Biodegradable compositions and articles made from cellulose acetate
By developing melt-processable cellulose acetate compositions containing cellulose acetate, plasticizers, and other components, the problem of compostability and biodegradability of disposable consumer products in existing technologies has been solved, achieving highly efficient and environmentally friendly performance.
Patent Information
- Application Number
- CN202180010071.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-08-07
- Filing Date
- 2021-01-20
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2041-01-20
AI Technical Summary
Existing technologies struggle to provide single-use consumer products with sufficient performance characteristics that are compostable and/or biodegradable, especially in cases of food contamination or inadequate waste management systems, leading to significant amounts of plastic waste leaking into the environment.
A melt-processable cellulose acetate composition has been developed, comprising cellulose acetate, plasticizers, and other additional components such as fillers, additives, biodegradable polymers, and stabilizers, ensuring at least 90% disintegration within 12 weeks under industrial composting conditions.
This invention achieves efficient disintegration of cellulose acetate compositions within 12 weeks while maintaining performance characteristics, making them suitable for single-use consumer products and reducing environmental pollution.
Smart Images

Figure BDA0003754471700000021 
Figure BDA0003754471700000511 
Figure BDA0003754471700000521
Abstract
Description
Background Art
[0001] Waste disposal is a well-known global issue, especially with the large number of consumer products, such as plastics or polymers, that are not considered biodegradable within acceptable time limits. The public would like to incorporate these types of waste into newer products by recycling, reusing or otherwise reducing the amount of waste in circulation or landfills. This is especially true for single-use plastic products / materials.
[0002] As consumer sentiment towards the environmental fate of single-use plastics (such as straws, takeaway cups and plastic bags) becomes a global trend, plastic bans are being considered / enacted in developed and developing countries around the world. For example, in the United States alone, bans have been extended from plastic shopping bags to straws, cutlery and clamshell packaging. Other countries have taken even more extreme measures, such as a selected list of ten single-use products that have been banned, restricted in use, or mandated to have extended producer responsibility throughout the European Union. As a result, industry leaders, brand owners and retailers have made ambitious commitments to implement recyclable, reusable or compostable packaging in the coming years. While recyclable materials are required in some applications, other applications are more suitable for compostable and / or biodegradable materials, such as when the products are contaminated with food or when there is a large amount of leakage into the environment due to inadequate waste management systems.
[0003] There is a need in the market for disposable consumer products that have adequate performance properties for their intended use and that are compostable and / or biodegradable.
[0004] It would be beneficial to provide products having such properties and also having significant contents of renewable, recycled and / or reused materials. Summary of the invention
[0005] The present application discloses a melt-processable and biodegradable cellulose acetate composition comprising at least one cellulose acetate, at least one plasticizer and at least one additional component selected from fillers, additives, biodegradable polymers, stabilizers or odor modifiers.
[0006] wherein the at least one plasticizer is present in an amount of 10 wt% to 25 wt% based on the total weight of the composition,
[0007] wherein the biodegradable polymer is present in an amount of 0 wt % to less than 50 wt % based on the total combined amount of the biodegradable polymer and cellulose acetate,
[0008] wherein the cellulose acetate composition is biodegradable when tested under industrial composting conditions according to ASTM D6400, and
[0009] wherein when the cellulose acetate composition is formed into a 10 mil film, the film exhibits at least 90% disintegration in not more than 12 weeks as measured according to the Disintegration Test Protocol described in the specification.
[0010] Additional compositions, articles, and methods are also disclosed herein. BRIEF DESCRIPTION OF THE DRAWINGS
[0011] Figure 1 The weight loss curves for Example 36, Example 37 and Foamazol 73S are described. DETAILED DESCRIPTION
[0012] Cellulose acetate
[0013] In an embodiment, the cellulose acetate used in the present invention can be any cellulose acetate known in the art and biodegradable. The cellulose acetate that can be used in the present invention generally comprises repeating units of the following structure:
[0014]
[0015] Where R 1 , R 2 and R 3 Independently selected from hydrogen or acetyl. For cellulose esters, the substitution level is usually expressed as a degree of substitution (DS), which is the average number of non-OH substituents per anhydroglucose unit (AGU). Typically, conventional cellulose contains three hydroxyl groups that can be replaced in each AGU unit; therefore, the value of DS can be between 0 and 3. Natural cellulose is a large polysaccharide, and even after pulping and purification, the degree of polymerization is between 250-5,000, so the assumption that the maximum DS is 3.0 is approximately correct. Since DS is a statistical average, a value of 1 does not guarantee that each AGU has a single substituent. In some cases, there may be unsubstituted anhydroglucose units, some with two substituents, some with three substituents, and generally the value is a non-integer. The total DS is defined as the average number of all substituents per anhydroglucose unit. The degree of substitution per AGU can also refer to a specific substituent, such as a hydroxyl or acetyl group. In an embodiment, n is an integer in the range of 25 to 250, or 25 to 200, or 25 to 150, or 25 to 100, or 25 to 75.
[0016] In an embodiment of the present invention, cellulose acetate has at least 2 anhydroglucose rings, and may have at least 50 to a maximum of 5,000 anhydroglucose rings, or at least 50 to less than 150 anhydroglucose rings. The number of anhydroglucose units per molecule is defined as the degree of polymerization (DP) of cellulose acetate. In an embodiment, the inherent viscosity (IV) of the cellulose ester may be about 0.2 to about 3.0 deciliters per gram, or about 0.5 to about 1.8, or about 1 to about 1.5, measured at a temperature of 25° C. in 100 ml of a 60 / 40 weight ratio phenol / tetrachloroethane solution for 0.25 grams of sample. In an embodiment, the DS / AGU of the cellulose acetate useful in the present invention may be about 1 to about 2.5, or 1 to less than 2.2, or 1 to less than 1.5, and the substituted ester is an acetyl group.
[0017] Cellulose acetate can be prepared by any method known in the art. Examples of methods for producing cellulose esters are taught in Kirk-Othmer, Encyclopedia of Chemical Technology, 5th Edition, Vol. 5, Wiley-Interscience, New York (2004), pp. 394-444. Cellulose, the starting material for the production of cellulose acetate, can be obtained in different grades and sources, such as from cotton linters, softwood pulp, hardwood pulp, corn fiber and other agricultural sources, as well as bacterial cellulose and the like.
[0018] One method of preparing cellulose acetate is to esterify cellulose by mixing cellulose with a suitable organic acid, anhydride and catalyst. The cellulose is then converted into a cellulose triester. The ester is then hydrolyzed by adding a water-acid mixture to the cellulose triester, which can then be filtered to remove any gel particles or fibers. Water is then added to the mixture to precipitate the cellulose ester. The cellulose ester can then be washed with water to remove reaction by-products, then dehydrated and dried.
[0019] The cellulose triester to be hydrolyzed may have three acetyl substituents. These cellulose esters may be prepared by many methods known to those skilled in the art. For example, cellulose esters may be prepared by heterogeneous acylation of cellulose in a mixture of carboxylic acid and anhydride in the presence of a catalyst such as H2SO4. Cellulose triesters may also be prepared by homogeneous acylation of cellulose dissolved in a suitable solvent such as LiCl / DMAc or LiCl / NMP.
[0020] Those skilled in the art will understand that the commercial term cellulose triesters also include cellulose esters that are not fully substituted with acyl groups. For example, cellulose triacetate commercially available from Eastman Chemical Company, Kingsport, TN, USA, typically has a DS of about 2.85 to about 2.99.
[0021] After esterification of cellulose to triester, some of the acyl substituents may be removed by hydrolysis or alcoholysis to obtain cellulose diester. As previously mentioned, the distribution of acyl substituents may be random or non-random, depending on the particular method used. Cellulose diesters may also be prepared directly without hydrolysis by using a limited amount of acylating agent. This method is particularly useful when the reaction is carried out in a solvent that dissolves cellulose. All of these methods produce cellulose esters that can be used in the present invention.
[0022] In one embodiment or in combination with any of the mentioned embodiments, the cellulose acetate is cellulose diacetate having a polystyrene equivalent number average molecular weight (Mn) of about 10,000 to about 100,000 as measured by gel permeation chromatography (GPC) according to ASTM D6474 using NMP as solvent and a polystyrene equivalent Mn. In an embodiment, the cellulose acetate composition comprises cellulose diacetate having a polystyrene equivalent number average molecular weight (Mn) of 10,000-90,000; or 10,000 to 80,000; or 10,000 to 70,000; or 10,000 to 60,000; or 10,000 to less than 60,000; or 10,000 to less than 55,000; or 10,000 to 50,000; or 10,000 to less than 50,000; or 10,000 to less than 45,000; or 10,000 to 40,000; or 10,000 to 30,000; or 20,000 to less than 60,000; or or 30,000 to less than 60,000; or 30,000 to less than 55,000; or 30,000 to 50,000; or 30,000 to less than 50,000; or 30,000 to less than 45,000; or 20,000 to 40,000; or 20,000 to 35,000; or 20,000 to 30,000; or 30,000 to less than 60,000; or 30,000 to less than 55,000; or 30,000 to 50,000; or 30,000 to less than 50,000; or 30,000 to less than 45,000; or 30,000 to 40,000; or 30,000 to 35,000; is measured by gel permeation chromatography (GPC) according to ASTM D6474 using NMP as solvent.
