Isothermal extrusion method for aluminum alloy profile
By measuring the initial heating temperature and microstructure of the aluminum alloy casting rod, the mold outlet temperature is calculated using Zener-Hollomon parameters, and a reasonable casting rod heating gradient is set, the problem of uneven temperature during isothermal extrusion of aluminum alloy in the prior art isothermal extrusion is solved. , achieving efficient extrusion process and product quality improvement.
Patent Information
- Application Number
- CN202210556432.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-05-20
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2042-05-20
AI Technical Summary
The prior art is difficult to achieve isothermal extrusion of aluminum alloys, mainly due to the inability to accurately measure the actual temperature of the profile at the mold outlet and the lack of reasonable reference basis for temperature gradient setting, resulting in uneven temperature during the extrusion process, affecting product quality and productivity.
By measuring the initial heating temperature of the aluminum alloy casting rod and the average subcrystal size of the microstructure of the profile, the mold outlet temperature is calculated using the Zener-Hollomon parameters, and then a reasonable casting rod heating temperature gradient is set to ensure the uniformity of the temperature during the extrusion process.
Isothermal extrusion of aluminum alloy profiles is achieved, the extrusion speed and uniformity of product shape, size, structure and performance are improved, and productivity and product quality are significantly improved.
Smart Images

Figure CN114939604B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of aluminum alloy material processing, and in particular to an isothermal extrusion method for aluminum alloy profiles. Background Art
[0002] In the conventional aluminum alloy hot extrusion process, the temperature and deformation of the cast rod are very uneven, which leads to uneven quality in terms of product size, shape, organization and performance. Isothermal extrusion can reduce these unevenness and is an ideal extrusion process. The characteristic of isothermal extrusion is to ensure that the temperature of the metal in the deformation zone near the die hole remains constant or basically constant throughout the extrusion process, and to try to maintain the uniformity of metal deformation resistance and metal flow, so as to obtain a higher extrusion speed. At the same time, the shape and size of the extruded profile are accurate, and the uniformity of organization and performance along the cross section and length direction is also improved. The use of isothermal extrusion can achieve the best results in the geometric dimensions, surface quality, internal organization and physical properties of the entire product head and tail, greatly improving productivity. Therefore, the implementation of isothermal extrusion is of great significance to improving the productivity and quality of extruded products.
[0003] The key technology of isothermal extrusion process is to control the temperature of the extruded product at the die outlet. Only when the temperature fluctuation is controlled within a very small range can isothermal extrusion be truly achieved. Therefore, in the technology of isothermal extrusion of billet temperature gradient extrusion, the reasonable setting of the heating gradient of the cast rod becomes the most critical issue. This leads to two practical problems: how to accurately measure the actual temperature of the profile at the die outlet, and how to reasonably set the heating gradient of the cast rod.
[0004] At present, there are two main methods for measuring the outlet temperature of profiles in industrial production: manual measurement with handheld thermocouples and infrared measurement. The common disadvantage of these two methods is that they cannot directly measure the actual temperature at the die outlet. The measured temperature is often the temperature of the profile 0.5-1.5m away from the die outlet (due to the structural limitation of the front beam of the extruder). At this time, the profile has been out of the die for a period of time and has been cooled by air. The actual temperature is much lower than the temperature at the die outlet. Therefore, if the heating gradient of the cast rod is set at this temperature, the isothermal extrusion effect cannot be truly achieved. Therefore, how to accurately measure the actual temperature of the profile at the die outlet becomes a key issue in realizing the isothermal extrusion process.
[0005] In the technology of achieving isothermal extrusion by the billet temperature gradient extrusion method, there is currently no reasonable reference basis for setting the temperature gradient in the industry. It is often set based on a rough estimate based on experience, and the ultimate true isothermal extrusion effect is often difficult to fully achieve. Summary of the invention
[0006] The object of the present invention is to overcome the defects of the prior art and provide an isothermal extrusion method for aluminum alloy profiles, which associates the profile structure with the actual temperature, and realizes accurate temperature measurement by inferring the actual temperature through the profile structure according to the Z parameter, and then realizes reasonable setting of the gradient heating temperature gradient of the aluminum alloy profile by accurately calculating the outlet temperature of the extrusion die.
