An ultrapure manganese and its preparation method
By using a composite smelting process with low-melting-point and high-melting-point metal additives and a two-stage vacuum distillation process, the problem of impurity control in high-purity manganese has been solved, achieving efficient preparation of ultra-pure manganese, meeting the needs of the microelectronics industry, simplifying the production process, and reducing energy consumption and pollution.
Patent Information
- Application Number
- CN202210547948.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-05-18
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2042-05-18
AI Technical Summary
Existing technologies struggle to effectively control the content of gaseous element impurities in high-purity manganese, leading to copper migration and integrated circuit reliability issues. Furthermore, the production process is cumbersome, energy-intensive, and causes severe environmental pollution.
By employing a composite smelting process combining low-melting-point and high-melting-point metal additives with a two-stage vacuum distillation process, impurities are separated through vacuum smelting and two-stage distillation to prepare ultrapure manganese, reducing the total content of non-gaseous element impurities to below 10 ppm and the total content of gaseous elements to below 50 ppm.
It has achieved high-purity production of ultrapure manganese, meeting the needs of the microelectronics industry, simplifying the process, reducing energy consumption and environmental pollution, and is suitable for large-scale production.
Smart Images

Figure CN114990362B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of ultrapure metal preparation technology, specifically relating to ultrapure manganese and its preparation method. Background Technology
[0002] The development of the microelectronics industry, especially very large-scale integrated circuits (VLSI), has had a profound impact on human society. In integrated circuits, various devices such as diodes, transistors, resistors, and capacitors are formed by depositing and etching on silicon wafers. These devices are connected to each other using wires made of special materials. Traditional semiconductor processes often use aluminum as the interconnecting wire; however, when the wiring size is as small as 0.18μm, aluminum wires suffer from severe electromigration, high resistivity, and shallow junction penetration. These defects can easily lead to chip failure. As wiring sizes rapidly decrease, copper has gradually replaced aluminum as the mainstream material for interconnects. However, copper itself has a strong migration ability, which may contaminate the silicon substrate or insulating film. Adding high-purity manganese to high-purity copper can effectively suppress copper migration and improve the reliability of integrated circuits. Therefore, the demand for high-purity manganese has surged. In the field of magnetic storage, manganese alloys are important antiferromagnetic materials. By sputtering IrMn or PtMn layers to form an internal magnetic field, magnetic random access memory (MRAM) can achieve fieldless switching. However, impurities such as gaseous elements (C, H, O, N, S, and Cl) can affect the switching performance of magnetic layers in MRAM. Therefore, there is an urgent need for high-purity manganese with low gaseous element impurity content.
[0003] Currently, the main production processes for high-purity manganese of 5N and above are electrolytic refining and vacuum distillation. For example, invention CN105200453A uses two electrolytic refining processes to prepare 5N grade Mn, but this process is cumbersome, energy-intensive, and causes serious environmental pollution. More importantly, the content of impurities such as gaseous elements is uncontrollable. Invention CN202111161334.3 uses a vacuum distillation process to prepare high-purity manganese with a purity of 4N5 to 5N, however, its C, H, O, and N contents are too high, approximately 100 ppm. Furthermore, in the examples of CN202111161334.3 verifying the technical effect, only 11 impurity elements were analyzed using GDMS (assuming the total content of the 11 impurity elements and manganese is 100%), indicating that the purity assessment criteria in the examples are not strict.
[0004] In view of the above problems, there is an urgent need to develop a method for preparing ultrapure manganese with low content of gaseous elemental impurities in order to meet the demand for high-purity manganese in the integrated circuit industry. Summary of the Invention
[0005] In order to solve the above-mentioned technical problems, the inventors of this invention, based on their research in the field and through a large number of experiments, have provided an ultrapure manganese and its preparation method.
[0006] Specifically, the present invention first provides a method for preparing ultrapure manganese, comprising the following steps:
[0007] Raw manganese is mixed with low-melting-point metal additives and then vacuum smelted to obtain crude manganese.
[0008] The crude manganese was mixed with a high-melting-point metal additive to obtain a mixture. The mixture was then separated by two-stage distillation under low vacuum conditions to obtain manganese vapor. The manganese vapor was collected to obtain ultrapure manganese.
[0009] In the two-stage distillation, the first stage distillation essentially separates impurities with melting points lower than that of manganese from the mixture, while the second stage distillation separates manganese from the mixture.
[0010] The term “substantially separating impurities with melting points below the manganese melting point from the mixture” as used herein means that the content of impurities with melting points below the manganese melting point from the mixture is less than 5 ppm, preferably less than 1 ppm.
[0011] Compared with the traditional method of smelting and distilling raw manganese, this invention incorporates low-melting-point metal additives and high-melting-point metal additives for composite smelting and distillation, and adopts a two-stage distillation process. The resulting ultrapure manganese has a total non-gaseous element impurity content of less than 10 ppm and a total gaseous element content of less than 50 ppm, which meets the demand of the microelectronics industry for ultrapure manganese. Moreover, the purity is stable and it is easy to achieve large-scale production.
[0012] According to an embodiment of the present invention, the electrolytic manganese sheet is a commercially available electrolytic manganese sheet, and its purity is tested to be 2N-3N according to the metallurgical industry standard YB / T 051-2015.
