Double-layer pipe interface friction coefficient testing device and method

By designing a double-layer tube interface friction coefficient test device, the high-temperature interface friction coefficient of the double-layer tube is measured by heating and air pressure control, the problem of large measurement deviation in the prior art is solved, and the accuracy of the thermal bending forming environment of titanium alloy materials is achieved. Reflect, improve the accuracy of measurement results.

CN114993931BActive Publication Date: 2024-12-06DALIAN SHUANGHANG FORMING TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210576808.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-05-25
Publication Date
2024-12-06
Estimated Expiration
2042-05-25

AI Technical Summary

Technical Problem

The existing testing methods cannot accurately measure the interfacial friction coefficient of the double-layer tube structure at high temperatures, especially in the thermal bending and forming process of titanium alloy materials. Traditional methods have problems such as changes in contact surfaces, strain influence and deviations, which are difficult to apply. Interface friction process in pipe structure.

Method used

A double-layer tube interface friction coefficient testing device is designed, including a working mold frame, heating device, compressed air source, mechanical sliding device and compression device. By heating the double-layer tube, the measurement between the inner sealed tube and the outer tube is measured. The friction force and contact area are used to calculate the friction coefficient using the air pressure controller and force sensor to ensure the accuracy of the measurement.

Benefits of technology

Improve the accuracy of the test of high-temperature friction coefficient of the double-layer tube interface, avoid the deviation problem of traditional methods, can accurately guide and solve wrinkle problems in metal hot pressing and bending forming, and use servo motor and air pressure control to achieve high-temperature titanium tube displacement Dual control and air pressure reduce heat loss.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114993931B_ABST
    Figure CN114993931B_ABST
Patent Text Reader

Abstract

The present invention discloses a device and method for testing the high-temperature interface friction coefficient of a double-layer tube, and relates to the field of metal forming manufacturing technology. The device includes: a working mold frame, a double-layer tube, a heating device, a compressed gas source, an air pressure control cabinet, a mechanical sliding device, and a data acquisition device; the method includes: sealing the inner tube with a head to form a closed tube; hot-fitting the closed tube into the outer tube to form a double-layer tube; the double-layer tube is clamped on the working mold frame and connected to the mechanical sliding device; after the heating device heats the double-layer tube to the target temperature, compressed gas is introduced; the mechanical sliding device drives the closed tube to move axially relative to the outer tube; the data acquisition device is provided with force, displacement, temperature, and air pressure sensors to collect data, and the high-temperature interface friction coefficient of the double-layer tube is calculated by formula. The high-temperature interface friction coefficient measured by the device and method of the present invention has high accuracy, which solves the problem that there is no suitable measurement method for the high-temperature interface friction coefficient of double-layer tubes of heterogeneous materials, and reduces the energy consumption of high-temperature interface friction coefficient testing.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of metal forming and manufacturing, and in particular to a device and method for testing the friction coefficient of a double-layer pipe interface. Background Art

[0002] Tube bending is a common forming technology for preparing integral elbows, ring shells and other parts. The bending of large-sized thin-walled tubes is affected by the inner compressive stress and the outer tensile stress, and it is very easy to wrinkle on the inside and reduce the thickness of the outer wall. In order to suppress wrinkling defects, a double-layer tube structure is often used as the original blank for bending. After bending, the outer tube is removed to obtain an inner thin-walled bent tube. Titanium alloy ring shells are an important structural form of fuel tanks for aerospace and other carriers. Titanium alloys have high strength, low elastic modulus and poor plasticity at room temperature. Its overall bending is extremely difficult and needs to be bent in a heated state. Therefore, hot bending of double-layer tube structures is an advanced technology for manufacturing large-sized thin-walled bent titanium tubes.

[0003] During the double-layer tube bending process, there is friction at the interface of the tube blank of different materials, which has a great influence on the material flow and deformation behavior. The interface friction affects the thinning and distribution of the wall thickness of the inner titanium tube on the outer side of the bending tension. For the inner side, the interface friction reduces the compressive stress on the inner side to a certain extent, causing the stress neutral layer to move and the trend of instability wrinkling to change. Therefore, it is necessary to measure the high-temperature interface friction coefficient to control the friction effect of the double-layer tube deformation.

[0004] For the interface friction coefficient, the existing testing methods mainly include reciprocating friction test method, cup drawing friction test method, strip tensile bending test method and flat plate sliding friction test method.

[0005] The cup-shaped drawing friction test method uses a punch to draw the sheet into a cup shape. By recording the punch force and the blank holder force, the friction coefficient can be calculated. The disadvantages of the cup-shaped drawing friction test method are: the friction area of ​​the contact surface changes during the test, there are many influencing factors, and the force conditions are relatively complex, so the results obtained have certain deviations.

[0006] The strip tensile bending test method uses front and rear clamps to clamp the strip, and uses the force controlled by the motor to keep the rear clamp clamped while pulling the strip with the front clamp, so that the strip slides around the tool pin, and the piezoelectric torque sensor on the tool pin directly measures the friction and obtains the friction coefficient. The defects of this test method are: 1) The obtained friction coefficient value depends on the test configuration, such as the pin radius; 2) The strain changes near the instrument pin and the test machine clamp are not considered, and the obtained value is somewhat different from the actual friction coefficient.