[0007] To achieve the above-mentioned purpose of the invention, the present invention proposes an isothermal extrusion method for aluminum alloy profiles, which measures the initial heating temperature of the aluminum alloy cast rod to be extruded, and measures the average subgrain size of the profile microstructure at each measurement position selected on the profile after extrusion, obtains the mold outlet temperature at each measurement position by Z parameter calculation, and sets the gradient heating temperature of the cast rod according to the comparison calculation between the mold outlet temperature and the initial heating temperature, thereby realizing isothermal extrusion.
[0008] Preferably, the mold outlet temperature is calculated by selecting a measurement position at the head of the profile and behind the head, and obtaining the lnZ function relationship of the profile deformation at the head of the profile and at a measurement position behind the head according to the relationship between the Z parameter, the deformation rate and the temperature.
[0009] Preferably, after comparing the die outlet temperature with the initial heating temperature, the temperature increase value at each measuring position is obtained; and according to the temperature increase value and the preset profile extrusion temperature, the gradient heating temperature of the cast rod is calculated.
[0010] Preferably, the lnZ function relationship is:
[0011]
[0012] Where Q is the deformation activation energy / J / mol, R is the gas constant, R=8.341 / J / (mol·K), T is the deformation temperature / K, T F is the initial heating temperature of the profile, T R is the mold outlet temperature at a certain measurement position after the head, Z F and Z R are the Z values of the profile head and a certain measuring position behind the head, respectively. F parameter.
[0013] Preferably, during the isothermal extrusion process, obtaining the gradient heating temperature comprises the following steps:
[0014] S1, measuring the initial heating temperature of the aluminum alloy profile to be extruded before extrusion;
[0015] S2, selecting each measurement position according to the setting requirements, taking the metallographic sample of the profile in each measurement position, measuring the average subgrain size of the microstructure of the profile at each measurement position, and calculating the Z parameter of the profile structure at each measurement position;
[0016] S3, select a certain measuring position at the head and the back of the profile, and obtain the lnZ function relationship of the profile deformation at a certain measuring position at the head and the back of the profile according to the relationship between the Z parameter, the deformation rate and the temperature:
[0017]
[0018] The die outlet temperature of the profile at a certain measuring position behind the head is calculated, where Q is the deformation activation energy / J / mol, R is the gas constant, R=8.341 / J / (mol·K), T is the deformation temperature / K, T F is the initial heating temperature of the profile, T R is the mold outlet temperature at a certain measurement position after the head, Z F and Z R are the Z values of the profile head and a certain measuring position behind the head, respectively. F parameter;
[0019] S4, repeat the calculation process of step S3 to obtain the mold outlet temperature of the profile at other measurement positions;
[0020] S5, comparing the die outlet temperature of the profile at each measuring position with the initial heating temperature of the profile before extrusion to obtain the temperature increase value of each profile section;
[0021] S6, calculating the gradient heating temperature of the cast rod according to the temperature increase value and the preset profile extrusion temperature.
[0022] Preferably, in S2, EBSD metallographic observation samples are prepared for the cross-section of the profile structure at each measuring position, and the average size of subgrains of the microstructure of the profile at each measuring position is measured.
[0023] The preset profile extrusion temperature is the die outlet temperature of each part of the profile after extrusion set according to the process requirements, and the selection of the measurement position is the measurement position on the profile selected according to the length of the profile, process requirements, etc.
[0024] Preferably, the setting of the gradient heating temperature of the cast rod corresponds to the measuring position of the profile.