[0013] Preferably, the temperature of the mixture in the first stage of distillation is 1250–1300°C;
[0014] More preferably, the distillation time for the first stage of distillation is 0.5–2 hours, and the absolute pressure during distillation is 10. -5 ~10 -2 Pa. Under the above conditions, the present invention, through a first-stage distillation, allows impurities in the melt with melting points lower than that of manganese to fully volatilize and condense on a condenser plate.
[0015] In a preferred embodiment, 1) before the first stage of distillation, crude manganese and high-melting-point metal additives are mixed and placed in a crucible, and a vacuum is drawn to an absolute pressure of 10. -5 Pa level or below 10 -51) Apply a vacuum continuously at a pressure of 5–10 °C / min until the melt temperature reaches 1250–1300 °C; 2) Begin the first stage of distillation, maintaining the melt temperature in the crucible at 1250–1300 °C and the condenser temperature at 500–900 °C; the distillation time is 0.5–2 h, preferably 1 h; 3) After the first stage of distillation, stop heating and perform vacuum cooling, with an absolute pressure of 10 MPa. -5 Pa level or below 10 -5 The furnace should be opened only after it has cooled to room temperature and been filled with high-purity nitrogen or argon gas.
[0016] Preferably, the temperature of the mixture in the second stage of distillation is 1350–1450°C;
[0017] Further preferably, the absolute pressure during the second stage of distillation is 10. -5 ~10 -2 Pa. Under the above conditions, the present invention, through a second-stage distillation, allows non-volatile impurities to remain in the melt, while manganese vapor condenses on a condenser plate, thus obtaining ultrapure manganese.
[0018] In a preferred embodiment, 1) before the second stage distillation, the condenser plate from the first stage distillation is removed and replaced with a new condenser plate, and a vacuum is drawn to an absolute pressure of 10. -5 Pa level or below 10 -5 1) Maintain a vacuum and heat at 5–10 °C / min until the melt temperature in the crucible reaches 1350–1450 °C; 2) Begin the second stage of distillation, keeping the melt temperature in the crucible at 1350–1450 °C and the condenser temperature at 500–1100 °C; 3) After the second stage of distillation, stop heating and perform vacuum cooling at an absolute pressure of 10 Pa. -5 Pa level or below 10 -5 The sample is in the Pa range. After cooling to room temperature, high-purity nitrogen or argon is introduced, the furnace is opened, and the sample is removed.
[0019] Preferably, the low-melting-point metal is selected from one or more of zinc, calcium, magnesium, and aluminum; the amount of the low-melting-point metal additive is 1 to 10% based on the mass of the raw material manganese.
[0020] More preferably, the low-melting-point metal is calcium and magnesium in a mass ratio of 1 to 3:1; and the amount of the low-melting-point metal additive is 2 to 5% based on the mass of the raw material manganese. The present invention unexpectedly discovered that by selecting the above-mentioned low-melting-point metal additive with specific content and composition, the content of various impurities in ultrapure manganese can be effectively reduced, especially the content of gaseous elements such as S, C, H, O, N, and Cl is significantly reduced.
[0021] Preferably, the high-melting-point metal is selected from one or more of tungsten, molybdenum, tantalum, rhenium, and iridium; the mass ratio of crude manganese to the high-melting-point metal is in the range of 1 to 20:1.
[0022] More preferably, the mass ratio of the crude manganese to the high-melting-point metal is in the range of 10 to 15:1. Studies have found that the present invention, by mixing the aforementioned high-melting-point metal additive with the aforementioned vacuum-melted crude manganese in a specific ratio and then performing a two-stage distillation process, is beneficial for further reducing the content of impurities such as Fe, Co, Ni, Cr, V, and Ti.
[0023] Preferably, the vacuum melting is vacuum induction melting or vacuum arc melting, and an inert gas, preferably argon, is introduced during melting; the absolute pressure during vacuum melting is 10. 4 Pa level or below 10 4 Pa level, preferably 10 3 Pa level, even better at 1×10 3 Pa~9×10 3 Pa. In this invention, when vacuum induction melting or vacuum arc melting with absolute pressure of the aforementioned magnitude is used, the content of gaseous elements and metallic impurities with melting points lower than that of manganese can be reduced. In particular, under vacuum conditions, the content of gaseous elements such as C, H, and O can be further reduced. Introducing an inert gas during melting can prevent manganese from evaporating.
[0024] Preferably, the surface of the raw manganese is chemically cleaned with an acidic solution before mixing the raw manganese with the low-melting-point metal additive.
[0025] More preferably, the pH of the acidic solution is 3–6.8, and more preferably 5–6. The acidic solution includes, but is not limited to, hydrochloric acid, sulfuric acid, acetic acid, and hydrogen peroxide. Surface chemical cleaning can effectively remove the oxide layer from the surface of electrolytic manganese.
[0026] Preferably, the method further includes: after the vacuum melting, the resulting block is subjected to surface mechanical processing to obtain crude manganese;
[0027] The surface machining is preferably performed by any one or a combination of turning, milling, planing, and grinding. The raw material manganese in this invention is vacuum-melted and cast into a block. After surface machining, oxygen elements introduced by slight oxidation of the manganese surface can be better prevented from entering the later products. It also removes impurities introduced by the mold during the casting process.