[0007] The plate sliding friction test method uses the chuck part of the tensile device to clamp the strip steel, so that the strip steel moves at a constant speed with the tensile device. The strip steel is compressed by the compression device under a given load, and the friction coefficient can be calculated based on the compression load and the tensile load. However, as the pressure increases, the actual contact area between the material plate and the compression device will inevitably increase due to the deformation of the material, causing the measured friction coefficient to gradually deviate from the normal value.

[0008] The reciprocating friction test method mainly consists of a test head and a thin plate sample. The contact between the end face of the test head and the thin plate sample forms a point contact and can apply a high contact pressure usually encountered in metal forming applications. The disadvantage of this method is that the point contact state between the test material and the test head is different from the surface contact state of the double-layer material, and it is not suitable for the measurement of the friction coefficient of the double-layer material contact; moreover, the adhesion effect of the reciprocating material cannot be eliminated.

[0009] In summary, the existing methods are not applicable to the interface friction process of tube structures. At the same time, since titanium alloy materials need to be hot formed, the measured friction coefficient should be the high-temperature interface friction coefficient.

[0010] Therefore, there is an urgent need for a device and method for measuring the high-temperature friction coefficient of the interface of a double-layer tube structure to solve the above-mentioned problems existing in the prior art. Summary of the invention

[0011] The purpose of the present invention is to provide a double-layer pipe interface friction coefficient testing device and method to solve the above-mentioned problems existing in the prior art, improve the accuracy of high-temperature friction coefficient testing of the double-layer pipe interface, and avoid the problem of large deviation in traditional friction measurement methods.

[0012] To achieve the above object, the present invention provides the following solutions:

[0013] The present invention provides a double-layer pipe interface friction coefficient testing device, comprising:

[0014] A working mold frame, used for carrying a double-layer tube, wherein the double-layer tube comprises an outer tube and an inner closed tube, wherein the outer tube is heat-shrink-fitted onto the outer side of the inner closed tube, and the inner wall of the outer tube matches the outer wall of the inner closed tube;

[0015] A heating device, used to heat the double-layer tube to a preset temperature, wherein a temperature sensor is provided on the double-layer tube;

[0016] A compressed gas source is connected to the inner closed tube and is used to introduce compressed gas into the inner closed tube. The compressed gas source is connected to a gas pressure controller and is used to control the pressure of the gas delivered to the closed tube.

[0017] A mechanical sliding device connected to the inner closed tube and used to drive the inner closed tube to move axially relative to the outer tube, the mechanical sliding device being connected to a force sensor and a displacement sensor;

[0018] A pressing device, used for pressing the outer tube onto the working mold frame when the inner closed tube and the outer sleeve move relative to each other;

[0019] A data acquisition device is connected to the force sensor, the displacement sensor, the temperature sensor and the air pressure controller, and is used to collect load data and displacement data of the mechanical sliding device, temperature data of the double-layer tube and air pressure data of the air pressure controller.

[0020] Preferably, the heating device adopts an induction heating coil, which is sleeved on the outside of the double-layer tube. The induction heating coil is also connected to an induction heater. The induction heater can adjust the power of the induction heating coil to heat the double-layer tube to a preset temperature through the temperature data feedback of the double-layer tube measured by the temperature sensor.

[0021] Preferably, the outer wall of the double-layer tube is wrapped with a thermal insulation layer to reduce heat loss when the heating device heats the double-layer tube.

[0022] Preferably, the outer layer tube is a steel tube; the inner layer closed tube includes a titanium tube, an upper head and a lower head, the upper and lower ends of the titanium tube are respectively sealed and connected with the upper head and the lower head, the upper head is processed with a flange hole, and the mechanical sliding device is connected to the upper head through a flange.

[0023] Preferably, the inner closed tube and the outer tube are interference fit to compensate for the different thermal expansion amounts of the steel tube and the titanium tube after heating.

[0024] Preferably, the mechanical sliding device adopts a servo motor.

[0025] Preferably, the lower end cap is provided with an air inlet hole, the air inlet hole is connected to the compressed air source through an air pipe, the air pressure controller adopts an air pressure control cabinet, which is used to control the pressurization rate to reach a preset pressure and realize pressure maintenance, and the air pressure control cabinet is installed on the air pipe between the compressed air source and the lower end cap;

[0026] The gas pressure in the double-layer tube can ensure that the double-layer tube does not produce plastic yield.

[0027] Preferably, the working mold frame comprises a mold frame lower table and a mold frame upper top surface, the mold frame lower table surface is mounted with mold frame columns, and the mold frame upper top surface is mounted on the mold frame columns and can move up and down along the mold frame columns;

[0028] The outer tube is installed on the lower table of the mold frame by bolts, and a heat insulating gasket is arranged between the outer tube and the lower table of the mold frame to prevent the heat from being transferred to the lower table of the mold frame and causing damage and heat loss of the double tube when the heating device heats the double tube;

[0029] An upper through hole for the mechanical sliding device to pass through is provided on the top surface of the mold frame, a lower through hole and a flange hole for the air pipe of the compressed air source device to pass through are provided on the lower surface of the mold frame, and the double-layer tube is connected to the flange hole on the lower surface of the mold frame by screws.

