A method for preparing large-size bars by controlled rolling and controlled cooling
Through multiple temperature control and slow cooling control technology, combined with deformation-induced phase change, the problem of uneven deformation of the surface and core part in large-scale bars is solved, and the uniformity and strength of cross-sectional performance are improved .
Patent Information
- Application Number
- CN202210585022.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-05-27
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2042-05-27
AI Technical Summary
The prior art is difficult to achieve the control of rolling and cooling of large-scale bars, and the deformation of the surface and core parts is uneven, resulting in differences in cross-sectional performance of the finished product, especially in bars with specifications of ≥Ф80mm.
Using multiple temperature control and slow cooling technology, combined with deformation-induced phase change technology, the steel billet heating is finely controlled through a stepping beam heating furnace, rough rolling is rolled at a lower volume, and the intermediate billet is continuously rolled, and the diameter reduction unit is reduced. Slow cooling to avoid temperature differences caused by intense water cooling, prompting the γ→α phase transition to occur in advance, and refine the tissue and grains.
The uniformity of cross-sectional structure and performance of large-sized rods is achieved, the strength and hardness of the finished product are improved, the internal stress and temperature differences are reduced, and the yield strength, tensile strength and impact toughness are significantly improved.
Smart Images

Figure CN114985461B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a controlled rolling and controlled cooling preparation method for a large-size bar, belonging to the technical field of special steel bar rolling. Background Art
[0002] The reason why special steel materials can be widely used and become an important basic material that is indispensable in the national economy is that they have special chemical composition, special properties and meet special usage requirements. In order to achieve these characteristics, it is necessary to strengthen the steel materials by adding alloying elements or heat treatment to the steel to achieve different strength and toughness performance matching. However, the strengthening effect of simply adding a large amount of alloying elements to the steel is limited and not economical, and it is difficult to meet the needs of a large number of applications of special steels. The microstructure of the material can also be refined and strengthened by heat treatment (normalizing, etc.), which has obvious effects, but it consumes a lot of energy and brings environmental problems such as pollutant emissions. How to efficiently and economically improve the strength, toughness and other properties of steel has become an issue that must be considered in the development of special steel products.
[0003] Since the TMCP technology was officially developed in the 1980s, after decades of development, it has become an indispensable technology in the field of medium and thick plate rolling and has been widely used. Simply put, the rolling technology method that comprehensively uses controlled rolling and controlled cooling is called TMCP technology. It does not rely on alloy elements. It controls the cooling of steel by online control of rolling temperature and relatively cheap cooling water. It is a process that saves alloys and energy and has great application value and environmental significance. Controlled rolling and controlled cooling are developed as manufacturing technologies for medium and thick plates, and have also been promoted and applied as a broad TMCP technology in the production of hot-rolled strip, steel sections, and bars. It is an indispensable technology for the production of high-grade special steels. This technology is to carry out a certain degree of rapid cooling in the temperature region of austenite to ferrite phase transformation after controlled rolling, so that the phase transformation structure is more refined than that of simple controlled rolling, and at the same time, higher strength is obtained. It is a control technology for phase transformation of the controlled austenite based on "controlling the austenite state". By controlling the phase transformation process from austenite (γ) to ferrite (α), a wide range of phase transformation structures are obtained, and the phase transformation structures in different ranges show the characteristics of a wide range of performance changes, and the main performance changes are strength and toughness indicators. The generalized TMCP rolling technology is also gradually applied to bar rolling, especially in the field of special steel rolling. Common controlled rolling and controlled cooling technology applications in special steel bar rolling include: inhibiting the precipitation of bearing steel network carbides through the water penetration process after rolling, producing ultrafine grain gear steel through controlled rolling and cooling, and improving the mechanical properties of non-quenched and tempered steel through low temperature rolling technology. Compared with traditional TMCP application fields such as medium and thick plates, the research and application of controlled rolling and controlled cooling in bar lines, especially medium and large-sized bars, is not very mature.
