Fluorine-containing positive electrode active material for lithium secondary battery and lithium secondary battery containing the same
By introducing fluorine and heat treatment into the positive electrode active material of lithium secondary battery, layered structures and ordered crystals are formed, the side reaction problems caused by high nickel content are solved, and battery performance with high capacity and long cycle life is achieved.
Patent Information
- Application Number
- CN202080089922.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-12-26
- Filing Date
- 2020-12-24
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2040-12-24
AI Technical Summary
The existing positive electrode active materials of lithium secondary batteries have high nickel content during the circulation process, resulting in side reactions, resulting in deterioration of cycle life characteristics and reduced capacity.
By introducing fluorine into the positive electrode active material, the oxidation number of nickel is controlled, and a layered structure and an ordered crystal structure are formed, the side reaction between the electrolyte and the positive electrode is suppressed, and the fluorine-containing crystal coating is formed through heat treatment to stabilize lithium The path of movement of ions.
It realizes that while maintaining high discharge capacity under high nickel content, it improves cycle life characteristics and structural stability, and extends the service life of the battery.
Smart Images

Figure CN114982008B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a positive electrode active material and a lithium secondary battery including the same, and more particularly, to a positive electrode active material for a lithium secondary battery having improved cycle life and capacity characteristics by including fluorine, and a lithium secondary battery including the same. Background Art
[0002] With the development of portable mobile electronic devices such as smart phones, MP3 players and tablet personal computers, the demand for secondary batteries that can store electrical energy has exploded. In particular, with the emergence of portable devices that require high energy density, medium and large energy storage systems, and electric vehicles, the demand for lithium secondary batteries is increasing.
[0003] As the demand for such lithium secondary batteries increases, research and development of positive electrode active materials for lithium secondary batteries have been conducted. For example, Korean Patent Application Publication No. 10-2014-0119621 (Korean Patent Application No. 10-2013-0150315) discloses a secondary battery having high voltage capacity and long cycle life characteristics due to controlling the type and composition of alternative metals in a precursor for preparing a lithium-rich positive electrode active material and controlling the type and amount of added metals. Summary of the invention
[0004] Technical issues
[0005] An object of the present invention is to provide a fluorine-containing positive electrode active material for a lithium secondary battery having high capacity and improved cycle characteristics while containing a large amount of nickel, and a lithium secondary battery containing the same.
[0006] Another object of the present invention is to provide a fluorine-containing positive electrode active material for a lithium secondary battery and a lithium secondary battery comprising the same, wherein the fluorine-containing positive electrode active material has a layered structure that has enhanced structural stability due to control of the oxidation number of nickel by adding fluorine and shows low capacity drop even after long-term cycling.
[0007] The objects to be achieved by the present invention are not limited to the above objects.
[0008] Technical Solution
[0009] In order to achieve the above object, the present invention provides a fluorine-containing positive electrode active material for a lithium secondary battery and a lithium secondary battery comprising the same.
[0010] According to one embodiment, a positive electrode active material for a lithium secondary battery has a layered structure and contains lithium, a transition metal, fluorine (F), and oxygen, wherein the layered structure includes a lithium layer consisting only of lithium and a transition metal layer consisting only of a transition metal including nickel, wherein nickel includes Ni in terms of oxidation number. 3+ and Ni 2+ , and Ni 2+ with Ni 3+ The ratio (Ni 2+ / Ni 3 + ) increases with the increase of fluorine content.
[0011] In one embodiment, the layered structure may further include a first mixed layer and a second mixed layer each containing lithium and a transition metal, wherein the lithium content in the first mixed layer may be higher than the transition metal content, and the transition metal content in the second mixed layer may be higher than the lithium content.
[0012] In one embodiment, the first mixed layer and the second mixed layer in the positive electrode active material can be stacked adjacent to each other and repeated alternately and regularly to form a layered structure, and the first mixed layer and the second mixed layer stacked adjacent to each other can be configured so that the transition metal of the first mixed layer and the lithium of the second mixed layer can correspond to each other.
[0013] In one embodiment, the first mixed layer and the second mixed layer stacked adjacent to each other may have an ordered structure, wherein the ordered structure may be formed so that the n1 lithium ions and n2 transition metal ions of the first mixed layer may correspond to the n1 transition metal ions and n2 lithium ions of the second mixed layer, respectively (wherein n1 and n2 are the same or different natural numbers), and the unit cell formed by the ordered structure may include a long-range ordered lattice with an increased a-axis lattice constant.
[0014] In one embodiment, a lattice formed by the first mixed layer and the second mixed layer stacked adjacent to each other may include a super lattice having an a-axis twice as long as a lattice formed by the lithium layer and the transition metal layer.
[0015] In one embodiment, the peak (I) of the (003) plane in the X-ray diffraction spectrum of the positive electrode active material obtained by XRD analysis using CuKα radiation after the electrochemical reaction is (003) ) and the peak value (I (104) ) ratio (I (003) / I (104) ) can be reduced by less than 1%.
[0016] In one embodiment, the peak value (I (003) ) and the peak value (I (104)) ratio (I (003) / I (104) ) can be 1.71 or less.
[0017] In one embodiment, in an XPS spectrum of Ni2P obtained by X-ray photoelectron spectroscopy (XPS), Ni 2+ The peak area can be larger than Ni 3+ The peak area of Ni 2+ with Ni 3+ The ratio (Ni 2 + / Ni 3+ ) can be from 49% to 130%.
[0018] In one embodiment, at a binding energy of 850 eV to 860 eV, Ni 2+ The peak area of Ni 3+ The ratio of the peak areas can be from 0.49:1 to 1.3:1.
[0019] In one embodiment, the positive electrode active material may include secondary particles consisting of a group of a plurality of primary particles, and at least one of the primary particles may include a fluorine-containing grain coating at a grain boundary between the primary particles.
[0020] In one embodiment, the positive electrode active material may be represented by the following Formula 1:
[0021] [Formula 1]
[0022] Li 1-x M 1-y [Li x M y ]O 2-z F z
[0023] wherein x+y=1; 0.005≤z≤0.02; and M is any one of the following: Ni; Ni and Co; Ni and Mn; Ni, Co and Mn; Ni and Al; Ni, Co and Al; Ni, Mn and Al; and Ni, Co, Mn and Al.
[0024] In one embodiment, Ni 2+ with Ni 3+ The ratio (Ni 2+ / Ni 3+ ) can be reduced as the nickel content in Formula 1 increases.
[0025] In one embodiment, the layered structure may also include a first mixed layer and a second mixed layer, each containing lithium and a transition metal; the lithium content in the first mixed layer is higher than the transition metal content, and the transition metal content in the second mixed layer is higher than the lithium content; the first mixed layer and the second mixed layer in the positive electrode active material are stacked adjacent to each other and repeated alternately and regularly to form a layered structure; and the electron diffraction pattern of the
[010] zone axis or the
[100] zone axis of the layered structure may show: a first diffraction spot group, in which one or more diffraction spots having a first intensity and corresponding to the lattice formed by the lithium layers and the transition metal layers stacked adjacent to each other are aligned in one direction; and a second diffraction spot group, in which one or more diffraction spots having a second intensity lower than the first intensity of the diffraction spots of the first diffraction group and corresponding to the lattice formed by the first mixed layer and the second mixed layer stacked adjacent to each other are aligned in one direction.