[0030] Preferably, the pressing device comprises a lower pressing block and a cylinder, the lower pressing block can press the outer tube, and a heat insulating gasket is provided at the contact position between the lower pressing block and the outer tube to prevent the heat from being transferred to the lower pressing block and causing damage and heat loss of the double tube when the heating device heats the double tube;

[0031] The lower pressing block is installed below the upper top surface of the mold frame, and a lower pressing block through hole corresponding to the upper through hole is opened on the lower pressing block; the cylinder is connected to the upper top surface of the mold frame and can drive the upper top surface of the mold frame and the lower pressing block to move.

[0032] The present invention also provides a method for testing the friction coefficient of a double-layer pipe interface, using the above-mentioned double-layer pipe interface friction coefficient testing device, comprising the following steps:

[0033] Step 1), according to preset parameters, an inner tube and an outer tube are obtained respectively, wherein the inner tube and the outer tube are a titanium tube and a steel tube respectively, and the steel tube and the titanium tube are assembled into a double-layer tube by shrink-fitting;

[0034] Step 2), sealing the inner tube to form an inner closed tube, installing the double-layer tube to the working mold frame, and heating the double-layer tube to a preset temperature;

[0035] Step 3), introducing compressed gas into the inner closed tube to make the gas pressure in the inner closed tube reach a preset pressure;

[0036] Step 4), pulling the inner closed tube at a constant speed to a specified displacement, and recording the load of the mechanical sliding device;

[0037] Step 5), calculate the friction coefficient.

[0038] Preferably, in step 1), the outer diameter of the titanium tube is D1, the inner diameter of the titanium tube is d, the wall thickness of the titanium tube is t1, and the length of the titanium tube is H; the outer diameter of the steel tube is D2, the inner diameter of the steel tube is D1, the wall thickness of the steel tube is t2, and the length of the steel tube is H.

[0039] Preferably, in step 1), the temperature range of the heat-fitting is 850-900°C, and the interference is calculated according to the test temperature. The calculation formula of the interference is δ=α Fe D(T1-T0)-α Ti D(T1-T0); where D is the interface diameter at high temperature test temperature, α Fe and α Ti is the thermal expansion coefficient of the steel pipe and the titanium pipe at high temperature, T1 is the temperature of the steel pipe and the titanium pipe, and T0 is the room temperature.

[0040] Preferably, in step 2), an upper head and a lower head with a diameter of d are obtained, the upper head is welded to one end of the titanium tube, and the lower head is welded to the other end of the titanium tube to form a closed titanium tube; the titanium tube is welded by one of arc welding and laser welding.

[0041] Preferably, in step 2), the double-layer tube is installed on the working mold frame, the induction heating coil and the thermal insulation layer are installed, and the cylinder is started to make the lower pressure block press the steel tube with a preset pressure. The pressure is large enough not to cause the double-layer tube to yield, and the yield limit is determined by the material with a smaller yield limit in the double-layer tube at the test temperature.

[0042] Preferably, in step 2), the double-layer tube is heated to a preset temperature of 850-900°C.

[0043] Preferably, in step 3), the preset gas pressure range in the double-layer tube should ensure that the double-layer tube does not produce plastic yield, and the calculation formula of the gas pressure is P = σ si ln[r m / (r m -t1)]+(1-r m 2 / b 2 )σ so / 2, where P is the gas pressure, σ si is the material yield limit of the titanium tube, r m is the inner wall radius of the steel tube, t1 is the wall thickness of the titanium tube, b is the outer wall radius of the steel tube, σ so is the material yield limit of the steel pipe.

[0044] Preferably, in step 4), the displacement range of the inner closed tube is 0-H, the speed range is 0-v, the speed is kept uniform, and the size is adjusted according to the needs of the test grouping. The contact area between the titanium tube and the steel tube is calculated using the formula S=πD(H-vt), where S is the contact area; D is the outer diameter of the titanium tube; H is the length of the titanium tube; v is the movement speed of the titanium tube; and t is the time.

[0045] Preferably, in step 5), the friction coefficient is calculated using the formula μPS=F, where μ is the friction coefficient; P is the pressure; S is the contact area; and F is the servo motor load. By taking multiple tests with different speeds v and internal pressures P and collecting sufficient data, the friction coefficient μ can be calculated using the above formula.

[0046] Compared with the prior art, the present invention has achieved the following technical effects:

[0047] The present invention drives the inner closed tube to move at a constant speed through a mechanical sliding device, measures the pulling force generated by the mechanical sliding device on the inner closed tube through a force sensor, and the pulling force is the same as the friction force between the inner closed tube and the outer closed tube, so that the friction force can be obtained; the air pressure in the inner closed tube is controlled by an air pressure controller; the displacement of the inner closed tube relative to the outer closed tube is obtained by a displacement sensor, and then the contact area between the inner closed tube and the outer closed tube is obtained, and then according to the contact area between the inner closed tube and the outer tube, the air pressure in the inner closed tube and the friction force, the double-layer tube interface friction coefficient can be measured through μPS=F. The present invention can heat the double-layer tube through a heating device to measure its high-temperature interface friction coefficient.

[0048] The present invention adopts a double-layer tube measurement method to measure the high-temperature interface friction coefficient, restores the environment and force conditions in metal hot press bending, improves the accuracy of the measurement results, avoids the problem of large deviation in traditional friction measurement methods, and can be used to guide the solution of problems such as wrinkling in metal hot press bending involving high-temperature interface friction.