[0023] The most common commercial cellulose diesters are prepared by an initial acid-catalyzed heterogeneous acylation of cellulose to form cellulose triesters. After obtaining a homogeneous solution of the cellulose triesters in the corresponding carboxylic acids, the cellulose triesters are hydrolyzed until the desired degree of substitution is obtained. After separation, random cellulose diesters are obtained. That is, the relative degree of substitution (RDS) at each hydroxyl group is approximately equal.
[0024] The cellulose acetate useful in the present invention may be prepared using techniques known in the art and may be selected from various types of cellulose esters, such as those available from Eastman Chemical Company, Kingsport, Tennessee, USA, such as Eastman TM Cellulose acetate CA 398-30 and Eastman TM Cellulose acetate CA 398-10.
[0025] In embodiments of the invention, cellulose acetate can be prepared by converting cellulose into cellulose esters using reactants obtained from recycled materials (e.g., recycled plastic component syngas sources). In embodiments, such reactants can be cellulosic reactants, including organic acids and / or anhydrides used in esterification or acylation reactions of cellulose, for example, as discussed herein.
[0026] In one embodiment of the invention or in combination with any of the mentioned embodiments, or in combination with any of the mentioned embodiments, there is provided a cellulose acetate composition comprising at least one recycled cellulose acetate, wherein the cellulose acetate has at least one substituent on an anhydroglucose unit (AU) derived from a recycled content material (e.g., recycled plastic content syngas).
[0027] In one aspect, biodegradable cellulose acetate can be formulated into a cellulose acetate composition together with a plasticizer and at least one of a filler, an additive, a biopolymer, a stabilizer, and / or an odor modifier. Examples of additives include waxes, compatibilizers, biodegradation promoters, dyes, pigments, colorants, gloss control agents, lubricants, antioxidants, viscosity modifiers, antifungal agents, antifogging agents, thermal stabilizers, impact modifiers, antibacterial agents, softeners, release agents, and combinations thereof. It should be noted that the same type of compound or material can be identified as or included in multiple categories of components in the cellulose acetate composition. For example, polyethylene glycol (PEG) can be used as a plasticizer or as an additive that does not have plasticizer function, such as a hydrophilic polymer or a biodegradation promoter, for example, wherein a lower molecular weight PEG has a plasticizing effect, while a higher molecular weight PEG acts as a hydrophilic polymer but does not have a plasticizing effect.
[0028] In an embodiment, the cellulose acetate composition comprises biodegradable cellulose acetate (BCA) and at least one plasticizer. The plasticizer reduces the melting temperature, Tg and / or melt viscosity of cellulose acetate. In an embodiment, the plasticizer is a plasticizer that meets food standards. Meet food standards means to meet applicable food additives and / or food contact regulations, wherein the plasticizer is approved for use or recognized as safe by at least one (national or regional) food safety management agency (or organization), such as listed in the 21CFR food additive regulations or generally recognized as safe (GRAS) plasticizers by the U.S. Food and Drug Administration (FDA). In an embodiment, the plasticizer that meets food standards is triacetin. In an embodiment, examples of food-compliant plasticizers that may be considered may include triacetin, triethyl citrate, polyethylene glycol, benzoate plasticizers (Benzoflex), propylene glycol, polysorbate sucrose octaacetate, acetylated triethyl citrate, acetyl tributyl citrate, Admex, tripropionin, Scandiflex, poloxamer copolymers, polyethylene glycol succinate, diisobutyl adipate, polyvinyl pyrrolidone, and ethylene glycol tribenzoate.
[0029] In embodiments, the plasticizer may be present in an amount sufficient to allow the cellulose acetate composition to be melt processed (or thermoformed) in conventional melt processing equipment into useful articles (e.g., disposable plastic articles). In embodiments, the plasticizer is present in an amount of 1 wt%-40 wt% for most thermoplastic processing, based on the weight of the cellulose acetate composition; or 15 wt%-25 wt%, or 13 wt%-17 wt% for profile extrusion; or 19 wt%-22 wt% for sheet extrusion; or 23 wt%-27 wt% for injection molding. In embodiments, profile extrusion, sheet extrusion, thermoforming, and injection molding may be accomplished using plasticizer levels in the range of 13 wt%-30 wt%, or 13 wt%-25 wt%, or 15 wt%-30 wt%, or 15 wt%-25 wt%, based on the weight of the cellulose acetate composition.
[0030] In an embodiment, the plasticizer is a biodegradable plasticizer. Some examples of biodegradable plasticizers include triacetin, triethyl citrate, acetyl triethyl citrate, polyethylene glycol, benzoate-containing plasticizers such as Benzoflex TM Plasticizer series, poly(alkyl succinates) such as poly(butyl succinate), polyether sulfones, adipate-based plasticizers, soybean oil epoxides such as Paraplex TM Plasticizer series, sucrose-based plasticizer, dibutyl sebacate, tributyrin, sucrose acetate isobutyrate, Resolflex TMPlasticizer series, triphenyl phosphate, glycolate, polyethylene glycol, 2,2,4-trimethyl-1,3-pentanediol diisobutyrate and polycaprolactone.
[0031] In an embodiment, the cellulose acetate composition comprises a biodegradable CA component and a biodegradable polymer component, the biodegradable CA component comprising at least one BCA, and the biodegradable polymer component comprising at least one other biodegradable polymer (other than BCA). In an embodiment, the other biodegradable polymer can be selected from polyhydroxyalkanoates (PHA and PHB), polylactic acid (PLA), polycaprolactone polymers (PCL), polybutylene adipate terephthalate (PBAT), polyethylene succinate (PES), polyvinyl acetate (PVA), polybutylene succinate (PBS) and copolymers (e.g., polybutylene succinate-adipate (PBSA)), cellulose esters, cellulose ethers, starch, proteins, derivatives thereof, and combinations thereof. In an embodiment, the cellulose acetate composition comprises two or more biodegradable polymers. In an embodiment, the cellulose acetate composition contains a biodegradable polymer (other than BCA) in an amount of 0.1 wt% to less than 50 wt%, or 1 wt% to 40 wt%, or 1 wt% to 30 wt%, or 1 wt% to 25 wt%, or 1 wt% to 20 wt%, based on the cellulose acetate composition. In an embodiment, the cellulose acetate composition contains a biodegradable polymer (other than BCA) in an amount of 0.1 wt% to less than 50 wt%, or 1 wt% to 40 wt%, or 1 wt% to 30 wt%, or 1 wt% to 25 wt%, or 1 wt% to 20 wt%, based on the total amount of BCA and the biodegradable polymer. In an embodiment, at least one biodegradable polymer comprises a weight average molecular weight (Mw) of 10,000 to 1,000,000, or 50,000 to 1,000,000, or 100,000 to 1,000,000, or 250,000 to 1,000,000, or 500,000 to 1,000,000, or 600,000 to 1,000,000, or 600 ,000 to 900,000, or 700,000 to 800,000, or 10,000 to 500,000, or 10,000 to 250,000, or 10,000 to 100,000, or 10,000 to 50,000, measured using gel permeation chromatography (GPC) with a refractive index detector and polystyrene standards using a dichloromethane solvent. In an embodiment, the PHA may include polyhydroxybutyrate-co-hydroxyhexanoate.
[0032] In certain embodiments, the cellulose acetate composition comprises at least one stabilizer. Although it is desirable that the cellulose acetate composition be composable and / or biodegradable, an amount of stabilizer may be added to provide a selected shelf life or stability to light exposure, oxidative stability, or hydrolytic stability, for example. In various embodiments, stabilizers may include: UV absorbers, antioxidants (ascorbic acid, BHT, BHA, etc.), other acids and free radical scavengers, epoxidized oils such as epoxidized soybean oil, or combinations thereof.
[0033] Antioxidants can be divided into several categories, including primary antioxidants and secondary antioxidants. It is generally known that primary antioxidants are basically used as free radical terminators (scavengers). It is generally known that secondary antioxidants decompose hydroperoxides (ROOH) into non-reactive products before they decompose into alkoxy and hydroxyl radicals. Secondary antioxidants are often used in combination with free radical scavengers (primary antioxidants) to achieve a synergistic inhibitory effect, and the secondary AO is used to extend the life of the phenolic primary AO.
