Reflective film and bead planting method for reflective film

By controlling the thickness of the wet glue layer and the amount of solvent during the bead planting process of the reflective film, and using the bead suction unit to remove stray beads and floating beads, the problem of stray beads and floating beads during the bead planting process is solved, and an efficient reflective film is achieved Preparation, improves the gloss and brightness uniformity of the film.

CN114994816BActive Publication Date: 2024-10-01SVG TECH GRP CO LTD +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210591829.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-05-27
Publication Date
2024-10-01
Estimated Expiration
2042-05-27

AI Technical Summary

Technical Problem

During the bead planting process of the reflective film, the bead planting glue easily overflows during the rolling process, resulting in the appearance of stray beads and floating beads, which affects the surface gloss and performance of the film.

Method used

Using a device including a bead planting unit, a bead suction unit and a drying unit, by controlling the thickness of the wet glue layer and the amount of solvent, rubber rollers and steel rollers are used for bead planting, and transmission between the bead planting unit and the drying unit A bead suction unit is installed on the path to remove stray beads and floating beads to ensure the cleanliness of the dry glue layer.

Benefits of technology

It effectively reduces the appearance of stray beads and floating beads, improves the surface gloss and brightness uniformity of the reflective film, is suitable for high-end product needs, and improves production efficiency and yield.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114994816B_ABST
    Figure CN114994816B_ABST
Patent Text Reader

Abstract

The present application discloses a reflective film and a beading method for the reflective film, and the beading method includes: applying adhesive on the surface of the base film to form a wet adhesive layer, wherein the thickness of the wet adhesive layer is 15%-35% of the particle size of the glass beads; implanting the glass beads in the bead groove into the wet adhesive layer by means of a rubber roller and a steel roller; performing wind-force bead suction treatment on the surface of the wet adhesive layer by means of a bead suction unit to remove excess glass beads on the surface of the wet adhesive layer; drying the wet adhesive layer to convert the wet adhesive layer into a dry adhesive layer, wherein the thickness of the dry adhesive layer is 10%-30% of the particle size of the glass beads. The present application first controls the thickness of the wet adhesive layer and the amount of solvent and other parameters to reduce the phenomenon of adhering miscellaneous beads on the wet adhesive layer; secondly, the bead groove, the glass beads and the base film are all subjected to a static electricity removal treatment to reduce the phenomenon of floating beads; finally, before the wet adhesive layer is dried and cured, the miscellaneous beads and floating beads on the surface of the wet adhesive layer are removed by means of a bead suction unit, so that a dry adhesive layer without miscellaneous beads or floating beads on the surface is prepared.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application belongs to the technical field of reflective film preparation technology, and in particular, relates to a reflective film and a method for implanting beads on the reflective film. Background Art

[0002] Reflective film is a film structure that can effectively reflect incident light. Therefore, it is widely used in traffic warning labels, road condition warning labels, etc. The core structure that plays a reflective role in reflective film is the glass beads embedded in the base film of the reflective film. The method of embedding glass beads in the base film of the reflective film is called the beading method.

[0003] In one implementation, the bead implanting method of the reflective film can be achieved by the following steps: firstly coating an adhesive layer on the base film, then implanting glass micro beads into the adhesive layer, and finally drying the adhesive layer implanted with the glass micro beads.

[0004] However, this bead planting method has the following technical difficulties: when the bead planting glue is used to plant glass microbeads, the bead planting glue is easily squeezed and overflowed during the rolling process, and the overflowed glue will adhere to the excess miscellaneous beads; in addition, when the glass microbeads are implanted in the base film, a large number of floating beads will appear on the base film due to electrostatic adsorption and other reasons. The presence of miscellaneous beads and floating beads not only requires a lot of manpower and material resources to remove in the subsequent process, but also easily causes the surface of the reflective film to be easily scratched and the brightness to be uneven, affecting the performance of the reflective film. Summary of the invention

[0005] In order to solve the above technical problems, the present application provides a reflective film and a method for implanting beads on the reflective film.