[0025] The present invention also provides an isothermal extrusion method for an aluminum alloy profile, wherein obtaining the gradient heating temperature comprises the following steps:
[0026] S1, measuring the initial heating temperature of the aluminum alloy profile to be extruded before extrusion;
[0027] S2, selecting each measurement position according to the setting requirements, taking the metallographic sample of the profile in each measurement position, measuring the average subgrain size of the microstructure of the profile at each measurement position, and calculating the Z parameter of the profile structure at each measurement position;
[0028] S3, select a certain measuring position at the head and the back of the profile, and obtain the lnZ function relationship of the profile deformation at a certain measuring position at the head and the back of the profile according to the relationship between the Z parameter, the deformation rate and the temperature:
[0029]
[0030] The die outlet temperature of the profile at a certain measuring position behind the head is calculated, where Q is the deformation activation energy / J / mol, R is the gas constant, R=8.341 / J / (mol·K), T is the deformation temperature / K, T F is the initial heating temperature of the profile, T R is the mold outlet temperature at a certain measurement position after the head, Z F and Z R are the Z values of the profile head and a certain measuring position behind the head, respectively. F parameter;
[0031] S4, repeat the calculation process of step S3 to obtain the mold outlet temperature of the profile at other measurement positions;
[0032] S5, comparing the die outlet temperature of the profile at each measuring position with the initial heating temperature of the profile before extrusion to obtain the temperature increase value of each profile section;
[0033] S6, calculating the gradient heating temperature of the cast rod according to the temperature increase value and the preset profile extrusion temperature.
[0034] Preferably, the Z parameter of the profile structure at each measurement position is calculated in S3 by the following formula:
[0035] lnZ=A+Bδ -1 .
[0036] Preferably, in step S4, the lnZ function relationship of the profile deformation at the profile head and a certain measuring position behind the profile head is obtained by the following formula of the relationship between the Z parameter, the deformation rate and the temperature:
[0037]
[0038] in, is the strain rate / s -1 .
[0039] Preferably, in step S4, the Z of the profile head during the extrusion process FParameters and Z of the extruded profile at a certain measurement position after the head R The relationship between the parameters is:
[0040]
[0041] Preferably, in S2, EBSD metallographic observation samples are prepared for the cross-section of the profile structure at each measuring position, and the average size of subgrains of the microstructure of the profile at each measuring position is measured.
[0042] The invention obtains the effect of isothermal extrusion by quantitatively analyzing the degree of temperature rise during the extrusion process. Since the microstructure of the profile is usually composed of a surface coarse-grained layer and an internal fibrous deformation structure containing equiaxed subgrains, the invention uses the subgrain size in the microstructure of each part of the profile and the Zener-Hollomon parameter to infer the real temperature of the profile at the outlet of the extrusion die, thereby calculating the actual deformation temperature of the extrusion process, and then inferring the gradient heating temperature of the cast rod. By associating the profile structure with the actual temperature, the accurate inference of the outlet temperature of the extrusion die is achieved, and the accurate setting of the gradient heating temperature during isothermal extrusion of the cast rod profile is achieved, thereby providing a reasonable and accurate temperature gradient calculation method for realizing isothermal extrusion by the gradient heating extrusion method of the billet.
[0043] At the same time, the gradient heating temperature set by the present invention makes the temperature of the metal in the deformation zone near the die hole always remain constant or substantially constant, maintains the uniformity of metal deformation resistance and metal flow, and makes the die surface pressure constant or substantially constant, thereby obtaining a higher extrusion speed, and at the same time, the shape and size of the extruded profile are accurate, and the uniformity of the structure and performance along the cross section and length direction is also improved. The use of isothermal extrusion can achieve the best effect in the geometric size, surface quality, internal structure and physical properties of the entire product head and tail, greatly improving productivity. BRIEF DESCRIPTION OF THE DRAWINGS
[0044] Figure 1 It is a schematic diagram of the aluminum alloy round profile before isothermal extrusion of the present invention;
[0045] Figure 2 It is a schematic diagram of the initial stage of isothermal extrusion of the aluminum alloy profile of the present invention;
[0046] Figure 3 It is a schematic diagram of the middle stage of isothermal extrusion of the aluminum alloy profile of the present invention;
[0047] Figure 4 It is a schematic diagram of the later stage of isothermal extrusion of the aluminum alloy profile of the present invention;
[0048] Figure 5 It is a flow chart of the isothermal extrusion method of aluminum alloy profiles of the present invention;
[0049] Figure 6The figure is a flow chart of the isothermal extrusion method according to a specific embodiment of the present invention. DETAILED DESCRIPTION
[0050] The specific embodiments of the present invention are described in detail below in conjunction with the accompanying drawings, but it should be understood that the protection scope of the present invention is not limited by the specific embodiments. The structural, method, or functional changes made by ordinary technicians in the field according to these embodiments are all included in the protection scope of the present invention.