[0034] "Primary antioxidants" are antioxidants that act by reacting with peroxide free radicals via hydrogen transfer to quench the free radicals. Primary antioxidants typically contain reactive hydroxyl or amino groups, such as in hindered phenols and secondary aromatic amines. Examples of primary antioxidants include BHT, Irganox TM 1010, 1076, 1726, 245, 1098, 259 and 1425; Ethanox TM 310, 376, 314 and 330; Evernox TM 10, 76, 1335, 1330, 3114, MD 1024, 1098, 1726, 120, 2246 and 565; Anox TM 20, 29, 330, 70, IC-14 and 1315; Lowinox TM 520, 1790, 22IB46, 22M46, 44B25, AH25, GP45, CA22, CPL, HD98, TBM-6, and WSP; Naugard TM 431, PS48, SP and 445; Songnox TM 1010, 1024, 1035, 1076CP, 1135LQ, 1290PW, 1330FF, 1330PW, 2590 PW and 3114FF; and ADK Stab AO-20, AO-30, AO-40, AO-50, AO-60, AO-80 and AO-330.
[0035] "Secondary antioxidants" are often called hydroperoxide decomposers. They work by reacting with hydroperoxides, breaking them down into non-reactive and heat-stable products that are not free radicals. They are often used in combination with primary antioxidants. Examples of secondary antioxidants include organophosphorus (e.g., phosphites, phosphonites) and organosulfur compounds. The phosphorus and sulfur atoms of these compounds react with peroxides, converting the peroxides into alcohols. Examples of secondary antioxidants include Ultranox 626, Ethanox TM 368, 326 and 327; Doverphos TM LPG11, LPG12, DPS-680, 4, 10, S480, S-9228, S-9228T; Evernox TM 168 and 626; Irgafos TM 126 and 168; Weston TM DPDP, DPP, EHDP, PDDP, TDP, TLP and TPP; Mark TM CH 302, CH 55, TNPP, CH 66, CH 300, CH 301, CH 302, CH 304, and CH 305; ADK Stab 2112, HP-10, PEP-8, PEP-36, 1178, 135A, 1500, 3010, C, and TPP; Weston 439, DHOP, DPDP, DPP, DPTDP, EHDP, PDDP, PNPG, PTP, PTP, TDP, TLP, TPP, 398, 399, 430, 705, 705T, TLTTP, and TNPP; Alkanox 240, 626, 626A, 627AV, 618F, and 619F; and Songnox TM 1680FF, 1680PW, 6280FF.
[0036] In an embodiment, the cellulose acetate composition comprises at least one stabilizer, wherein the stabilizer comprises one or more secondary antioxidants. In an embodiment, the stabilizer comprises a first stabilizer component selected from one or more secondary antioxidants and a second stabilizer component selected from one or more primary antioxidants, citric acid, or a combination thereof.
[0037] In an embodiment, the stabilizer comprises one or more auxiliary antioxidants, based on the total weight of the composition, in an amount of 0.01wt%-0.8wt%, or 0.01wt%-0.7wt%, or 0.01wt%-0.5wt%, or 0.01wt%-0.4wt%, or 0.01wt%-0.3wt%, or 0.01wt%-0.25wt%, or 0.01wt%-0.2wt%, or 0.05wt%-0.8wt%, or 0.05wt%-0.7wt%, or 0.05wt%-0. In one embodiment, the stabilizer comprises an auxiliary antioxidant, which is a phosphite compound. In one embodiment, the stabilizer comprises an auxiliary antioxidant and another auxiliary antioxidant, which is a phosphite compound, and the other auxiliary antioxidant is DLTDP.
[0038] In a subclass of this class, the stabilizer further comprises a second stabilizer component comprising one or more primary antioxidants, wherein the amount of the primary antioxidant is in the range of 0.05wt%-0.7wt%, or 0.05wt%-0.6wt%, or 0.05wt%-0.5wt%, or 0.05wt%-0.4wt%, or 0.05wt%-0.3wt%, or 0.1wt%-0.6wt%, or 0.1wt%-0.5wt%, or 0.1wt%-0.4wt%, or 0.1wt%-0.3wt%, based on the total weight of the composition. In another subclass of this class, the stabilizer further comprises a second stabilizer component comprising citric acid, the amount of which is in the range of 0.05wt%-0.2wt%, or 0.05wt%-0.15wt%, or 0.05wt%-0.1wt% of the total amount of citric acid, based on the total weight of the composition. In another subclass of this class, the stabilizer further comprises a second stabilizer component comprising one or more primary antioxidants and citric acid, the amounts of which are as discussed herein. In a subclass of this class, the stabilizer comprises less than 0.1wt% of the primary antioxidant or does not contain the primary antioxidant, based on the total weight of the composition. In a subclass of this class, the stabilizer comprises less than 0.05wt% of the primary antioxidant or does not contain the primary antioxidant, based on the total weight of the composition.
[0039] In an embodiment, the cellulose acetate composition comprises at least one filler. In an embodiment, the type and amount of filler present can improve biodegradability and / or compostability. In an embodiment, the cellulose acetate composition comprises at least one filler selected from the group consisting of carbohydrates (sugars and salts), cellulose and organic fillers (wood flour, wood fiber, hemp, carbon, coal particles, graphite, and starch), mineral and inorganic fillers (calcium carbonate, talc, silica, titanium dioxide, glass fiber, glass spheres, boron nitride, aluminum trihydrate, magnesium hydroxide, calcium hydroxide, aluminum oxide, and clay), food waste or byproducts (egg shells, wine lees, and coffee grounds), desiccants (e.g., calcium sulfate, magnesium sulfate, magnesium oxide, calcium oxide), alkaline fillers (e.g., Na 2 CO 3 MgCO 3 ) or a combination (e.g., a mixture) of such fillers. In an embodiment, the cellulose acetate composition may include at least one filler that also functions as a colorant additive. In an embodiment, the colorant additive filler may be selected from the group consisting of: carbon, graphite, titanium dioxide, opacifiers, dyes, pigments, toners, and combinations thereof. In an embodiment, the cellulose acetate composition may include at least one filler that also functions as a stabilizer or flame retardant.
[0040] In an embodiment, the cellulose acetate composition comprises at least one plasticizer (as described herein) in an amount of 1 wt%-40wt%, or 5wt%-40wt%, or 10wt%-40wt%, or 13wt%-40wt%, or 15wt%-40wt%, or greater than 15wt%-40wt%, or 17wt%-40wt%, or 20wt%-40wt%, or 25wt%-40wt%, or 5wt%-35wt%, or 10wt%-35wt%, or 13wt%-35wt%, or 15wt%-35wt%, or greater than 15wt%-35wt%, or 17wt%-35wt%, or 20wt%-35wt%, or 5wt%-30wt%, or 10wt%-30wt%, or 13wt%-30wt%, or 15wt%-35wt%, or greater than 15wt%-35wt%, or 17wt%-35wt%, or 20wt%-35wt%, or 5wt%-30wt%, or 10wt%-30wt%, or 13wt%-30wt%, or 15wt%-35wt%, or greater than 15wt%-35wt%, or 17wt%-35wt%, or 20wt%-35wt%, or 5wt%-30wt%, or 30wt%, or greater than 15wt%-30wt%, or 17wt%-30wt%, or 5wt%-25wt%, or 13wt%-25wt%, or 15wt%-25wt%, or greater than 15wt%-25wt%, or 17wt%-25wt%, or 5wt%-20wt%, or 10wt%-20wt%, or 13wt%-20wt%, or 15wt%-20wt%, or Greater than 15wt%-20wt%, or 17wt%-20wt%, or 5wt%-17wt%, or 10wt%-17wt%, or 13wt%-17wt%, or 15wt%-17wt%, or greater than 15wt%-17wt%, or 5wt%-less than 17wt%, or 10wt%-less than 17wt%, or 13wt%-less than 17wt%, or 15wt%-less than 17wt%.In an embodiment, the cellulose acetate composition further comprises at least one filler (as described herein) in an amount of 1 wt%-60 wt%, or 5 wt%-55 wt%, or 5 wt%-50 wt%, or 5 wt%-45 wt%, or 5 wt%-40 wt%, or 5 wt%-35 wt%, or 5 wt%-30 wt%, or 5 wt%-25 wt%, or 10 wt%-55 wt%, or 10 wt%-50 wt%, or 10 wt%-45 wt%, or 10 wt%-40 wt%, or 10 ...%. %-35wt%, or 10wt%-30wt%, or 10wt%-25wt%, or 15wt%-55wt%, or 15wt%-50wt%, or 15wt%-45wt%, or 15wt%-40wt%, or 15wt%-35wt%, or 15wt%-30wt%, or 15wt%-25wt%, or 20wt%-55wt%, or 20wt%-50wt%, or 20wt%-45wt%, or 20wt%-40wt%, or 20wt%-35wt%, or 20wt%-30wt%. In an embodiment, at least one plasticizer comprises a plasticizer that meets food standards or is a plasticizer that meets food standards. In an embodiment, the plasticizer that meets food standards comprises triacetin or is triacetin. In an embodiment, the filler comprises calcium carbonate or is calcium carbonate.