[0004] Patent No. CN107185968A discloses a controlled rolling and controlled cooling method for high-quality steel bars. This method is a typical controlled rolling and controlled cooling arrangement on a continuous rolling line. The racks are arranged relatively compactly, the rolling speed is fast, and the deformation time is relatively short. Due to the capacity limitation of the continuous rolling mill, the existing controlled rolling technology cannot achieve deformation with a large amount of reduction, so it is not conducive to the uniform penetration of the deformation into the core of the rolled piece, and it is easy to cause uneven deformation of the surface and the core of large-sized bars. Since the static recovery and static recrystallization time of austenite cannot be controlled during continuous rolling and rough rolling, the faster rolling speed and deformation speed make it impossible to accurately control the austenite recrystallization and non-recrystallization processes, and the control of the combination of deformation and phase change processes is not very sufficient. The invention controls cooling by using a 2-stage water tank for cooling before intermediate rolling and finishing rolling, a 3-stage water tank for cooling before the finishing mill and the sizing mill (RSM), and a 5-stage water tank for cooling after the RSM. On the rolling line before RSM, the bar exit speed and water penetration speed are relatively fast. The existing technology for large-sized bars often causes the surface to be completely cooled to a lower temperature below the phase transition point while the core remains near or above the phase transition point. The disadvantage is that strong water cooling easily leads to a large temperature difference between the core and the surface, which ultimately leads to differences in the cross-sectional properties of the finished bars. The existing invention uses a remedial method for extending the recovery time after rolling to improve the uneven cross-sectional temperature caused by strong water penetration cooling before rolling for small and medium-sized bars with specifications of Ф12-70mm, but no effective solution is proposed for the controlled rolling and controlled cooling method of large-sized bars (especially ≥Ф80mm). Summary of the invention
[0005] The technical problem to be solved by the present invention is to provide a preparation method of large-size bars by controlled rolling and controlled cooling in response to the above-mentioned prior art, which breaks through the current technical difficulties of controlled rolling and controlled cooling of large-size bars, and solves the problem of the difficulty of penetrating the deformation of the core of large bars through a rough rolling and large reduction rolling process. For large-size bars (especially Ф≥80mm), multiple temperature controls and slow controlled cooling before fine rolling are performed to control the deformation and temperature of austenite recrystallization and non-recrystallization zones. At the same time, deformation-induced phase transformation technology is used to promote the γ→α phase transformation to occur in advance to refine the structure and grains, thereby solving the problem of uniformity of structure and performance at different positions of the cross section of large-size bars.
[0006] The technical solution adopted by the present invention to solve the above problem is: a preparation method of large-size bars by controlled rolling and controlled cooling, the preparation method comprising the following steps:
[0007] Step 1: Heating the continuous casting billet: The continuous casting billet is placed in a walking beam heating furnace with multiple temperature control zones for heating;
[0008] Step 2: Descaling: After the high-temperature continuous casting billet comes out of the furnace, it passes through the high-pressure water impact force of the descaling box to remove the iron oxide scale on the high-temperature continuous casting billet;
[0009] Step 3: Primary heating: The high-temperature continuous casting billet is heated once before entering the rough rolling mill;
[0010] Step 4: Rough rolling: The continuous casting billet after the first temperature treatment is rolled at high temperature with large reduction;
[0011] Step 5: Head cutting: remove the defects of the head of the intermediate billet;
[0012] Step 6: Secondary heating: The intermediate billet after cutting is subjected to secondary heating before entering the continuous rolling mill;
[0013] Step 7: Continuous rolling: The continuous rolling unit rolls the rectangular intermediate billet into an intermediate round bar;
[0014] Step 8: Cut the head and tail, and divide into multiple lengths: Cut off the head and tail of the middle round rod, and divide the middle round rod into several sections according to the multiple lengths;
[0015] Step 9: Three-time temperature waiting: The segmented bars are subjected to three-time temperature waiting by blowing or air convection;
[0016] Step 10: Finish rolling: After three times of warming, the product enters the sizing mill and is rolled into bars with a diameter of 60 to 150 mm.
[0017] Step 11: Water cooling: The bars after finish rolling enter the multi-stage water tank for water cooling;
[0018] Step 12: Cut to length: Cut the cooled bar into the required length or single length;
[0019] Step 13: Cooling on the cooling bed: The bar enters the cooling bed and cools slowly;
[0020] Step 14: Piece collection: Pack and collect the bars and stack them offline.
[0021] In the step 1, eight temperature control zones are provided in the walking beam heating furnace: the temperature of zone eight is ≤800°C, the temperature of zone seven is 700-900°C, the temperature of zone six is 900-1000°C, the temperature of zone five is 1000-1100°C, the temperature of zone four is 1050-1260°C, the temperature of zone three is 1100-1260°C, the temperature of zone two is 1100-1280°C, the temperature of zone one is 1150-1280°C, and the total heating time is 3.5-8h.