[0051] like Figure 1-4 As shown, it is a schematic diagram of the whole process of isothermal extrusion before the start, early, middle and late stages of extrusion of aluminum alloy cast bars (or round bars, round ingots) using a gradient heating method. The cast bars to be extruded are placed in an extrusion barrel, and the front end is extruded by the front beam and the machine base of the extruder to fix the extrusion die base and the die, and the rear end is connected to the extrusion rod through an extrusion pad. The heating gradient of the cast bars in the figure is set according to the measurement position selected on the profile. In this embodiment, three gradient heating temperatures are set, namely T1, T2 and T3. The temperature of the profile at the die outlet corresponding to each measurement position on the profile is set to t1, t2 and t3. Of course, in other embodiments of the present invention, the measurement position of the profile and the temperature heating gradient of the corresponding cast bars can be set to n according to the actual situation in theory, and n is a natural number greater than or equal to 2.
[0052] Under ideal conditions, that is, when the extrusion speed remains unchanged and the extrusion barrel and the mold reach a state of thermal equilibrium, isothermal extrusion can be achieved by setting a reasonable cast rod heating gradient. For example, assuming that the cast rod temperature gradient in the figure is ΔT1=T1-T2, ΔT2=T2-T3, then the temperature of the profile extrusion at the mold outlet should be consistent, that is, t1=t2=t3. In actual production, ΔT1, ΔT2, and ΔTn are all estimated based on experience and are not the most reasonable temperature gradients. In addition, since the extrusion barrel and the mold have not reached a state of thermal equilibrium, these factors together lead to the inability to achieve isothermal extrusion. Among them, the unreasonable cast rod heating temperature gradient is the main reason why isothermal extrusion cannot be achieved.
[0053] When the alloy grade, extrusion speed, extrusion ratio and other conditions are determined, the structure and performance of the profile mainly depend on the temperature of the profile at the die outlet. Different outlet temperatures will lead to different microstructures and mechanical properties. For example, if t1≠t2≠t3, the microstructures of the profiles corresponding to t1, t2 and t3 are significantly different. The difference is mainly reflected in the different subgrain sizes at different positions of the profile. The present invention uses the subgrain sizes in the microstructure of each part of the profile and the Zener-Hollomon parameters to infer the true temperature of the profile at the outlet of the extrusion die, thereby calculating the actual deformation temperature of the extrusion process, and then inferring the heating temperature gradient of the cast rod.
[0054] Since the microstructure of the profile is usually composed of a surface coarse-grained layer and an internal fibrous deformed structure containing equiaxed subgrains, the size of the subgrains has the following relationship with the Z parameter:
[0055] lnZ=A+Bδ -1 (I)
[0056] Where Z is the Zener-Hollomon parameter, A and B are material constants, and δ is the average subgrain size. The relationship between the Z parameter and the deformation rate and temperature is as follows:
[0057]
[0058] in is the strain rate / s -1 Q is the deformation activation energy / J / mol, R is the gas constant, R=8.341 / J / (mol·K), and T is the deformation temperature / K.
[0059] Considering that during the constant speed extrusion process, the deformation rate of the material at the center of the cross section of the profile at different positions are the same, the difference is the deformation temperature T. The deformation temperature of the profile head during extrusion is assumed to be the initial deformation temperature T F , then the Z of the corresponding profile head F Parameters and Z of the extruded profile at a certain measurement position after the head R The parameters have the following relationship:
[0060]
[0061]
[0062] From this we can conclude that:
[0063]
[0064] Expressing equation (5) as a function of lnZ, we obtain:
[0065]
[0066] The initial deformation temperature of the profile head is T F and Z of the profile head F The parameters can be obtained through constitutive equations and microstructure characterization, so the deformation temperature T of the profile at different measurement positions during deformation R It can be calculated by the above formula, and then the extruded cast rod can be gradient heated to obtain the same temperature gradient as the temperature rise, so as to ensure that the extrusion is carried out at an isothermal condition.