[0026] In one embodiment, the first diffraction spot group and the second diffraction spot group may be arranged alternately and regularly with each other, and the first diffraction spot group and the second diffraction spot group may be spaced apart from each other.
[0027] In one embodiment, the layered structure may also include a first mixed layer and a second mixed layer, each containing lithium and a transition metal, wherein the lithium content in the first mixed layer may be higher than the transition metal content, the transition metal content in the second mixed layer may be higher than the lithium content, the lithium and the transition metal in the first mixed layer may be arranged alternately, the transition metal and lithium in the second mixed layer may be arranged alternately, and the lattice formed by the first mixed layer and the second mixed layer stacked adjacent to each other may include a superlattice.
[0028] In one embodiment, the transition metal includes any one or more of nickel (Ni), manganese (Mn), and cobalt (Co), wherein the oxidation number of nickel is 2+ and 3+, and the oxidation number of manganese is 3+ or 4+, and the oxidation number of cobalt can be 3+.
[0029] In one embodiment, the primary particle may include a rod-shaped particle formed in a plate-like shape having a major axis and a minor axis in cross section, and the rod-shaped particle may be oriented such that the major axis thereof faces a central portion of the secondary particle.
[0030] In one embodiment, the transition metal may include any one or more of nickel (Ni), manganese (Mn) and cobalt (Co), wherein at least one of the transition metals may have a concentration gradient in at least a portion of the secondary particle from the center of the secondary particle toward its surface.
[0031] In one embodiment, nickel (Ni) may be included in an amount of 70 mol % or more.
[0032] According to another aspect of the present invention, one embodiment of the present invention includes a lithium secondary battery, which includes: a positive electrode, the positive electrode comprising the above-mentioned positive electrode active material for a lithium secondary battery; a negative electrode, the negative electrode facing the positive electrode and composed of graphite or lithium metal; an isolation member between the positive electrode and the negative electrode; and an electrolyte solution or a solid electrolyte containing a lithium salt.
[0033] Beneficial Effects
[0034] According to the present invention as described above, a fluorine-containing positive electrode active material for a lithium secondary battery and a lithium secondary battery containing the same can be provided, wherein the fluorine-containing positive electrode active material has a high nickel content and has improved cycle life characteristics due to suppression of side reactions between an electrolyte and the positive electrode active material while maintaining a high discharge capacity.
[0035] In addition, according to the present invention, a fluorine-containing positive electrode active material for a lithium secondary battery and a lithium secondary battery containing the same can be provided, wherein the fluorine-containing positive electrode active material has a layered structure and a new crystal structure maintained during long-term cycles while having a high nickel content (Ni-rich) and thus has improved stability and reliability. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] Figure 1 A secondary particle according to one embodiment of the present invention is schematically shown.
[0037] Figure 2 is a schematic cross-sectional view of a positive electrode active material according to one embodiment of the present invention.
[0038] Figure 3 The movement of lithium ions in a positive electrode active material according to one embodiment of the present invention is schematically shown.
[0039] Figure 4 Schematically showing images of the positive electrode active material before and after addition of fluorine and heat treatment according to Example 1 of the present invention (a and b) and the ordered structure of the positive electrode active material formed by addition of fluorine (c).
[0040] Figure 5 Graphs showing the electrochemical capacity (a) and cycle-life characteristics (b) of button cells employing the positive electrode active materials of Examples 1 to 3 according to the present invention and Comparative Example 1 are depicted.
[0041] Figure 6 is a graph showing the resistance of button cells using the positive electrode active materials of Comparative Example 1 and Example 2 according to the present invention.
[0042] Figure 7Graphs showing the cycle characteristics and resistance versus SOC of full cells employing the positive electrode active materials of Comparative Example 1 and Example 2 according to the present invention are depicted.
[0043] Figure 8 A TEM image showing the ordered structure of the positive electrode active material according to Example 2 after 2000 cycles is shown.
[0044] Fig. 9 A TEM image showing the ordered structure of the positive electrode active material according to Example 2 after 5000 cycles is shown.
[0045] Fig.10 The results of XRD analysis for examining the c-axis length and the a-axis length of the positive electrode active materials according to Comparative Example 1 and Example 2 after cycling are shown.
[0046] Fig.11 A graph (a) showing a peak on the (003) plane and a peak on the (104) plane in the positive electrode active material according to Example 2 and a graph (b) showing a ratio between the peaks are depicted.
[0047] Fig.12 XRD patterns according to Example 2, Example 3, Comparative Example 1, and Comparative Example 2 are shown.
[0048] Fig.13 XPS charts according to Example 2, Example 3, Comparative Example 1, and Comparative Example 2 are shown.
[0049] Fig.14 Selected-area electron diffraction (SAED) patterns of the
[010] zone axis according to Comparative Example 1 and Example 2 are shown.
[0050] Fig.15 High-angle annular dark field (HAADF) images of the
[010] zone axis according to Comparative Example 1 and Example 2 are shown. DETAILED DESCRIPTION
[0051] Hereinafter, preferred embodiments of the present invention will be described in detail with reference to the accompanying drawings. However, the technical spirit of the present invention is not limited to the embodiments disclosed herein, and may be embodied in other forms. On the contrary, the embodiments disclosed herein are provided so that the present disclosure will be thorough and complete, and the spirit of the present invention will be fully conveyed to those skilled in the art.
[0052] Throughout this specification, when any component is referred to as being "on" another component, this refers not only to the case where the component is directly on another component, but also to the case where a third component exists between the two components. In addition, in the drawings, in order to effectively describe the technical content, the thickness of the film and the region are exaggerated.
[0053] In addition, in different embodiments of this specification, terms such as first, second, third, etc. are used to describe different components, but these components should not be limited by these terms. These terms are only used to distinguish any component from another component. Therefore, the component referred to as the first component in any embodiment may also be referred to as the second component in other embodiments. Each embodiment described and illustrated herein also includes its supplementary embodiment. In addition, as used herein, the term "and / or" includes at least one of the related enumerated items.
[0054] In this specification, unless otherwise specified in its context, singular expressions include plural expressions. The terms "comprise", "include", "have", etc. are intended to indicate the presence of the mentioned features, numbers, steps, components, or combinations thereof, but do not exclude the possibility of the presence or addition of one or more other features, numbers, steps, components, or combinations thereof.
[0055] In the following description, when related known functions or configurations may obscure the subject matter of the present invention, a detailed description thereof will be omitted.
[0056] In addition, in the present specification, the expression "the proportion of the first crystal structure in a specific part is higher than the proportion of the second crystal structure" means that the specific part includes both the first crystal structure and the second crystal structure, and not only means that the proportion of the first crystal structure in the specific part is higher than the proportion of the second crystal structure, but also means that the specific part only has the first crystal structure.
[0057] Furthermore, in the present specification, the crystal system may be composed of the following seven systems: triclinic system, monoclinic system, orthorhombic system, tetragonal system, trigonal or rhombohedral system, hexagonal system, and cubic system.
[0058] Furthermore, in the present application, “mol %” is interpreted as meaning the content of any metal in the positive electrode active material or the positive electrode active material precursor based on 100% of the sum of metals other than lithium and oxygen in the positive electrode active material or the positive electrode active material precursor.
[0059] Figure 1 A secondary particle according to one embodiment of the present invention is schematically shown. Figure 2 is a schematic cross-sectional view of a positive electrode active material according to one embodiment of the present invention. Figure 3The movement of lithium ions in a positive electrode active material according to one embodiment of the present invention is schematically shown.