[0049] Furthermore, other technical solutions in the present invention have achieved the following technical effects compared with the prior art:

[0050] 1. The present invention adopts a servo motor and an air pressure control cabinet to realize dual control of the displacement process of the high-temperature titanium tube and the air pressure inside the tube, thereby realizing the measurement of the high-temperature interface friction coefficient of the double-layer tube under different process parameters;

[0051] 2. The present invention uses a double-layer tube measurement method and introduces a thermal insulation layer and a thermal insulation gasket, which can effectively reduce the heat loss during the friction coefficient measurement process. The experimental process can truly reflect the high temperature environment of the actual tube bending process;

[0052] 3. The double-layer tube in the present invention adopts induction heating rather than the traditional environmental heating furnace heating method, which significantly improves the heating efficiency and shortens the process cycle. At the same time, it can avoid the heat loss of the tube during the transfer process from the heating furnace and improve the accuracy of the measurement results. BRIEF DESCRIPTION OF THE DRAWINGS

[0053] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0054] Figure 1 Schematic diagram of the structure of a double-layer tube interface friction coefficient testing device in an embodiment of the present invention;

[0055] Figure 2 Schematic diagram of the process of testing the friction coefficient of the double-layer tube interface in an embodiment of the present invention;

[0056] Figure 3 Schematic diagram of the moving position of the double-layer tube interface friction coefficient testing device in an embodiment of the present invention;

[0057] Figure 4 Schematic diagram of the stress state of the inner closed tube in the method for testing the coefficient of friction at the interface of a double-layer tube in an embodiment of the present invention;

[0058] Figure 5 Schematic diagram of the stress state of the inner closed tube unit body in the method for testing the interface friction coefficient of the double-layer tube in an embodiment of the present invention.

[0059] Explanation of the reference numerals: 1- lower table of mold frame; 2- mold frame column; 3- upper top surface of mold frame; 4- induction heating coil; 5- temperature control box; 6- titanium tube; 7- steel tube; 8- upper head; 9- lower head; 10- lower pressure block; 11- servo motor; 12- compressed air source; 13- air pressure control cabinet; 14- cylinder; 15- thermal insulation layer; 16- thermal insulation gasket. DETAILED DESCRIPTION

[0060] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0061] The purpose of the present invention is to provide a double-layer pipe interface friction coefficient testing device and method to solve the above-mentioned problems existing in the prior art, improve the accuracy of high-temperature friction coefficient testing of the double-layer pipe interface, and avoid the problem of large deviation in traditional friction measurement methods.

[0062] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the present invention is further described in detail below with reference to the accompanying drawings and specific embodiments.

[0063] Embodiment 1

[0064] like Figure 1 As shown, a double-layer tube interface friction coefficient testing device is provided in this embodiment, which mainly includes a working mold frame, a heating device, a compressed air source device, a mechanical sliding device and a pressing device; wherein, the working mold frame is used to carry the double-layer tube, the double-layer tube includes an outer tube and an inner closed tube, both ends of the inner closed tube are closed, the outer tube is heat-fitted on the outer side of the inner closed tube, the inner wall of the outer tube and the outer wall of the inner closed tube are interference fit, the outer tube and the inner closed tube are preferably circular tubes, or other shapes of tubes can be selected according to work needs, such as square tubes, irregular tubes, etc.; the heating device is used to heat the double-layer tube to simulate a high-temperature environment and realize a high-temperature interface friction coefficient test; the compressed air source device is connected to the inner closed tube, and is used to introduce compressed gas into the inner closed tube to establish gas pressure in the double-layer tube; the mechanical sliding device is connected to the inner closed tube, and is used to drive the inner closed tube to move axially relative to the outer tube; the pressing device is used to press the outer tube against the working mold frame when the inner closed tube moves.

[0065] In this embodiment, the heating device preferably uses an induction heating coil 4, which is sleeved on the outside of the double-layer tube, one end of the induction heating coil 4 is connected to the positive electrode of the induction heater, and the other end of the induction heating coil 4 is connected to the negative electrode of the induction heater; the induction heater is also connected to a temperature control box 5 to control the heating temperature of the induction heating coil 4, and the temperature control box 5 can also be connected to a temperature sensor, which is installed on the double-layer tube. In this embodiment, the double-layer tube is heated by the induction heating coil 4 to a preset temperature. Alternatively, other heating devices can be selected according to work needs, such as a current self-resistance heating device or an electric heating water pipe.

[0066] In this embodiment, the outer wall of the double-layer pipe is wrapped with a thermal insulation layer 15, and the thermal insulation layer 15 is made of commonly used thermal insulation materials, such as aluminum foil thermal insulation materials, rock wool thermal insulation materials, etc.

[0067] In this embodiment, the outer tube and the inner closed tube are preferably made of different materials; further, the outer tube is a steel tube 7, the material of the steel tube 7 is stainless steel or low carbon steel, preferably stainless steel; the inner closed tube includes a titanium tube 6, the material of the titanium tube 6 is titanium alloy, and the titanium alloy is preferably one of α-type titanium alloy or α+β-type titanium alloy; preferably, the length of the steel tube 7 is the same as that of the titanium tube 6, and the inner diameter of the steel tube 7 is equal to the outer diameter of the titanium tube 6. Among them, the outer tube and the inner closed tube can also be made of other materials according to work needs.

