal alkyl reagent is preferably selected from one or more of aluminoxane, alkylaluminum, alkylzinc and alkylmagnesium reagents. The alkylaluminum is further preferably selected from one or more of trimethylaluminum, triethylaluminum, tri-n-butylaluminum, tri-n-propylaluminum, triisobutylaluminum, triisopropylaluminum, tripentylaluminum, trihexylaluminum, trioctylaluminum, diethylaluminum hydride and diisobutylaluminum hydride; the aluminoxane is further preferably selected from one or more of methylaluminoxane (MAO), dried aluminoxane (DMAO) and modified aluminoxane (MMAO). The alkylzinc is further preferably diethylzinc; the alkylmagnesium is further preferably selected from one or more of diethylmagnesium, di-n-propylmagnesium, diisopropylmagnesium and dibutylmagnesium.
[0059] The present invention also provides a method for catalyzing the polymerization of styrene and its derivatives, comprising the following steps:
[0060] Under anhydrous and oxygen-free conditions, styrene monomers or styrene derivative monomers are subjected to homopolymerization or copolymerization reaction under the catalysis of the binuclear cyclopentadienyl group IV metal catalyst composition of the present invention.
[0061] In the present invention, the molar ratio of the styrene monomer or styrene derivative monomer to the binuclear cyclopentadienyl group-four metal catalyst of formula I in the binuclear cyclopentadienyl group-four metal catalyst composition is preferably (50-1000000):1, further preferably (1000-500000):1, and more preferably (5000-100000):1.
[0062] In the present invention, the temperature of the homopolymerization or copolymerization reaction is preferably 0-180°C, more preferably 20-160°C, further preferably 40-120°C, most preferably 50-100°C; most preferably 60-80°C; the time is preferably 1 min to 100 h, more preferably 10 min to 24 h, most preferably 30 min to 12 h, and most preferably 60 min to 4 h.
[0063] In the present invention, the styrene monomer is one or more of styrene, p-methylstyrene and p-tert-butylstyrene, and the styrene derivative monomer is a styrene derivative containing a long-chain alkane with 2 to 25 carbon atoms in the para position of styrene. The polymerization of the styrene monomer can be the homopolymerization of each of the above monomers, or the copolymerization of two or more of the above monomers.
[0064] The above polymerization can be carried out in bulk or in an organic solvent; the organic solvent used for the polymerization of the styrene monomer or styrene derivative monomer of the present invention is not particularly limited, and is preferably selected from one or a mixture of saturated alkanes, aromatic hydrocarbons, halogenated aromatic hydrocarbons and cycloalkanes. Preferably, it is one or a mixture of n-hexane, decahydronaphthalene, cyclohexane, petroleum ether, benzene, toluene and xylene.
[0065] The present invention provides a dinuclear cyclopentadienyl Group IV metal catalyst for the polymerization of styrene monomers, which has a structure of Formula I. Compared with the corresponding mononuclear cyclopentadienyl Group IV metal catalyst or the cyclopentadienyl dinuclear rare earth catalyst bridged by a long chain group or a rigid group, the dinuclear cyclopentadienyl Group IV metal catalyst of the present invention exhibits a significant bimetallic synergistic effect in the process of catalyzing olefin polymerization, and can produce ultra-high molecular weight syndiotactic polystyrene under a very wide temperature range.
[0066] In order to further illustrate the present invention, the binuclear cyclopentadienyl Group IV metal catalyst provided by the present invention, its preparation method, composition and application are described in detail below in conjunction with the examples, but they should not be construed as limiting the scope of protection of the present invention.