[0041] In an embodiment, the cellulose acetate composition may include at least one odor modifying additive, depending on the application, such as a disposable food contact application. In an embodiment, depending on the application and the components used in the cellulose acetate composition, suitable odor modifying additives may be selected from the group consisting of: vanillin, Pennyroyal M-1178, almonds, cinnamon, spices, spice extracts, volatile organic compounds or small molecules, and Plastidor. In an embodiment, the odor modifying additive may be vanillin. In an embodiment, the cellulose acetate composition may include the odor modifying additive in an amount of 0.01 wt%-1 wt%, or 0.1 wt%-0.5 wt%, or 0.1 wt%-0.25 wt%, or 0.1 wt%-0.2 wt%, based on the total weight of the composition. The mechanism of the odor modifying additive may include masking, capturing, supplementing, or a combination of these.
[0042] As described above, the cellulose acetate composition may include other additives. In an embodiment, the cellulose acetate composition may include at least one compatibilizer. In an embodiment, the compatibilizer may be a non-reactive compatibilizer or a reactive compatibilizer. The compatibilizer may enhance the ability of the cellulose acetate or another component to achieve a desired small particle size to improve the dispersion of the selected component in the composition. In such an embodiment, the biodegradable cellulose acetate may be in the continuous phase or the discontinuous phase of the dispersion, depending on the desired formulation. In an embodiment, the compatibilizer used may improve the mechanical and / or physical properties of the composition by changing the interfacial interaction / bonding between the biodegradable cellulose acetate and another component (e.g., other biodegradable polymers).
[0043] In an embodiment, the cellulose acetate composition comprises a compatibilizer in an amount of about 1 wt% to about 40 wt%, or about 1 wt% to about 30 wt%, or about 1 wt% to about 20 wt%, or about 1 wt% to about 10 wt%, or about 5 wt% to about 20 wt%, or about 5 wt% to about 10 wt%, or about 10 wt% to about 30 wt%, or about 10 wt% to about 20 wt%, based on the weight of the cellulose acetate composition.
[0044] In an embodiment, the cellulose acetate composition may include a biodegradation agent and / or decomposer, if desired, for example, a hydrolysis aid or any intended degradation promoter additive may be added to or contained in the cellulose acetate composition, added during or after the manufacture of biodegradable cellulose acetate (BCA), and melt or solvent blended with BCA to prepare the cellulose acetate composition. In an embodiment, the additive may promote hydrolysis by releasing acidic or alkaline residues, and / or accelerate light (UV) or oxidative degradation and / or promote the growth of selective microbial colonies to aid decomposition and biodegradation in compost and soil media. In addition to promoting degradation, these additives may have additional functions, such as improving the processability of the product or improving desired mechanical properties.
[0045] One group of examples of possible decomposing agents include inorganic carbonates, synthetic carbonates, nepheline syenite, talc, magnesium hydroxide, aluminum hydroxide, diatomaceous earth, natural or synthetic silica, calcined clay, etc. In embodiments, it may be desirable that these additives are well dispersed in the cellulose acetate composition matrix. The additives may be used alone or in combination of two or more.
[0046] Another group of examples of possible decomposing agents are aromatic ketones used as oxidative decomposing agents, including benzophenone, anthraquinone, anthrone, acetylbenzophenone, 4-octylbenzophenone, etc. These aromatic ketones can be used alone or in combination of two or more.
[0047] Other examples include transition metal compounds used as oxidative decomposition agents, such as cobalt or magnesium salts, such as aliphatic carboxylic acid (C12-C20) salts of cobalt or magnesium, or cobalt stearate, cobalt oleate, magnesium stearate and magnesium oleate; or anatase titanium dioxide, or titanium dioxide. Mixed phase titanium dioxide particles in which both rutile and anatase crystal structures are present in the same particle can be used. The photoactive agent particles can have a relatively high surface area, such as about 10 to about 300 sq.m / g, or 20 to 200 sq.m / g, measured by the BET surface area method. If desired, the photoactive agent can be added to the plasticizer. These transition metal compounds can be used alone or in combination of two or more.
[0048] Examples of rare earth compounds that can be used as oxidative decomposition agents include rare earths belonging to Group 3A of the periodic table and their oxides. Specific examples include cerium (Ce), yttrium (Y), neodymium (Nd), rare earth oxides, hydroxides, rare earth sulfates, rare earth nitrates, rare earth acetates, rare earth chlorides, rare earth carboxylates, etc. More specific examples include cerium oxide, cerium sulfate, ammonium cerium sulfate, ammonium cerium nitrate, cerium acetate, lanthanum nitrate, cerium chloride, cerium nitrate, cerium hydroxide, cerium octoate, lanthanum oxide, yttrium oxide, scandium oxide, etc. These rare earth compounds can be used alone or in combination of two or more.
[0049] In one embodiment, the BCA composition includes an additive having pro-degradation functionality to enhance biodegradability, the additive including a transition metal salt or a chemical catalyst containing a transition metal (e.g., cobalt, manganese, and iron). The transition metal salt may include tartrate, stearate, oleate, citrate, and chloride. The additive may also include a free radical scavenging system and one or more inorganic or organic fillers, such as chalk, talc, silicon dioxide, wollastonite, starch, cotton, recycled paperboard, and plant matter. The additive may also include enzymes, bacterial cultures, expanders, CMC, sugars, or other energy sources. The additive may also include hydroxylamine esters and thio compounds.
[0050] In certain embodiments, other possible biodegradation and / or decomposition agents may include swelling agents and disintegrants. Swelling agents may be hydrophilic materials that increase in volume after absorbing water and exert pressure on the surrounding matrix. Disintegrants may be additives that promote the decomposition of the matrix into smaller fragments in an aqueous environment. Examples include minerals and polymers, including cross-linked or modified polymers and swellable hydrogels. In an embodiment, the BCA composition may include water-swelling minerals or clays and their salts, such as synthetic hectorite and bentonite; hydrophilic polymers, such as poly (acrylic acid) and salts, poly (acrylamide), poly (ethylene glycol) and poly (vinyl alcohol); polysaccharides and gums, such as starch, alginates, pectin, chitosan, psyllium, xanthan gum; guar gum, locust bean gum; and modified polymers, such as cross-linked PVP, sodium starch glycolate, carboxymethyl cellulose, gelatinized starch, cross-linked sodium carboxymethyl cellulose; or combinations of these additives.
[0051] In an embodiment, the BCA composition may include an alkaline additive that can increase the decomposition or degradation of the composition or an article made from (or including) the composition. Examples of alkaline additives that can be used as oxidative decomposition agents include alkaline earth metal oxides, alkaline earth metal hydroxides, alkaline earth metal carbonates, alkali metal carbonates, alkali metal bicarbonates, ZnO, and alkaline Al 2 O 3 In an embodiment, at least one alkaline additive may be MgO, Mg(OH) 2 MgCO 3 , CaO, Ca(OH) 2 、CaCO 3 、NaHCO 3 、Na 2 CO 3 、K2CO 3 、ZnΟKHCO 3 or basic Al 2 O 3 In one aspect, alkaline earth metal oxides, ZnO and alkaline Al 2 O 3 Can be used as alkaline additives. In embodiments, combinations of different alkaline additives, or combinations of alkaline additives with other additives can be used. In embodiments, the pH of the alkaline additive is greater than 7.0 to 10.0, or 7.1 to 9.5, or 7.1 to 9.0, or 7.1 to 8.5, or 7.1 to 8.0, measured in a mixture / solution of 1 wt % water.
[0052] Examples of organic acid additives that can be used as oxidative decomposers include acetic acid, propionic acid, butyric acid, valeric acid, citric acid, tartaric acid, oxalic acid, malic acid, benzoic acid, formates, acetates, propionates, butyrates, valerates, citrates, tartrates, oxalates, malates, maleic acid, maleates, phthalic acid, phthalates, benzoates, and combinations thereof.