[0006] In the first aspect, the present application provides a bead planting method for a reflective film, the bead planting method is implemented based on a bead planting device, the bead planting device includes a bead planting unit, a bead suction unit and a drying unit arranged in sequence, wherein the bead planting unit includes a matching rubber roller and a steel roller, and a bead groove; the bead groove is used to hold glass beads; the bead planting method includes: applying adhesive on the surface of the base film to form a wet glue layer, wherein the thickness of the wet glue layer is 15%-35% of the particle size of the glass beads; implanting the glass beads in the bead groove into the wet glue layer through the rubber roller and the steel roller, wherein the bead groove, the glass beads and the base film are all connected to a static electricity removal device; performing wind-force bead suction treatment on the surface of the wet glue layer through the bead suction unit to remove excess glass beads on the surface of the wet glue layer; drying the wet glue layer to transform the wet glue layer into a dry glue layer, wherein the thickness of the dry glue layer is 10-30% of the particle size of the glass beads.

[0007] In one feasible embodiment, the bead suction unit includes at least one bead suction tube distributed along the transmission direction from the bead planting unit to the drying unit; the air suction port of the bead suction tube is toward the surface of the wet glue layer and forms an angle of 105°±10° with the surface of the wet glue layer.

[0008] In one achievable manner, the air suction port of the bead suction tube spans across the width direction of the wet glue layer surface, wherein the width direction of the wet glue layer surface refers to a direction perpendicular to the transmission direction from the bead planting unit to the drying unit.

[0009] In one achievable method, the adhesive is coated on the surface of the base film to form a wet adhesive layer, comprising: coating the adhesive on the surface of the base film; controlling the base film coated with the adhesive to pre-dry from a first preset temperature to a second preset temperature according to a preset heating strategy, so that the solvent content in the obtained wet adhesive layer is 25%-50%, wherein the second preset temperature is greater than the first preset temperature.

[0010] In an implementable manner, the pre-drying time is 2-3 minutes, the first preset temperature is 40°C, and the second preset temperature is 80°C.

[0011] In an achievable manner, the drying temperature for drying the wet adhesive layer is 135° C., and the drying time is 3-7 minutes.

[0012] In one possible implementation, the method further includes: scraping a focusing layer on the dry adhesive layer; and making a reflecting layer on the focusing layer.

[0013] In an implementable manner, the base film is any one of PET, acrylic, polyester or UV resin materials.

[0014] In one implementation, the base film has a thickness of at least 50 μm.

[0015] In a second aspect, the present application provides a reflective film, which is prepared by the bead planting method for the reflective film as described in any one of the first aspects.

[0016] In summary, the present application provides a reflective film and a method for implanting beads on the reflective film. First, the thickness of the wet adhesive layer and the amount of solvent and other parameters are controlled to reduce the phenomenon of adhering miscellaneous beads on the wet adhesive layer; secondly, when the glass microbeads in the bead groove are implanted into the wet adhesive layer by means of a rubber roller and a steel roller, the bead groove, the glass microbeads and the base film are all treated with anti-static treatment to reduce the phenomenon of floating beads; finally, before the wet adhesive layer is dried and cured, the miscellaneous beads and floating beads on the surface of the wet adhesive layer are further removed by a bead suction unit, so that a dry adhesive layer with no miscellaneous beads or floating beads on the surface is prepared. Furthermore, based on the prepared dry adhesive layer with a clean surface, a focusing layer can be directly scraped on the dry adhesive layer, and a reflecting layer, an adhesive layer and a peeling layer can be made on the focusing layer. Among them, the focusing layer prepared based on the above-mentioned dry adhesive layer has no flowery appearance and uniform brightness, which is suitable for high-end product requirements. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the following briefly introduces the drawings required for use in the embodiments or the description of the prior art. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0018] Figure 1 A schematic diagram of the structure of a bead planting device provided in an embodiment of the present application;

[0019] Figure 2 A top view of a bead suction unit provided in an embodiment of the present application;

[0020] Figure 3 A side view of a bead suction tube provided in an embodiment of the present application;

[0021] Figure 4 A process flow chart of a method for implanting beads on a reflective film provided in an embodiment of the present application.