[0067] Preparation Example 1 of Complex 1
[0068] Under anhydrous and oxygen-free conditions, slowly drip 10 mmol of butyl lithium n-hexane solution into a Schlenk bottle containing 5 mmol of ligand 1 in tetrahydrofuran (10 mL) at -30°C. In addition, slowly drip 10 mmol of [Et3NH][BPh4] in tetrahydrofuran (5 mL) into another Schlenk bottle containing 10 mmol of Ti(CH2Ph)4 in tetrahydrofuran (8 mL) at room temperature, and react at room temperature for 2 hours. Then pour the lithium salt solution of ligand 1 into the alkyl titanium reaction system Ti(CH2Ph)3(BPh4), and stir the reaction at room temperature for 40 minutes. Remove all solvents under vacuum, extract with 20 mL of toluene, filter, and collect the filtrate. After concentrating the filtrate, add an appropriate amount of n-hexane, and place it in a -30°C refrigerator to stand for crystallization. The yield of complex 1 is 53%. 1 H NMR (400MHz, C6D6): δ7.04 (12H, C6H5), 6.91 (4H, C5H4), 6.78 (4H, C5H4), 6.62-6.59 (18H, C6H5), 3.14 (12H, CH2), 0.55 (6H, SiMe2).
[0069]
[0070] Complex 2 Preparation Example 2
[0071] Under anhydrous and oxygen-free conditions, 10 mmol of butyl lithium n-hexane solution was slowly dripped into a Schlenk bottle containing 5 mmol of ligand 2 in toluene (10 mL) at -30°C, and reacted at this temperature for 2 hours. Then, it was added to a reaction bottle containing 10 mmol of Ti(CH2Ph)3Cl in toluene solution, and reacted at room temperature for 1 hour, and then the solid product was filtered out, and the filtered filtrate was vacuum concentrated, and an appropriate amount of n-hexane was added. Complex 2 was precipitated in a mixed solution of toluene and n-hexane at -30°C, and the yield was 58%. 1 H NMR (400 MHz, C6D6): δ7.03 (12H, C6H5), 6.86 (4H, C5H4), 6.73 (4H, C5H4), 6.61-6.57 (18 H, C6H5), 3.14 (12H, CH2Ph), 4.31 (2H, CH2Cp2).
[0072]
[0073] Preparation Example 3 of Complex 3
[0074] According to the method of Example 1 for preparing complex 1, the lithium salt of ligand 3 was reacted with 2 times the amount of the corresponding titanium ion pair reagent Ti(CH2SiMe3)3(BPh4) to obtain complex 3 with a yield of 61%.
[0075]
[0076] Complex 4 Preparation Example 4
[0077] According to the method of Example 1 for preparing complex 1, the lithium salt of ligand 4 was reacted with 2 times the amount of the corresponding titanium ion pair reagent Ti(CH2SiMe3)3(BPh4) to obtain complex 4 with a yield of 51%.
[0078]
[0079] Complex 5 Preparation Example 5
[0080] According to the method of Example 2 for preparing complex 2, the lithium salt of ligand 5 was reacted with the corresponding titanium compound Ti(CH2Ph)3Cl to obtain complex 5 with a yield of 64%.
[0081]
[0082] Complex 6 Preparation Example 6
[0083] According to the method of Example 2 for preparing complex 2, the lithium salt of ligand 6 was reacted with the corresponding titanium compound Ti(CH3)3Cl to obtain complex 6 with a yield of 59%.
[0084]
[0085] Complex 7 Preparation Example 7
[0086] According to the method of Example 2 for preparing complex 2, the lithium salt of ligand 7 was reacted with the corresponding titanium ion pair reagent Ti(CH2C6H4Me)3(BPh4) to obtain complex 7 with a yield of 62%.
[0087]
[0088] Preparation Example 8 of Complex 8
[0089] According to the method of Example 2 for preparing complex 2, the lithium salt of ligand 8 was reacted with the corresponding titanium compound Ti(CH2C6H4Me)3Cl to obtain complex 8 with a yield of 71%.
[0090]
[0091] Complex 9 Preparation Example 9
[0092] According to the method of Example 2 for preparing complex 2, the lithium salt of ligand 9 was reacted with the corresponding titanium compound Ti(CH2Ph)3Cl to obtain complex 9 with a yield of 59%.