[0022] The working pressure of the descaling machine in step 2 is ≥20MPa.
[0023] The first waiting temperature in step three is 950-1100° C.; the second waiting temperature in step six is 830-950° C.; the third waiting temperature in step nine is 10-50° C. above Ar3.
[0024] The primary waiting temperature is 980-1030°C; the secondary waiting temperature is 830-880°C.
[0025] In the step 4, the rough rolling reduction is ≥60 mm, the rough rolling ratio is 3 to 7, and the number of completed rolling passes is 5 to 13.
[0026] The rolling interval is controlled by controlling the residence time of the rolled piece on the roller table of the slab opening machine, and the residence time is 1 to 5 seconds.
[0027] In the step eight, a hydraulic cutting device is used to cut the intermediate blank, and the cutting length is ≥50mm.
[0028] In the step 10, the deformation amount of each pass is controlled to be ≥ 20%, and the cumulative deformation amount is controlled to be ≥ 60%.
[0029] The water pressure of each water tank in step 11 is 0.5-1.0 MPa, and the final cooling temperature of the bar surface is ≥600°C.
[0030] Compared with the prior art, the advantages of the present invention are: a method for preparing large-size bars by controlled rolling and controlled cooling;
[0031] 1. Conventional heating furnaces only control four sections, namely, the preheating section, the first heating section, the second heating section, and the soaking section. The temperature control area of the process adopted by the present invention is more refined, and the heating temperature and heating time of the steel type in a certain area can be accurately controlled according to the thermoplasticity difference of the steel. The alloy elements or micro-alloy elements in the steel can be fully dissolved during heating, and the austenite of the steel billet is more uniform. Since the residence time of the steel billet at high temperature can be accurately controlled to avoid the coarsening of the austenite grains at high temperature, the heating uniformity of the steel billet is better than that of the traditional process method.
[0032] 2. Continuous rolling cannot achieve large-scale deformation. For large-size bars, due to the limited deformation, rolling deformation often only stays on the surface and cannot penetrate into the center of the bar. The uniformity of the structure and performance of the controlled rolled bars is difficult to ensure. The rough rolling of the present invention adopts a semi-continuous rolling process with a large reduction function. Its technical advantage is that a larger rolling reduction can better penetrate the center of the continuous casting billet, promote the welding of defective structures in the core of the continuous casting billet, and break up coarse columnar crystals, so as to obtain better finished product low-magnification structure and more uniform cross-sectional properties. The present invention utilizes reciprocating rolling intermittent time control to allow austenite to fully undergo static recovery and static recrystallization. Its beneficial effect is that it can accurately control the rolling process of rough-rolled austenite in the crystallization zone to obtain more refined austenite equiaxed grains.
[0033] 3. Before continuous rolling, the present invention adopts a secondary temperature treatment to control the rolling temperature and deformation of the unrecrystallized austenite zone. In this stage, a lower rolling temperature and continuous rolling deformation accumulation are adopted to control the unrecrystallized austenite grains to be continuously elongated and flattened, thereby increasing the area of the grain boundary per unit area. The beneficial effect is to promote the formation of high-density dislocations and a large number of deformation bands in the austenite crystals, increase the ferrite nucleation rate, and thus obtain finer grains and structures.
[0034] 4. The present invention does not use water or spray water for cooling during the entire cooling process before rolling, which is very different from the traditional cooling control method. The present invention adopts a transverse cooling bed for three times of temperature control cooling in the sizing unit (RSM). Through a relatively mild cooling method, the cooling intensity of the core and surface of the large-sized bars is controlled to be relatively consistent and the temperature is relatively uniform. It has significant innovation and has the beneficial effect of avoiding the large difference in core and surface temperature caused by intense water cooling of large-sized bars, which leads to differences in organization and performance.