[0028] In a preferred embodiment, the preparation method includes the following steps:
[0029] 1) Using electrolytic manganese flakes as raw material, the oxide layer is removed by surface chemical cleaning. The surface chemical cleaning uses an acidic solution, including but not limited to hydrochloric acid, sulfuric acid, acetic acid, hydrogen peroxide, etc. Its pH value is 3-6.8, preferably 5-6;
[0030] 2) Add low-melting-point metal additives and perform vacuum melting, introducing argon gas during melting at an absolute pressure of 10. 4 Pa level or below 10 4 Pa level, preferably 10 3 Pa level, even better at 1×10 3 Pa~9×10 3 Pa.
[0031] 3) The surface of the cast sample is machined by any combination of one or more processes such as turning, milling, planing, and grinding to obtain crude manganese;
[0032] 4) First-stage distillation: The crude manganese is mixed with the high-melting-point metal additive and placed in a crucible under vacuum until 10 °C. -5 The pressure is on the order of Pa, and a vacuum is continuously applied. The mixture is then heated at a rate of 5–10 °C / min until the melt temperature reaches 1250–1300 °C. Distillation then begins for 0.5–2 hours, preferably 1 hour. Heating is subsequently stopped, and the mixture is cooled under vacuum at an absolute pressure of 10 MPa. -5 The pressure is in the Pa range, and the furnace is finally cooled to room temperature. High-purity nitrogen or argon gas must be introduced before the furnace can be opened.
[0033] 5) Second-stage distillation: First, remove the multi-stage condenser used in the first distillation and replace it with a brand new multi-stage condenser. Then, evacuate to 10°C. -5 The pressure is on the order of Pa, and a vacuum is continuously applied. The mixture is then heated at a rate of 5–10 °C / min until the melt temperature reaches 1350–1450 °C. Distillation then begins, followed by vacuum cooling to room temperature at an absolute pressure of 10 MPa. -5 Pa level. Pour in high-purity nitrogen or argon gas, open the furnace, and remove the sample.
[0034] The present invention also provides an ultrapure manganese, which is prepared according to the above-described method for preparing ultrapure manganese.
[0035] The beneficial effects of this invention are at least as follows:
[0036] This invention provides ultrapure manganese and its preparation method. Employing an improved process, it can purify 2N-3N electrolytic manganese to 5N or even higher, with the total content of non-gaseous element impurities below 10 ppm, the total content of gaseous elements below 50 ppm, and the gaseous element content ≤1 ppm C, ≤20 ppm H, ≤20 ppm O, ≤30 ppm N, ≤2 ppm S, and ≤20 ppm Cl. This meets the ultrapure manganese requirements of the microelectronics industry. The process is simple, consumes little energy, causes minimal environmental pollution, provides stable purity, and is easily scalable for mass production. Attached Figure Description
[0037] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0038] Figure 1 This is a schematic diagram of the distillation apparatus used in an embodiment of the present invention, wherein 1-crucible, 2-multi-stage condenser, 3-heating coil, and 4-condenser cover.
[0039] Figure 2 This is a process flow diagram of the method for preparing ultrapure manganese provided in the embodiments of the present invention. Detailed Implementation
[0040] The present invention will now be described by way of preferred embodiments. It should be understood by those skilled in the art that these embodiments are for illustrative purposes only and are not intended to limit the scope of the invention.
[0041] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. The following embodiments are used to illustrate the present invention, but are not intended to limit the scope of the present invention. Where specific techniques or conditions are not specified in the embodiments, they shall be performed in accordance with the techniques or conditions described in the literature in the art, or in accordance with the product instructions. Reagents or instruments used without specified manufacturers are all conventional products that can be purchased through legitimate channels.
[0042] Figure 1 This is a schematic diagram of the distillation apparatus used in Examples 1-4, wherein 1-crucible (the horizontal position of the crucible), 2-multi-stage condenser plate, 3-heating coil, and 4-condenser cover.
[0043] Figure 2 This is a process flow diagram of the preparation method of ultrapure manganese provided in Examples 1-4 of the present invention.
[0044] Example 1
[0045] An ultrapure manganese and its preparation method. See also: Figure 2 The specific steps are as follows:
[0046] 1. Use 1 kg of commercially available 3N grade electrolytic manganese flakes as raw material, and perform surface chemical cleaning with dilute hydrochloric acid (pH value 5) until the surface of the electrolytic manganese flakes has a silvery-white metallic luster. Then, clean with distilled water and alcohol in sequence, and dry.
[0047] 2. Electrolytic manganese flakes, after surface chemical cleaning, are mixed with low-melting-point metal additives (2 wt.% Ca, 1 wt.% Mg) and placed in a vacuum induction furnace at an absolute pressure of 3.5 × 10⁻⁶. 3 The smelting process begins at Pa. After smelting is complete, the sample is removed, the surface layer is removed, and crude manganese is obtained.
[0048] 3. For the high melting point metal additive, bulk tungsten with an average diameter of about 10 mm is selected, and the mass ratio of tungsten to manganese is 1:10.
[0049] 4. In the first distillation, the crude manganese is mixed with the high-melting-point metal additive and placed in a crucible, then placed in... Figure 1 In the distillation apparatus shown, a vacuum of 1 × 10⁻⁶ was applied. -5 Pa; heating is started at a rate of 5℃ / min, the melt temperature in the crucible is 1250℃, the first distillation begins, the temperature of the multi-stage condenser is 510~820℃, and the absolute pressure during distillation is maintained at 10. -5 ~10 -2 Pa; distillation time is 1 hour, heating is stopped after distillation; vacuum cooling, vacuum is applied to 10°C during cooling. -5 Pa level; after cooling to room temperature, introduce high-purity nitrogen gas and start the furnace.