[0067] right Figure 1-4Taking the round ingot shown as an example, the initial heating temperature of the head end of the cast rod for extrusion is 480°C, and the head, middle and tail of the profile are selected as measurement positions. According to the above method, the temperatures of the head, middle and tail of the profile at the mold outlet are t1=500°C, t2=520°C, and t3=540°C, which means that the temperature rises at the head, middle and tail measurement positions of the extruded profile are 20°C, 40°C and 60°C respectively. Therefore, the temperature gradients between the head, middle and tail measurement positions of the corresponding cast rod for extrusion should correspond to this. If you want to obtain a profile with an extrusion temperature, that is, a preset profile extrusion temperature of 520°C, the gradient heating temperatures of the head, middle and tail of the cast rod should be set to 500°C, 480°C and 460°C respectively.
[0068] Therefore, if Figure 5 As shown, during the isothermal extrusion process of the aluminum alloy profile of the present invention, the acquisition of the gradient heating temperature at each measuring position of the profile includes the following steps:
[0069] S1, measure the initial heating temperature T of the aluminum alloy profile to be extruded at the beginning of extrusion F ;
[0070] S2, according to the process, the length of the profile and other settings, each measurement position to be measured is selected, and the metallographic sample of the profile in each measurement position is taken. The EBSD metallographic observation sample is made on the cross section of the profile structure at each measurement position, and the average subgrain size of the microstructure of the profile at each measurement position is measured, and the Z parameter of the profile structure at each measurement position is calculated by the following formula:
[0071] lnZ=A+Bδ -1
[0072] S3, select the head of the profile and a certain measurement position behind the head, according to the relationship between Z parameter, deformation rate and temperature,
[0073]
[0074] The lnZ value and lnZ function relationship of the profile deformation at the head and a certain measuring position behind the head of the aluminum alloy profile are obtained:
[0075]
[0076] in, is the strain rate / s -1 Q is the deformation activation energy / J / mol, R is the gas constant, R=8.341 / J / (mol·K), T is the deformation temperature / K, Z F and Z R are the Z parameters of the profile head and a certain measurement position behind the head,
[0077] Calculate the die outlet temperature T of a selected section of the profile after the head R .
[0078] S4, repeat the calculation process of step S3 to obtain the mold outlet temperature at other measurement positions;
[0079] S5, set the die outlet temperature T of each profile segment R Compared with the initial heating temperature before profile extrusion, the temperature increase value of each measuring position is obtained;
[0080] S6, adjusting the heating setting temperature of each measuring position according to the temperature increase value and the preset profile extrusion temperature, and calculating the gradient heating temperature of the cast rod.
[0081] The preset profile extrusion temperature is the die outlet temperature of each part of the profile after extrusion set according to the process requirements, and the selection of the measurement position is the measurement position on the profile selected according to the length of the profile, process requirements, etc. The setting of the gradient heating temperature of the cast rod, such as the number of temperature gradients, corresponds to the measurement position and measurement number of the profile. If the preset gradient heating temperature is a 3-stage gradient, it is necessary to select at least 3 points on the profile for sampling.
[0082] The calculation process of the gradient heating temperature is described below with a specific embodiment.
