A kind of organic silicon synthetic leather foam coating and preparation method thereof
Through the in-situ construction method of the water-in-oil system, the vulcanization and foaming of the silicone synthetic leather foam coating are realized in steps, which solves the problems of difficulty in coordinating the foaming and vulcanization rates and insufficient adhesion in the existing technology. , improves the polarity and mechanical properties of the coating, and enhances the adhesion to polar substrates.
Patent Information
- Application Number
- CN202210428866.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-04-22
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2042-04-22
AI Technical Summary
The existing silicone synthetic leather foam coating technology has problems such as difficulty in coordinating foaming and vulcanization rates, difficulty in regulating cell size and coating physical properties, and insufficient mechanical strength and interlayer adhesion of the coating.
Using the in-situ construction method of water-in-oil system, water-based polyurethane and hydroxyl silicone oil are mixed to form an emulsion. After adding curing agent and catalyst, it is coated and baked to achieve vulcanization and foaming in steps, using water volatilization to cause pores to form Silicone synthetic leather foam coating.
It achieves more controllable cell structure and coating physical properties, improves the polarity and mechanical properties of the coating, enhances the adhesion with polar substrates, and solves the coordination problems and bonding problems in traditional processes. The problem of insufficient power.
Smart Images

Figure CN114892418B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of synthetic leather, and in particular relates to an organic silicon synthetic leather foaming coating and a preparation method thereof. Background Art
[0002] As a type of organic chemical material that can be produced without relying on petroleum resources, silicone has many excellent properties such as high and low temperature resistance, aging resistance, wear resistance, hydrophobicity and physiological inertness due to its unique -Si-O-Si- structure. It has been widely used in the leather / synthetic leather field in the form of additives for many years. With the continuous advancement of the cleanness of the synthetic leather industry and the continuous improvement of manufacturing technology, in recent years, silicone materials have begun to be used in the manufacture of synthetic leather in the form of coatings, that is, the new generation of silicone synthetic leather. The construction of silicone synthetic leather coating is mainly based on the silylation reaction system between vinyl silicone oil and hydrogen-containing silicone oil. The production process does not require the use of any organic solvents, no gas is generated, and environmental pollution can be greatly reduced. The product has no volatile organic compounds (VOCs). In view of its unique resources, performance and environmental advantages, synthetic leather based on silicone coating materials can meet the market demand for high-quality ecological synthetic leather today and has great development prospects.
[0003] However, as an emerging product, silicone synthetic leather has a short history of development. Compared with the mainstream polyurethane synthetic leather on the market, it still has many imperfections. Among them, in terms of synthetic leather structure, traditional polyurethane synthetic leather is usually composed of five parts: surface effect layer, surface layer, intermediate foaming layer, adhesive layer and substrate. Each part plays a vital role in the overall performance of synthetic leather. However, due to the mismatch between manufacturing technology and coating materials, the foaming coating technology that can be applied to silicone synthetic leather is relatively scarce. The foaming layer plays a key role in giving synthetic leather a full feel, foaming feel and fullness, as well as improving the quality and market competitiveness of synthetic leather. Therefore, combining the physical property requirements and process characteristics of synthetic leather, enriching the preparation technology of silicone foaming coating will lay an important foundation for the further promotion and application of silicone synthetic leather.
[0004] Chinese patent CN111691193A discloses a foamed silicone synthetic leather and a preparation method thereof; the invention discloses a foamed silicone synthetic leather, which is composed of a surface layer, a foaming layer and a base layer stacked in sequence; the surface layer includes vinyl polysiloxane, vinyl MQ silicone resin, white carbon black, hydrogen-containing polysiloxane, platinum catalysts and inhibitors; the foaming layer includes vinyl polysiloxane, vinyl MQ silicone resin, α, ω-dihydroxy polysiloxane, hydroxy silicone oil, white carbon black, hydrogen-containing polysiloxane, platinum catalysts, inhibitors and tackifiers. The foamed silicone synthetic leather uses chemical foaming to prepare the foaming layer, and the foaming layer has a uniform distribution of pore size and a uniform spherical shape, which reduces the amount of silicone used and thus reduces the cost, but has good mechanical properties and lightweight characteristics. The invention also provides a preparation method for foamed silicone synthetic leather, which is simple and easy to operate, easy to promote, and has low equipment and site cost investment, and is suitable for industrial-scale production.