[0050] 5. For the second distillation, first remove the multi-stage condenser from the first distillation and replace it with a brand new multi-stage condenser; then begin evacuating to 10°C. -5 Pa level; then heating was started at a rate of 5℃ / min, and the melt temperature in the crucible was 1400℃, initiating the second distillation; the temperature of the condenser was 570~1050℃; the distillation time was 4 hours, and after the second distillation, vacuum cooling was performed, with a vacuum level of 10 during cooling. -5 The sample was taken at the Pa level, cooled to room temperature, filled with high-purity nitrogen, and the furnace was opened to remove the ultrapure manganese sample.
[0051] The purity of the samples was analyzed by glow discharge mass spectrometry (GDMS) and overflow gas analysis (EGA). C, H, O, and N were measured by EGA, and the remaining elements were measured by GDMS.
[0052] After the first distillation in Example 1, the material in the crucible was analyzed by GDMS, and the results are shown in Table 1.
[0053] Table 1
[0054] element content element content element content element content Li 0.02 Ni 6.8 Sn 0.38 Hf <0.01 Be <0.01 Cu 1 Sb 0.55 Ta <0.01 B 0.17 Zn 0.5 Te <0.05 W 0.14 F <0.05 Ga <0.05 I <0.05 Re <0.05 Na 0.9 Ge <0.05 Cs <0.01 Os <0.01 Mg 0.9 As 0.35 Ba <0.01 Ir <0.01 Al 0.08 Se 0.9 La <0.01 Pt <0.01 Si 1 Br <0.05 Ce <0.03 Au <0.05 P 0.59 Rb <0.05 Pr <0.01 Hg <0.05 S 0.5 Sr <0.05 Nd <0.01 Tl <0.05 Cl <0.01 Y <0.05 Sm <0.01 Pb <0.05 K 0.9 Zr <0.05 Eu <0.01 Bi <0.01 Ca 0.58 Nb 0.05 Gd <0.01 Th <0.005 Sc <0.05 Mo 4.9 Tb <0.01 U <0.005 Ti 4 Ru <0.01 Dy <0.01 V 2 Rh <0.01 Ho <0.01 Cr 5 Pd <0.05 Er <0.01 Mn principal component Ag <0.05 Tm <0.01 Fe 3 Cd <0.05 Yb <0.01 Co 5 In <0.05 Lu <0.01
[0055] As can be seen from Table 1, after one distillation, the content of impurities with melting points lower than that of manganese in the crucible material is below 1 ppm.
[0056] The composition of the ultrapure manganese obtained in Example 1 is shown in Table 2.
[0057] Table 2 shows the content of ultrapure manganese obtained in Example 1, in ppm and wt.
[0058] element content element content element content element content Li <0.01 Ni 0.53 Sn 0.38 Hf <0.01 Be <0.01 Cu 0.13 Sb 0.55 Ta <0.01 B 0.02 Zn <0.1 Te <0.05 W 0.14 F <0.05 Ga <0.05 I <0.05 Re <0.05 Na 0.31 Ge <0.05 Cs <0.01 Os <0.01 Mg 0.5 As 0.21 Ba <0.01 Ir <0.01 Al 0.08 Se 0.5 La <0.01 Pt <0.01 Si 0.45 Br <0.05 Ce <0.01 Au <0.05 P 0.29 Rb <0.05 Pr <0.01 Hg <0.05 S 0.31 Sr <0.05 Nd <0.01 Tl <0.05 Cl <0.01 Y <0.05 Sm <0.01 Pb <0.05 K 0.07 Zr <0.05 Eu <0.01 Bi <0.01 Ca 0.57 Nb 0.05 Gd <0.01 Th <0.005 Sc <0.05 Mo 0.2 Tb <0.01 U <0.005 Ti 0.04 Ru <0.01 Dy <0.01 H <15 V <0.01 Rh <0.01 Ho <0.01 C 0.08 Cr 0.03 Pd <0.05 Er <0.01 N <5 Mn principal component Ag <0.05 Tm <0.01 O 9 Fe 0.13 Cd <0.05 Yb <0.01 Co 0.39 In <0.05 Lu <0.01
[0059] Example 2
[0060] An ultrapure manganese and its preparation method. The specific steps are as follows:
[0061] 1. Use 1 kg of commercially available 3N grade electrolytic manganese flakes as raw material. Perform surface chemical cleaning with a mixture of hydrogen peroxide and water (pH value 5.5) until the surface of the electrolytic manganese flakes has a silvery-white metallic luster. Then, clean with distilled water and alcohol in sequence, and dry.
[0062] 2. Electrolytic manganese flakes, after surface chemical cleaning, are mixed with low-melting-point metal additives (0.5 wt.% Ca, 2 wt.% Mg, and 1 wt.% Zn) and placed in a vacuum induction furnace at an absolute pressure of 5 × 10⁻⁶. 3 The smelting process begins at Pa. After smelting is complete, the sample is removed, the surface layer is removed, and crude manganese is obtained.
[0063] 3. The high-melting-point metal additive is tungsten powder with an average diameter of 100μm and a tungsten to manganese mass ratio of 1:15.