[0068] In this embodiment, the upper and lower ends of the titanium tube 6 are respectively sealed with an upper head 8 and a lower head 9, and the mechanical sliding device is connected to the upper head 8; wherein the upper head 8 and the lower head 9 are respectively welded to the upper and lower ends of the titanium tube 6 to play a sealing role, and the welding method is preferably one of laser welding or argon arc welding. Alternatively, the sealed connection between the upper head 8 and the lower head 9 and the titanium tube 6 can also be achieved by other methods, such as threaded connection.

[0069] In this embodiment, the outer tube and the inner closed tube are interference fit to compensate for the different thermal expansion amounts of the outer tube and the inner closed tube after heating.

[0070] In this embodiment, the mechanical sliding device preferably uses a servo motor 11, which is connected to the upper head 8; specifically, the output shaft of the servo motor 11 is connected to a lead screw, which is connected to a slider, and the lead screw is driven to rotate by the servo motor 11, thereby driving the slider to move along the lead screw, and the slider is connected to the upper head 8 through a connecting rod, so that the entire inner closed tube can be driven to move; a flange hole is also provided on the upper head 8 to facilitate connection with the connecting rod; this embodiment uses the speed control mode of the servo motor 11 to pull out the inner closed tube at a uniform speed, wherein the servo motor 11 can measure the load F1 through its own force sensor. Alternatively, other mechanical sliding devices such as cylinders, linear motors, etc. can be selected according to work needs.

[0071] In this embodiment, the compressed air source device includes a compressed air source 12 and an air pressure control cabinet 13. An air hole is provided on the lower head 9, and the air hole is connected to the compressed air source 12 through an air pipe; the air pressure control cabinet 13 is installed on the air pipe between the compressed air source 12 and the lower head 9, and its two ends are respectively connected to the compressed air source 12 and the inner closed tube. The air pressure control cabinet 13 is used to control the gas pressure delivered to the inner closed tube.

[0072] Furthermore, the compressed gas provided by the compressed gas source 12 is preferably one of air, nitrogen, helium and argon; the gas pressure in the double-layer tube ensures that the double-layer tube does not produce plastic yield, and is preferably 0.1-10 MPa.

[0073] In this embodiment, the double-layer tube is preferably arranged vertically, and the working mold frame includes a mold frame lower table surface 1 and a mold frame upper top surface 3, and the mold frame lower table surface 1 and the mold frame upper top surface 3 are respectively located at the upper and lower ends of the double-layer tube; wherein, the double-layer tube can also be selected to be arranged horizontally as needed, at this time, the mold frame lower table surface 1 and the mold frame upper top surface 3 are respectively located at the two ends of the double-layer tube.

[0074] In this embodiment, a mold frame column 2 is installed on the mold frame lower table 1, and the mold frame upper top surface 3 is installed on the mold frame column 2 and can move up and down along the mold frame column 2; the bottom of the outer layer tube is installed on the mold frame lower table 1 by bolts, and a heat insulation gasket 16 is arranged between the outer layer tube and the mold frame lower table 1. Specifically, a fixing boss is arranged on the outer edge of the bottom side of the outer layer tube, and bolt holes are arranged on the fixing boss and the mold frame lower table 1, and the fixing boss and the mold frame lower table 1 are fixed by passing bolts through the bolt holes. Furthermore, an upper through hole for the mechanical sliding device to pass through is opened at the center position of the mold frame upper top surface 3, and a lower through hole for the air pipe of the compressed air source device to pass through is opened on the mold frame lower table 1.

[0075] In this embodiment, the clamping device includes a lower clamping block 10 and a cylinder 14. The lower clamping block 10 can clamp the outer tube, and a heat insulating gasket 16 is provided at the contact position between the lower clamping block 10 and the outer tube; the lower clamping block 10 is installed below the upper surface 3 of the mold frame, and a lower clamping block through hole corresponding to the upper through hole is provided on the lower clamping block 10 to facilitate the passage of the mechanical sliding device; the cylinder 14 is connected to the top of the upper surface 3 of the mold frame, and can drive the upper surface 3 of the mold frame and the lower clamping block 10 to move, thereby achieving the clamping and loosening of the top of the outer tube. Among them, a plurality of cylinders 14 can be provided, and the plurality of cylinders 14 are evenly distributed along the circumference, and preferably two are provided, and the two cylinders 14 are symmetrically arranged, and the two cylinders 14 apply pressures F2 and F3 to the upper surface 3 of the mold frame respectively.

[0076] Embodiment 2

[0077] like Figure 2 As shown, this embodiment provides a method for testing the friction coefficient of a double-layer pipe interface, using the double-layer pipe interface friction coefficient testing device in Embodiment 1, and mainly comprising the following steps:

[0078] 1) Install double-layer pipe;

[0079] 2) heating the double-layer tube to a preset temperature, preferably 850° C.-900° C.;

[0080] 3) Introduce compressed gas into the inner closed tube to make the gas pressure in the inner closed tube reach a preset pressure;

[0081] 4) Pull the inner closed tube to a specified displacement and record the load of the mechanical sliding device;

[0082] 5) Calculate the friction coefficient.