[0035] 5. The present invention maintains the rolling temperature at a certain temperature slightly higher than the phase transformation point, so that the deformation temperature can be maintained near Ar3, so that the starting temperature of the γ→α phase transformation is higher than the equilibrium phase transformation temperature, and the phase transformation is induced in advance by the accumulation of a large amount of deformation at low temperature, that is, the phase transformation is induced by deformation, thereby producing ultrafine ferrite grains. Different from the traditional method of controlling the organizational transformation by rapid water cooling, the present invention introduces the influence of deformation during the phase transformation process, and refines the grains through deformation-induced phase transformation, which has obvious effects and more uniform nucleation transformation. The water penetration after rolling of the present invention is only used as a means to further refine the organization, increase the supercooling of the pearlite transformation, and further refine the pearlite lamellar spacing to improve the strength and hardness of the rod. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] Figure 1 This is a process layout diagram of a method for preparing a large-size bar by controlled rolling and controlled cooling according to an embodiment of the present invention;
[0037] In the figure, 1 is a walking-beam heating furnace, 2 is a high-pressure water descaling box, 3 is a roller table for warming up before rough rolling, 4 is a two-roller reversible billet opening machine, 5 is a hydraulic head cutting device, 6 is a roller table for warming up before continuous rolling, 7 is a first continuous rolling unit, 8 is a second continuous rolling unit, 9 is a flying shear, 10 is a rack-type transverse cooling bed, 11 is a sizing unit, 12 is a water-penetrating tank, 13 is a grinding wheel saw, and 14 is a cooling bed. DETAILED DESCRIPTION
[0038] The present invention is further described in detail below with reference to the accompanying drawings.
[0039] Embodiment 1
[0040] Combination Figure 1Taking the production of a steel bar with a diameter of 80 mm as an example, the production method of the present invention is further described. The continuous casting billet is a medium carbon steel containing 0.4C-1.4Mn-0.1V-0.06S (%). The preparation method comprises the following steps:
[0041] Step 1: Heating the continuous casting billet: Cold load the continuous casting billet with a specification of 300*340mm into the walking-beam heating furnace 1 for heating. The walking-beam heating furnace has eight temperature control zones, and the temperature of each zone is controlled: the temperature of zone eight is 655℃, the temperature of zone seven is 810℃, the temperature of zone six is 954℃, the temperature of zone five is 1047℃, the temperature of zone four is 1105℃, the temperature of zone three is 1171℃, the temperature of zone two is 1203℃, the temperature of zone one is 1205℃, and the total heating time is 6h.
[0042] Step 2: Dephosphorization: After the high-temperature continuous casting billet is taken out of the furnace, the iron oxide scale on the surface of the high-temperature continuous casting billet is removed by the impact force of the high-pressure water descaling box 2, and the descaling working pressure is 28MPa.
[0043] Step 3: One-time warming: Before entering the rough rolling mill, the steel is warmed once on the pre-rough rolling warming roller table 3, and the warming temperature is 1000°C.
[0044] Step 4: Rough rolling: The Ф850 two-roller reversible billet mill 4 rolls the continuous casting billet after the first warming at high temperature with a large reduction. The reduction of the 1st, 3rd, 5th and 7th passes is 60mm, the rough rolling ratio is 3.3, the rolling passes are completed in 9 passes, the interval time of the rolled piece on the roller is 2 seconds, and the final rolling temperature is 940°C. The rolling interval time is controlled to allow the austenite to fully undergo static recovery and static recrystallization processes. Among them, the final rolling temperature of the rough rolling is slightly higher than the austenite non-recrystallization temperature Tnr, ensuring that the rolling of the austenite in the crystallization zone is completed after the rough rolling, thereby obtaining more refined austenite equiaxed grains.
[0045] Step 5: Head cutting: The hydraulic head cutting device 5 is used to cut off the head of the intermediate billet. The head cutting length is 120mm to reduce rolling accidents caused by the head biting problem of the rolled piece.
[0046] Step 6: Secondary warming: After the rough rolling is completed, the intermediate billet is subjected to secondary warming on the warming roller 6 before being sent to the continuous rolling unit. The warming temperature is 860°C. During the continuous rolling, all the rolling is carried out in the austenite non-crystallization zone.
[0047] Step 7: Continuous rolling: The continuous rolling mill group uses two 650 Ф rolling mills and two 450 Ф rolling mills in a horizontal and vertical alternating manner. The two 650 Ф rolling mills form the first continuous rolling mill group 7, and the two 450 Ф rolling mills form the second continuous rolling mill group 8. The number of stands can be increased or decreased according to different rolling specifications. The rectangular intermediate billet is rolled into an intermediate round bar of a certain size.