[0064] 4. For the first distillation, mix the crude manganese with the high-melting-point metal additive and place the mixture in a crucible. Evacuate to a vacuum of 1×10⁻⁶. -5 Pa; heating is started at a rate of 5℃ / min, the melt temperature in the crucible is 1270℃, the first distillation begins, the temperature of the multi-stage condenser is 510~850℃, and the absolute pressure during distillation is maintained at 10. -5 ~10 -2 Pa; distillation time is 1 hour, heating is stopped after distillation; vacuum cooling, vacuum is applied to 10°C during cooling. -5 Pa level; after cooling to room temperature, introduce high-purity nitrogen gas and start the furnace.
[0065] 5. For the second distillation, first remove the multi-stage condenser from the first distillation and replace it with a brand new multi-stage condenser; then begin evacuating to 10°C.-5 Pa level; then heating was started at a rate of 5℃ / min, and the melt temperature in the crucible was 1450℃, initiating the second distillation; the temperature of the condenser was 610~1080℃; the distillation time was 6h, and after the second distillation, vacuum cooling was performed, with a vacuum level of 10℃ during cooling. -5 The sample was taken at the Pa level, cooled to room temperature, filled with high-purity nitrogen, and the furnace was opened to remove the ultrapure manganese sample.
[0066] The purity analysis method is the same as in Example 1. The composition of ultrapure manganese obtained in Example 2 is shown in Table 3.
[0067] Table 3 shows the ultrapure manganese content obtained in Example 2, in ppm and wt.
[0068]
[0069]
[0070] Example 3
[0071] An ultrapure manganese and its preparation method. The specific steps are as follows:
[0072] 1. Use 1 kg of commercially available 3N grade electrolytic manganese flakes as raw material, and perform surface chemical cleaning with dilute hydrochloric acid (pH value 6) until the surface of the electrolytic manganese flakes has a silvery-white metallic luster. Then, clean with distilled water and alcohol in sequence, and dry.
[0073] 2. Electrolytic manganese flakes, after surface chemical cleaning, are mixed with low-melting-point metal additives (2 wt.% Ca, 4 wt.% Al, and 4 wt.% Zn) and placed in a vacuum induction furnace at an absolute pressure of 4 × 10⁻⁶. 3 The smelting process begins at Pa. After smelting is complete, the sample is removed, the surface layer is removed, and crude manganese is obtained.
[0074] 3. Molybdenum powder with an average diameter of 90 μm was selected as the high melting point metal additive, and the mass ratio of molybdenum to manganese was 1:15.
[0075] 4. For the first distillation, mix the crude manganese with the high-melting-point metal additive and place the mixture in a crucible. Evacuate to a vacuum of 1×10⁻⁶. -5 Pa; heating is started at a rate of 5℃ / min, the melt temperature in the crucible is 1290℃, the first distillation begins, the temperature of the multi-stage condenser is 520~870℃, and the absolute pressure during distillation is maintained at 10. -5 ~10 -2 Pa; distillation time is 1 hour, heating is stopped after distillation; vacuum cooling, vacuum is applied to 10°C during cooling. -5 Pa level; after cooling to room temperature, introduce high-purity nitrogen gas and start the furnace.
[0076] 5. For the second distillation, first remove the multi-stage condenser from the first distillation and replace it with a brand new multi-stage condenser; then begin evacuating to 10°C. -5 Pa level; then heating was started at a rate of 5℃ / min, and the melt temperature in the crucible was 1430℃, initiating the second distillation; the temperature of the condenser was 600~1070℃; the distillation time was 6h, and after the second distillation, vacuum cooling was performed, with a vacuum level of 10℃ during cooling. -5 The sample was taken at the Pa level, cooled to room temperature, filled with high-purity nitrogen, and the furnace was opened to remove the ultrapure manganese sample.
[0077] The purity analysis method is the same as in Example 1. The composition of ultrapure manganese obtained in Example 3 is shown in Table 4.
[0078] Table 4. Content of ultrapure manganese obtained in Example 3 (unit: ppm, wt)
[0079] element content element content element content element content Li <0.01 Ni 0.78 Sn 0.12 Hf <0.01 Be <0.01 Cu 2 Sb 0.2 Ta <0.01 B 0.01 Zn <0.2 Te <0.05 W 0.1 F <0.05 Ga <0.05 I <0.05 Re <0.05 Na 0.2 Ge <0.05 Cs <0.01 Os <0.01 Mg 0.85 As 0.21 Ba <0.01 Ir <0.01 Al 0.05 Se 0.5 La <0.01 Pt <0.01 Si 0.45 Br <0.05 Ce <0.01 Au <0.05 P 0.29 Rb <0.05 Pr <0.01 Hg <0.05 S 0.2 Sr <0.05 Nd <0.01 Tl <0.01 Cl <0.01 Y <0.01 Sm <0.01 Pb <0.05 K 0.08 Zr <0.05 Eu <0.01 Bi <0.01 Ca 0.33 Nb 0.05 Gd <0.05 Th <0.005 Sc <0.05 Mo 0.25 Tb <0.01 U <0.005 Ti 0.04 Ru <0.01 Dy <0.01 H 10 V <0.01 Rh <0.01 Ho <0.01 C 0.05 Cr 0.03 Pd <0.05 Er <0.01 N 7 Mn principal component Ag <0.01 Tm <0.01 O 10 Fe 0.13 Cd <0.01 Yb <0.01 Co 1 In <0.05 Lu <0.01
[0080] Example 4
[0081] An ultrapure manganese and its preparation method. The specific steps are as follows:
[0082] 1. Use 1 kg of commercially available 3N grade electrolytic manganese flakes as raw material, and perform surface chemical cleaning with dilute hydrochloric acid (pH value 5) until the surface of the electrolytic manganese flakes has a silvery-white metallic luster. Then, clean with distilled water and alcohol in sequence, and dry.
