Viscosity-enhancing polyol composition and method for preparing polyurethane sealing foam therefrom
By using a tackifying polyol composition and isocyanate to form a two-component system in the sealing material, the problems of anti-flowability and permanent foam deformation in the on-site reaction of materials A and B are solved, and the efficient sealing and production efficiency are improved. The sealing of irregular shape accessories replaces the shortcomings of traditional EPDM foam strips.
Patent Information
- Application Number
- CN202210748640.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-06-28
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2042-06-28
AI Technical Summary
In the on-site reaction of materials A and B, the problems of insufficient flow resistance of sealing materials and permanent foam deformation caused by gas-phase silica have not been effectively solved by the prior art.
Using a viscosity-enhancing polyol composition, comprising polyether polyol, polymer polyol, amine organics, vapor phase silica, water, surfactants and catalysts, the sealing foam is enhanced by forming strong hydrogen bonds and cohesion. Flow resistance and curing network, cast using a two-component system with isocyanate.
It achieves efficient flow resistance and low permanent deformation, improves sealing effect and production efficiency, and is suitable for sealing of irregular shape accessories, replacing the shortcomings of traditional EPDM foam strips.
Smart Images

Figure BDA0003717537350000061 
Figure BDA0003717537350000071
Abstract
Description
Technical Field
[0001] The invention relates to a tackifying polyol composition, which is suitable for polyurethane on-site pouring foaming reaction molding and is used for sealing special-shaped plastic parts of household appliances, lighting fixtures, electronic product chassis, cabinets, distribution cabinets and the like. Background Art
[0002] In the fields of construction, home appliances, automobiles, electromechanics, etc., sealing materials are essential chemical products. They are used for joint sealing and non-structural bonding and assembly, and can play the role of anti-seepage, anti-leakage, anti-vibration and sealing. Due to the limitations of the scenarios in these applications, the anti-sagging and anti-flow of sealing material polymers are one of the key properties that people generally pay attention to. Improving the viscosity of polymers is currently a common technology to achieve anti-sagging performance.
[0003] Due to its unique molecular structure and large specific surface area, fumed silica can form a network structure through hydrogen bonding, which can effectively increase the viscosity of the polymer. It is also beneficial to the production and storage of products, such as thixotropy, anti-settling of fillers, and physical property reinforcement.
[0004] Due to the thixotropy of the fumed silica thickening polymer, the low viscosity during production due to the stirring shear force is conducive to uniform mixing, and the increased viscosity after standing is conducive to storage and anti-sagging requirements during construction. This technology is widely used in single-component sealing materials.
[0005] In order to adjust the reaction curing speed and the ratio of raw materials on a continuous production line, two-component sealing materials A and B are often used. A and B materials are mixed and poured onto the seal at high speed on site by a glue coating machine. The requirements for anti-sagging and anti-flow performance are higher, otherwise the required shape of the sealing material cannot be obtained. In this application process, the thixotropic disadvantage of fumed silica is also highlighted. After the A and B materials are mixed at high speed, there is still a problem of flowability.
[0006] Some patents have also been disclosed in this field. Patent CN106190000 solves the waterproof problem of sealing foam. Although patent CN110016313 solves the flow problem, it uses a higher proportion of fumed silica and a large amount of powder filler, and a large amount of powder filler will bring new problems. Patent CN110724246 solves the adhesion and appearance problems of sealing materials. Patent CN111892690 solves the resilience problem of sealing materials. Patent CN112375527 solves the density problem of sealing materials. None of the above patents solve the problem of the anti-flowability of A and B materials in the field reaction, and the problem of permanent deformation of key indicators of sealing foam.
[0007] The present invention starts from the characteristics of the raw material molecular structure, utilizes the cohesive force and reaction activity between molecules, and unexpectedly finds that the shortcomings in the application of fumed silica can be solved. Summary of the invention
[0008] The object of the present invention is to provide a viscosity-enhancing polyol composition to solve the problems of anti-flowing property and permanent deformation of foam in the on-site reaction of materials A and B.
[0009] The present invention also provides a method for preparing polyurethane sealing foam, and the viscosity-enhancing polyol composition of the present invention is used in the preparation process.