[0083] In this embodiment, step 1) mainly includes the following steps:

[0084] 11) Obtaining the outer tube and the inner closed tube respectively according to preset parameters; wherein the outer tube is preferably a steel tube 7, and the inner closed tube is preferably a titanium tube 6, and the preset parameters mainly include the outer diameter, inner diameter, length, wall thickness, etc. of the titanium tube 6 and the steel tube 7;

[0085] 12) placing the steel tube 7 in a heating furnace and heating it to a preset temperature, taking it out and shrink-fitting the steel tube 7 and the titanium tube 6 to form a double-layer tube;

[0086] 13) According to the preset parameters, the upper end cap 8 and the lower end cap 9 are respectively obtained, and the upper end cap 8 is welded to one end of the titanium tube 6, and the lower end cap 9 is welded to the other end of the titanium tube 6 to form a closed titanium tube; wherein the preset parameters mainly include the diameter and thickness of the upper end cap 8 and the lower end cap 9, and the welding method is one of laser welding and argon arc welding;

[0087] 14) Install the double-layer tube on the mold frame.

[0088] In this embodiment, the outer diameter of the titanium tube 6 is D, the inner diameter of the titanium tube 6 is d, the wall thickness of the titanium tube 6 is t1, and the length of the titanium tube 6 is H; the outer diameter of the steel tube 7 is D2, the inner diameter of the steel tube 7 is D, the wall thickness of the steel tube 7 is t2, and the length of the steel tube 7 is H; the diameter of the upper head 8 and the lower head 9 is d. At room temperature, the titanium tube 6 and the steel tube 7 are interference fit, and the interference amount is calculated according to the test temperature, and the formula is δ=α Fe D(T1-T0)-α Ti D(T1-T0), where D is the interface diameter at high temperature test temperature (i.e., the inner diameter of the steel tube 7 or the outer diameter of the titanium tube 6), α Fe and α Ti They are the thermal expansion coefficients of the steel tube 7 and the titanium tube 6 at high temperatures, T1 is the temperature of the steel tube 7 and the titanium tube 6, and T0 is the room temperature.

[0089] In this embodiment, the method further includes the following steps before step 2):

[0090] The induction heating coil 4 and the heat-insulating layer 15 are installed, and the cylinder 14 is started to make the pressing block 10 press the top end of the steel pipe 7 with a preset pressure.

[0091] In this embodiment, in step 3), the compressed gas introduced is preferably one of air, nitrogen, helium, and argon; the gas pressure in the closed titanium tube ensures that the double-layer tube does not produce plastic yield, preferably 0.1-10MPa. Further, the gas pressure calculation formula is P = σ si ln[r m / (r m -t1)]+(1-r m 2 / b 2 )σ so / 2, where P is the gas pressure, σsi is the material yield limit of titanium tube 6, r m is the inner wall radius of the steel tube 7, t1 is the wall thickness of the titanium tube 6, b is the outer wall radius of the steel tube 7, σ so is the material yield limit of the steel pipe 7.

[0092] In this embodiment, in step 4), the servo motor 11 is used to pull the closed titanium tube into which compressed gas is passed to a displacement s at a preset speed, with a speed range of 0-v and a displacement range of 0-H; the changes in the servo motor load and the gas pressure in the double-layer tube are recorded, and the time t is recorded.

[0093] In this embodiment, in step 5), the friction coefficient is calculated using the formula F=μPπD(Hs).

[0094] Embodiment 3

[0095] like Figure 1 as well as Figure 3-Figure 5 As shown, this embodiment takes the titanium alloy-steel high temperature interface friction coefficient as an example for detailed description:

[0096] In this embodiment, the titanium tube 6 and the upper and lower heads 8 and 9 are preferably made of the same material, TC4 titanium alloy. The outer diameter of the titanium tube 6 is 200 mm, the inner diameter is 196 mm, the wall thickness is 2 mm, and the length is 200 mm. The outer diameter of the steel tube 7 is 210 mm, the inner diameter is 200 mm, and the wall thickness is 5 mm. The heating temperature of the material is 850°C.

[0097] The specific steps of the TC4 titanium alloy-steel high temperature interface friction coefficient test method in this embodiment are as follows:

[0098] According to the design, the size of titanium tube 6 and steel tube 7 is determined, and the double-layer tube is assembled. The interference is calculated according to the test temperature, and the formula is δ=α Fe D(T-T0)-α Ti D(T-T0), where D is the interface diameter at high temperature test temperature 200mm, α Fe The thermal expansion coefficient of the steel pipe 7 at high temperature is 14.4×10 -6 / K,α Ti The thermal expansion coefficient of the titanium tube 6 at high temperature is 9.4×10 -6 / K, T is the temperature of the steel tube 7 and the titanium tube 6 850°C, T0 is the room temperature 20°C, and the calculated interference is 0.83mm.

[0099] The two ends of the titanium tube 6 and the upper head 8 and the lower head 9 are surface treated and welded together to form a closed titanium tube; the welding method is laser welding.

[0100] The induction heating coil 4 and the thermal insulation layer 15 are installed on the outer wall of the double-layer tube to heat the closed titanium tube to a preset temperature;

[0101] Compressed gas is injected into the heated closed titanium tube to build up internal pressure in the tube. The compressed gas is one of the inert gases nitrogen and argon. The gas pressure should ensure that the double-layer tube does not yield. The calculation formula is: P = σ si ln[r m / (r m -t1)]+(1-r m 2 / b 2 )σ so / 2, the yield stress of titanium alloy at 850℃ is 129.56MPa, the yield stress of stainless steel at 850℃ is 37.27MPa, r m The inner wall radius of the steel tube 7 is 100 mm, r is the inner wall radius of the titanium tube 6 is 98 mm, t1 is the wall thickness of the titanium tube 6 is 2 mm, and b is the outer wall radius of the steel tube 7 is 105 mm. The calculated gas pressure is no more than 4.35 MPa, and the gas pressure P is taken as 2 MPa.