[0048] Step 8: Cutting the head and tail, and dividing into sections according to multiple lengths: Use the flying shears 9 to cut off the head and tail areas of the middle round rod, and divide the middle round rod into several sections according to multiple lengths.
[0049] Step 9: Three-time temperature waiting: The segmented bars are sent to the rack-type transverse cooling bed 10 for three-time temperature waiting. The middle round bars are quickly cooled to 810°C on the rack-type transverse cooling bed by blowing or air convection. No water is passed or sprayed for cooling during the entire cooling process.
[0050] Step 10: Finish rolling: After the three waiting temperatures are reached, the temperature of the intermediate round bar is maintained at 810°C, and then enters the high-precision sizing unit 11 for rolling, with a deformation of 20% per pass, a cumulative deformation of 60%, and a final rolling specification of Ф80mm. The rolling temperature is maintained at a certain temperature slightly higher than the phase transformation point, so that the deformation temperature can be maintained near Ar3, so that the starting temperature of the γ→α phase transformation is higher than the equilibrium phase transformation temperature, and the accumulation of a large deformation at low temperature can induce the phase transformation in advance, that is, through deformation-induced phase transformation, to produce ultra-fine ferrite grains.
[0051] Step 11: Water cooling: The rolled bar enters the three-stage water tank 12 for water cooling. The water pressure of each water tank is 0.5 MPa. The final cooling surface red-return temperature of the bar is 610°C, which further refines the transformation structure, reduces the lamellar spacing of pearlite, and improves the strength, hardness and plasticity of the bar.
[0052] Step 12: Cutting to length: After the rod is pierced with water, it is cut into a fixed length of 7m using a grinding wheel saw 13, so as to meet the delivery size requirements of the rod.
[0053] Step 13: Cooling on a cooling bed: The bar enters the cooling bed 14 and is slowly cooled to further reduce the temperature difference between the center and the surface and the internal stress.
[0054] Step 14: Piece collection: After the cooling bed is off-line, automatic packaging equipment is used to pack, collect and stack the pieces off-line.
[0055] The comparison results of Example 1 and Comparative Example 1, which are large-size bars of Ø80 mm that are directly rolled without conventional processes such as controlled rolling and controlled cooling, are shown in Table 1 (comparison results of macrostructure rating) and Table 2 (comparison results of grain structure and performance).
[0056] Table 1
[0057] project Steel grade composition Rolling specification / mm Generally loose Loose center Ingot segregation Example 1 0.4C-1.4Mn-0.1V-0.06S(%) Ф80 1 1 1 Comparative Example 1 0.4C-1.4Mn-0.1V-0.06S(%) Ф80 1.5 1.5 1
[0058] Table 2
[0059]
[0060] Embodiment 2
[0061] Combined with Figure 1Taking the production of a steel bar with a diameter of 80 mm as an example, the production method of the present invention is further described. The continuous casting billet is a medium carbon steel containing 0.35C-1.3Mn-0.12V-0.05S (%). The preparation method comprises the following steps:
[0062] Step 1: Heating the continuous casting billet: The continuous casting billet with a specification of 300*340mm is cold loaded into the walking-beam heating furnace 1 for heating. The walking-beam heating furnace has eight temperature control zones, and the temperature of each zone is controlled: the temperature of zone eight is 667℃, the temperature of zone seven is 809℃, the temperature of zone six is 961℃, the temperature of zone five is 1053℃, the temperature of zone four is 1102℃, the temperature of zone three is 1175℃, the temperature of zone two is 1197℃, the temperature of zone one is 1210℃, and the total heating time range is 6h.
[0063] Step 2: Dephosphorization: After the high-temperature continuous casting billet is taken out of the furnace, the iron oxide scale on the surface of the high-temperature continuous casting billet is removed by the impact force of the high-pressure water descaling box 2, and the descaling working pressure is 27MPa.
[0064] Step 3: First warming: Before entering the rough rolling mill, the steel is warmed once on the warming roller before rough rolling, and the warming temperature is 1000℃.