[0010] In order to achieve the above invention object, the technical solution adopted by the present invention is as follows:
[0011] The first aspect of the present invention provides a tackifying polyol composition (hereinafter referred to as component A), comprising the following components:
[0012] Polyols, including at least one of polyether polyols, polymer polyether polyols, and polyester polyols;
[0013] Amine organic matter;
[0014] Fumed silica;
[0015] Water, surfactants, catalysts, color pastes and other additives;
[0016] Taking the weight of the viscosity-enhancing polyol composition as 100%, the contents of the components are: 94-96.5% polyol, 0.5-2% amine organic matter, 0.8-1.3% fumed silica, 0.45-0.55% water, 0.5-0.8% surfactant, 0.6-0.9% catalyst and 0.4-0.6% color paste.
[0017] In component A of the present invention, the polyether polyol can be obtained by starting with one or more of propylene glycol, glycerol and trimethylolpropane and polymerizing with propylene oxide and / or ethylene oxide, and the hydroxyl value is preferably 20-50 mgKOH / g; the polymer polyether polyol is formed by graft polymerization of one or two monomers of styrene and acrylonitrile in the polyether polyol, and the hydroxyl value is preferably 19-35 mgKOH / g; the polyester polyol is formed by condensation of adipic acid or phthalic anhydride with one or more of ethylene glycol, diethylene glycol or butanediol, and the hydroxyl value is preferably 35-115 mgKOH / g; preferably, the polyol comprises the following substances (the weight ratio refers to the weight ratio in the tackifying polyol composition):
[0018] Polyether polyol 1, glycerol-initiated, ethylene oxide-terminated, hydroxyl value 32-36 mgKOH / g, or polyether polyol 2, glycerol-initiated, ethylene oxide-terminated, hydroxyl value 26-30 mgKOH / g; weight ratio 45-60%;
[0019] Polyether polyol 3, propylene glycol initiator, ethylene oxide end-capping, hydroxyl value 25-30 mgKOH / g; weight ratio 8-20%;
[0020] Polymer polyether polyol 4, polyether polyol 1 is a base polyether, styrene and acrylonitrile are grafted and polymerized, and the hydroxyl value is 19-23 mgKOH / g; the weight ratio is 0-10% (for example, 1%, 2%, 3%, 4%, ...);
[0021] Polyester polyol 5, polycondensation product of adipic acid, EG and BDO, hydroxyl value 50-60 mgKOH / g, or polyester polyol 6, polycondensation product of adipic acid, EG and DEG, hydroxyl value 50-60 mgKOH / g; weight ratio 20-40%.
[0022] In component A of the present invention, the amine organic matter includes but is not limited to at least one of ethylenediamine, diethyltoluenediamine, dimethylthiotoluenediamine, 4,4'-bis-sec-butylaminodiphenylmethane, 4,4'-bis-diaminodiphenylmethane and 3,3'-dichloro-4,4'-diaminodiphenylmethane.
[0023] In the component A of the present invention, the fumed silica is a nanometer-sized white powder generated by high-temperature hydrolysis of silicon halides in a hydrogen-oxygen flame, and the specific surface area of the aggregate is greater than 200 m 2 / g.
[0024] In component A of the present invention, the surfactant is a polysiloxane modified by copolymerization of ethylene oxide and propylene oxide, which plays the role of emulsification, nucleation and foam stabilization. Commercially available products include B8715, DC6070 and the like.
[0025] In component A of the present invention, the catalyst includes but is not limited to one or more of triethylenediamine, bisdimethylaminoethyl ether, dimorpholine diethyl ether, N,N-dimethylcyclohexylamine, N-ethylmorpholine, N-methyldicyclohexylamine, pentamethyldiethylenetriamine, triethylamine and dimethylethanolamine, preferably one or two of triethylenediamine and bisdimethylaminoethyl ether.
[0026] The second aspect of the present invention provides a method for preparing a polyurethane sealing foam, using the tackifying polyol composition (component A) and component B isocyanate of the present invention;
[0027] Wherein, the weight ratio of component A to component B is 100:17-28; preferably, the weight ratio of component A to component B is 100:20-25.
[0028] The isocyanate component B of the present invention includes but is not limited to urethane-modified diphenylmethane diisocyanate prepolymer, a mixture of diphenylmethane diisocyanate and polymethylene polyphenyl isocyanate, with an NCO content of 23.5-24.5% and a viscosity of 250-350 mPa·S.