[0060] Reference Figures 1 to 3 , a positive electrode active material according to an embodiment of the present invention may include a secondary particle 100 having an approximately spherical shape. The secondary particle 100 may be divided into a central portion 10 and a surface portion 20, and may be formed by aggregation of a plurality of primary particles 30. The primary particles 30 may form a layered structure.
[0061] In the secondary particle 100, the primary particles 30 constituting the central portion 10 and the primary particles 30 constituting the surface portion 20 may have the same or different sizes, and the primary particles 30 constituting the surface portion 20 may be arranged in a shape having a major axis and a minor axis, and at least a portion of the primary particles 30 constituting the surface portion 20 may be oriented toward the central portion 10 of the secondary particle 100. At least a portion of the primary particles 30 constituting the surface portion 20 may be arranged in a radial form.
[0062] The secondary particle 100 may be composed of one or more metals including lithium, and at least a portion of the one or more metals may be configured to have a concentration gradient in the central portion 10 and the surface portion 20. Alternatively, in the secondary particle 100, a gap may be formed between the central portion 10 and the surface portion 20, or the crystal form between the central portion 10 and the surface portion 20 may be different, or an image difference between the central portion 10 and the surface portion 20 may be created by manufacturing the central portion 10 and then making the surface portion 20 surround the central portion 10. Therefore, the secondary particle may be configured in a core-shell form.
[0063] The primary particle 30 may extend radially from an area in the secondary particle toward the surface portion 20 of the secondary particle. The area in the secondary particle may be the central portion 10 of the secondary particle. In other words, at least a portion of the primary particle 30 may include a rod-shaped particle formed into a sheet-like shape. The rod-shaped particle may be oriented so that its major axis faces the central portion of the secondary particle.
[0064] A moving path of metal ions (e.g., lithium ions) and electrolyte can be provided between the primary particles 30, that is, between the primary particles 30 extending in the direction D from the central portion 10 of the secondary particle toward the surface portion 20 thereof. Therefore, the positive electrode active material according to one embodiment of the present invention can improve the charging and discharging efficiency of the secondary battery.
[0065] According to one embodiment, in the direction from the center 10 of the secondary particle toward the surface 20 of the secondary particle, the length of the primary particle 30 relatively adjacent to the surface 20 of the secondary particle may be longer than that of the primary particle 30 relatively adjacent to the center portion 10 of the secondary particle. In other words, in at least a portion of the secondary particle extending from the center portion 10 of the secondary particle to the surface 20, the length of the primary particle 30 may increase toward the surface 20.
[0066] Figure 4 Schematically showing images of a positive electrode active material before and after addition of fluorine and heat treatment according to one embodiment of the present invention (a and b) and an ordered structure of the positive electrode active material formed by addition of fluorine (c).
[0067] One embodiment of the present invention includes a positive electrode active material for a lithium secondary battery having a layered structure and comprising lithium, a transition metal, fluorine (F), and oxygen, wherein the layered structure includes a lithium layer consisting only of lithium and a transition metal layer consisting only of a transition metal including nickel. In terms of oxidation number, nickel may include Ni 3+ and Ni 2+ , and Ni 2+ with Ni 3+ The ratio (Ni 2+ / Ni 3+ ) may increase as the fluorine content increases. A fluorine-containing positive electrode active material for a lithium secondary battery may be prepared by preparing a metal composite hydroxide using a transition metal containing nickel, mixing the metal composite hydroxide with a lithium compound to prepare a sintered body, and mixing the sintered body with a fluorine compound, followed by heat treatment. For example, in the positive electrode active material, nickel (Ni) may be included in an amount of 70 mol% or more.
[0068] Generally, in nickel-rich layered positive electrode active materials having a nickel content of 70 mol% or more, high capacity can be achieved by nickel, but there is a problem that side reactions occur with the electrolyte on the surface of the positive electrode active material during the cycle, and the resulting by-products deteriorate the cycle life characteristics.
[0069] Such side reactions lead to unnecessary electrolyte consumption, thereby depleting the electrolyte in the lithium secondary battery, and byproducts composed of organic materials accumulate on the electrode surface, thereby reducing the coulombic efficiency of the lithium secondary battery and causing instability. In addition, during the charging and discharging process, the byproducts may cause the crystal structure of the particles of the positive electrode active material to deteriorate, thereby degrading the cycle life characteristics. In particular, in nickel-rich positive electrode active materials, byproducts lead to inhibition of the H2 to H3 phase transition, resulting in rapid degradation of the cycle life characteristics.
[0070] On the other hand, in the case of the positive electrode active material according to this embodiment, the oxidation number of nickel can be controlled by adding fluorine and heat treatment. Specifically, Ni 2+ with Ni 3+ The ratio (Ni 2+ / Ni 3+ ) can increase with the increase of fluorine content.
[0071] The positive electrode active material may have a layered structure, wherein the layered structure may include a first mixed layer and a second mixed layer each containing lithium and a transition metal, in addition to a lithium layer composed only of lithium and a transition metal layer composed only of a transition metal. The content of lithium in the first mixed layer may be higher than the content of the transition metal, the content of the transition metal in the second mixed layer may be higher than the content of lithium, and the nickel contained in the first mixed layer may be nickel (Ni) with a specific oxidation number of +3. 3+ ) includes nickel (Ni 2+ ), and specifically, only nickel (Ni 2+ )composition.
[0072] The positive electrode active material may include secondary particles composed of a plurality of primary particles, and at least one of the primary particles may include a fluorine-containing grain coating at the grain boundary between the primary particles. A metal composite hydroxide containing a transition metal is mixed with a lithium compound and then prepared into a sintered body, and the prepared sintered body is mixed with a fluorine compound using a ball mill or the like. Thus, the surface of the sintered body is coated with a fluorine compound (F) (see Figure 4 Then, when the sintered body is heat-treated at 300° C. to 700° C., specifically about 400° C., the fluorine compound applied to the surface of the sintered body may be uniformly diffused into the sintered body and may be formed as a grain coating at the grain boundary between primary particles.
[0073] After the sintered body is mixed with the fluorine compound, heat treatment may be performed at 300° C. to 700° C. If the heat treatment is performed at less than 300° C., the fluorine compound may be difficult to uniformly diffuse into the sintered body, and if the heat treatment is performed at more than 700° C., the electrochemical properties of the positive electrode active material may deteriorate.
[0074] The primary particles on which the grain coating is formed can prevent the occurrence of side reactions with the electrolyte at the boundaries between the primary particles even after long-term cycling, thereby maintaining the lithium ion movement path (Li + The primary particles can prevent the occurrence of side reactions with the electrolyte during the charge / discharge process and prevent the layered structure from being transformed into a cubic crystal structure during the charge / discharge process. For example, the primary particles on which the fluorine-containing grain coating is formed can include rod-shaped particles.