[0022] Attached icon description

[0023] 10-bead planting unit, 20-bead suction unit, 30-drying unit, 40-winding unit;

[0024] 101-rubber roller, 102-steel roller, 103-bead groove, 201-bead suction tube, 202-air suction pump, 203-air suction port;

[0025] 100-base film, 200-wet adhesive layer, 300-glass beads, 400-dry adhesive layer. DETAILED DESCRIPTION

[0026] The following will be combined with the drawings in the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by those skilled in the art without creative work are within the scope of protection of this application.

[0027] The embodiment of the present application provides a method for planting beads on a reflective film, which is implemented based on a bead planting device. Based on the bead planting device, the embodiment of the present application provides a method for planting beads on a reflective film, which can solve the technical problem that miscellaneous beads and floating beads are difficult to remove.

[0028] The bead implanting device provided in the embodiment of the present application will first be described with reference to the accompanying drawings.

[0029] like Figure 1 As shown, the bead planting device provided by the present application includes a bead planting unit 10, a bead suction unit 20 and a drying unit 30 which are arranged in sequence.

[0030] The bead implanting unit 10 comprises a rubber roller 101, a steel roller 102 and a bead groove 103, wherein the rubber roller 101, the steel roller 102 and the bead groove 103 cooperate with each other to implant the glass micro beads in the bead groove 103 into the wet glue layer of the base film.

[0031] The present application does not limit the structure of the rubber roller 101 and the steel roller 102, as long as the glass beads can be implanted by rolling. For example, the rubber roller 101 and the steel roller 102 are two non-coaxial roller-shaped structures rotating in opposite directions, wherein the rubber roller 101 has a smooth surface, and the steel roller 102 has grooves arranged in an array, wherein the size of the grooves is adapted to the size of the glass beads.

[0032] The base film treated by the bead planting unit 10 needs to be dried by the drying unit 30 so that the glass beads are solidified on the base film. The present application also provides a bead suction unit 20 between the bead planting unit 10 and the drying unit 30, which can remove the miscellaneous beads and floating beads on the base film by wind power before the glass beads are solidified on the base film.

[0033] The present application does not limit the structure of the bead suction unit 20. In one possible implementation, Figure 2 As shown, the bead suction unit 20 in the present application includes at least one bead suction tube 201 , wherein each bead suction tube 201 is connected to an air suction pump 202 , and the air suction pump 202 provides air suction power for the bead suction tube 201 .

[0034] If the bead suction unit 20 includes a plurality of bead suction tubes 201, the plurality of bead suction tubes 201 may be distributed along the direction of the base film being transported from the bead planting unit 10 to the drying unit 30. In this way, during the process of the base film being transported from the bead planting unit 10 to the drying unit 30, the plurality of bead suction tubes 201 in the bead suction unit 20 may be used to remove the miscellaneous beads and floating beads attached to the base film.

[0035] The present application does not limit the structure of each bead suction tube 201. In one possible implementation, Figure 2 and Figure 3 As shown, the bead suction tube 201 is a long tubular structure, and an opening of a preset width is opened in the length direction of the bead suction tube 201, which serves as an air suction port 203. When working, the air suction port 203 faces the base film direction, and the angle α with the transmission direction of the base film is 105°±10°, so that the bead suction tube 201 can be prevented from forming a vacuum state perpendicular to the surface of the base film, thereby improving the suction force.

[0036] like Figure 1 As shown, after the drying unit 30, the bead implanting device provided in the present application may further include a winding unit 40, and the winding unit 40 is used to perform a winding operation on the structure after the glass beads are solidified on the base film.