[0005] The existing technology uses a chemical foaming method based on the principle of dehydrogenation between silicon hydrogen and hydroxyl groups. This method performs foaming and coating vulcanization simultaneously, which will cause problems such as difficulty in coordinating the foaming and vulcanization rates and difficulty in controlling the foaming process, thereby increasing the difficulty of actual process operation, and making it difficult to control the pore size and coating properties.
[0006] The existing technology uses a single component of silicone to prepare the foaming layer. Since silicone is a non-polar polymer, and the synthetic leather substrate is mostly a polar material, such as polyethylene terephthalate (PET), nylon, etc., there will still be problems of insufficient mechanical strength of the coating and insufficient interlayer adhesion. Summary of the invention
[0007] The purpose of the present invention is to address the deficiencies of the above-mentioned prior art and to provide a method for preparing a silicone synthetic leather foam coating in combination with the physical property requirements of the synthetic leather foam coating, comprising the following steps:
[0008] (1) adding water-based polyurethane to hydroxy silicone oil at a rate of 10-50 mL / h, mixing, and obtaining a hydroxy silicone oil-water-based polyurethane water-in-oil emulsion; the mass ratio of the water-based polyurethane to the hydroxy silicone oil is 30-50:50-70;
[0009] (2) adding a curing agent and a catalyst to the hydroxy silicone oil-aqueous polyurethane water-in-oil emulsion, mixing and coating the mixture on the surface of the release paper to obtain a coating to be cured; the mass ratio of the hydroxy silicone oil, the curing agent and the catalyst is 100:2:0.1-0.3;
[0010] (3) baking the coating to be cured and then drying it to obtain the organic silicone synthetic leather foam coating.
[0011] Preferably, in step (1), 50-70 parts of hydroxy silicone oil are added to a batching tank and placed under a disperser, and fully stirred at a speed of 100-500 r / min. Under continuous stirring conditions, 30-50 parts of aqueous polyurethane are slowly added to the hydroxy silicone oil at a speed of 10-50 mL / h using a peristaltic pump, and after the addition is completed, a hydroxy silicone oil-aqueous polyurethane oil-in-water emulsion can be obtained.
[0012] Preferably, in step (2), the coating thickness is 0.8-1.0 mm.
[0013] Preferably, in step (3), the baking temperature is 50-80° C. and the baking time is 3-5 min.
[0014] Preferably, in step (3), the drying temperature is 100-120° C. and the drying time is 1-2 min.
[0015] Preferably, the hydroxy silicone oil is α,ω-dihydroxy polysiloxane with a viscosity of 5000-20000 mPa·s.
[0016] Preferably, the waterborne polyurethane is a polyester waterborne polyurethane or a polyether waterborne polyurethane, and has a solid content of 20-40wt%. The introduction of waterborne polyurethane not only causes pores, but also improves the polarity and mechanical properties of the silicone foam coating, thereby improving the adhesion between the silicone foam coating and the polar substrate of synthetic leather, laying a material foundation for the manufacture of high-property silicone synthetic leather.
[0017] Preferably, the curing agent is one or more of methyl orthosilicate, ethyl orthosilicate and butyl orthosilicate.
[0018] Preferably, the catalyst is bismuth isooctanoate and / or bismuth neodecanoate.
[0019] The present invention also provides an organic silicon synthetic leather foam coating prepared by the above preparation method.
[0020] The present invention uses a water-in-oil system precursor to in-situ construct an organosilicon synthetic leather foam coating, which can achieve vulcanization and foaming in steps, thus overcoming the problem of difficulty in coordinating the foaming and vulcanization rates in traditional processes.