[0053] Examples of other hydrophilic polymers or biodegradation promoters may include glycols, polyethylene glycols, polyethers and polyols or other biodegradable polymers such as poly(glycolic acid), poly(lactic acid), polyethylene glycol, polypropylene glycol, polydioxanes, polyoxalates, poly(α-esters), polycarbonates, polyanhydrides, polyacetals, polycaprolactones, poly(orthoesters), polyamino acids, aliphatic polyesters such as polybutylene succinate, polyethylene succinate, starch, regenerated cellulose or aliphatic-aromatic polyesters such as PBAT.
[0054] In embodiments, examples of colorants may include carbon black, iron oxides such as red or blue iron oxide, titanium dioxide, silicon dioxide, cadmium red, calcium carbonate, kaolin, aluminum hydroxide, barium sulfate, zinc oxide, aluminum oxide; and organic pigments such as azo and diazo and triazine pigments, condensed azo, azo lakes, naphthol pigments, anthracene pyrimidines, benzimidazolone, carbazole, diketopyrrolopyrrole, flavanone, indigo pigments, isoindolinone, isoindolinone, isoanthrone violet, metal Complex pigments, oxazines, perylenes, pyrenones, pyranthrones, pyrazoloquinazolinones, quinolinephthalones, triarylcarbonium pigments, triphenodioxazines, xanthenes, thioindigos, indanthrones, isoindanthrones, anthraquinones, anthraquinones, isodibenzanthrones, triphenodioxazines, quinacridones and the phthalocyanine series, especially copper phthalocyanine and its core halogenated derivatives, as well as acid lakes, basic and mordant dyes, and isoindolinone pigments, as well as plants and vegetable dyes, and any other useful colorants or dyes.
[0055] In an embodiment, the gloss control agent for adjusting the glossiness and filler may include silica, talc, clay, barium sulfate, barium carbonate, calcium sulfate, calcium carbonate, magnesium carbonate, and the like.
[0056] Suitable flame retardants may include silica, metal oxides, phosphates, catechol phosphates, resorcinol phosphates, borates, inorganic hydrates, and aromatic polyhalides.
[0057] Antifungal and / or antibacterial agents include polyene antifungals (e.g., natamycin, chastomycin, filipin, nystatin, amphotericin B, candesin and hamycin), imidazole antifungals such as miconazole (available as from WellSpring Pharmaceuticals), ketoconazole (available as Available from McNeil Consumer Healthcare), clotrimazole (available as and LOTRAMIN Commercially available from Merck and commercially available from Bayer), econazole, omoconazole, bifonazole, butoconazole, fenticonazole, isoconazole, oxiconazole, sertaconazole (available as commercially available from OrthoDematologics), sulconazole, and tioconazole; triazole antifungals such as fluconazole, itraconazole, isavuconazole, ravuconazole, posaconazole, voriconazole, terconazole, and albaconazole, thiazole antifungals such as abafungin, allylamine antifungals such as terbinafine (available as commercially available from Novartis Consumer Health), naftifine (available as commercially available from McDevitt Pharmaceuticals) and butenafine (available as LOTRAMIN commercially available from Merck), echinocandin antifungals (e.g., anidulafungin, caspofungin, and micafungin), polygonaldialdehyde, benzoic acid, ciclopirox, tolnaftate (e.g., available as Commercially available from MDS Consumer Health, Inc.), undecylenic acid, flucytosine, 5-flucytosine, griseofulvin, haloprogin, octanoic acid, and any combination thereof.
[0058] Viscosity modifiers useful for altering the melt flow index or viscosity of the biodegradable cellulose acetate composition that can be used include polyethylene glycol, polypropylene glycol, and glycerin.
[0059] In embodiments, other components that may be included in the BCA composition may serve as mold release agents or lubricants (e.g., fatty acids, ethylene glycol distearate), anti-caking agents or lubricants (e.g., fatty acid esters, metal stearates (e.g., zinc stearate), and waxes), anti-fogging agents (e.g., surfactants), thermal stabilizers (e.g., epoxy stabilizers, derivatives of epoxidized soybean oil (ESBO), linseed oil, and sunflower oil), antistatic agents, foaming agents, antimicrobial agents, impact modifiers, or reinforcing fibers. More than one component may be present in a BCA composition. It should be noted that in a BCA composition, additional components may have more than one function. The different (or specific) functionality of any particular additive (or component) of a BCA composition may depend on its physical properties (e.g., molecular weight, solubility, melting temperature, Tg, etc.) and / or the amount of such additive / component in the overall composition. For example, polyethylene glycol may act as a plasticizer at one molecular weight, or act as a hydrophilic agent (with little or no plasticizing effect) at another molecular weight.
[0060] In an embodiment, if necessary, a fragrance can be added. Examples of fragrances can include spices, spice extracts, herbal extracts, essential oils, smelling salts, volatile organic compounds, volatile small molecules, methyl formate, methyl acetate, methyl butyrate, ethyl acetate, ethyl butyrate, isoamyl acetate, amyl butyrate, amyl valerate, octyl acetate, myrcene, geraniol, nerol, citral, citronellal, citronellol, linalool, nerolidol, limonene, camphor, terpineol, α-ionone, thujone, benzaldehyde, eugenol, isoeugenol, cinnamon Aldehydes, ethyl maltol, vanilla, vanillin, cinnamyl alcohol, aniseoxide, anethole, estragole, thymol, furanone, methanol, rosemary, lavender, citrus, freesia, apricot blossom, greens, peach, jasmine, rosewood, pine, thyme, oakmoss, musk, vetiver, myrrh, black currant, bergamot, grapefruit, gum arabic, passionflower, sandalwood, tonka bean, citrus, neroli, violet leaf, gardenia, red fruit, ylang-ylang, acaciafarnesiana), mimosa, tonka bean, wood, ambergris, daffodil, hyacinth, narcissus, blackcurrant buds, iris, raspberry, lily of the valley, sandalwood, vetiver, cedarwood, neroli, strawberry, carnation, oregano, honey, civet, heliotrope, caramel, coumarin, patchouli, dewberry, helonial, coriander, allspice, labdanum, cassie, aldehydes, orchid, amber, orris, tuberose, palmarosa, cinnamon, nutmeg, moss, styrax, pineapple , foxglove, tulip, wisteria, clematis, ambergris, gum, resin, civet, plum, castoreum, civet, myrrh, geranium, rose purple, kalanchoe, spicy carnation, galbanum, petitgrain, iris, honeysuckle, pepper, raspberry, benzoin, mango, coconut, orange peel (hesperides), castoreum, osmanthus, oakmoss, nectarine, mint, fennel, cinnamon, orris, apricot, plumeria, marigold, rose otto, narcissus, tolu balsam, frankincense, amber, orange blossom, vetiver, opoponax, white musk, wood melon, rock sugar, jackfruit, honeydew melon, lotus, lily of the valley, mulberry, wormwood, ginger, juniper berry, spicebush, peony, violet, lemon, lime, hibiscus, white rum, basil, lavender, balsamics, polygonum multiflorum, osmanthus, karokarunde, white orchid, calla lily, white rose, hairy lily, marigold, ambergris, ivy, grass, hevea, spearmint, clary sage, cottonwood, grape, brimbelle, lotus, cyclamen , orchid, glycine, tiare flower, wild ginger flower, green osmanthus, passion flower, blue rose, bay oil, acacia (cassie), African marigold, Anatolian rose, Auvergne narcissus, English broom, English broom chocolate, Bulgarian rose, Chinese patchouli, Chinese gardenia, Calabrian mandarin, Comoros tuberose, Ceylon cardamom, Caribbean passion flower, Damascus rose, Georgia peach, white Madonna lily, Egyptian jasmine, Egyptian marigold, Ethiopian civet, acacia (Farnesiancassie), Florentine iris, French jasmine, French kalanchoe, French hyacinth, Guinea orange, Guyana wacapua, Grasse orange leaf, Grasse rose, Grasse tuberose, Haitian vetiver, Hawaiian pineapple, Israeli basil, Indian sandalwood, Indian Ocean vanilla, Italian bergamot, Italian iris, Jamaican pepper, May rose, Madagascar ylang-ylang, Madagascar vanilla, Moroccan jasmine, Moroccan rose, Moroccan oakmoss, Moroccan orange blossom, Mysore sandalwood, Oriental rose, Russian leather, Russian coriander, Sicily mandarin, South African marigold, South African tonka bean, Singapore patchouli, Spanish orange blossom, Sicily lime, Reunion vetiver, Turkish rose, Thai benzoin, Tunisian orange blossom, Yugoslav oakmoss, Virginia cedarwood, Utah yarrow, West Indian rosewood, etc. and any combination thereof.