[0037] The bead planting method of the reflective film provided in the embodiment of the present application is described below with reference to the accompanying drawings.

[0038] like Figure 4 As shown, the bead planting method of the reflective film provided in the embodiment of the present application includes the following steps:

[0039] Step S1 : applying adhesive on the surface of the base film 100 to form a wet adhesive layer 200 , wherein the thickness of the wet adhesive layer 200 is 15%-35% of the particle size of the glass microbeads 300 .

[0040] The base film 100 is the basic material for preparing the reflective film, and the base film 100 provides a carrier for the implanted beads. The present application does not limit the material of the base film 100, and the base film 100 can be one or more materials selected from PET, acrylate, polyester or UV resin.

[0041] To facilitate subsequent operations such as coating and hot pressing on the base film 100 , the thickness of the base film 100 may be greater than 50 μm, for example, the thickness of the base film 100 is 50 μm, 60 μm or 70 μm.

[0042] The present application does not limit the type of adhesive. For example, the adhesive may be solvent-based glue.

[0043] The present application can prevent glue overflow when the glass beads 300 are implanted into the wet glue layer 200 by limiting the thickness of the wet glue layer 200 , thus greatly alleviating the problem of foreign beads adhering to the wet glue layer 200 .

[0044] It should be noted here that the miscellaneous beads in the embodiment of the present application refer to the excess glass beads adhered to the wet glue layer 200; the floating beads refer to the excess glass beads stacked on the glass beads embedded in the wet glue layer 200 due to electrostatic adsorption.

[0045] In order to further alleviate the problem of foreign beads adhering to the wet glue layer 200, the present application can form the wet glue layer 200 through the following steps: first, an adhesive is coated on the surface of the base film 100; then, the base film 100 coated with the adhesive is controlled to be pre-dried from a first preset temperature to a second preset temperature according to a preset heating strategy, so that the solvent content in the obtained wet glue layer 200 is 25%-50%, wherein the second preset temperature is greater than the first preset temperature.

[0046] Among them, according to the preset temperature increase strategy, the pre-drying is gradually performed from the first preset temperature to the second preset temperature, so that the solvent in the adhesive can be gradually volatilized, so that a wet adhesive layer 200 with a smooth surface can be prepared.

[0047] The present application does not limit the preset temperature increase strategy. For example, the preset temperature increase strategy may be to use a fixed temperature increase rate and control the time for gradual pre-drying from 40° C. to 80° C. to be 3 minutes.

[0048] After the pre-drying process is completed, the wet adhesive layer 200 is in a semi-dry state, and the wet adhesive layer 200 in this state is not easy to adhere to foreign beads.

[0049] The amount of solvent in the present application refers to the percentage of the solvent in the wet adhesive layer to the total amount of solvent and solute in the wet adhesive layer.

[0050] Step S2, implanting the glass micro beads 300 in the bead groove 103 into the wet glue layer 200 through the glue roller 101 and the steel roller 102, wherein the bead groove 103, the glass micro beads 300 and the base film 100 are all connected to a static electricity removal device.

[0051] like Figure 1 As shown, the base film 100 with the wet glue layer 200 formed thereon enters between the rubber roller 101 and the steel roller 102 for bead planting. The bead groove 103 provides glass beads 300 for the wet glue layer 200. As the rubber roller 101 and the steel roller 102 rotate, the glass beads 300 entering the steel roller 102 from the bead groove 103 adhere to the wet glue layer 200 passing through, and the matching rubber roller 101 presses the glass beads 300 adhered to the wet glue layer 200 into the wet glue layer 200.

[0052] It should be noted that the above step S2 is the main step where the phenomenon of miscellaneous beads and floating beads occurs. Since in step S1 of the embodiment of the present application, the problem of miscellaneous beads adhering to the wet adhesive layer 200 can be reduced by controlling the thickness and solvent amount of the wet adhesive layer 200. To further reduce the phenomenon of floating beads, in step S2 of the embodiment of the present application, the bead groove 103, the glass beads 300 and the base film 100 are all connected to a static electricity removal device.