[0021] The technical solution of the present invention has the following advantages over the prior art:
[0022] (1) For the first time, an in-situ preparation method for water-in-oil silicone foam coatings was proposed. This method does not require the use of any emulsifiers or foaming agents. It utilizes the volatilization of water in a two-component room temperature / low temperature curing silicone rubber system to form pores, providing a new idea for the construction of silicone synthetic leather foam coatings.
[0023] (2) The introduction of waterborne polyurethane (WPU) not only causes pores, but also forms an interpenetrating network with the silicone component, thereby effectively improving the polarity and mechanical properties of the silicone foam coating and the adhesion to the polar substrate, laying a material foundation for the manufacture of high-property silicone synthetic leather.
[0024] (3) The in-situ construction method of the foaming coating based on the oil-in-water system can realize the vulcanization and foaming in steps, which effectively overcomes the problem of the difficulty in coordinating the foaming and vulcanization rates in the traditional foaming process, and the pore structure and coating properties are more controllable. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 Flow chart for in-situ preparation of silicone synthetic leather foam coating. DETAILED DESCRIPTION
[0026] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments so that those skilled in the art can better understand the present invention and implement it, but the embodiments are not intended to limit the present invention.
[0027] Example 1
[0028] (1) Preparation of hydroxy silicone oil-aqueous polyurethane water-in-oil emulsion:
[0029] 70 parts of 5000mPa·s α,ω-dihydroxy polysiloxane were added into the batching tank and placed under a disperser, and fully stirred at a speed of 100r / min. Under continuous stirring conditions, 30 parts of aliphatic polyester waterborne polyurethane with a solid content of 20wt% were slowly added into the α,ω-dihydroxy polysiloxane at a speed of 10mL / h using a peristaltic pump, and after the addition was completed, a hydroxy silicone oil-waterborne polyurethane oil-water emulsion was obtained;
[0030] (2) In-situ preparation of silicone-polyurethane interpenetrating network foaming coating:
[0031] Methyl orthosilicate is added to the water-in-oil emulsion prepared in step (1), and the mass ratio of hydroxy silicone oil to methyl orthosilicate is controlled to be 100:2. Then, 0.3 parts of bismuth neodecanoate is added, mixed evenly and then quickly applied to the surface of the release paper. The coating thickness is controlled to be 0.8 mm, and then placed in a 50° C. oven for curing for 3 min. After the organic silicon component is completely cured, the oven temperature is raised to 100° C. and continued to dry for 2 min to remove internal moisture, thereby obtaining an organic silicon-polyurethane interpenetrating network foaming coating.
[0032] This coating does not use any organic solvents during its preparation and use. After comparative testing, compared with a single-component silicone foam coating, the mechanical strength of the coating is increased from 1.8MPa to 2.8MPa, and the peel strength between the coating and the base fabric is increased from 35N / 3cm to 45N / 3cm.
[0033] Embodiment 2:
[0034] (1) Preparation of hydroxy silicone oil-aqueous polyurethane water-in-oil emulsion:
[0035] 60 parts of 10000mPa·s α,ω-dihydroxy polysiloxane were added into the batching tank and placed under a disperser, and stirred at 200r / min. Under continuous stirring, 40 parts of aliphatic polyether waterborne polyurethane with a solid content of 30wt% were slowly added into the α,ω-dihydroxy polysiloxane at a speed of 20mL / h using a peristaltic pump, and after the addition was completed, a hydroxy silicone oil-waterborne polyurethane oil-water emulsion was obtained;
[0036] (2) In-situ preparation of silicone-polyurethane interpenetrating network foaming coating:
[0037] Add ethyl orthosilicate to the water-in-oil emulsion prepared in step (1), control the mass ratio of hydroxy silicone oil to ethyl orthosilicate to be 100:2, then add 0.2 parts of bismuth neodecanoate, mix well and quickly apply it on the surface of release paper, control the coating thickness to 0.8 mm, and then place it in a 60° C. oven for curing for 3 minutes. After the organic silicon component is completely cured, increase the oven temperature to 110° C. and continue drying for 1 minute to remove internal moisture, thereby obtaining an organic silicon-polyurethane interpenetrating network foaming coating.