[0083] A 6061 alloy round ingot with a specification of φ178*500mm is extruded on an extruder with a tonnage of 18MN to produce an extruded sheet with a cross-sectional specification of 20*40mm. The profile extrusion length is 15.6m, the extrusion ratio is 30, the extrusion speed is 3mm / s, and the initial heating temperature of the ingot before extrusion is 490℃, that is, the initial heating temperature T of the original ingot at the die mouth before extrusion F The initial heating temperature is 490℃, which is also the initial temperature of the plate after extrusion. The three measurement positions of the head, middle and tail of the profile are selected. The die outlet temperatures of the head, middle and tail of the extruded plate are set to t1, t2 and t3 respectively. Then, metallographic samples are taken from the head, middle and tail of the profile with a length of 15.6 meters respectively, and EBSD metallographic observation samples are made for their cross sections. After measurement, the following results are obtained:
[0084] The average size of the initial microstructure subgrains is 2.03 μm;
[0085] The average size of the head tissue subgrains is 2.12 μm;
[0086] The average size of subgrains in the middle structure is 2.25 μm;
[0087] The average subgrain size of the tail structure is 2.32 μm;
[0088] Substitute the above subcrystal measurement results into the following formula to calculate
[0089] lnZ=A+Bδ -1
[0090]
[0091] For 6061 alloy, its material constants A = 27.4, B = 61, Q = 249.67KJ / mol, gas constant R = 8.341 / J / (mol·K). Since the initial heating temperature of the ingot at the die mouth is 490°C, it is considered that the initial temperature of the plate after extrusion is 490°C. According to the above formula, it can be calculated:
[0092] LqCy 初 =27.4+61*2.03 -1 =57.449
[0093] LqCy 头 =27.4+61*2.32 -1 =53.693
[0094] LqCy 中 =27.4+61*2.65 -1 =50.419
[0095] LqCy 尾 =27.4+61*2.86 -1 =48.728
[0096] Further calculations yield:
[0097] t1=522℃
[0098] t2=554℃
[0099] t3=572℃
[0100] Therefore, the die outlet temperatures at the head, middle and tail measuring positions of the profile during the actual extrusion process are 522°C, 554°C and 572°C respectively. It can be seen that the temperatures of the head, middle and tail of the extruded profile are 32°C, 64°C and 82°C higher than the initial heating temperature of the ingot before extrusion. Therefore, in order to ensure that the profile at the die outlet temperature during the extrusion process, that is, the preset profile extrusion temperature is 560°C, the heating temperature of the ingot should be set according to a certain gradient. According to the calculated temperature rise value, the gradient heating temperatures of the head, middle and tail of the ingot can be set to 528°C, 496°C and 478°C respectively.
[0101] The foregoing description of specific exemplary embodiments of the present invention is for the purpose of illustration and demonstration. These descriptions are not intended to limit the present invention to the precise form disclosed, and it is clear that many changes and variations can be made based on the above teachings. The purpose of selecting and describing the exemplary embodiments is to explain the specific principles of the present invention and its practical application, so that those skilled in the art can realize and utilize various different exemplary embodiments of the present invention and various different selections and changes. The scope of the present invention is intended to be limited by the claims and their equivalents.
Claims
1. An isothermal extrusion method for an aluminum alloy profile, characterized in that: Measuring the initial heating temperature of the aluminum alloy casting rod to be extruded, and measuring the average subgrain size of the profile microstructure at each measurement position selected on the profile after extrusion, obtaining the die outlet temperature at each measurement position by Z parameter calculation, obtaining the temperature increase value at each measurement position by comparing the die outlet temperature with the initial heating temperature, and calculating the gradient heating temperature of the casting rod according to the temperature increase value and the preset profile extrusion temperature, thereby realizing isothermal extrusion; The calculation of the mold outlet temperature is performed by selecting a certain measuring position at the head of the profile and the back of the head, and obtaining the lnZ function relationship of the profile deformation at a certain measuring position at the head of the profile and the back of the head according to the relationship between the Z parameter, the deformation rate and the temperature: Where Q is the deformation activation energy / J / mol, R is the gas constant, R=8.341 / J / (mol·K), T is the deformation temperature / K, T F is the initial heating temperature of the profile, T R is the mold outlet temperature at a certain measurement position after the head, Z F and Z R They are the Z parameters of the profile head and a certain measurement position behind the head respectively.