[0093]
[0094] Preparation Example 10 of Complex 10
[0095] According to the method of Example 1 for preparing complex 1, the lithium salt of ligand 10 was reacted with the corresponding titanium ion pair Ti(CH2Ph)3(BPh4) to obtain complex 10 with a yield of 63%.
[0096]
[0097] Preparation Example 11 of Complex 11
[0098] According to the method of Example 1 for preparing complex 1, the lithium salt of ligand 7 was reacted with zirconium ion pair Zr(CH2C6H4Me)3(BPh4) to obtain complex 11 with a yield of 62%;
[0099]
[0100] Complex 12 Preparation Example 12
[0101] According to the method of Example 1 for preparing complex 1, the lithium salt of ligand 7 was reacted with the hafnium ion pair Hf(CH2Ph)3(BPh4) to obtain complex 12 with a yield of 54%;
[0102]
[0103] Complex 13 Preparation Example 13
[0104] According to the method of Example 2 for preparing complex 2, the lithium salt of ligand 11 is reacted with the titanium compound Ti(CH2Ph)3Cl to obtain complex 13 with a yield of 51%.
[0105]
[0106] Complex 14 Preparation Example 14
[0107] According to the method of Example 2 for preparing complex 2, the lithium salt of ligand 12 is reacted with the titanium compound Ti(CH2Ph)3Cl to obtain complex 14 with a yield of 60%.
[0108]
[0109] Preparation Example 15 of Complex 15
[0110] According to the method of Example 2 for preparing complex 2, the lithium salt of ligand 13 is reacted with the titanium compound Ti(CH2Ph)3Cl to obtain complex 15 with a yield of 47%.
[0111]
[0112] Complex 16 Preparation Example 16
[0113] According to the method of Example 2 for preparing complex 2, the lithium salt of ligand 14 is reacted with the titanium compound Ti(CH2Ph)3Cl to obtain complex 16 with a yield of 51%.
[0114]
[0115] Complex 17 Preparation Example 17
[0116] According to the method of Example 2 for preparing complex 2, the lithium salt of ligand 17 is reacted with the titanium compound Ti(CH2Ph)3Cl to obtain complex 17 with a yield of 68%.
[0117]
[0118] Comparative Complex 1 Preparation Example 1
[0119] Under anhydrous and oxygen-free conditions, 10 mmol of butyl lithium n-hexane solution was slowly dripped into a Schlenk bottle containing 5 mmol of ligand 1 in ether (10 mL) at -30°C. After reacting at -30°C for 1 hour, the ether solution was added to a Schlenk bottle containing 10 mmol of TiCl4 ether (8 mL) solution. After reacting at room temperature for 2 hours, 30 mmol of KCH2Ph was added to the above reaction bottle. After reacting at room temperature for 4 hours, all solvents were removed by vacuum decompression, extracted with 20 mL of toluene, filtered, and the filtrate was collected. After concentrating the filtrate, an appropriate amount of n-hexane was added, and the filtrate was placed in a -30°C refrigerator to obtain a small amount of solid matter. The H NMR spectrum analysis showed that it was a mixture that was difficult to distinguish. The reaction failed and the target complex 1 was not obtained.
[0120]
[0121] Polymerization Example 1: Complex 1 catalyzes styrene homopolymerization
[0122] Under anhydrous and oxygen-free conditions, 5 μmol of complex 1 and 10 μmol of [Ph3C][B(C6F5)4] were reacted in 3 mL of toluene at room temperature for 20 min, and then 200 μmol of Al i Bu3 was used to prepare a catalyst composition solution (4 mL in total). The catalyst composition toluene solution was then injected into a reaction bottle containing 10 mL of styrene monomer and 46 mL of toluene solvent. The reaction was carried out at 70°C for 120 min, and then ethanol acidified with hydrochloric acid was added to terminate the polymerization reaction, thereby obtaining 8.9 g of polystyrene. The polymerization activity was 4.45×10 5 g / mol Ti h. Molecular weight M n =121×10 4 g / mol, molecular weight distribution M w / M n =2.39, T m =270℃, syndiotactic stereotacticity rrrr>99%.