[0083] 2. Electrolytic manganese flakes, after surface chemical cleaning, are mixed with low-melting-point metal additives (2 wt.% Ca, 6 wt.% Al) and placed in a vacuum induction furnace at an absolute pressure of 8 × 10⁻⁶. 3 The smelting process begins at Pa. After smelting is complete, the sample is removed, the surface layer is removed, and crude manganese is obtained.
[0084] 3. For the high melting point metal additive, tantalum powder with an average diameter of 130μm and a tantalum to manganese mass ratio of 1:15 is selected.
[0085] 4. For the first distillation, mix the crude manganese with the high-melting-point metal additive and place the mixture in a crucible. Evacuate to a vacuum of 1×10⁻⁶. -5 Pa; heating is started at a rate of 5℃ / min, the melt temperature in the crucible is 1270℃, the first distillation begins, the temperature of the multi-stage condenser is 510~850℃, and the absolute pressure during distillation is maintained at 10. -5 ~10 -2 Pa; distillation time is 1 hour, heating is stopped after distillation; vacuum cooling, vacuum is applied to 10°C during cooling. -5 Pa level; after cooling to room temperature, introduce high-purity nitrogen gas and start the furnace.
[0086] 5. For the second distillation, first remove the multi-stage condenser from the first distillation and replace it with a brand new multi-stage condenser; then begin evacuating to 10°C. -5 Pa level; then heating was started at a rate of 5℃ / min, and the melt temperature in the crucible was 1430℃, initiating the second distillation; the temperature of the condenser was 600~1070℃; the distillation time was 8h, and after the second distillation, vacuum cooling was performed, with a vacuum level of 10℃ during cooling. -5 The sample was taken at the Pa level, cooled to room temperature, filled with high-purity nitrogen, and the furnace was opened to remove the ultrapure manganese sample.
[0087] The purity analysis method is the same as in Example 1. The composition of ultrapure manganese obtained in Example 4 is shown in Table 5.
[0088] Table 5. Content of ultrapure manganese obtained in Example 4 (unit: ppm, wt)
[0089] element content element content element content element content Li <0.01 Ni 0.48 Sn 0.2 Hf <0.01 Be <0.01 Cu 1 Sb 0.2 Ta <0.01 B 0.01 Zn <0.2 Te <0.05 W 0.1 F <0.05 Ga <0.05 I <0.05 Re <0.05 Na 0.2 Ge <0.05 Cs <0.01 Os <0.01 Mg 0.33 As 0.21 Ba <0.01 Ir <0.01 Al 0.05 Se 0.5 La <0.01 Pt <0.01 Si 0.3 Br <0.05 Ce <0.01 Au <0.05 P 0.4 Rb <0.05 Pr <0.01 Hg <0.05 S 0.3 Sr <0.05 Nd <0.01 Tl <0.01 Cl <0.01 Y <0.01 Sm <0.01 Pb <0.05 K 0.05 Zr <0.05 Eu <0.01 Bi <0.01 Ca 0.2 Nb 0.05 Gd <0.05 Th <0.005 Sc <0.05 Mo 0.15 Tb <0.01 U <0.005 Ti 0.04 Ru <0.01 Dy <0.01 H 13 V <0.01 Rh <0.01 Ho <0.01 C 0.05 Cr 0.04 Pd <0.05 Er <0.01 N 6 Mn principal component Ag <0.01 Tm <0.01 O 12 Fe 0.13 Cd <0.01 Yb <0.01 Co 0.05 In <0.05 Lu <0.01
[0090] Comparative Example 1
[0091] The only difference between Comparative Example 1 and Example 1 is that Comparative Example 1 involves only one distillation step, without a primary distillation step, and the distillation parameters are consistent with the secondary distillation parameters of Example 1. The purity analysis method for Comparative Example 1 is the same as that for Example 1, and the manganese content obtained is shown in Table 6.
[0092] Table 6 shows the manganese content obtained in Comparative Example 1, in ppm and wt.