[0075] In the positive electrode active material in which a grain coat layer is formed on at least a portion of primary particles by adding fluorine and heat treatment, Ni 2+ with Ni 3+ The ratio (Ni 2+ / Ni 3+ ) can be increased. + The ionic radius is Ni 2+ The ionic radius is And Ni 3+ The ionic radius is or greater. 2+ The ionic radius of Li + The ionic radius of Ni 3+ In comparison, Ni 2+ In probability, it is favorable to + In addition, in this embodiment, by controlling the addition of fluorine and the heat treatment, the sites of lithium ions and nickel ions can be regularly moved toward each other, thereby providing a positive electrode active material having a value extended to a new lattice constant. In the positive electrode active material, Ni can be increased by adding fluorine and heat treatment. 2+ with Ni 3+ The ratio (Ni 2+ / Ni 3+ ), and the first mixed layer and the second mixed layer can be formed by site exchange between lithium in the initial lithium layer and nickel in the transition metal layer.
[0076] For example, the first mixed layer may be formed by regular site exchange between lithium in a layer consisting only of lithium and nickel in an adjacent layer consisting only of transition metals. In this case, the nickel moved to the first mixed layer may be Ni 2+ . 2+ with Ni 3+ The ratio (Ni 2+ / Ni 3+ ) can be controlled by adding fluorine and heat treatment. 2+ with Ni 3+ The ratio (Ni 2+ / Ni 3+ ) is higher than a predetermined level, the first mixed layer and the second mixed layer adjacent to each other can be Li + with Ni 2+ or Ni 3+ The regular site exchange between lithium and nickel is not an irregular mixture (cation mixing). + with Ni 2+ The regular site exchange between Li+ with Ni 3+ The regular site exchange between + Can be with you 2+ The first mixed layer can be formed by providing Ni at the lithium site in the layer composed only of lithium. 2+ The second mixed layer can be formed by providing Li at the nickel site in the layer composed of only the transition metal containing nickel. + And formed.
[0077] In the positive electrode active material, the first mixed layer and the second mixed layer may be stacked adjacent to each other and alternately and regularly repeated to form a layered structure, and the first mixed layer and the second mixed layer stacked adjacent to each other may be arranged so that the transition metal of the first mixed layer and the lithium of the second mixed layer correspond to each other. Specifically, the first mixed layer and the second mixed layer stacked adjacent to each other may be arranged so that the transition metal of the first mixed layer and the lithium of the second mixed layer correspond to each other.
[0078] More specifically, the first mixed layer and the second mixed layer stacked adjacent to each other may have a cation ordered structure, wherein the cation ordered structure may be formed such that n1 lithium ions and n2 transition metal ions of the first mixed layer may correspond to n1 transition metal ions and n2 lithium ions of the second mixed layer, respectively (wherein n1 and n2 are the same or different natural numbers).
[0079] The unit cell formed by the ordered structure may include a long-range ordered lattice with an increased a-axis lattice constant. The lattice formed by the first mixed layer and the second mixed layer stacked adjacent to each other may include a superlattice whose a-axis is twice as long as the a-axis of the lattice formed by the lithium layer and the transition metal layer.
[0080] In the positive electrode active material according to the embodiment, the fluorine-containing grain coating layer and the ordered structure formed by the addition of fluorine and the heat treatment can suppress the side reaction at the interface between the positive electrode active material and the electrolyte.
[0081] In addition, the grain coating can further improve the electrochemical performance during the charge / discharge process by making the interface between primary particles more stable. In addition, the ordered structure can maximize the lattice stability so that the crystallinity and lattice structure can be stably maintained even in repeated charge and discharge cycles.
[0082] The positive electrode active material can be represented by the following Formula 1:
[0083] [Formula 1]
[0084] Li1-xM 1-y [Li x M y ]O2-z F z
[0085] wherein x+y=1; 0.005≤z≤0.02; M is Ni; Ni and Co; Ni and Mn; and any one of Ni, Co and Mn.
[0086] In formula 1, Li 1-x It can represent a lithium layer composed only of lithium, M 1-y It can represent a transition metal layer consisting only of transition metals, [Li x M y ] can represent the first mixed layer and the second mixed layer.
[0087] In formula 1, Ni 2+ with Ni 3+ The ratio (Ni 2+ / Ni 3+ ) can decrease with the increase of nickel content. In addition, Ni 2+ with Ni 3+ The ratio (Ni 2+ / Ni 3+ ) can increase with the fluorine content.
[0088] The transition metal may include at least one of nickel (Ni), manganese (Mn), and cobalt (Co), wherein the oxidation number of nickel may be 2+ and 3+, the oxidation number of manganese may be 3+ or 4+, and the oxidation number of cobalt may be 3+.
[0089] The transition metal includes any one or more of nickel (Ni), manganese (Mn) and cobalt (Co), wherein at least one of the transition metals may have a concentration gradient from the center toward the surface of the secondary particle in at least a portion of the secondary particle.
[0090] Specifically, at least one of the transition metals may be provided with a concentration gradient from the central portion to the surface portion of the secondary particle, or may be provided with a concentration gradient from the center of the secondary particle to a predetermined portion of the secondary particle and provided at a constant concentration from the predetermined portion of the secondary particle to the surface, or may be provided at a constant concentration from the center of the secondary particle to a predetermined portion thereof and provided with a concentration gradient from the predetermined portion to the surface of the secondary particle.
[0091] The positive electrode active material may include secondary particles consisting of a group of multiple primary particles, wherein the secondary particles may include microcracks extending from the outermost surface of the secondary particles to the inside of the secondary particles, and the microcracks are channels through which the electrolyte penetrates the secondary particles. In a secondary battery using a positive electrode active material, the secondary particles can maintain 80% or more of the initial specific capacity after 5000 charge / discharge cycles at a discharge rate of 1C. That is, the positive electrode active material according to this embodiment can maintain 80% or more of the initial specific capacity after long-term cycling, for example, 2000 cycles or 5000 cycles. In this case, even if the electrolyte penetrates the inside of the positive electrode active material, due to the high stability (crystallinity) of the grain coating on the primary particles constituting the positive electrode active material, no side reaction occurs. This is because, although the positive electrode active material according to this embodiment may generate microcracks during long-term cycling, even when the electrolyte penetrates the secondary particles through the microcracks, problems such as overall collapse of the secondary particles will not occur.
[0092] The positive electrode active material according to one embodiment of the present invention may be a secondary particle composed of a plurality of primary particles, wherein the secondary particle may have an approximately spherical shape. The primary particle is oriented from the central portion of the secondary particle toward its surface portion, and the shape of the primary particle in the central portion may be different from the shape of the primary particle in the surface portion.
[0093] After many cycles, microcracks may form in the spaces between primary particles in the secondary particles of the positive electrode active material.
[0094] Generally, in a positive electrode active material in which the cross-sectional area of microcracks is 20% or more, the electrolyte penetrates the center of the secondary particles during charge and discharge and causes a side reaction, so that the structure of the primary particles collapses rapidly, causing its capacity to decrease during cycling.
[0095] On the other hand, when the cross-sectional area of the microcracks in the positive electrode active material according to the embodiment is 20% or more, in a secondary battery using the positive electrode active material, after 5000 charge / discharge cycles at a discharge rate of 1C, the positive electrode active material can maintain 80% or more of the initial specific capacity and can exhibit excellent cycle characteristics. That is, the positive electrode active material according to the embodiment of the present invention can prevent the penetration of the electrolyte due to the grain coating and the ordered structure even when microcracks are formed, and even when the electrolyte penetrates the positive electrode active material, it can exhibit excellent characteristics without reducing the capacity due to the ordered structure with low reactivity with the electrolyte due to high crystallinity (stability).