[0029] It needs to be further explained and illustrated that the polyol composition component A of the present invention has achieved unexpected results in the preparation of polyurethane sealing foam, and has excellent anti-flowing property. It may be that the N atom of the amine compound, the carbonyl group of the polyester polyol and the hydroxyl group on the surface of the fumed silica form a hydrogen bond with stronger binding force, and the polyester polyol molecule has a stronger cohesive force, which is not easy to be destroyed under a certain shear force, and maintains the shape of the cast. Another factor may be that the amine organic matter reacts very quickly with the isocyanate, quickly forming a solidified network, which can also further improve the anti-flowing property. The anti-flowing property is reflected in the appearance size of the foam strip cast on the accessory by the glue coating machine, the ratio of the width d of the bottom plane of the foam strip to the height h of the highest point of the foam strip to the bottom plane, that is, the smaller the d / h ratio, the better the anti-flowing property. However, the d / h ratio is not the smaller the better, and the d / h ratio range is better between 1 / 1-2 / 1. The use effect of the sealing foam strip is related to the permanent deformation of the foam strip. The smaller the permanent deformation, the better the sealing effect, and the ideal permanent deformation is less than 10%. The density of the foam will affect the hardness and compressibility of the foam. The foam density is 400-450kg / m 3 The effect shown is better.
[0030] The present invention prepares the sealing foam from the polyol composition component A by the following method: the component A and the isocyanate component B form a two-component system, the material temperature is 20-25°C, the components A and B are fully mixed by a glue coating machine and then directly poured on the sealing part of the accessory, forming in one step, with high efficiency and good consistency, and no need for secondary pasting. By changing the diameter of the pores of the pouring head, the requirements of different sealing strip sizes can be met.
[0031] The beneficial effects of the present invention are: high production efficiency, smooth foam strip appearance, good connection, good sealing effect, and it is also suitable for sealing irregularly shaped accessories, and can completely replace the existing EPDM foam strip sealing technology. At present, EPDM foam strips need to be manually pasted, which has the disadvantages of poor connection at the interface and difficulty in bonding special-shaped accessories. DETAILED DESCRIPTION
[0032] The present invention is further described below by way of examples, but the present invention is not limited to these examples.
[0033] Viscosity test method: in accordance with GB / T 12008.7-2010
[0034] NCO test standard: in accordance with GB / T 12009.4-2016
[0035] Permanent deformation test: in accordance with GB / T 1683-2018
[0036] Diethyltoluenediamine, dimethylthiotoluenediamine, 4,4'-bis-sec-butylaminodiphenylmethane, 3,3'-dichloro-4,4'-diaminodiphenylmethane industrial products
[0037] Catalyst 1: Bis(dimethylaminoethyl)ether
[0038] Catalyst 2: 33% triethylenediamine in DPG solution
[0039] Polyether polyol 1: glycerol-based, ethylene oxide-capped, hydroxyl value 32-36 mgKOH / g;
[0040] Polyether polyol 2: glycerol-initiated, ethylene oxide-terminated, hydroxyl value 26-30 mgKOH / g;
[0041] Polyether polyol 3: Propylene glycol-based, ethylene oxide-capped, hydroxyl value 25-30 mgKOH / g;
[0042] Polymer polyol 4: Polyether polyol 1 is the base polyether, styrene and acrylonitrile are grafted and polymerized, and the hydroxyl value is 19-23 mgKOH / g;
[0043] Polyester polyol 5: polycondensate of adipic acid, EG and BDO, hydroxyl value 50-60 mgKOH / g;
[0044] Polyester polyol 6: polycondensate of adipic acid, EG and DEG, hydroxyl value 50-60 mgKOH / g;
[0045] Fumed silica: A nanometer-sized white powder generated by high-temperature hydrolysis of silicon halides in a hydrogen-oxygen flame. The specific surface area of the aggregate is greater than 200 m 2 / g.
[0046] Diphenylmethane diisocyanate: containing 4,4'-MDI, 2,4'-MDI;
[0047] Polymeric MDI: A mixture of diphenylmethane diisocyanate and polymethylene polyphenyl isocyanate.
[0048] Isocyanate component B: a mixture of polyether polyol 1 or 2 modified diphenylmethane diisocyanate prepolymer and polymethylene polyphenyl isocyanate, with an NCO content of 23.5-24.5% and a viscosity of 250-350 mPa·S.
[0049] Example
[0050] According to the weight proportion of the raw materials in Table 1 (in terms of the effective content of each component), first add the polyol into the barrel of the disperser, then add the fumed silica, stir at a low speed (50-100 rpm) until the fumed silica is wetted, and then stir and disperse into the polyol raw materials at a high speed (800-1000 rpm). Then add the remaining other components, stir and mix for 30 minutes, and obtain the viscosity-enhancing polyol composition component A of the present invention.