[0102] The closed titanium tube into which the compressed gas is introduced is pulled out to a preset position s=100 mm at a preset speed v=2 mm / s using the speed control mode of the servo motor 11 , and the load F of the servo motor is recorded.

[0103] During the test, the titanium tube 6 is subjected to a uniform force F and a friction force, the two forces are equal in magnitude and opposite in direction; the friction force is affected by the internal pressure P = 2MPa and the contact area between the titanium tube 6 and the steel tube 7, and the contact area between the titanium tube 6 and the steel tube 7 is affected by the speed v = 2mm / s and the time t = 50s. At this time, the formula is:

[0104] Friction force: μPS = F

[0105] The contact area between the titanium tube 6 and the steel tube 7: S = πD (H-vt)

[0106] In the formula, μ is the friction coefficient; P is the pressure; S is the contact area; F is the servo motor load; D is the outer diameter of the titanium tube 6; H is the length of the titanium tube 6; v is the movement speed of the titanium tube 6; and t is the time.

[0107] After calculation, the friction coefficient μ is obtained.

[0108] By taking multiple tests, using different speeds v and internal pressures P, and collecting enough data to obtain several sets of curves that change with time, the average value of the friction coefficient μ can be calculated using the above formula.

[0109] In summary, the double-layer tube interface friction coefficient testing device and method of the present invention, through induction heating of the closed titanium tube, can make the closed titanium tube quickly reach the forming temperature in a short time, significantly improve the heating efficiency, avoid the disadvantage that the traditional environmental furnace heating is limited by the size of the pipe fittings, and reduce the manufacturing cost of the components; at the same time, the double-layer tube measurement method is used to measure the high-temperature interface friction coefficient, which restores the environmental and stress conditions in the metal hot press bending forming, improves the accuracy of the measurement results, avoids the problem of large deviation of the traditional friction measurement method, and can be used to guide the solution of problems such as wrinkling in the metal hot press bending forming involving high-temperature interface friction.

[0110] The present specification uses specific examples to illustrate the principles and implementation methods of the present invention. The above examples are only used to help understand the method and core idea of ​​the present invention. At the same time, for those skilled in the art, according to the idea of ​​the present invention, there will be changes in the specific implementation methods and application scope. In summary, the content of this specification should not be understood as limiting the present invention.

Claims

1. A double-layer pipe interface friction coefficient testing device, characterized in that: include: A working mold frame, used for carrying a double-layer tube, wherein the double-layer tube comprises an outer tube and an inner closed tube, wherein the outer tube is sleeved on the outer side of the inner closed tube, and the inner wall of the outer tube matches the outer wall of the inner closed tube; A heating device, used to heat the double-layer tube to a preset temperature, and a temperature sensor is provided on the double-layer tube; A compressed gas source is connected to the inner closed tube and is used to introduce compressed gas into the inner closed tube. The compressed gas source is connected to a gas pressure controller and is used to control the pressure of the gas delivered to the closed tube. A mechanical sliding device connected to the inner closed tube and used to drive the inner closed tube to move axially relative to the outer tube, the mechanical sliding device being connected to a force sensor and a displacement sensor; A pressing device, used for pressing the outer tube onto the working mold frame when the inner closed tube and the outer sleeve move relative to each other; A data acquisition device is connected to the force sensor, the displacement sensor, the temperature sensor and the air pressure controller, and is used to collect load data and displacement data of the mechanical sliding device, temperature data of the double-layer tube and air pressure data of the air pressure controller.

2. The double-layer pipe interface friction coefficient testing device according to claim 1 is characterized in that: The heating device adopts an induction heating coil, which is sleeved on the outside of the double-layer tube. The induction heating coil is also connected to an induction heater. The induction heater can adjust the power of the induction heating coil through the temperature data feedback of the double-layer tube measured by the temperature sensor to heat the double-layer tube to a preset temperature; The outer wall of the double-layer pipe is also wrapped with a heat-insulating layer to reduce heat loss when the heating device heats the double-layer pipe.

3. The double-layer pipe interface friction coefficient testing device according to claim 1, characterized in that: The outer tube is a steel tube; the inner closed tube includes a titanium tube, an upper end cap and a lower end cap, the upper and lower ends of the titanium tube are respectively sealed and connected with the upper end cap and the lower end cap, the upper end cap is processed with a flange hole, and the mechanical sliding device is connected to the upper end cap through a flange; The inner closed tube and the outer tube are interference fit to compensate for the different thermal expansion amounts of the steel tube and the titanium tube after heating.

4. The double-layer pipe interface friction coefficient testing device according to claim 1 or 3, characterized in that: The mechanical sliding device adopts a servo motor.