[0053] In the present application, the anti-static devices connected to the bead groove 103, the glass beads 300 and the base film 100 may be the same or different, and the present application does not limit this.

[0054] Among them, before entering between the rubber roller 101 and the steel roller 102, the glass microbeads 300 are stored in the bead groove 103, and the bead groove 103 is filled with a large number of glass microbeads for entering the plant stage. In the embodiment of the present application, the glass microbeads 300 are treated to remove static electricity before entering the plant stage to prevent the glass microbeads 300 from having static electricity themselves. The present application does not limit the structure of the static electricity removal device for removing static electricity from the glass microbeads 300. In one feasible way, a conductive wire for removing static electricity can be placed in the bead groove 103 that holds the glass microbeads 300. At the same time, the bead groove 103 is also connected to the static electricity removal device, so that the static electricity on the glass microbeads 300 can be conducted away; in another feasible way, water can also be placed in the bead groove 103, and a large number of glass microbeads can be immersed in the water, so that the glass microbeads 300 will not carry static electricity. The bead groove 103 is generally a metal structure, so the static electricity removal device for removing static electricity on the bead groove 103 can be connected to any position that can form electrical conduction with the bead groove 103 .

[0055] For the base film 100 , the surface of the base film 100 facing away from the wet adhesive layer 200 may be connected to a static electricity removal device.

[0056] Step S3: performing wind-force bead suction treatment on the surface of the wet glue layer 200 by using the bead suction unit 20 to remove excess glass beads on the surface of the wet glue layer 200.

[0057] In the embodiment of the present application, the path and time for the base film 100 to be transferred from the bead planting unit 10 to the drying unit 30 are fully utilized, and a bead suction unit 20 is arranged on the transfer path to remove the miscellaneous beads and floating beads attached to the wet glue layer 200 before the wet glue layer 200 is cured.

[0058] When implementing step S3, the bead suction tube 201 in the bead suction unit 20 can be controlled to be close to the wet glue layer 200, but no pressure is applied to the wet glue layer 200. Among them, the air suction port 203 of the bead suction tube 201 spans the width direction of the surface of the wet glue layer 200, and the width direction of the surface of the wet glue layer 200 refers to the perpendicular direction to the transmission direction of the bead planting unit 10 to the drying unit 30. In addition, the air suction port 203 of the bead suction tube 201 is oriented toward the surface of the wet glue layer 200 and forms an angle of 105°±10° with the surface of the wet glue layer 200. In this way, the miscellaneous beads and floating beads can be removed on the path of the base film 100 to the drying unit 30, and there is no need to add operations such as removing miscellaneous beads and floating beads after drying.

[0059] It should be noted that the above description is only based on the example of setting the bead suction tube 201 on one side of the surface of the wet glue layer 200, and does not limit the position of the bead suction tube 201. For example, the bead suction tube 201 can also be set on the side of the base film 100 facing away from the wet glue layer 200. In this way, the miscellaneous beads and floating beads on both surfaces of the base film 100 can be adsorbed.

[0060] Step S4 , drying the wet adhesive layer 200 to transform the wet adhesive layer 200 into a dry adhesive layer 400 , wherein the thickness of the dry adhesive layer 400 is 10%-30% of the particle size of the glass beads 300 .

[0061] After the wet adhesive layer 200 is dried in step S4, the wet adhesive layer 200 is solidified and transformed into a dry adhesive layer 400. The present application does not limit the drying temperature and drying time of the drying process. For example, the drying temperature may be 135° C. and the drying time may be 3-7 minutes.