[0123] Polymerization Example 2: Complex 2 catalyzes styrene homopolymerization
[0124] Under anhydrous and oxygen-free conditions, 5 μmol of complex 2 was reacted with 10 μmol of [Ph3C][B(C6F5)4] in 3 mL of toluene at room temperature for 20 min, and then 200 μmol of Al iBu3 was used to prepare a catalyst composition solution (4 mL in total). The catalyst composition toluene solution was then injected into a reaction bottle containing 10 mL of styrene monomer and 46 mL of toluene solvent. The reaction was carried out at 70°C for 120 min, and then ethanol acidified with hydrochloric acid was added to terminate the polymerization reaction, thereby obtaining 8.5 g of polystyrene. The polymerization activity was 4.25×10 5 g / mol Ti h. Molecular weight M n =117×10 4 g / mol, molecular weight distribution M w / M n =2.41, T m =272℃, syndiotactic stereotacticity rrrr>99%.
[0125] Polymerization Example 3: Complex 3 catalyzes styrene homopolymerization
[0126] Under anhydrous and oxygen-free conditions, 5 μmol of complex 3 and 10 μmol of [PhNMe2H][B(C6F5)4] were reacted in 3 mL of toluene at room temperature for 30 min, and then 200 μmol of Al i Bu3 was used to prepare a catalyst composition solution (4 mL in total). The catalyst composition toluene solution was then injected into a reaction bottle containing 10 mL of styrene monomer and 46 mL of toluene solvent. The reaction was carried out at 80°C for 120 min, and then ethanol acidified with hydrochloric acid was added to terminate the polymerization reaction, thereby obtaining 8.8 g of polystyrene. The polymerization activity was 4.4×10 5 g / mol Ti h. Molecular weight M n =109×10 4 g / mol, molecular weight distribution M w / M n =2.42, T m =269℃, syndiotactic stereotacticity rrrr>99%.
[0127] Polymerization Example 4: Complex 4 catalyzes styrene homopolymerization
[0128] Under anhydrous and oxygen-free conditions, 5 μmol of complex 4 and 10 μmol of [Ph3C][B(C6F5)4] were reacted in 3 mL of toluene at room temperature for 20 min, and then 400 μmol of Al i Bu3 was used to prepare a catalyst composition solution (4 mL in total). The catalyst composition toluene solution was then injected into a reaction bottle containing 15 mL of styrene monomer and 71 mL of toluene solvent. The reaction was carried out at 80°C for 120 min, and then ethanol acidified with hydrochloric acid was added to terminate the polymerization reaction, producing 13.1 g of polystyrene. The polymerization activity was 6.6×10 5g / mol Ti h. Molecular weight M n =151×10 4 g / mol, molecular weight distribution M w / M n =2.39, T m =271℃, syndiotactic stereotacticity rrrr>99%.
[0129] Polymerization Example 5: Complex 5 catalyzes styrene homopolymerization
[0130] Under anhydrous and oxygen-free conditions, 5 μmol of complex 5 was reacted with 10 μmol of [Ph3C][B(C6F5)4] in 3 mL of toluene at room temperature for 20 min, and then 200 μmol of Al i Bu3 was used to prepare a catalyst composition solution (4 mL in total). The catalyst composition toluene solution was then injected into a reaction bottle containing 10 mL of styrene monomer and 46 mL of toluene solvent. The reaction was carried out at 70°C for 120 min, and then ethanol acidified with hydrochloric acid was added to terminate the polymerization reaction, producing 8.7 g of polystyrene. The polymerization activity was 4.35×10 5 g / mol Ti h. Molecular weight M n =130×10 4 g / mol, molecular weight distribution M w / M n =2.31, T m =270℃, syndiotactic stereotacticity rrrr>99%.