[0065] Step 4: Rough rolling: The Ф850 two-roller reversible billet mill rolls the continuous casting billet after the first warming at high temperature with a large reduction. The reduction of the 1st, 3rd, 5th and 7th passes is 60mm, the rough rolling ratio is 3, the rolling passes are completed in 7 passes, the interval time of the rolled piece on the roller is 2 seconds, and the final rolling temperature is 953℃. The rolling interval time is controlled to allow the austenite to fully undergo static recovery and static recrystallization processes. Among them, the final rolling temperature of rough rolling is slightly higher than the austenite non-recrystallization temperature Tnr, ensuring that the rolling of austenite in the crystallization zone is completed after the rough rolling, thereby obtaining more refined austenite equiaxed grains.
[0066] Step 5: Head cutting: The hydraulic head cutting device 5 is used to cut off the head of the intermediate billet. The head cutting length is 110mm to reduce rolling accidents caused by the head biting problem of the rolled piece.
[0067] Step 6: Secondary warming: After the rough rolling is completed, the intermediate billet is subjected to secondary warming on the warming roller table before being sent to the continuous rolling unit. The warming temperature is 860°C. During the continuous rolling, all the rolling is carried out in the austenite non-crystallization zone.
[0068] Step 7: Continuous rolling: The continuous rolling unit uses two horizontal and vertical alternating Ф650 rolling mills. The number of stands can be increased or decreased according to different rolling specifications. The rectangular intermediate billet is rolled into an intermediate round bar of a certain size.
[0069] Step 8: Cutting the head and tail, and dividing into sections according to multiple lengths: Use the flying shears 9 to cut off the head and tail areas of the middle round rod, and divide the middle round rod into several sections according to multiple lengths.
[0070] Step 9: Three-time temperature waiting: The segmented bars are sent to the rack-type transverse cooling bed 10 for three-time temperature waiting. The middle round bars are quickly cooled to 810°C on the rack-type transverse cooling bed by blowing or air convection. No water is passed or sprayed for cooling during the entire cooling process.
[0071] Step 10: Finish rolling: After the three waiting temperatures are reached, the temperature of the intermediate round bar is maintained at 810°C, and then enters the high-precision sizing unit 11 for rolling, with a deformation of 20% per pass, a cumulative deformation of 60%, and a final rolling specification of Ф1400mm. The rolling temperature is maintained at a certain temperature slightly higher than the phase transformation point, so that the deformation temperature can be maintained near Ar3, so that the starting temperature of the γ→α phase transformation is higher than the equilibrium phase transformation temperature, and the accumulation of a large deformation at low temperature can induce the phase transformation in advance, that is, through deformation-induced phase transformation, to produce ultra-fine ferrite grains.
[0072] Step 11: Water cooling: The rolled bar enters the three-stage water tank 12 for water cooling. The water pressure of each water tank is 0.5 MPa. The final cooling surface red-return temperature of the bar is 630°C, which further refines the transformation structure, reduces the lamellar spacing of pearlite, and improves the strength, hardness and plasticity of the bar.
[0073] Step 12: Cutting to length: After passing through water pipe, the bar is cut into 6m length with a grinding wheel saw to meet the delivery size requirements of the bar.
[0074] Step 13: Cooling on a cooling bed: The bar enters the cooling bed 14 and is slowly cooled to further reduce the temperature difference between the center and the surface and the internal stress.
[0075] Step 14: Piece collection: After the cooling bed is off-line, automatic packaging equipment is used to pack, collect and stack the pieces off-line.
[0076] Comparative Example 2 is a large-size bar with a diameter of 80 mm that is directly rolled without conventional processes such as controlled rolling and controlled cooling. The comparison results with Example 2 are shown in Table 3 (comparison results of macrostructure rating) and Table 4 (comparison results of grain structure and performance).
[0077] Table 3
[0078] project Steel grade composition Rolling specification / mm Generally loose Loose center Ingot segregation Example 2 0.35C-1.3Mn-0.12V-0.05S(%) Ф140 1 1 1 Comparative Example 2 0.35C-1.3Mn-0.12V-0.05S(%) Ф140 1.5 1.5 1
[0079] Table 4
[0080]
[0081] It can be seen from the comparison results of macrostructure rating in Table 1 and Table 3 that the process of the present invention has an obvious effect on the macrostructure defects of welded continuous casting billets, and can obtain better finished macrostructure and more uniform cross-sectional properties than conventional processes.