[0062] In summary, the bead implanting method for the reflective film provided in the embodiment of the present application first controls the parameters such as the thickness and the amount of solvent of the wet glue layer 200 to reduce the phenomenon of miscellaneous beads adhering to the wet glue layer 200; secondly, when the glass microbeads 300 in the bead groove 103 are implanted into the wet glue layer 300 by the glue roller 101 and the steel roller 102, the bead groove 103, the glass microbeads 300 and the base film 100 are all subjected to anti-static treatment to reduce the phenomenon of floating beads; finally, before the wet glue layer 200 is dried and cured, the miscellaneous beads and floating beads on the surface of the wet glue layer 200 are further removed by the bead suction unit 20, so that a dry glue layer 400 with no miscellaneous beads or floating beads on the surface is prepared.

[0063] Based on the prepared dry adhesive layer 400 with a clean surface, a focusing layer can be directly scraped on the dry adhesive layer 400, and a reflective layer, an adhesive layer and a peeling layer can be made on the focusing layer. Among them, the focusing layer prepared based on the above dry adhesive layer 400 has no flowery appearance and uniform brightness, which is suitable for high-end product requirements.

[0064] In addition, due to the use of the bead planting method for the reflective film provided in the embodiment of the present application, the miscellaneous beads and floating beads are greatly reduced, and there is no need for additional bead removal operations in the subsequent processes. Therefore, the production efficiency and yield of the bead planting method of the present application are improved.

[0065] The advantages of the bead implanting method for the reflective film provided in the embodiment of the present application are described below through experimental data.

[0066] The first set of experiments

[0067] In the first group of experiments of the present application, Experimental Example 1 adopts the bead planting method of the reflective film provided in the embodiment of the present application to prepare a dry adhesive layer, and a focusing layer is scraped on the dry adhesive layer; a reflecting layer is made on the focusing layer to obtain a reflective film. In the remaining experimental examples and comparative examples of the first group of experiments, the thickness of the wet adhesive layer is adjusted under the condition that other parameters in Experimental Example 1 remain unchanged to determine the effect of the thickness of the wet adhesive layer on the prepared reflective film. For specific experimental parameters, see Table 1.

[0068] Table 1 The first set of experimental parameters and experimental results

[0069]

[0070] The second set of experiments

[0071] In the second group of experiments of the present application, Experimental Example 4 adopts the bead planting method of the reflective film provided in the embodiment of the present application to prepare a dry adhesive layer, and a focusing layer is scraped on the dry adhesive layer; a reflecting layer is made on the focusing layer to obtain a reflective film. In the remaining experimental examples and comparative examples of the second group of experiments, the amount of solvent in the wet adhesive layer is adjusted under the condition that other parameters in Experimental Example 4 remain unchanged to determine the effect of the amount of solvent in the wet adhesive layer on the prepared reflective film. For specific experimental parameters, see Table 2.

[0072] Table 2 The second set of experimental parameters and experimental results

[0073]

[0074]

[0075] The third group of experiments

[0076] In the third group of experiments of the present application, Experimental Example 7 adopts the bead planting method of the reflective film provided in the embodiment of the present application to prepare a dry adhesive layer, and a focusing layer is scraped on the dry adhesive layer; a reflective layer is made on the focusing layer to obtain a reflective film. In the remaining experimental examples and comparative examples of the third group of experiments, the steps of the bead planting method are adjusted under the condition that other parameters in Experimental Example 7 remain unchanged. For specific experimental parameters, see Table 3.

[0077] Table 3 Experimental parameters and results of the third group

[0078]

[0079] It should be noted that in the above-mentioned first, second and third experiments, the retroreflection coefficient of the reflective film can be detected by using a retroreflectometer.

[0080] According to the first group of experiments, when the ratio of the wet adhesive layer thickness to the glass bead particle size is controlled at 15%-35%, there are no impurities or floating beads on the surface of the prepared dry adhesive layer, and the corresponding retroreflection coefficient of the prepared reflective film is 75-80d / lx / m 2 When the ratio of the wet adhesive layer thickness to the glass microbead particle size exceeds 35%, there are miscellaneous beads and floating beads on the surface of the prepared dry adhesive layer, and the retroreflection coefficient of the corresponding prepared reflective film drops to 65-70d / lx / m 2 .