[0131] Polymerization Example 6: Complex 6 catalyzes styrene homopolymerization
[0132] Under anhydrous and oxygen-free conditions, 5 μmol of complex 6 was reacted with 10 μmol of [Ph3C][B(C6F5)4] in 3 mL of toluene at room temperature for 20 min, and then 200 μmol of Al i Bu3 was used to prepare a catalyst composition solution (4 mL in total). The catalyst composition toluene solution was then injected into a reaction bottle containing 10 mL of styrene monomer and 46 mL of toluene solvent. The reaction was carried out at 70°C for 60 min, and then ethanol acidified with hydrochloric acid was added to terminate the polymerization reaction, thereby obtaining 8.5 g of polystyrene. The polymerization activity was 8.8×10 5 g / mol Ti h. Molecular weight M n =83×10 4 g / mol, molecular weight distribution M w / M n =2.27, T m =271℃, syndiotactic stereotacticity rrrr>99%.
[0133] Polymerization Example 7: Complex 7 catalyzes styrene homopolymerization
[0134] Under anhydrous and oxygen-free conditions, 5 μmol of complex 7 was reacted with 10 μmol of [Ph3C][B(C6F5)4] in 3 mL of toluene at room temperature for 20 min, and then 200 μmol of Al i Bu3 was used to prepare a catalyst composition solution (4 mL in total). The catalyst composition toluene solution was then injected into a reaction bottle containing 10 mL of styrene monomer and 46 mL of toluene solvent. After the reaction was carried out at 20°C for 4 h, ethanol acidified with hydrochloric acid was added to terminate the polymerization reaction, and 6.8 g of polystyrene was obtained. The polymerization activity was 1.7×10 5 g / mol Ti h. Molecular weight M n =137×10 4 g / mol, molecular weight distribution M w / M n =2.76, T m =270℃, syndiotactic stereotacticity rrrr>99%. Figure 1 and 2 They are the DSC curve and carbon NMR spectrum of the obtained polystyrene, respectively.
[0135] Polymerization Example 8: Homopolymerization of p-methylstyrene catalyzed by Complex 8
[0136] Under anhydrous and oxygen-free conditions, 5 μmol of complex 8 and 10 μmol of [Ph3C][B(C6F5)4] were reacted in 3 mL of toluene at room temperature for 20 min, and then 200 μmol of Al i Bu3 was used to prepare a catalyst composition solution (4 mL in total). The catalyst composition toluene solution was then injected into a reaction bottle containing 10 mL of p-methylstyrene monomer and 46 mL of toluene solvent. After the reaction was carried out at 60°C for 120 min, ethanol acidified with hydrochloric acid was added to terminate the polymerization reaction, and 8.8 g of poly-p-methylstyrene was obtained. The polymerization activity was 4.4×10 5 g / mol Ti h. Molecular weight M n = 134×10 4 g / mol, molecular weight distribution M w / M n =2.21, syndiotactic stereoregularity rrrr>99%. Figure 3 : This is the hydrogen nuclear magnetic resonance spectrum of the obtained poly(p-methylstyrene).
[0137] Polymerization Example 9: Complex 9 catalyzes styrene homopolymerization
[0138] Under anhydrous and oxygen-free conditions, 5 μmol of complex 9 and 10 μmol of [Ph3C][B(C6F5)4] were reacted in 3 mL of toluene at room temperature for 20 min, and then 200 μmol of Al i Bu3 was used to prepare a catalyst composition solution (4 mL in total). The catalyst composition toluene solution was then injected into a reaction bottle containing 3.3 mL of styrene monomer and 46 mL of toluene solvent. The reaction was polymerized at 40°C for 60 min, and then ethanol acidified with hydrochloric acid was added to terminate the polymerization reaction, yielding 2.7 g of polystyrene. The polymerization activity was 2.7×10 5 g / mol Ti h. Molecular weight M n =64×10 4 g / mol, molecular weight distribution M w / M n =2.36, T m =272℃, syndiotactic stereotacticity rrrr>99%.