[0061] In embodiments, the cellulose acetate composition may be extrudable, moldable, castable, thermoformable, or 3D printable. In embodiments, the cellulose acetate composition is melt processable and may be formed into useful molded articles that are biodegradable and / or compostable, such as disposable food contact articles. In embodiments, the articles are non-persistent. Environmentally "non-persistent" means that when the biodegradable cellulose acetate reaches an advanced level of disintegration, it becomes susceptible to complete consumption by natural microbial populations. Degradation of the biodegradable cellulose acetate ultimately results in its conversion to carbon dioxide, water, and biomass. In an embodiment, an article is provided comprising a cellulose acetate composition (discussed herein) having a maximum thickness of up to 150 mils, or 140 mils, or 130 mils, or 120 mils, or 110 mils, or 100 mils, or 90 mils, or 80 mils, or 70 mils, or 60 mils, or 50 mils, or 40 mils, or 30 mils, or 25 mils, or 20 mils, or 15 mils, or 10 mils, and being biodegradable and compostable (i.e., passing the industrial or home compostability tests / standards discussed herein). In embodiments, articles are provided comprising a cellulose acetate composition (discussed herein) having a maximum thickness of up to 150 mils, or 140 mils, or 130 mils, or 120 mils, or 110 mils, to 100 mils, or 90 mils, or 80 mils, or 70 mils, or 60 mils, or 50 mils, or 40 mils, or 30 mils, or 25 mils, or 20 mils, or 15 mils, or 10 mils, and being environmentally non-durable.
[0062] In embodiments, cellulose acetate compositions and any articles made from or comprising such compositions comprise biodegradable cellulose acetate (BCA) containing some recycled content. In embodiments, the recycled content is provided by a reactant derived from a recycled material, which reactant is the source of one or more acetyl groups on the BCA. In embodiments, the reactant is derived from recycled plastic. In embodiments, the reactant is derived from recycled plastic component syngas. "Recycled plastic component syngas" refers to syngas obtained from a syngas operation utilizing a feedstock containing at least some recycled plastic content, as more fully described in the various embodiments below. In embodiments, the recycled plastic component syngas can be prepared according to any method for producing syngas described herein; can contain or consist of any syngas composition or syngas composition stream described herein; or can be made from any feedstock composition described herein.
[0063] In an embodiment, the feedstock (for syngas operation) may be a combination of one or more granular fossil fuel sources and granular recycled plastic. In one embodiment or in any of the mentioned embodiments, the solid fossil fuel source may include coal. In an embodiment, the feedstock is fed to a gasifier along with an oxidant gas, and the feedstock is converted to syngas.
[0064] In embodiments, recycled plastic content syngas is utilized to prepare at least one chemical intermediate in a reaction scheme to prepare recycled BCA. In embodiments, the recycled plastic content syngas may be a component of a feedstock (for preparing at least one CA intermediate) from other sources including syngas, hydrogen, carbon monoxide, or a combination thereof. In one embodiment or any of the mentioned embodiments, the sole source of syngas used to prepare the CA intermediate is recycled plastic content syngas.
[0065] In an embodiment, the CA intermediate prepared using recycled component syngas (e.g., recycled plastic component syngas) can be selected from methanol, acetic acid, methyl acetate, acetic anhydride, and combinations thereof. In an embodiment, the CA intermediate can be at least one reactant or at least one product in one or more of the following reactions: (1) conversion of syngas to methanol; (2) conversion of syngas to acetic acid; (3) conversion of methanol to acetic acid, e.g., carbonylation of methanol to produce acetic acid; (4) production of methyl acetate from methanol and acetic acid; and (5) conversion of methyl acetate to acetic anhydride, e.g., carbonylation of methyl acetate and methanol to acetic acid and acetic anhydride.
[0066] In an embodiment, recycled plastic content syngas is used to produce at least one cellulosic reactant. In an embodiment, recycled plastic content syngas is used to produce at least one recycled BCA.
[0067] In an embodiment, recycled plastic content syngas is used to make acetic anhydride. In an embodiment, syngas containing recycled plastic content syngas is first converted to methanol, which is then used in a reaction scheme to make acetic anhydride. "RPS acetic anhydride" refers to acetic anhydride derived from recycled plastic content syngas. Derived from means that at least some of the raw material source material (which is used in any reaction scheme to make the CA intermediate) has a certain amount of recycled plastic content syngas.
[0068] In an embodiment, RPS acetic anhydride is used as a CA intermediate reactant for esterification of cellulose to produce recycled BCA, as discussed more fully above. In an embodiment, RPS acetic acid is used as a reactant to produce cellulose acetate or cellulose diacetate.
[0069] In an embodiment, recycled CA is produced from a cellulosic reactant comprising acetic anhydride derived from recycled plastic content syngas.
[0070] In an embodiment, the recycled plastic content syngas comprises a gasification product from a gasification feedstock. In an embodiment, the gasification product is produced by a gasification process using a gasification feedstock comprising recycled plastic. In an embodiment, the gasification feedstock comprises coal.
[0071] In an embodiment, the gasification feedstock comprises a liquid slurry comprising coal and recycled plastic. In an embodiment, the gasification method comprises gasifying the gasification feedstock in the presence of oxygen.
[0072] In one aspect, a recycled BCA composition is provided, comprising at least one biodegradable cellulose ester having at least one substituent on an anhydroglucose unit (AGU), the anhydroglucose unit being derived from one or more chemical intermediates, at least one of which is obtained at least in part from recycled plastic component syngas.
[0073] In embodiments, the recycled BCA is biodegradable and contains components derived from renewable sources, such as cellulose from wood or cotton linters, and components derived from recycled material sources, such as recycled plastics. Thus, in embodiments, a melt-processable material is provided that is biodegradable and contains renewable and recycled components, i.e., is made from renewable and recycled sources.
[0074] The degree of substitution of biodegradable cellulose acetate useful in embodiments of the present invention can be in the range of 1.0 to 2.5. In some cases, the average degree of substitution of cellulose acetate as described herein can be at least about 1.0, 1.05, 1.1, 1.15, 1.2, 1.25, 1.3, 1.35, 1.4, 1.45, or 1.5 and / or no more than about 2.5, 2.45, 2.4, 2.35, 2.3, 2.25, 2.2, 2.15, 2.1, 2.05, 2.0, 1.95, 1.9, 1.85, 1.8, or 1.75.
[0075] In embodiments, the number average molecular weight (Mn) of the biodegradable cellulose acetate may be no greater than 100,000, or no greater than 90,000, as measured using gel permeation chromatography as polystyrene equivalents using N-methyl-2-pyrrolidone (NMP) as a solvent. In some cases, the Mn of the biodegradable cellulose acetate may be at least about 10,000, at least about 20,000, 25,000, 30,000, 35,000, 40,000, or 45,000, and / or no greater than about 100,000, 95,000, 90,000, 85,000, 80,000, 75,000, 70,000, 65,000, 60,000, or 50,000.
[0076] In an embodiment, the article containing BCA can be biodegradable and has a certain degree of degradation. The degree of degradation can be characterized by the weight loss of the sample in a given time period exposed to certain environmental conditions. In some cases, the BCA composition can show at least about 5%, 10%, 15% or 20% weight loss after being buried in the soil for 60 days, and / or can show at least about 15%, 20%, 25%, 30% or 35% weight loss after being exposed to a typical urban composter for 15 days. However, the degradation rate can vary according to the specific end use of the article and the composition and specific test of the article. Exemplary test conditions are provided in U.S. Patent No. 5,970,988 and U.S. Patent No. 6,571,802.
[0077] In some embodiments, the BCA composition can be in the form of a biodegradable disposable (shaped / molded) article. It has been found that the BCA composition as described herein can exhibit an increased level of environmental non-persistence, characterized by better than expected degradation under various environmental conditions. The BCA-containing articles described herein can meet or exceed the qualified standards for industrial compostability, home compostability, and / or soil biodegradability established by international test methods and authoritative agencies.
[0078] To be considered "compostable", a material must meet the following four criteria: (1) the material should pass the biodegradation requirement in tests under controlled composting conditions at elevated temperatures (58°C) according to ISO 14855-1 (2012), which is equivalent to 90% absolute biodegradation or 90% relative to a control polymer, (2) the material must achieve 90% disintegration when tested under aerobic composting conditions according to ISO 16929 (2013); (3) the tested material must meet all requirements for volatile solids, heavy metals, and fluorine as specified in ASTM D6400 (2012), EN 13432 (2000), and ISO 17088 (2012); and (4) the material should not have a negative impact on plant growth. As used herein, the term "biodegradable" generally refers to the biological transformation and consumption of organic molecules. Biodegradability is an inherent property of the material itself, and materials can exhibit varying degrees of biodegradability depending on the specific conditions to which they are exposed. The term "disintegrable" refers to the tendency of a material to physically break down into smaller pieces when exposed to certain conditions. Disintegration depends on the material itself as well as the physical size and construction of the article being tested. Ecotoxicity measures the effect of a material on plant life and determines the amount of heavy metals in a material according to procedures established by standard test methods.