5. The double-layer pipe interface friction coefficient testing device according to claim 3, characterized in that: The lower end cap is provided with an air inlet hole, which is connected to the compressed air source through an air pipe. The air pressure controller adopts an air pressure control cabinet, which is used to control the pressurization rate to reach a preset pressure and maintain the pressure. The air pressure control cabinet is installed on the air pipe between the compressed air source and the lower end cap; The gas pressure in the double-layer tube can ensure that the double-layer tube does not produce plastic yield.

6. The double-layer pipe interface friction coefficient testing device according to claim 5, characterized in that: The working mold frame comprises a mold frame lower table and a mold frame upper top surface, the mold frame lower table surface is installed with a mold frame column, and the mold frame upper top surface is installed on the mold frame column and can move up and down along the mold frame column; The outer tube is installed on the lower table of the mold frame by bolts, and a heat insulating gasket is arranged between the outer tube and the lower table of the mold frame to prevent the heat from being transferred to the lower table of the mold frame and causing damage and heat loss of the double tube when the heating device heats the double tube; An upper through hole for the mechanical sliding device to pass through is provided on the top surface of the mold frame, a lower through hole and a flange hole for the air pipe of the compressed air source device to pass through are provided on the lower surface of the mold frame, and the double-layer tube is connected to the flange hole on the lower surface of the mold frame by screws.

7. The double-layer pipe interface friction coefficient testing device according to claim 6, characterized in that: The pressing device comprises a lower pressing block and a cylinder, the lower pressing block can press the outer tube, and a heat insulating gasket is provided at the contact position between the lower pressing block and the outer tube to prevent the heat from being transferred to the lower pressing block and causing damage and heat loss of the double tube when the heating device heats the double tube; The lower pressing block is installed below the upper top surface of the mold frame, and a lower pressing block through hole corresponding to the upper through hole is opened on the lower pressing block; the cylinder is connected to the upper top surface of the mold frame and can drive the upper top surface of the mold frame and the lower pressing block to move.

8. A method for testing the friction coefficient of a double-layer pipe interface, characterized in that: The double-layer pipe interface friction coefficient testing device as described in any one of claims 1 to 7 comprises the following steps: Step 1), according to preset parameters, an inner tube and an outer tube are obtained respectively, wherein the inner tube and the outer tube are a titanium tube and a steel tube respectively, and the steel tube and the titanium tube are assembled into a double-layer tube by shrink-fitting; Step 2), sealing the inner tube to form an inner closed tube, installing the double-layer tube to the working mold frame, and heating the double-layer tube to a preset temperature; Step 3), introducing compressed gas into the inner closed tube to make the gas pressure in the inner closed tube reach a preset pressure; Step 4), pulling the inner closed tube at a constant speed to a specified displacement, and recording the load of the mechanical sliding device; Step 5), calculate the friction coefficient.

9. The method for testing the coefficient of friction at the interface of a double-layer pipe according to claim 8, characterized in that: In the step 1), the outer diameter of the titanium tube is D1, the inner diameter of the titanium tube is d, the wall thickness of the titanium tube is t1, and the length of the titanium tube is H; the outer diameter of the steel tube is D2, the inner diameter of the steel tube is D1, the wall thickness of the steel tube is t2, and the length of the steel tube is H; In step 1), the temperature range of the heat-fitting is 850-900°C, and the interference is calculated according to the test temperature. The calculation formula of the interference is δ=α Fe D(T1-T0)-α Ti D(T1-T0); where D is the interface diameter at high temperature test temperature, α Fe and α Ti is the thermal expansion coefficient of the steel tube and the titanium tube at high temperature, T1 is the temperature of the steel tube and the titanium tube, and T0 is the room temperature; In the step 2), an upper head and a lower head with a diameter of d are obtained, the upper head is welded to one end of the titanium tube, and the lower head is welded to the other end of the titanium tube to form a closed titanium tube; the titanium tube is welded by arc welding or laser welding; In the step 2), the double-layer tube is installed on the working mold frame, the induction heating coil and the thermal insulation layer are installed, and the cylinder is started to make the lower pressing block press the steel tube with a preset pressure, the pressure is large enough not to make the double-layer tube yield, and the yield limit is determined by the material with a smaller yield limit in the double-layer tube at the test temperature; In the step 2), the preset temperature of the double-layer tube heating is 850-900°C.

10. The method for testing the friction coefficient of the double-layer pipe interface according to claim 8, characterized in that: In step 3), the preset gas pressure range in the double-layer tube should ensure that the double-layer tube does not produce plastic yield. The calculation formula of gas pressure is P = σ si ln[r m / (r m -t1)]+(1-r m 2 / b 2 )σ so / 2, where P is the gas pressure, σ si is the material yield limit of the titanium tube, r m is the inner wall radius of the steel tube, t1 is the wall thickness of the titanium tube, b is the outer wall radius of the steel tube, σ so is the material yield limit of the steel pipe; In the step 4), the displacement range of the inner closed tube is 0-H, the speed range is 0-v, the speed is kept uniform, and the size is adjusted according to the test grouping needs. The contact area between the titanium tube and the steel tube is calculated using the formula S=πD(H-vt), where S is the contact area; D is the outer diameter of the titanium tube; H is the length of the titanium tube; v is the movement speed of the titanium tube; t is time; In the step 5), the friction coefficient is calculated using the formula μPS=F, where μ is the friction coefficient; P is the pressure; S is the contact area; and F is the servo motor load. Multiple tests are conducted with different speeds v and internal pressures P to collect data and calculate the friction coefficient μ.