[0139] Polymerization Example 10: Complex 1 catalyzes styrene homopolymerization
[0140] Under anhydrous and oxygen-free conditions, 5 μmol of complex 1 and 10 μmol of [Ph3C][B(C6F5)4] were reacted in 3 mL of toluene at room temperature for 20 min, and then 200 μmol of Al i Bu3 was used to prepare a catalyst composition solution (4 mL in total). The catalyst composition toluene solution was then injected into a reaction bottle containing 13.2 mL of styrene monomer and 50 mL of toluene solvent. The reaction was carried out at 100°C for 4 h, and then ethanol acidified with hydrochloric acid was added to terminate the polymerization reaction, producing 11.7 g of polystyrene. The polymerization activity was 2.9×10 5 g / mol Ti h. Molecular weight M n =142×10 4 g / mol, molecular weight distribution M w / M n =2.58, T m =271℃, syndiotactic stereotacticity rrrr>99%.
[0141] Polymerization Example 11: Complex 1 catalyzes styrene homopolymerization
[0142] Under anhydrous and oxygen-free conditions, 5 μmol of complex 1 and 10 μmol of [Ph3C][B(C6F5)4] were reacted in 3 mL of toluene at room temperature for 20 min, and then 200 μmol of Al iBu3 was used to prepare a catalyst composition solution (4 mL in total). The catalyst composition toluene solution was then injected into a reaction bottle containing 13.2 mL of styrene monomer and 50 mL of toluene solvent. After the reaction was carried out at 180°C for 1 min, ethanol acidified with hydrochloric acid was added to terminate the polymerization reaction, and 0.9 g of polystyrene was obtained. The polymerization activity was 5.4×10 6 g / mol Ti h. Molecular weight M n =6.4×10 4 g / mol, molecular weight distribution M w / M n =1.87, T m =271℃, syndiotactic stereotacticity rrrr>99%.
[0143] Polymerization Example 12: Complex 1 catalyzes styrene homopolymerization
[0144] Under anhydrous and oxygen-free conditions, 5 μmol of complex 1 and 10 μmol of [Ph3C][B(C6F5)4] were reacted in 3 mL of toluene at room temperature for 20 min, and then 200 μmol of Al i Bu3 was used to prepare a catalyst composition solution (4 mL in total). The catalyst composition toluene solution was then injected into a reaction bottle containing 13.2 mL of styrene monomer and 50 mL of toluene solvent. The reaction was carried out at 0°C for 100 h, and then ethanol acidified with hydrochloric acid was added to terminate the polymerization reaction to obtain 9.5 g of polystyrene. The polymerization activity was 9.5×10 3 g / mol Ti h. Molecular weight M n =358×10 4 g / mol, molecular weight distribution M w / M n =2.67, T m =271℃, syndiotactic stereotacticity rrrr>99%.
[0145] In order to fully reveal the characteristics of binuclear catalysts in the styrene polymerization process, the present invention synthesized a mononuclear catalyst comparative complex 1 with similar structure and conducted comparative experiments under the same conditions. Comparative complex 1 was synthesized according to the method described in Organometallic 1989, 8, 476.
[0146]
[0147] Comparative Polymerization Example 1: Comparative Complex 1 Catalyzed Styrene Homopolymerization
[0148] According to the reaction conditions of Polymerization Example 7, 10 μmol of comparative complex 1 and 10 μmol of [Ph3C][B(C6F5)4] were reacted in 3 mL of toluene at room temperature for 20 min, and then 200 μmol of Al i Bu3 was used to prepare a catalyst composition solution (4 mL in total). The catalyst composition toluene solution was then injected into a reaction bottle containing 10 mL of p-methylstyrene monomer and 46 mL of toluene solvent. After the reaction was carried out at 60°C for 5 min, ethanol acidified with hydrochloric acid was added to terminate the polymerization reaction, and 8.4 g of polystyrene was obtained. The polymerization activity was 1.68×10 6 g / mol Ti h. Molecular weight M n =35.4×10 4 g / mol, molecular weight distribution M w / M n =1.85, syndiotactic stereotacticity rrrr>99%.