[0096] According to another aspect of the present invention, one embodiment of the present invention includes a lithium secondary battery, which includes: a positive electrode, the positive electrode comprising the above-mentioned positive electrode active material; a negative electrode, the negative electrode facing the positive electrode and composed of graphite or lithium metal; an isolation member between the positive electrode and the negative electrode; and an electrolyte solution or a solid electrolyte containing a lithium salt.
[0097] According to another aspect of the present invention, an embodiment of the present invention may include a method for preparing a positive electrode active material for a lithium secondary battery comprising an ordered structure substituted with lithium and a transition metal, the method comprising the following steps: preparing a metal composite hydroxide with a transition metal by a coprecipitation method; preparing a sintered body by sintering the metal composite hydroxide with a lithium compound; mixing the sintered body with a fluorine compound, and then heat treating it at 300°C to 700°C.
[0098] The transition metal may include nickel (Ni).
[0099] In the step of preparing the sintered body, the metal composite hydroxide may be pre-sintered at a certain temperature and then sintered at a temperature higher than the pre-sintering temperature.
[0100] Subsequently, the sintered body may be mixed with a fluorine compound such as ammonium fluoride (NH4F), and then heat-treated at 300°C to 700°C to form a fluorine-containing grain coating on at least a portion of the surface of the sintered body. The positive electrode active material may include secondary particles composed of a group of primary particles and having an approximately spherical shape, and the grain coating may be formed on at least one of the primary particles at a grain boundary between the primary particles.
[0101] The sintered body and the fluorine compound may be mixed together using a ball mill at room temperature before the heat treatment. By mixing the sintered body and the fluorine compound under pressure using a ball mill, the fluorine compound may be diffused into the sintered body after the heat treatment.
[0102] Hereinafter, examples of the present invention and comparative examples will be described. However, the following examples are merely preferred examples of the present invention, and the scope of the present invention is not limited by the following examples.
[0103] 1. Preparation of Positive Electrode Active Materials
[0104] Example 1 (F0.5-concentration gradient type NCM80)
[0105] 10 liters of distilled water were placed in a coprecipitation reactor (volume: 40 liters), and then N2 gas was supplied to the reactor at a rate of 6 liters / minute, and stirred at 350rpm while the reactor temperature was maintained at 40°C. Nickel sulfate aqueous solution (NiSO4·6H2O, Samchun Chemicals), cobalt sulfate aqueous solution (CoSO4·7H2O, Samchun Chemicals) and manganese sulfate aqueous solution (MnSO4·H2O, Samchun Chemicals) were mixed together to prepare a 2M metal solution so that the molar ratio between nickel (Ni), cobalt (Co) and manganese (Mn) was 80:5:15. The prepared 2M metal solution and 16M ammonia solution (NH4OH, JUNSEI) were continuously introduced into the reactor at a rate of 0.561 liters / hour and 0.08 liters / hour, respectively. During the coprecipitation reaction, the pH in the reactor was checked and the pH was maintained at 11.4 by adding NaOH (aq.) solution to the reactor.
[0106] A coprecipitation reaction was carried out in a reactor, during which nanoparticle hydroxide was first formed, and then nickel-cobalt-manganese-tungsten hydroxide slowly accumulated on the surface of the nanoparticle hydroxide to form a micron-sized precursor. Next, the prepared precursor was washed with distilled water several times, filtered through a filter, and dried in a drying oven at 110°C for 12 hours to obtain [Ni 0.80 Co 0.05 Mn 0.15 ](OH)2 metal complex hydroxide.
[0107] The obtained [Ni 0.80 Co 0.05 Mn 0.15 ](OH)2 metal composite hydroxide and LiOH·H2O were uniformly mixed together so that the molar ratio of Li:(Ni+Co+Mn) was 1.01:1. Then, the mixture was sintered at 770°C for 10 hours to obtain Li[Ni 0.80 Co 0.05 Mn 0.15 Then, the sintered body was mixed with ammonium fluoride (NH4F) and then heat-treated at 400°C to obtain a positive electrode active material powder containing 0.5 mol% of fluorine.
[0108] Example 2 (F1-concentration gradient type NCM80)
[0109] A positive electrode active material powder was obtained in the same manner as in Example 1, except that the sintered body was mixed with ammonium fluoride (NH4F) and then heat-treated at 400°C so that it contained 1 mol% of fluorine.
[0110] Example 3 (F2-concentration gradient type NCM80)
[0111] A positive electrode active material powder was obtained in the same manner as in Example 1, except that the sintered body was mixed with ammonium fluoride (NH4F) and then heat-treated at 400°C so that it contained 2 mol% of fluorine.
[0112] Comparative Example 1 (Concentration Gradient NCM80)
[0113] In the same manner as in Example 1, a sintered body of Li[Ni 0.80 Co 0.05 Mn 0.15 ]The positive electrode active material powder composed of MgO2 is different in that the process of mixing the sintered body with ammonium fluoride (NH4F) and heat treating the mixture is omitted.
[0114] Comparative Example 2 (F10-concentration gradient type NCM80)
[0115] A positive electrode active material powder was obtained in the same manner as in Example 1, except that the sintered body was mixed with ammonium fluoride (NH4F) and then heat-treated at 400°C so that it contained 10 mol% of fluorine.
[0116] The contents of Examples 1 to 3, Comparative Example 1 and Comparative Example 2 are shown in Table 1 below.
[0117] [Table 1]
[0118] distinguish Metal complex hydroxide F content Example 1 Gradient NCM = 80:5:15 0.5mol% Example 2 Gradient NCM = 80:5:15 1mol% Example 3 Gradient NCM = 80:5:15 2mol% Comparative Example 1 Gradient NCM = 80:5:15 0 Comparative Example 2 Gradient NCM = 80:5:15 10mol%
[0119] 2. Preparation of half-cells and full-cells using the examples and comparative examples
[0120] Half cells and full cells were fabricated using the positive electrode active materials according to the above-described Examples and Comparative Examples.
[0121] In order to manufacture half-cells and full cells, the powdered positive electrode active material prepared according to each of the embodiments and comparative examples, poly(vinylidene fluoride) and carbon black were added to N-methylpyrrolidone (0.4 g per g of positive electrode active material) at a weight ratio of 90:4.5:5.5, and then uniformly mixed together to prepare positive electrode slurries. Aluminum foil was coated with each of the prepared positive electrode slurries, rolled, and then dried under vacuum to prepare positive electrodes.
[0122] To manufacture a half-cell using the prepared positive electrode active material, an aluminum foil was coated with each of the prepared positive electrode active material slurries so that the loading level of the positive electrode active material was 5 mg / cm 2 (Meaning that when a sample of 1 cm is taken from the aluminum foil coated with the positive electrode active material 2The positive electrode was prepared by uniformly dissolving 2 wt% of vinylene carbonate (VC) and 1.2 mol / L of lithium salt LiPF6 as additives in ethylene carbonate:ethyl methyl carbonate (EC:EMC=3:7 v / v) as a solvent. As a half-cell, a 2032 button-type half-cell (hereinafter referred to as a button cell) using Li metal as a negative electrode was manufactured.