[0081] According to the second group of experiments, when the amount of solvent in the wet adhesive layer is controlled at 25%-50%, there are no impurities or floating beads on the surface of the prepared dry adhesive layer, and the corresponding retroreflection coefficient of the prepared reflective film is 75-80d / lx / m 2 When the solvent content of the wet adhesive layer exceeds 50%, although there are no miscellaneous beads or floating beads on the surface of the prepared dry adhesive layer, when the solvent content of the wet adhesive layer exceeds 50%, the ratio of the thickness of the corresponding prepared dry adhesive layer to the particle size of the glass microbeads is reduced to 9%-10%, and the retroreflection coefficient of the corresponding reflective film is reduced to 65-70d / lx / m 2 .

[0082] According to the third group of experiments, for reflective films with the same wet adhesive layer thickness, wet adhesive layer solvent volume, and dry adhesive layer thickness, during the preparation process, the bead groove, micro beads, and base film are treated with anti-static treatment, and the bead absorption unit is treated. The surface of the prepared dry adhesive layer has no miscellaneous beads or floating beads, and the corresponding reflective film has a retroreflective coefficient of 80d / lx / m 2 However, during the preparation process, the bead groove, microbeads and base film were not treated with anti-static treatment, and / or the bead absorption unit was not treated, and the surface of the prepared dry adhesive layer had miscellaneous beads and floating beads, and the corresponding retroreflection coefficient of the reflective film was reduced to 70-75d / lx / m 2 .

[0083] In summary, the retroreflective coefficient of the reflective film prepared by the method for producing the reflective film provided in the embodiment of the present application can reach 80d / lx / m 2 , the surface is not blooming and the brightness is uniform, meeting the needs of high-end products.

[0084] The embodiment of the present application also provides a reflective film, which is prepared by the bead implantation method of the reflective film provided in the embodiment of the present application. The reflective film includes a base film 100 and a dry adhesive layer 400 stacked in sequence, wherein glass microbeads 300 are implanted in the dry adhesive layer 400, and the thickness of the dry adhesive layer 400 is 10%-30% of the particle size of the glass microbeads 300. Furthermore, the reflective film provided in the embodiment of the present application can also be stacked with a focusing layer, a reflection layer, an adhesive layer, and a peeling layer on the surface of the glass microbeads 300 in sequence.

[0085] Embodiment 1

[0086] The bead planting method of the reflective film provided in the first embodiment of the present application comprises the following steps:

[0087] A polyester material with a thickness of about 50 μm is further coated on the PET with a thickness of 75 μm to obtain a base film, and an adhesive is further coated on the base film.

[0088] The base film coated with the adhesive is pre-dried, wherein the pre-drying temperature is gradually increased from 40° C. to 80° C. during the pre-drying process, and the pre-drying process is completed within 2-3 minutes to obtain a wet adhesive layer, wherein the solvent content in the wet adhesive layer is 25%, and the thickness of the wet adhesive layer is 15% of the particle size of the glass beads.

[0089] The glass beads will sink deeply into the wet glue layer under the pressure of about 2-5kg from the rubber roller and steel roller, and can be arranged neatly on the wet glue layer without overflowing glue or disorderly arrangement of glue-carrying beads (i.e., no miscellaneous beads). Among them, the glass beads, base film and bead groove are all connected to the static elimination device.

[0090] The beads and floating beads on the surface of the wet glue layer are removed by the bead suction unit. The bead suction tube in the bead suction unit is close to the wet glue layer, but does not press the wet glue layer, and the air suction port of the bead suction tube faces the surface of the wet glue layer and forms an angle of 105°±10° with the surface of the wet glue layer, ensuring that the static floating beads are removed by the suction power. The parameters of the suction pump are wind pressure 22kpa, air volume 165m 3 / h, power above 1100W.