[0038] This coating does not use any organic solvents during its preparation and use. After comparative testing, compared with a single-component silicone foam coating, the mechanical strength of the coating is increased from 1.8MPa to 3.2MPa, and the peel strength between the coating and the base fabric is increased from 35N / 3cm to 48N / 3cm.
[0039] Embodiment 3:
[0040] (1) Preparation of hydroxy silicone oil-aqueous polyurethane water-in-oil emulsion:
[0041] 50 parts of 20000mPa·s α,ω-dihydroxy polysiloxane were added into the batching tank and placed under the disperser, and fully stirred at a speed of 500r / min. Under continuous stirring conditions, 50 parts of aromatic polyether-type waterborne polyurethane with a solid content of 40wt% were slowly added into the α,ω-dihydroxy polysiloxane at a speed of 50mL / h using a peristaltic pump, and after the addition was completed, a hydroxy silicone oil-waterborne polyurethane oil-water emulsion was obtained;
[0042] (2) In-situ preparation of silicone-polyurethane interpenetrating network foaming coating:
[0043] Add butyl orthosilicate to the water-in-oil emulsion prepared in step (1), control the mass ratio of hydroxy silicone oil to butyl orthosilicate to be 100:2, then add 0.1 parts of bismuth isooctanoate, mix well and quickly apply it on the surface of release paper, control the coating thickness to 1.0 mm, and then place it in an oven at 80° C. for curing for 5 min. After the organic silicon component is completely cured, increase the oven temperature to 120° C. and continue drying for 1 min to remove internal moisture, thereby obtaining an organic silicon-polyurethane interpenetrating network foaming coating.
[0044] This coating does not use any organic solvents during its preparation and use. After comparative testing, compared with a single-component silicone foam coating, the mechanical strength of the coating is increased from 1.8MPa to 3.9MPa, and the peel strength between the coating and the base fabric is increased from 35N / 3cm to 50N / 3cm.
[0045] Obviously, the above embodiments are merely examples for clear explanation and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived from these are still within the protection scope of the invention.
Claims
1. A method for preparing a silicone synthetic leather foam coating, It is characterized in that The steps include: (1) adding waterborne polyurethane to hydroxy silicone oil at a rate of 10-50 mL / h, mixing, and obtaining a hydroxy silicone oil-waterborne polyurethane water-in-oil emulsion; the mass ratio of the waterborne polyurethane to the hydroxy silicone oil is 30-50:50-70; and the viscosity of the hydroxy silicone oil is 5000-20000 mPa·s; (2) adding a curing agent and a catalyst to the hydroxy silicone oil-waterborne polyurethane water-in-oil emulsion, mixing and coating the mixture on the surface of the release paper to obtain a coating to be cured; the mass ratio of the hydroxy silicone oil, the curing agent and the catalyst is 100:2:0.1-0.3; The curing agent is one or more of methyl orthosilicate, ethyl orthosilicate and butyl orthosilicate; (3) baking and drying the coating to be cured to obtain the silicone synthetic leather foam coating; In the step (3), the baking temperature is 50-80°C and the baking time is 3-5 min; In the step (3), the drying temperature is 100-120°C and the drying time is 1-2 min; The waterborne polyurethane is a polyester waterborne polyurethane or a polyether waterborne polyurethane, and has a solid content of 20-40 wt%.
2. The preparation method according to claim 1, It is characterized in that In the step (1), the hydroxy silicone oil is stirred at 100-500 r / min before mixing.
3. The preparation method according to claim 1, It is characterized in that In the step (2), the coating thickness is 0.8-1.0 mm.
4. The preparation method according to claim 1, It is characterized in that The hydroxy silicone oil is α, ω-dihydroxy polysiloxane.
5. The preparation method according to claim 1, It is characterized in that The catalyst is bismuth isooctanoate and / or bismuth neodecanoate.
6. A silicone synthetic leather foam coating prepared according to the preparation method according to any one of claims 1 to 5.