2. The isothermal extrusion method of an aluminum alloy profile according to claim 1, characterized in that: The steps include: S1, measuring the initial heating temperature of the aluminum alloy cast rod to be extruded at the beginning of extrusion; S2, selecting each measurement position according to the setting requirements, taking the metallographic sample of the profile at each measurement position, measuring the average size of the subgrains of the microstructure of the profile at each measurement position, and calculating the Z parameter of the profile structure at each measurement position; S3, selecting a certain measuring position at the head and the back of the profile, and obtaining the lnZ function relationship of the profile deformation at the head and the back of the profile according to the relationship between the Z parameter, the deformation rate and the temperature; S4, repeat the calculation process of step S3 to obtain the mold outlet temperature of the profile at other measurement positions; S5, comparing the die outlet temperature of the profile at each measuring position with the initial heating temperature at the beginning of extrusion to obtain the temperature increase value at each measuring position; S6, calculating the gradient heating temperature of the cast rod according to the temperature increase value and the preset profile extrusion temperature.
3. The isothermal extrusion method of an aluminum alloy profile according to claim 2, characterized in that: In S2, EBSD metallographic observation samples are prepared for the cross-section of the profile structure at each measuring position, and the average size of subgrains in the microstructure of the profile at each measuring position is measured.
4. An isothermal extrusion method for aluminum alloy profiles, characterized in that: The steps include: S1, measuring the initial heating temperature of the aluminum alloy cast rod to be extruded at the beginning of extrusion; S2, selecting each measurement position according to the setting requirements, taking the metallographic sample of the profile at each measurement position, measuring the average size of the subgrains of the microstructure of the profile at each measurement position, and calculating the Z parameter of the profile structure at each measurement position; S3, select a certain measuring position at the head and the back of the profile, and obtain the lnZ function relationship of the profile deformation at a certain measuring position at the head and the back of the profile according to the relationship between the Z parameter, the deformation rate and the temperature: The die outlet temperature of the profile at a certain measuring position behind the head is calculated, where Q is the deformation activation energy / J / mol, R is the gas constant, R=8.341 / J / (mol·K), T is the deformation temperature / K, T F is the initial heating temperature of the profile, T R is the mold outlet temperature at a certain measurement position after the head, Z F and Z R They are the Z parameters of the profile head and a certain measurement position behind the head; S4, repeat the calculation process of step S3 to obtain the mold outlet temperature of the profile at other measurement positions; S5, comparing the die outlet temperature of the profile at each measuring position with the initial heating temperature at the beginning of extrusion to obtain the temperature increase value at each measuring position; S6, calculating the gradient heating temperature of the cast rod according to the temperature increase value and the preset profile extrusion temperature.
5. The isothermal extrusion method of an aluminum alloy profile according to claim 4, characterized in that: In S3, the Z parameter of the profile structure at each measurement position is calculated by the following formula: lnZ=A+Bδ -1 Where A and B are material constants, and δ is the average subgrain size.
6. The isothermal extrusion method of an aluminum alloy profile according to claim 4, characterized in that: In S4, the lnZ function relationship of the profile deformation at the head of the profile and a certain measuring position behind the head is obtained by the following formula of the relationship between the Z parameter, the deformation rate and the temperature: in, is the strain rate / s -1 .
7. The isothermal extrusion method of an aluminum alloy profile according to claim 4, characterized in that: In S4, the ZF parameter of the profile head during the extrusion process and the ZF parameter of the extruded profile at a certain measuring position after the head are R The relationship between the parameters is:
8. The isothermal extrusion method of an aluminum alloy profile according to claim 4, characterized in that:In S2, EBSD metallographic observation samples are prepared for the cross-section of the profile structure at each measuring position, and the average size of subgrains in the microstructure of the profile at each measuring position is measured.
Citation Information
Patent Citations
Method for controlling speed regulation of isothermal extrusion of industrial aluminum profiles for transportation
CN102049426A
Isothermal extrusion processing method of square pipe aluminum alloy section
CN104959395A
Isothermal extrusion process based on temperature segmented control
CN105945081A
Production method of railway vehicle electrical cabinet aluminum profile
CN106623465A
Aluminum section bar equal-temperature extrusion system and extrusion method thereof
CN106694595A