[0091] The base film treated with beads is dried at 135° C. for 3-7 minutes, and the wet adhesive layer is solidified to become a dry adhesive layer, wherein the thickness of the dry adhesive layer is 10% of the particle size of the micro beads.

[0092] The surface of the dry adhesive layer prepared through the above steps of the embodiment of the present application is clean and free of miscellaneous beads and floating beads.

[0093] The same and similar parts between the various embodiments in this specification can refer to each other, especially the embodiment part corresponding to the reflective film can refer to the bead planting method part of the reflective film.

[0094] The present application is described in detail above in conjunction with specific implementation methods and exemplary examples, but these descriptions cannot be understood as limiting the present application. Those skilled in the art understand that, without departing from the spirit and scope of the present application, a variety of equivalent replacements, modifications or improvements can be made to the technical solution of the present application and its implementation methods, all of which fall within the scope of the present application. The scope of protection of the present application shall be subject to the attached claims.

Claims

1. A method for planting beads on a reflective film, characterized in that: The bead planting method is implemented based on a bead planting device, which includes a bead planting unit, a bead suction unit and a drying unit arranged in sequence, wherein the bead planting unit includes a matched rubber roller and a steel roller, and a bead trough; the bead trough is used to hold glass microbeads; The bead implantation method comprises: Applying adhesive on the surface of the base film to form a wet adhesive layer, wherein the thickness of the wet adhesive layer is 15%-35% of the diameter of the glass beads, and the adhesive is a solvent-based glue; Controlling the base film coated with the adhesive to pre-dry from a first preset temperature to a second preset temperature according to a preset temperature increase strategy, so that the solvent content in the obtained wet adhesive layer is 25%-50%, wherein the second preset temperature is greater than the first preset temperature, and the solvent content is a percentage of the total amount of solvent and solute in the wet adhesive layer; The glass beads in the bead groove are implanted into the wet glue layer by means of the rubber roller and the steel roller in a rolling manner, wherein the bead groove, the glass beads and the base film are all connected to a static elimination device so that the bead groove, the glass beads and the base film are free of static electricity; The surface of the wet glue layer is subjected to wind-forced bead suction treatment by the bead suction unit to remove excess glass beads from the surface of the wet glue layer; the bead suction unit includes at least one bead suction tube distributed along the transmission direction from the bead planting unit to the drying unit; the air suction port of the bead suction tube is directed toward the surface of the wet glue layer and forms an angle of 105°±10° with the surface of the wet glue layer; The wet adhesive layer is dried to transform the wet adhesive layer into a dry adhesive layer, wherein the thickness of the dry adhesive layer is 10-30% of the particle size of the glass beads.

2. The method for implanting beads according to claim 1, wherein: The air suction port of the bead suction tube spans the width direction of the wet glue layer surface, wherein the width direction of the wet glue layer surface refers to the perpendicular direction to the transmission direction from the bead planting unit to the drying unit.

3. The method for implanting beads according to claim 1, wherein: The pre-drying time is 2-3 minutes, the first preset temperature is 40°C, and the second preset temperature is 80°C.

4. The method for implanting beads according to claim 1, wherein: The drying temperature for the drying treatment of the wet adhesive layer is 135° C., and the drying time is 3-7 minutes.

5. The method for implanting beads according to claim 1, wherein: Also includes: scraping a focusing layer on the dry adhesive layer; A reflective layer is formed on the focusing layer.

6. The method for implanting beads according to claim 1, wherein: The base film is any one of PET, acrylate, polyester or UV resin materials.

7. The method for implanting beads according to claim 1, wherein: The base film has a thickness of at least 50 μm.

8. A reflective film, characterized in that: The reflective film is prepared by the bead planting method of the reflective film as described in any one of claims 1 to 7.