[0079] When tested under aerobic composting conditions at ambient temperature (28°C ± 2°C) according to ISO 14855-1 (2012), the CA composition (or an article comprising the same) may exhibit at least 70% biodegradation within a period of no more than 50 days. In some cases, when tested under these conditions (also referred to as "home composting conditions"), the CA composition (or an article comprising the same) may exhibit at least 70% biodegradation within a period of no more than 49, 48, 47, 46, 45, 44, 43, 42, 41, 40, 39, 38 or 37 days. These conditions may not be aqueous or anaerobic. In some cases, the CA composition (or an article comprising the same) may exhibit at least about 71%, 72%, 73%, 74%, 75%, 76%, 77%, 78%, 79%, 80%, 81%, 82%, 83%, 84%, 85%, 86%, 87%, or 88% total biodegradation when tested under home composting conditions according to ISO 14855-1 (2012) for a period of 50 days. This may represent at least about 95%, 97%, 99%, 100%, 101%, 102%, or 103% relative biodegradation when compared to cellulose subjected to the same testing conditions.
[0080] To be considered "biodegradable", a material must show a total biodegradation of at least 90% (e.g., compared to the initial sample) under home composting conditions according to French Standard NF T 51-800 and Australian Standard AS 5810, or after both the reference and the test item have reached a steady state, the biodegradation is at least 90% of the maximum degradation of the appropriate reference material. The maximum test duration for biodegradation under home composting conditions is 1 year. The CA compositions described herein may show at least 90% biodegradation in no more than 1 year, measured under home composting conditions according to 14855-1 (2012). In some cases, the CA compositions (or articles comprising them) may show at least about 91%, 92%, 93%, 94%, 95%, 96%, 97%, 98%, 99% or 99.5% biodegradation in no more than 1 year, or the CA compositions (or articles comprising them) may show 100% biodegradation in no more than 1 year, measured under home composting conditions according to 14855-1 (2012).
[0081] Additionally, or in the alternative, the CA compositions described herein (or articles comprising the same) may exhibit at least 90% biodegradation in no more than about 350, 325, 300, 275, 250, 225, 220, 210, 200, 190, 180, 170, 160, 150, 140, 130, 120, 110, 100, 90, 80, 70, 60, or 50 days as measured under home composting conditions according to ISO 14855-1 (2012). In some cases, the CA compositions (or articles comprising the same) may be at least about 97%, 98%, 99%, or 99.5% biodegradable in no more than about 70, 65, 60, or 50 days as tested under home composting conditions according to ISO 14855-1 (2012). Thus, according to, for example, French Standard NF T 51-800 and Australian Standard AS 5810, a CA composition (or an article comprising the same) may be considered biodegradable when tested under home composting conditions.
[0082] When tested under aerobic composting conditions at 58° C. (±2° C.) according to ISO 14855-1 (2012), the CA composition (or an article comprising the same) may exhibit at least 60% biodegradation within a period of no more than 45 days. In some cases, when tested under these conditions (also referred to as "industrial composting conditions"), the CA composition (or an article comprising the same) may exhibit at least 60% biodegradation within a period of no more than 44, 43, 42, 41, 40, 39, 38, 37, 36, 35, 34, 33, 32, 31, 30, 29, 28, or 27 days. These conditions may not be aqueous or anaerobic. In some cases, the CA composition (or article comprising the same) may exhibit at least about 65%, 70%, 75%, 80%, 85%, 87%, 88%, 89%, 90%, 91%, 92%, 93%, 94%, or 95% total biodegradation when tested under industrial composting conditions according to ISO 14855-1 (2012) for a period of 45 days. This may represent at least about 95%, 97%, 99%, 100%, 102%, 105%, 107%, 110%, 112%, 115%, 117%, or 119% relative biodegradation when compared to the same CA composition (or article comprising the same) subjected to the same testing conditions.
[0083] To be considered "biodegradable" under industrial composting conditions according to ASTM D6400 and ISO 17088, at least 90% of the organic carbon in the entire item (or each component present in an amount exceeding 1% by dry mass) must be converted into carbon dioxide at the end of the test period when compared to a control or an absolute value. According to European Standard ED 13432 (2000), after both the reference and the test item have reached a steady state, the material must show a total biodegradation of at least 90%, or a biodegradation of at least 90% of the maximum degradation of a suitable reference material. The maximum test duration for biodegradability under industrial composting conditions is 180 days. The CA composition described herein (or an article comprising the same) may show at least 90% biodegradation in no more than 180 days, measured under industrial composting conditions according to 14855-1 (2012). In some cases, the CA composition (or an article comprising the same) may exhibit at least about 91%, 92%, 93%, 94%, 95%, 96%, 97%, 98%, 99%, or 99.5% biodegradation in no more than 180 days, or the CA composition (or an article comprising the same) may exhibit 100% biodegradation in no more than 180 days, as measured under industrial composting conditions according to 14855-1 (2012).
[0084] Additionally, or in the alternative, the CA compositions described herein (or articles comprising the same) may exhibit at least 90% biodegradation in no more than about 175, 170, 165, 160, 155, 150, 145, 140, 135, 130, 125, 120, 115, 110, 105, 100, 95, 90, 85, 80, 75, 70, 65, 60, 55, 50, or 45 days, measured under industrial composting conditions according to ISO 14855-1 (2012). In some cases, the CA compositions (or articles comprising the same) may be at least about 97%, 98%, 99%, or 99.5% biodegradable in no more than about 65, 60, 55, 50, or 45 days, tested under industrial composting conditions according to ISO 14855-1 (2012). Thus, the CA compositions described herein (or articles comprising the same) can be considered biodegradable when tested according to ASTM D6400 and ISO 17088 under industrial composting conditions.
[0085] The CA composition (or an article comprising the same) may exhibit at least 60% biodegradation in soil in no more than 130 days, measured under aerobic conditions at ambient temperature according to ISO 17556 (2012). In some cases, when tested under these conditions (also referred to as "soil composting conditions"), the CA composition (or an article comprising the same) may exhibit at least 60% biodegradation over a period of no more than 130, 120, 110, 100, 90, 80, or 75 days. These conditions may not be aqueous or anaerobic. In some cases, when tested under soil composting conditions for a period of 195 days according to ISO 17556 (2012), the CA composition (or an article comprising the same) may exhibit at least about 65%, 70%, 72%, 75%, 77%, 80%, 82%, or 85% total biodegradation. This can represent a relative biodegradation of at least about 70%, 75%, 80%, 85%, 90%, or 95% when compared to the same CA composition (or article comprising the same) subjected to the same testing conditions.
[0086] according to According to the OKbiodegradable SOIL certification mark of DINCERTCO and the DIN Geprüft certification scheme for biodegradability in soil of DINCERTCO, to be considered "biodegradable" under soil composting conditions, a material must show a total biodegradation of at least 90% (e.g., compared to the initial sample), or a biodegradation of at least 90% of the maximum degradation of a suitable reference material after both the reference and the test item have reached a steady state. The maximum test time for biodegradability under soil composting conditions is 2 years. The CA composition described herein (or an article comprising the same) may show at least 90% biodegradation in no more than 2 years, 1.75 years, 1 year, 9 months, or 6 months, measured under soil composting conditions according to ISO 17556 (2012). In some cases, the CA composition (or an article comprising the same) may exhibit at least about 91%, 92%, 93%, 94%, 95%, 96%, 97%, 98%, 99%, or 99.5% biodegradation in no more than 2 years, or the CA composition (or an article comprising the same) may exhibit 100% biodegradation in no more than 2 years, as measured under soil composting conditions according to ISO 17556 (2012).
[0087] Additionally, or in the alternative, the CA compositions described herein (or articles comprising the same) may exhibit at least 90% biodegradation in no more than about 700, 650, 600, 550, 500, 450, 400, 350, 300, 275, 250, 240, 230, 220, 210, 200, or 195 days, as measured under soil composting conditions according to ISO 17556 (2012). In some cases, the CA compositions (or articles comprising the same) may be at least about 97%, 98%, 99%, or 99.5% biodegradable in no more than about 225, 220, 215, 210, 205, 200, or 195 days, as measured under soil composting conditions according to ISO 17556 (2012). Thus, the CA compositions described herein (or articles comprising the same) may meet the requirements of the Acceptable Use Certification Standards. The soil biodegradability mark of conformity is required by DIN CERTCO and meets the criteria of the DIN Geprüft soil biodegradability certification scheme of DIN CERTCO.