[0093] element content element content element content element content Li <0.01 Ni 1 Sn 0.44 Hf <0.01 Be <0.01 Cu 38 Sb 1.2 Ta <0.01 B 0.02 Zn <0.1 Te <0.05 W 0.14 F <0.05 Ga <0.05 I <0.05 Re <0.05 Na 0.5 Ge <0.05 Cs <0.01 Os <0.01 Mg 1.7 As 0.24 Ba <0.01 Ir <0.01 Al 0.08 Se 0.2 La <0.01 Pt <0.01 Si 7.6 Br <0.05 Ce <0.01 Au <0.05 P 0.29 Rb <0.05 Pr <0.01 Hg <0.05 S 4.8 Sr <0.05 Nd <0.01 Tl <0.05 Cl <0.01 Y <0.05 Sm <0.01 Pb <0.05 K 2.1 Zr <0.05 Eu <0.01 Bi <0.01 Ca 1 Nb 1 Gd <0.01 Th <0.005 Sc <0.05 Mo 0.2 Tb <0.01 U <0.005 Ti 0.04 Ru <0.01 Dy <0.01 H <15 V <0.01 Rh <0.01 Ho <0.01 C 0.08 Cr 0.83 Pd <0.05 Er <0.01 N <5 Mn principal component Ag <0.05 Tm <0.01 O 9 Fe 0.93 Cd <0.05 Yb <0.01 Co 0.32 In <0.05 Lu <0.01
[0094] Comparative Example 2
[0095] The only difference between Comparative Example 2 and Example 1 is that the commercially available electrolytic manganese is not surface-cleaned or smelted, but is directly used as the raw material for the two-step distillation. The purity analysis method for Comparative Example 2 is the same as that for Example 1, and the manganese content obtained is shown in Table 7.
[0096] Table 7 shows the manganese content obtained in Comparative Example 2, in ppm and wt.
[0097] element content element content element content element content Li <0.01 Ni 1 Sn 0.44 Hf <0.01 Be <0.01 Cu 0.05 Sb 0.1 Ta <0.01 B 0.02 Zn <0.1 Te <0.05 W 0.14 F <0.05 Ga <0.05 I <0.05 Re <0.05 Na 0.5 Ge <0.05 Cs <0.01 Os <0.01 Mg 0.3 As 0.24 Ba <0.01 Ir <0.01 Al 0.08 Se 0.2 La <0.01 Pt <0.01 Si 0.5 Br <0.05 Ce <0.01 Au <0.05 P 0.29 Rb <0.05 Pr <0.01 Hg <0.05 S 14 Sr <0.05 Nd <0.01 Tl <0.05 Cl <0.01 Y <0.05 Sm <0.01 Pb <0.05 K 0.7 Zr <0.05 Eu <0.01 Bi <0.01 Ca 0.5 Nb 1 Gd <0.01 Th <0.005 Sc <0.05 Mo 0.2 Tb <0.01 U <0.005 Ti 0.04 Ru <0.01 Dy <0.01 H <15 V <0.01 Rh <0.01 Ho <0.01 C 0.08 Cr 0.57 Pd <0.05 Er <0.01 N <5 Mn principal component Ag <0.05 Tm <0.01 O 600 Fe 0.57 Cd <0.05 Yb <0.01 Co 0.44 In <0.05 Lu <0.01
[0098] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, and not to limit them; although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some of the technical features; and these modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for preparing ultrapure manganese, characterized in that, Includes the following steps: Raw manganese is mixed with low-melting-point metal additives and then vacuum-melted to obtain crude manganese. Before mixing the raw manganese with the low-melting-point metal additives, the surface of the raw manganese is chemically cleaned with an acidic solution. The crude manganese is mixed with a high-melting-point metal additive to obtain a mixture. The mixture is then separated by two-stage distillation under low vacuum conditions to obtain manganese vapor. The manganese vapor is collected to obtain ultrapure manganese. The high-melting-point metal is selected from one or more of tungsten, molybdenum, tantalum, rhenium, and iridium. In the two-stage distillation, the first stage distillation essentially separates impurities with melting points below the melting point of manganese from the mixture, and the content of these impurities is below 5 ppm, while in the second stage distillation, manganese is separated from the mixture. The mixture obtained by mixing the crude manganese and the high-melting-point metal is placed in a crucible for the two-stage distillation, and the manganese vapor is collected using a condenser. The temperature of the condenser plate is 500~1100℃ when collecting the manganese vapor; The low-melting-point metal is selected from one or more of zinc, calcium, and magnesium.
2. The method for preparing ultrapure manganese according to claim 1, characterized in that, The temperature of the mixture in the first stage of distillation is 1250~1300℃.
3. The method for preparing ultrapure manganese according to claim 2, characterized in that, The distillation time for the first stage of distillation is 0.5~2 hours; And / or, the absolute pressure during the first stage of distillation is 10. -5 ~10 -2 Pa.
4. The method for preparing ultrapure manganese according to any one of claims 1 to 3, characterized in that, The temperature of the mixture in the second stage of distillation is 1350~1450℃.
5. The method for preparing ultrapure manganese according to claim 4, characterized in that, The absolute pressure during the second stage of distillation is 10. -5 ~10 -2 Pa.
6. The method for preparing ultrapure manganese according to any one of claims 1 to 3 and 5, characterized in that, The amount of the low-melting-point metal additive is 1 to 10% based on the mass of the raw material manganese.
7. The method for preparing ultrapure manganese according to claim 4, characterized in that, The amount of the low-melting-point metal additive is 1 to 10% based on the mass of the raw material manganese.
8. The method for preparing ultrapure manganese according to claim 6, characterized in that, The low-melting-point metal is calcium and magnesium in a mass ratio of 1 to 3:1; the amount of the low-melting-point metal additive is 2 to 5% based on the mass of the raw material manganese.
9. The method for preparing ultrapure manganese according to claim 7, characterized in that, The low-melting-point metal is calcium and magnesium in a mass ratio of 1 to 3:1; the amount of the low-melting-point metal additive is 2 to 5% based on the mass of the raw material manganese.