[0123] To manufacture a full battery using the prepared positive electrode active material, an aluminum foil was coated with each of the prepared positive electrode active material slurries so that the loading level of the positive electrode active material was 8.5 mg / cm 2 , thereby preparing a positive electrode. In addition, the prepared graphite slurry was used at 6.5 mg / cm 2 Aluminum foil was coated with a loading level of , rolled, and then dried under vacuum to prepare a negative electrode. The electrolyte used was obtained by uniformly dissolving 2 wt % of vinylene carbonate (VC) as an additive and 1.2 mol / L of lithium salt LiPF6 in ethylene carbonate: ethyl methyl carbonate (EC:EMC=3:7v / v) as a solvent. Each of the positive electrode, separator (Celgard, model 2320) and negative electrode was stacked in a pouch-type battery case and sealed with the prepared electrolyte to manufacture a pouch-type full battery.
[0124] 3. Evaluation of Examples and Comparative Examples
[0125] (1) Evaluation of capacity and cycle characteristics using half-cells
[0126] Each of the fabricated half-cells was subjected to 100 cycle charge / discharge tests by charging to 4.3 V and discharging to 2.7 V at a constant current of 0.5 C (1 C: 180 mA / g) at 30° C., and the recovered capacity (hereinafter referred to as 2.7 V to 4.3 V) was measured.
[0127] (2) Evaluation of capacity and cycle characteristics using full batteries
[0128] The fabricated full cell was cycled between 3.0 V (discharge voltage) and 4.2 V (charge voltage) at 25° C. at a constant current of 1 C, and the capacity and recovered capacity were measured.
[0129] (3) Microstructure analysis of metal composite hydroxides (precursors) and positive electrode active materials using SEM, TEM, XRD, and XPS
[0130] For the positive electrode active materials according to the embodiments and comparative examples and the metal composite hydroxides (precursors) before pre-sintering for forming the positive electrode active materials, the microstructure, crystal structure, etc. were analyzed by SEM (Nova Nano SEM 450, FEI). The positive electrode active material particles were cut and the cross-section of the positive electrode active material was imaged using a transmission electron microscope (TEM).
[0131] X-ray diffraction (XRD) analysis was performed using CuKα radiation as the X-ray diffraction light source. The analysis was performed at a scanning rate of 1° / min in the 2θ value range of 15° to 70° and at a scanning rate of 0.2° / min in the 2θ value range of 19° to 23°.
[0132] XPS analysis of the positive electrode active material was performed using a Quantum 2000 (Physical Electronics) system. XPS analysis was performed using a Quantum 2000 (Physical Electronics. Inc.) (accelerating voltage: 0.5 keV to 15 keV, 300 W, energy resolution: about 1.0 eV, minimum analysis area: 10 microns, sputtering rate: 0.1 nm / min).
[0133] Figure 4 Mapping images of the positive electrode active material according to Example 1 before and after fluorine coating and heat treatment, and a HAADF-TEM image of the ordered structure are shown.
[0134] Figure 5 Depicted are graphs showing the electrochemical capacity (a) and cycle life characteristics (b) of button cells using the positive electrode active materials according to Examples 1 to 3 of the present invention and Comparative Example 1. Table 2 below shows the values of the capacity and cycle life characteristics according to the Examples of the present invention and Comparative Examples.
[0135] [Table 2]
[0136]
[0137] Reference Figure 5From Table 2 above, it can be determined that the overall capacity is maintained even with the addition of fluorine. In addition, it can be determined that Examples 1 to 3 exhibit excellent cycle life characteristics compared to Comparative Example 1 to which fluorine is not added. For example, in the case of a half-cell, the change in 0.1C capacity and 0.5C capacity at a charge and discharge voltage of 2.7V to 4.3V at room temperature (25°C to 30°C) should be reduced by 5% or less relative to Comparative Example 1 to which fluorine is not added. On the other hand, it can be determined that in the case of Comparative Example 2, the capacity characteristics are deteriorated due to the excessively high fluorine content. In the case of Examples 1 to 3, the ordered structure controlled by the addition of fluorine and grain coating improves structural stability and thus improves long-term cycle characteristics. On the other hand, in the case of Comparative Example 2 in which the fluorine content is too high, the thickness of the grain coating formed at the grain boundaries of the primary particles becomes too large, so that the channel space for the movement of lithium ions may be reduced, thereby reducing the efficiency of the movement of lithium ions.
[0138] Figure 6 is a graph showing the resistance of button cells using the positive electrode active materials of Comparative Example 1 and Example 2 according to the present invention. Table 3 below shows the resistance values of Comparative Example 1 and Example 1 according to the present invention depending on the number of cycles.
[0139] [Table 3]
[0140] distinguish F content 25 cycles 50 cycles 75 cycles 100 cycles Comparative Example 1 0mol% 12.78Ω 17.83 21.4Ω 26.7Ω Example 2 1mol% 8.41Ω 8.64Ω 9.15Ω 9.92Ω
[0141] Reference Figure 6 From Table 3, it can be determined that, in the case of Comparative Example 1, the resistance value increases as the number of cycles increases, while in the case of Example 2, the resistance value hardly changes even when the number of cycles increases. That is, it can be determined that, in the case of Comparative Example 1, the positive electrode active material and the electrolyte undergo a side reaction during the cycle to generate resistance at the interface therebetween, while in the case of Example 2, the side reaction hardly occurs during the cycle. Therefore, it can be determined that, in the case of Example 2, the electrochemical characteristics remain constant during the cycle process with almost no change compared to the case of Example 1.
[0142] Figure 7 Graphs showing the cycle characteristics of full cells employing the positive electrode active materials of Comparative Example 1 and Example 2 according to the present invention and resistance versus SOC are depicted. Figure 8 A TEM image showing the ordered structure of the positive electrode active material according to Example 2 after 2000 cycles. Fig. 9 A TEM image showing the ordered structure of the positive electrode active material according to Example 2 after 5000 cycles is shown.
[0143] Table 4 shows the resistance values of Comparative Examples 1 and 2 depending on the SOC.
[0144] [Table 4]
[0145]
[0146] Reference Figure 7 and Table 4, showing the results of 2000 charge / discharge cycles at 1C using full batteries of Comparative Example 1 and Example 2, and it can be determined that, in the case of Comparative Example 1, the capacity decreases and the resistance increases as the number of cycles increases. On the other hand, it can be determined that, in the case of Example 2, the capacity hardly changes even when the number of cycles increases, and even after 5000 cycles, the capacity remains constant and the resistance does not change significantly. It can be determined that, in the case of Example 2, even during long-term cycles, due to the ordered structure and grain coating, side reactions with the electrolyte do not occur, and therefore Example 1 can exhibit stable electrochemical characteristics without structural collapse, while in the case of Comparative Example 1, changes in the crystal structure do occur during the cycling process, such as the separation of lithium ions from the lithium layer, and the partial layered structure changes to a cubic crystal structure, and therefore the electrochemical characteristics deteriorate. Reference Figure 7 By comparing (c) showing the cross section of the particles of Comparative Example 1 at 2000 cycles, (d) showing the cross section of the particles of Example 2 at 2000 cycles, and (e) showing the cross section of Example 2 at 5000 cycles, it can be determined that the microcracks in the particles themselves are almost similar, and the cross-sectional area of the microcracks is about 20% or more of the total area of the secondary particles. That is, it can be determined that even when the cross-sectional area of the microcracks is 20% or more, the structural stability of the positive electrode active material according to the embodiment of the present invention is maintained due to the grain coating formed by adding fluorine and heat treatment and the ordered structure controlled by adding fluorine and heat treatment, the positive electrode active material does not experience a decrease in capacity and an increase in resistance during the cycle process, and the positive electrode active material has excellent electrochemical characteristics.