[0051] Isocyanate B1: NCO content 23.5%, viscosity 347 mPa·S (25°C). Add 30.1 kg of polyether polyol 1 into the reactor, keep the material temperature at 40-80°C, then add 43.2 kg of diphenylmethane diisocyanate, keep the material temperature at 80°C and react for 3 hours. Then add 47.9 kg of polymeric MDI.
[0052] Isocyanate B2: NCO content 24.3%, viscosity 255 mPa·S (25°C). Add 27.9 kg of polyether polyol 2 to the reactor, keep the material temperature at 40-80°C, then add 43.2 kg of diphenylmethane diisocyanate, keep the material temperature at 80°C and react for 3 hours. Then add 52 kg of polymeric MDI.
[0053] The viscosity-enhancing polyol composition component A and the isocyanate component B constitute a two-component system. The components A and B are fully mixed by a glue coating machine and then directly poured on the sealing part of the accessory to form it in one step.
[0054] Table 1 Example
[0055]
[0056]
[0057] * Use glue coating machine to make samples, the pouring head diameter is 4mm, and use calipers to measure the width of the bottom plane of the foam strip and the height of the highest point from the bottom surface.
[0058] The examples are for the purpose of clearly illustrating the present invention, and are not intended to limit the present invention. A person skilled in the art can still make changes and adjustments to the raw material ratios, or replace similar raw materials on this basis, and the changes derived therefrom are still within the scope of protection of the present invention.
Claims
1. A tackifying polyol composition comprising the following components: Polyols; Amine organic matter, at least one selected from ethylenediamine, diethyltoluenediamine, dimethylthiotoluenediamine, 4,4'-bis-sec-butylaminodiphenylmethane, 4,4'-bis-diaminodiphenylmethane and 3,3'-dichloro-4,4'-diaminodiphenylmethane; Fumed silica; Additives, including water, surfactants and catalysts, color paste; Polyols include the following substances: Polyether polyol 1, glycerol-initiated, ethylene oxide-terminated, hydroxyl value 32-36 mgKOH / g, or polyether polyol 2, glycerol-initiated, ethylene oxide-terminated, hydroxyl value 26-30 mgKOH / g; weight ratio 45-60%; Polyether polyol 3, starting with propylene glycol, terminated with ethylene oxide, hydroxyl value of 25-30 mgKOH / g; weight ratio of 8-20%; Polymer polyether polyol 4, polyether polyol 1 as base polyether, styrene and acrylonitrile grafted polymerized, hydroxyl value 19-23 mgKOH / g; weight ratio 0-10%; Polyester polyol 5, polycondensation product of adipic acid, EG and BDO, hydroxyl value 50-60 mgKOH / g, or polyester polyol 6, polycondensation product of adipic acid, EG and DEG, hydroxyl value 50-60 mgKOH / g; weight ratio 20-40%.
2. The composition according to claim 1, wherein The viscosity-enhancing polyol composition comprises the following components based on 100% by weight: 94-96.5% of polyol, 0.5-2% of amine organic matter, 0.8-1.3% of fumed silica, 0.45-0.55% of water, 0.5-0.8% of surfactant, 0.6-0.9% of catalyst and 0.4-0.6% of color paste.
3. The composition according to any one of claims 1 to 2, wherein The fumed silica is a nanometer-sized white powder generated by high-temperature hydrolysis of silicon halides in a hydrogen-oxygen flame, and the specific surface area of the aggregate is greater than 200 m 2 / g.
4. The composition according to any one of claims 1 to 2, wherein The surfactant is ethylene oxide and propylene oxide copolyether modified polysiloxane.
5. The composition according to claim 4, wherein The surfactant is selected from B8715 and DC6070.
6. The composition according to any one of claims 1 to 2, wherein The catalyst comprises at least one of triethylenediamine, bis(dimethylaminoethyl)ether, dimorpholine diethyl ether, N,N-dimethylcyclohexylamine, N-ethylmorpholine, N-methyldicyclohexylamine, pentamethyldiethylenetriamine, triethylamine and dimethylethanolamine.
7. A polyurethane sealing foam comprising the tackifying polyol composition (component A) according to any one of claims 1 to 6 and isocyanate (component B); in, The weight ratio of component A to component B is 100:17-28.
8. The polyurethane sealing foam according to claim 7, wherein the B-component isocyanate has an NCO content of 23.5-24.5% and a viscosity of 250-350 mPa·s.
9. The polyurethane sealing foam according to claim 7 or 8, wherein components A and B are fully mixed by a glue coating machine and then directly poured on the sealing part of the accessory.