10. The method for preparing ultrapure manganese according to any one of claims 1-3, 5, 7-9, characterized in that, The mass ratio of crude manganese to the high-melting-point metal is in the range of 1 to 20:
1.
11. The method for preparing ultrapure manganese according to claim 4, characterized in that, The mass ratio of crude manganese to the high-melting-point metal is in the range of 1 to 20:
1.
12. The method for preparing ultrapure manganese according to claim 6, characterized in that, The mass ratio of crude manganese to the high-melting-point metal is in the range of 1 to 20:
1.
13. The method for preparing ultrapure manganese according to claim 10, characterized in that, The mass ratio of crude manganese to the high-melting-point metal is in the range of 10 to 15:
1.
14. The method for preparing ultrapure manganese according to claim 11 or 12, characterized in that, The mass ratio of crude manganese to the high-melting-point metal is in the range of 10 to 15:
1.
15. The method for preparing ultrapure manganese according to any one of claims 1-3, 5, 7-9, and 11-13, characterized in that, The vacuum melting is either vacuum induction melting or vacuum arc melting; an inert gas is introduced during the vacuum melting process, and the absolute pressure during the vacuum melting process is 10. 4 Pa level or below 10 4 Pa level.
16. The method for preparing ultrapure manganese according to claim 4, characterized in that, The vacuum melting is either vacuum induction melting or vacuum arc melting; an inert gas is introduced during the vacuum melting process, and the absolute pressure during the vacuum melting process is 10. 4 Pa level or below 10 4 Pa level.
17. The method for preparing ultrapure manganese according to claim 6, characterized in that, The vacuum melting is either vacuum induction melting or vacuum arc melting; an inert gas is introduced during the vacuum melting process, and the absolute pressure during the vacuum melting process is 10. 4 Pa level or below 10 4 Pa level.
18. The method for preparing ultrapure manganese according to claim 10, characterized in that, The vacuum melting is either vacuum induction melting or vacuum arc melting; an inert gas is introduced during the vacuum melting process, and the absolute pressure during the vacuum melting process is 10. 4 Pa level or below 10 4 Pa level.
19. The method for preparing ultrapure manganese according to claim 14, characterized in that, The vacuum melting is either vacuum induction melting or vacuum arc melting; an inert gas is introduced during the vacuum melting process, and the absolute pressure during the vacuum melting process is 10. 4 Pa level or below 10 4 Pa level.
20. The method for preparing ultrapure manganese according to claim 15, characterized in that, The absolute pressure during the vacuum melting is 10. 3 Pa level.
21. The method for preparing ultrapure manganese according to claim 20, characterized in that, The absolute pressure during the vacuum melting is 1×10⁻⁶. 3 Pa ~ 9×10 3 Pa.
22. The method for preparing ultrapure manganese according to any one of claims 1-3, 5, 7-9, 11-13, 16-21, characterized in that, The pH of the acidic solution is 3 to 6.
8.
23. The method for preparing ultrapure manganese according to claim 4, characterized in that, The pH of the acidic solution is 3 to 6.
8.
24. The method for preparing ultrapure manganese according to claim 6, characterized in that, The pH of the acidic solution is 3 to 6.
8.
25. The method for preparing ultrapure manganese according to claim 10, characterized in that, The pH of the acidic solution is 3 to 6.
8.
26. The method for preparing ultrapure manganese according to claim 14, characterized in that, The pH of the acidic solution is 3 to 6.
8.
27. The method for preparing ultrapure manganese according to claim 15, characterized in that, The pH of the acidic solution is 3 to 6.
8.
28. The method for preparing ultrapure manganese according to claim 22, characterized in that, The pH of the acidic solution is 5-6.
29. The method for preparing ultrapure manganese according to any one of claims 1-3, 5, 7-9, 11-13, 16-21, 23-28, characterized in that, Also includes: After the vacuum melting, the resulting block is subjected to surface machining to obtain crude manganese.
30. The method for preparing ultrapure manganese according to claim 4, characterized in that, Also includes: After the vacuum melting, the resulting block is subjected to surface machining to obtain crude manganese.
31. The method for preparing ultrapure manganese according to claim 6, characterized in that, Also includes: After the vacuum melting, the resulting block is subjected to surface machining to obtain crude manganese.
32. The method for preparing ultrapure manganese according to claim 10, characterized in that, Also includes: After the vacuum melting, the resulting block is subjected to surface machining to obtain crude manganese.
33. The method for preparing ultrapure manganese according to claim 14, characterized in that, Also includes: After the vacuum melting, the resulting block is subjected to surface machining to obtain crude manganese.
34. The method for preparing ultrapure manganese according to claim 15, characterized in that, Also includes: After the vacuum melting, the resulting block is subjected to surface machining to obtain crude manganese.
35. The method for preparing ultrapure manganese according to claim 22, characterized in that, Also includes: After the vacuum melting, the resulting block is subjected to surface machining to obtain crude manganese.
36. The method for preparing ultrapure manganese according to claim 29, characterized in that, The surface machining is selected from any one or more combinations of turning, milling, planing, and grinding.
37. An ultrapure manganese, characterized in that, It is prepared by the method for preparing ultrapure manganese according to any one of claims 1 to 36.
Citation Information
Patent Citations
Preparation process of electrolytic refined high-purity manganese
CN105200453A
Method for purifying metal manganese through vacuum distillation
CN113897501A