[0147] Figure 8 An image of the positive electrode active material of Example 2 after 2000 cycles is shown. Fig. 9 An image of the positive electrode active material of Example 2 after 5000 cycles is shown. Figure 8 and Fig. 9 It can be confirmed that the ordered structure is maintained.
[0148] Figure 8 and Fig. 9An electron diffraction pattern of a
[010] crystal zone axis or a
[100] crystal zone axis is shown. The electron diffraction pattern shows: a first diffraction spot group G1, in which one or more diffraction spots having a first intensity and corresponding to a lattice formed by a lithium layer and a transition metal layer stacked adjacent to each other are aligned in one direction; and a second diffraction spot group G2, in which one or more diffraction spots having a second intensity relatively lower than the first intensity of the diffraction spots of the first diffraction group G1 and corresponding to a lattice formed by a first mixed layer and a second mixed layer stacked adjacent to each other are aligned in one direction. The first diffraction spot group and the second diffraction spot group indicate an ordered structure.
[0149] Fig.10 Results of XRD analysis performed to examine the c-axis length and a-axis length after cycling of the positive electrode active materials according to Comparative Example 1 and Example 2 are shown. Table 5 below shows the c-axis length and a-axis length according to Comparative Example 1 and Example 2 after long-term cycling.
[0150] [Table 5]
[0151]
[0152] Reference Fig.10 As shown in Table 5, in the case of Comparative Example 1 (a), after a long-term cycle of 2000 cycles, the lithium ions in the lattice disappear, and vacancies of lithium ions appear in the lithium layer, so that the c-axis length of the crystal structure increases significantly, while the a-axis length hardly changes. Therefore, in the crystal structure of the primary particles constituting Comparative Example 1, the arrangement of the primary particles constituting the secondary particles is destroyed due to the increase in the c-axis length, and the channel of the lithium ions is blocked as a whole, thereby deteriorating the electrochemical characteristics. On the other hand, in the case of Example 2, the a-axis length and the c-axis length are almost unchanged until 2000 cycles and 5000 cycles, because the shape and arrangement of the initial primary particles are maintained. In the case of Example 2, during the long-term cycle, lithium and nickel are exchanged with each other between the layers consisting of lithium alone and the layers consisting of transition metals containing nickel, and thus lithium and transition metals are located at sites corresponding to each other between the first mixed layer (a layer formed by site exchange between lithium and nickel in the lithium layer) and the second mixed layer (a layer formed by site exchange between nickel and lithium in the transition metal layer), thereby forming an ordered structure. The unit cell formed by the ordered structure includes a long-range ordered lattice with an increased a-axis lattice constant. The long-range ordered lattice is composed of a superlattice whose a-axis is twice as long as the a-axis of the lattice formed by the lithium layer and the transition metal layer, and thus can improve the stability of the layered structure, thereby preventing the structural collapse of the layered structure.
[0153] Fig.11Depicted are a graph (a) showing a peak on the (003) plane and a peak on the (104) plane in the positive electrode active material according to Example 2, and a graph (b) showing the ratio between the peaks. Table 6 below shows the content of divalent nickel ions in the lithium layer, the peak of the (104) plane, and the ratio between the peaks.
[0154] [Table 6]
[0155] distinguish Comparative Example 1 Example 1 Example 2 Example 3 Comparative Example 2 F content 0mol% 0.5mol% 1mol% 2mol% 10mol% <![CDATA[Ni in the Li layer mountain 2+ (%)]]> 4.3 4.3% 4.7 4.8 6.8 <![CDATA[The increase rate (%) of Ni in the Li layer 2+ > 1 1 1.1 1.13 1.63 <![CDATA[I (003 / I (104) ]]> 1.74 1.74 1.72 1.71 1.59 <![CDATA[I (003) / I (104) Reduction rate of]]> 1 1 0.99 0.98 0.92
[0156] Reference Fig.11 and Table 6, which shows the Ni content in the first mixed layer (a layer having sites substituted by nickel in a layer composed only of lithium). 2+ The content (%) of Ni in the first mixed layer can be determined as the F content increases. 2+ The content (%) increases, and as the peak on the (003) plane (I (003) ) and the peak value on (104) surface (I (104) ) of the ratio I (003) / I (104) The reduction rate is 1% or less. Specifically, I (003) / I (104) It can be reduced by regular site exchange between nickel ions with an oxidation number of 2 and lithium ions. In addition, as the peak (I (003) ) and the peak value on (104) surface (I (104) ) of the ratio I (003) / I (104) Can be 1.71 or less.
[0157] Fig.12 XRD patterns according to Example 2, Example 3, Comparative Example 1, and Comparative Example 2 are shown.
[0158] Reference Fig.12 It can be confirmed that even when the ordered structure formed increases due to the increase in the amount of fluorine added, the crystal structure of the positive electrode active material does not change. This is because the ordered structure can form a certain regular lattice and thus maintain the layered structure of the positive electrode active material, and the lithium ions and nickel ions (oxidation number 2) formed in the first mixed layer or the second mixed layer have similar ion radii.
[0159] Fig.13 XPS charts according to Example 2, Example 3, Comparative Example 1, and Comparative Example 2 are shown. Fig.14 Selected area electron diffraction (SAED) of the
[010] zone axis according to Comparative Examples 1 and 2 is shown. Fig.15High angle annular dark field (HAADF) images of the
[010] zone axis according to Comparative Example 1 and Example 2 are shown. Table 7 below shows the nickel content of Examples 1 to 3 and Comparative Examples 1 and 2 depending on the oxidation number of nickel oxidation.
[0160] [Table 7]
[0161]
[0162] Reference Fig.13 From Table 7, it can be determined that, in terms of oxidation number, nickel includes Ni 3+ and Ni 2+ , and Ni 2+ with Ni 3+ The ratio (Ni 2+ / Ni 3+ ) increases with the increase of fluorine content. At this time, when Ni 2+ with Ni 3+ The ratio (Ni 2+ / Ni 3+ ) is within a certain range, an ordered structure between the first mixed layer and the second mixed layer is formed in the layered structure of the positive electrode active material, and thus during long-term cycling, the ordered structure between the first mixed layer and the second mixed layer and the layered structure thereby are more stably maintained without lithium ions being separated therefrom. In the XPS spectrum of Ni2P obtained by X-ray photoelectron spectroscopy (XPS), at a binding energy of 850 eV to 860 eV, Ni 2+ The peak area is larger than that of Ni 3+ The peak area of Ni 2+ with Ni 3+ The ratio (Ni 2+ / Ni 3 + ) can be 49.7% to 130%. In addition, at a binding energy of 850 eV to 860 eV, Ni 2+ The peak area of Ni 3+ The ratio of the peak areas of can be from 0.497:1 to 1.3:1.
[0163] Fig.15 An electron diffraction pattern of the
[010] zone axis according to Example 2 is shown.
[0164] Reference Fig.15 , it can be determined that the positive electrode active material of Example 2 has both a layered structure and an ordered structure. The layered structure is a structure in which lithium layers composed only of lithium and transition metal layers composed only of transition metals are alternately arranged. Fig.15As shown in the left figure of Figure 16, only diffraction spots (peaks) in the (012), (014) and (003) space groups are found. In the ordered structure, due to the site exchange of lithium and transition metal in the first mixed layer and the second mixed layer, diffraction spots (peaks) that do not appear in the layered structure appear, and the intensity of these diffraction spots is lower than that of the diffraction spots appearing in the layered structure.