[0149] It can be seen from the above embodiments that the present invention provides a dinuclear cyclopentadienyl Group IV metal catalyst for syndiotactic selective polymerization of styrene monomers, having a structure of Formula I; compared with the corresponding mononuclear cyclopentadienyl Group IV metal catalyst, the dinuclear cyclopentadienyl Group IV metal catalyst of the present invention exhibits a significant bimetallic synergistic effect in the process of catalyzing the polymerization of styrene monomers, can effectively inhibit chain transfer reactions, and produce higher molecular weight syndiotactic polystyrene and its derivatives.
[0150] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A dinuclear cyclopentadienyl group IV metal catalyst for the polymerization of styrene and its derivatives, characterized in that: It is selected from one of the following structures:
2. A method for preparing a binuclear cyclopentadienyl group IV metal catalyst for polymerization of styrene and its derivatives according to claim 1, characterized in that: The following steps are involved: The binuclear cyclopentadienyl group IV metal catalyst has a structure shown in Formula I: Step 1: Under anhydrous and oxygen-free conditions, 1 -U-Cp 2 The ligand is dissolved in an organic solvent to obtain a ligand solution; Step 2, reacting the ligand solution with twice the molar amount of an alkali metal reagent to obtain an alkali metal salt of the ligand; Step 3: The alkali metal salt of the ligand and twice the molar amount of (A)M(X 1 X 2 X 3 ) to obtain a binuclear cyclopentadienyl Group IV metal catalyst having a structure shown in Formula I; The (A)M(X 1 X 2 X 3 ) wherein A is selected from halogen, BH4 – 、[(C6H5)4B] – or [(C6F5)4B] – , M, X 1 , X 2 and X 3 , and the Cp 1 -U-Cp 2 Cp 1 , Cp 2 and U correspond to the substituent groups on each complex in claim 1.
3. A binuclear cyclopentadienyl group IV metal catalyst composition for catalyzing the polymerization of styrene and its derivatives, characterized in that: The invention comprises the binuclear cyclopentadienyl group-four metal catalyst, organic boron salt and main group metal alkyl reagent as claimed in claim 1; the molar ratio of the binuclear cyclopentadienyl group-four metal catalyst, organic boron salt and main group metal alkyl reagent is 1:(0-4):(0-4000).
4. The binuclear cyclopentadienyl Group IV metal catalyst composition according to claim 3, characterized in that: The organic boron salt is selected from the group consisting of [B(C6F5)4] – Negative ion organic boron salt, containing [1,4-(C6F5)3BC6F4B(C6F5)3] 2– One or more of anion organic boron salts, B(C6F5)3 and 1,4-(C6F5)2BC6F4B(C6F5)2; the main group metal alkyl reagent is selected from one or more of aluminoxane, alkyl aluminum, alkyl zinc and alkyl magnesium reagents.
5. A method for catalyzing the polymerization of styrene and its derivatives, characterized in that: The following steps are involved: Under anhydrous and oxygen-free conditions, homopolymerizing or copolymerizing styrene monomers or styrene derivative monomers under the catalysis of the binuclear cyclopentadienyl Group IV metal catalyst composition of claim 3 or 4; The styrene monomer is one or more of styrene, p-methylstyrene and p-tert-butylstyrene; the styrene derivative monomer is a styrene derivative containing a long-chain alkane with 2 to 25 carbon atoms at the para position of styrene.
6. The method according to claim 5, characterized in that The temperature of the homopolymerization or copolymerization reaction is 0 to 180° C., and the time is 1 minute to 100 hours.
Citation Information
Patent Citations
Synthetic method of bridged metallocene dinuclear catalyst
CN102993341A
Preparation and application of dual-core metallocene compound
CN108456234A
Dinuclear rare earth catalyst as well as preparation method and application thereof
CN113307896A
Binuclear metal catalyst, preparation method and application
CN114031703A