[0082] It can be seen from the grain structure and performance comparison results in Table 2 and Table 4 that the mechanical properties such as yield strength, tensile strength, and impact toughness of the embodiments of the present invention are significantly improved, and the results of impact toughness of the embodiments of the present invention are less volatile, and the performance is relatively uniform and stable. The present invention has a significant improvement in performance over the traditional process, and the organization and grain refinement effects of the present invention are also very obvious, which can solve the technical problems such as uneven organization and performance of large-size bars after controlled rolling and controlled cooling.
[0083] In addition to the above embodiments, the present invention also includes other implementation modes. Any technical solutions formed by equivalent transformation or equivalent replacement should fall within the protection scope of the claims of the present invention.
Claims
1. A method for preparing large-size bars by controlled rolling and controlled cooling, characterized in that: The preparation method comprises the following steps: Step 1: Heating the continuous casting billet: The continuous casting billet is placed in a walking beam heating furnace with multiple temperature control zones for heating; Step 2: Descaling: After the high-temperature continuous casting billet comes out of the furnace, it passes through the high-pressure water impact force of the descaling box to remove the iron oxide scale on the high-temperature continuous casting billet; Step 3: Primary heating: The high-temperature continuous casting billet is heated once before entering the rough rolling mill; the primary heating temperature is 950~1100℃; Step 4: Rough rolling: The continuous casting billet after the first temperature treatment is rolled at high temperature with large reduction; Step 5: Head cutting: remove the defects of the head of the intermediate billet; Step 6: Secondary heating: The intermediate billet after cutting is subjected to secondary heating before entering the continuous rolling mill; the secondary heating temperature is 830~950℃; Step 7: Continuous rolling: The continuous rolling unit rolls the rectangular intermediate billet into an intermediate round bar; Step 8: Cut the head and tail, and divide into multiple lengths: Cut off the head and tail of the middle round rod, and divide the middle round rod into several sections according to the multiple lengths; Step 9: Three-time temperature waiting: The segmented bars are heated three times by blowing or air convection; the three-time temperature waiting temperature is 10~50℃ above Ar3; Step 10: Finish rolling: After three times of warming, it enters the sizing unit for rolling and is rolled into bars with a diameter of 60~150mm; Step 11: Water cooling: The finished rolled bars enter a multi-stage water tank for water cooling; Step 12: Cut to length: Cut the cooled bar into the required length or single length; Step 13: Cooling on the cooling bed: The bar enters the cooling bed and cools slowly; Step 14: Piece collection: Pack and collect the bars and stack them offline; In the step 1, eight temperature control zones are provided in the walking beam heating furnace: the temperature of zone 8 is ≤800°C, the temperature of zone 7 is 700-900°C, the temperature of zone 6 is 900-1000°C, the temperature of zone 5 is 1000-1100°C, the temperature of zone 4 is 1050-1260°C, the temperature of zone 3 is 1100-1260°C, the temperature of zone 2 is 1100-1280°C, the temperature of zone 1 is 1150-1280°C, and the total heating time is 3.5-8h; In the step 10, the deformation amount of each pass is controlled to be ≥ 20%, and the cumulative deformation amount is controlled to be ≥ 60%.
2. The method for preparing large-size bars by controlled rolling and controlled cooling according to claim 1, characterized in that: The working pressure of the descaling box in step 2 is ≥20MPa.
3. The method for preparing large-size bars by controlled rolling and controlled cooling according to claim 1, characterized in that: The first temperature is 980-1030°C; the second temperature is 830-880°C.
4. The method for preparing large-size bars by controlled rolling and controlled cooling according to claim 1, characterized in that: In the step 4, the rough rolling reduction is ≥60 mm, the rough rolling ratio is 3-7, and the number of completed rolling passes is 5-13.
5. The method for preparing large-size bars by controlled rolling and controlled cooling according to claim 4, characterized in that: The rolling interval is controlled by controlling the residence time of the rolled piece on the roller table of the slab opening machine, and the residence time is 1~5s.
6. The method for preparing large-size bars by controlled rolling and controlled cooling according to claim 1, characterized in that: In the step eight, a hydraulic cutting device is used to cut the intermediate blank, and the cutting length is ≥50mm.
7. The method for preparing large-size bars by controlled rolling and controlled cooling according to claim 1, characterized in that: In the step 11, the water pressure of each water tank is 0.5-1.0 MPa, and the final cooling temperature of the bar surface is ≥600°C.