[0165] Specifically, in the ordered structure, the first mixed layer and the second mixed layer are stacked adjacent to each other and are alternately and regularly repeated to form a layered structure. The electron diffraction pattern of the
[010] crystal zone axis (or
[100] crystal zone axis) of the ordered structure shows: a first diffraction spot group G1, in which one or more diffraction spots having a first intensity and corresponding to a lattice formed by the lithium layer and the transition metal layer stacked adjacent to each other are aligned in one direction; and a second diffraction spot group G2, in which one or more diffraction spots having a second intensity relatively lower than the first intensity of the diffraction spots of the first diffraction group G1 and corresponding to a lattice formed by the first mixed layer and the second mixed layer stacked adjacent to each other are aligned in one direction.
[0166] The first diffraction spot group G1 and the second diffraction spot group G2 are alternately and regularly arranged with each other, and the first diffraction spot group G1 and the second diffraction spot group G2 may be spaced apart from each other at the same interval.
[0167] In the case of Example 2, Ni 2+ with Ni 3+ The ratio (Ni 2+ / Ni 3+ ) is increased by adding fluorine and heat treatment, and thus Ni 2+ The lithium of the adjacent layer composed only of lithium is site-exchanged to form a first mixed layer and a second mixed layer. In the electron diffraction pattern, the layer composed only of lithium shows no diffraction spots, while only the transition metal layer shows diffraction spots in the form of white spots ( Fig.12 On the other hand, when the first mixed layer and the second mixed layer are formed to form an ordered structure, diffraction spots are formed in only the portion shown in black to form a superlattice.
[0168] For example, in the first mixed layer, lithium and transition metal may be arranged alternately, and in the second mixed layer, transition metal and lithium may be arranged alternately. The lattice formed by the first mixed layer and the second mixed layer stacked adjacent to each other may include a superlattice, and the superlattice may have six lithium atoms and one transition metal atom.
[0169] Although the present invention has been described in detail with reference to preferred embodiments, the scope of the present invention is not limited to specific embodiments, but should be limited by the appended claims. In addition, those skilled in the art will appreciate that many modifications and variations are possible without departing from the scope of the present invention.
[0170] [Explanation of Reference Numerals]
[0171] 10: Center
[0172] 20: Surface part
[0173] 30: Primary particles
[0174] 100: Secondary particles
Claims
1. A positive electrode active material for a lithium secondary battery, the positive electrode active material having a layered structure and comprising lithium, a transition metal, fluorine (F) and oxygen, wherein the layered structure includes a lithium layer consisting only of lithium and a transition metal layer consisting only of a transition metal including nickel, In terms of oxidation number, the nickel includes Ni 3+ and Ni 2+ , and the Ni 2+ With the Ni 3+ The ratio (Ni 2+ / Ni 3+ ) increases with the increase of the fluorine content, wherein the layered structure further comprises a first mixed layer and a second mixed layer each containing lithium and a transition metal, wherein the first mixed layer and the second mixed layer are stacked adjacent to each other and are alternately and regularly repeated to form a layered structure, and the first mixed layer and the second mixed layer stacked adjacent to each other are configured such that the transition metal of the first mixed layer and the lithium of the second mixed layer correspond to each other, wherein a lattice formed by the first mixed layer and the second mixed layer stacked adjacent to each other comprises a superlattice, an a-axis of the superlattice being twice as long as an a-axis of a lattice formed by the lithium layer and the transition metal layer, wherein the content of lithium in the first mixed layer is higher than the content of the transition metal, and the content of the transition metal in the second mixed layer is higher than the content of lithium; and The electron diffraction pattern of the [010] zone axis or the [100] zone axis of the layered structure shows: a first diffraction spot group in which one or more diffraction spots having a first intensity and corresponding to a lattice formed by the lithium layer and the transition metal layer stacked adjacent to each other are aligned in one direction; and a second diffraction spot group, wherein one or more diffraction spots having a second intensity lower than the first intensity of the diffraction spots of the first diffraction spot group and corresponding to a lattice formed by the first mixed layer and the second mixed layer stacked adjacent to each other are aligned in one direction, The positive electrode active material is represented by the following formula 1: [Formula 1] Li 1-x M 1-y [Li x M y ]O 2-z F z wherein x+y=1; 0.005≤z≤0.02; and M is any one of the following: Ni; Ni and Co; Ni and Mn; Ni, Co and Mn; Ni and Al; Ni, Co and Al; Ni, Mn and Al; and Ni, Co, Mn and Al.
2. The positive electrode active material according to claim 1, wherein the first mixed layer and the second mixed layer stacked adjacent to each other have an ordered structure, wherein the ordered structure is formed so that n1 lithium ions and n2 transition metal ions of the first mixed layer correspond to n1 transition metal ions and n2 lithium ions of the second mixed layer, respectively, wherein n1 and n2 are the same or different natural numbers, and a unit cell formed by the ordered structure includes a long-range ordered lattice with an increased a-axis lattice constant.
3. The positive electrode active material according to claim 1, wherein the peak (I 003) of the (003) plane in the X-ray diffraction spectrum of the positive electrode active material obtained by XRD analysis using CuKα radiation after the electrochemical reaction is (003) ) and the peak value (I (104) ) ratio (I (003) / I (104) ) is reduced by less than 1%.
4. The positive electrode active material according to claim 3, wherein the peak value (I (003) ) and the peak value (I (104) ) of the ratio (I (003) / I (104) ) is 1.71 or less.
5. The positive electrode active material according to claim 1, wherein In the XPS spectrum of Ni2P obtained by X-ray photoelectron spectroscopy (XPS), Ni 2+ The peak area of Ni 3+ The ratio of the peak areas is 0.49:1 to 1.3:
1. 6 . The positive electrode active material according to claim 1 , wherein the positive electrode active material comprises secondary particles consisting of a group of a plurality of primary particles, and at least one of the primary particles comprises a grain coating layer comprising fluorine at a grain boundary between the primary particles. 7 . The positive electrode active material according to claim 1 , wherein the first diffraction spot group and the second diffraction spot group are arranged alternately and regularly with each other, and the first diffraction spot group and the second diffraction spot group are spaced apart from each other.
8. The positive electrode active material according to claim 1, wherein The lithium and transition metal in the first mixed layer are arranged alternately; and The transition metal and lithium in the second mixed layer are arranged alternately.
9. The positive electrode active material according to claim 6, wherein the primary particle comprises a rod-like particle formed into a sheet shape having a major axis and a minor axis in cross section, and the rod-like particle is oriented so that the major axis of the rod-like particle faces the central portion of the secondary particle.
10. The positive electrode active material according to claim 6, wherein the transition metal comprises any one or more of nickel (Ni), manganese (Mn) and cobalt (Co), wherein at least one of the transition metals has a concentration gradient from the center of the secondary particle toward the surface of the secondary particle in at least a portion of the secondary particle.
11. A lithium secondary battery comprising: A positive electrode comprising the positive electrode active material for a lithium secondary battery according to any one of claims 1 to 10; a negative electrode facing the positive electrode and composed of graphite or lithium metal; a separator between the positive electrode and the negative electrode; and An electrolyte solution or solid electrolyte containing a lithium salt.