[0088] In some embodiments, the CA compositions of the present invention (or articles comprising the same) may include less than 1 wt%, 0.75 wt%, 0.50 wt%, or 0.25 wt% of components of unknown biodegradability. In some cases, the CA compositions described herein (or articles comprising the same) may not include components of unknown biodegradability.
[0089] In addition to being biodegradable under industrial and / or home composting conditions, the CA compositions described herein (or articles comprising the same) may also be composted under home and / or industrial conditions. As previously described, a material is considered compostable if it meets or exceeds the requirements set forth in EN 13432 for biodegradability, disintegration capacity, heavy metal content, and ecotoxicity. The CA compositions described herein (or articles comprising the same) may exhibit sufficient compostability under home and / or industrial composting conditions to meet the requirements set forth in EN 13432 for biodegradability, disintegration capacity, heavy metal content, and ecotoxicity. Requirements for receiving OK compost and OK compost HOME certification marks.
[0090] In some cases, the CA compositions described herein (or articles comprising the same) may have volatile solids concentrations, heavy metals, and fluorine contents that meet all requirements specified in EN 13432 (2000). Alternatively, the CA compositions (or articles comprising the same) do not negatively affect compost quality (including chemical parameters and ecotoxicity tests).
[0091] In some cases, the CA composition (or an article comprising the same) may exhibit at least 90% disintegration in no more than 26 weeks, measured under industrial composting conditions according to ISO 16929 (2013). In some cases, under industrial composting conditions, the CA composition (or an article comprising the same) may exhibit at least about 91%, 92%, 93%, 94%, 95%, 96%, 97%, 98%, 99% or 99.5% disintegration in no more than 26 weeks, or under industrial composting conditions, the CA composition (or an article comprising the same) may exhibit 100% disintegration in no more than 26 weeks. Alternatively, or in addition, the CA composition (or an article comprising the same) may exhibit at least 90% disintegration in no more than about 26, 25, 24, 23, 22, 21, 20, 19, 18, 17, 16, 15, 14, 13, 12, 11, or 10 weeks under industrial composting conditions as measured according to ISO 16929. In some cases, the CA composition described herein (or an article comprising the same) may be at least 97%, 98%, 99%, or 99.5% disintegrated in no more than 12, 11, 10, 9, or 8 weeks under industrial composting conditions as measured according to ISO 16929 (2013).
[0092] In some cases, the CA composition (or an article comprising it) may exhibit at least 90% disintegration in no more than 26 weeks, measured under home composting conditions according to ISO 16929 (2013). In some cases, under home composting conditions, the CA composition (or an article comprising it) may exhibit at least about 91%, 92%, 93%, 94%, 95%, 96%, 97%, 98%, 99% or 99.5% disintegration in no more than 26 weeks, or under home composting conditions, the CA composition (or an article comprising it) may be 100% disintegrated in no more than 26 weeks. Alternatively, or additionally, at least 90% disintegration may be exhibited in no more than about 26, 25, 24, 23, 22, 21, 20, 19, 18, 17, 16 or 15 weeks under home composting conditions, as measured according to ISO 16929 (2013). In some cases, the CA compositions described herein (or articles comprising the same) may be at least 97, 98, 99, or 99.5% disintegrated in no more than 20, 19, 18, 17, 16, 15, 14, 13, or 12 weeks, measured under home composting conditions according to ISO 16929 (2013).
[0093] In an embodiment or in combination with any other embodiment, when the CA composition is formed into a film having a thickness of 0.13, or 0.25, or 0.38, or 0.51, or 0.64, or 0.76, or 0.89, or 1.02, or 1.14, or 1.27, or 1.40, or 1.52 mm, the film exhibits greater than 90% disintegration after 12 weeks according to a disintegration test protocol, as described in the specification or in an alternative to ISO 16929 (2013). In certain embodiments, when the CA composition is formed into a film having a thickness of 0.76, or 0.89, or 1.02, or 1.14, or 1.27, or 1.40, or 1.52 mm, the film exhibits greater than 90% disintegration after 12 weeks according to a disintegration test protocol, as described in the specification or in an alternative to ISO 16929 (2013). In certain embodiments, when the CA composition is formed into a film having a thickness of 0.13, or 0.25, or 0.38, or 0.51, or 0.64, or 0.76, or 0.89, or 1.02, or 1.14, or 1.27, or 1.40, or 1.52 mm, the film exhibits greater than 90%, or 95%, or 96%, or 97%, or 98%, or 99% disintegration after 12 weeks according to a disintegration test protocol, as described in the instructions or in an alternative protocol according to ISO 16929 (2013). In certain embodiments, when the CA composition is formed into a film having a thickness of 0.13, or 0.25, or 0.38, or 0.51, or 0.64, or 0.76, or 0.89, or 1.02, or 1.14, or 1.27, or 1.40, or 1.52 mm, the film exhibits greater than 90%, or 95%, or 96%, or 97%, or 98%, or 99% disintegration after 8, or 9, or 10, or 11, or 12, or 13, or 14, or 15, or 16 weeks according to a disintegration test protocol, as described in the specification or in an alternative to ISO 16929 (2013).
[0094] In some embodiments, the CA compositions described herein (or articles comprising the same) may be substantially free of photodegradants. For example, based on the total weight of the CA composition (or articles comprising the same), the CA composition (or articles comprising the same) may include no more than about 1, 0.75, 0.50, 0.25, 0.10, 0.05, 0.025, 0.01, 0.005, 0.0025, or 0.001 wt% of a photodegradant, or the CA composition (or articles comprising the same) may not include a photodegradant. Examples of such photodegradants include, but are not limited to, pigments used as photooxidation catalysts, and are optionally enhanced by the presence of one or more metal salts, oxidizable promoters, and combinations thereof. The pigment may include coated or uncoated anatase or rutile titanium dioxide, which may be present alone or in combination with one or more reinforcing components (e.g., various types of metals). Other examples of photodegradation agents include benzoin, benzoin alkyl ethers, benzophenone and its derivatives, acetophenone and its derivatives, quinones, thioxanthones, phthalocyanines and other photosensitizers, ethylene-carbon monoxide copolymers, aromatic ketone-metal salt sensitizers, and combinations thereof.
[0095] In one aspect, a biodegradable and / or compostable article comprising a CA composition, as described herein is provided. In an embodiment, the article is made of a moldable thermoplastic material comprising a CA composition, as described herein.
[0096] In an embodiment, the article is a disposable food contact article. Examples of such articles that can be prepared from the CA composition include cups, trays, multi-compartment plates, clamshell packaging, candy bars, films, sheets, trays and lids (e.g., thermoformed), straws, plates, bowls, portion cups, food packaging, liquid carrying containers, solid or gel carrying containers, and tableware. In an embodiment, the article can be a horticultural article. Examples of such articles that can be prepared from the CA composition include plant pots, plant labels, mulch films, and agricultural ground covers.
[0097] In another aspect, a CA composition is provided, comprising recycled BCA prepared by an integrated process comprising the following processing steps: (1) preparing a recycled plastic component synthesis gas in a synthesis gas operation using a feedstock containing a solid fossil fuel source and at least some recycled plastic component; (2) preparing at least one chemical intermediate from the synthesis gas; (3) reacting the chemical intermediate in a reaction scheme to prepare at least one cellulosic reactant for preparing the recycled BCA, and / or selecting the chemical intermediate as at least one cellulosic reactant for preparing the recycled BCA; and (4) reacting the at least one cellulosic reactant to prepare the recycled BCA; wherein the recycled BCA comprises at least one substituent on an anhydroglucose unit (AGU) derived from the recycled plastic component synthesis gas.
[0098] In an embodiment, process steps (1) to (4) are performed in a system that is fluid and / or gaseous connected (i.e., including the possibility of a combination of fluid and gaseous connected). It should be understood that in one or more reaction schemes for producing recycled BCA starting from recycled plastic component syngas, chemical intermediates can be temporarily stored in storage containers and subsequently reintroduced into the integrated process system.
[0099] In an embodiment, at least one chemical intermediate is selected from methanol, methyl acetate, acetic anhydride, acetic acid, or a combination thereof. In an embodiment, one chemical intermediate is methanol, and methanol is used in the reaction scheme to prepare a second chemical intermediate, namely acetic anhydride. In an embodiment, the cellulose reactant is acetic anhydride.
[0100] In an embodiment, a cellulose ester composition comprises a BCA (as described herein), a plasticizer composition, and a stabilizer composition, wherein the plasticizer composition comprises one or more food grade plasticizers, and the food grade plasticizer is present in an amount of 13 wt % to 25 wt %, or 14 wt % to 25 wt %, or 15 wt % to 25 wt %, or 16 wt % to 25 wt %, or 17 wt % to 25 wt %, or 13 wt % to 23 wt %, or 14 wt % to 22 wt %, or 15 wt % to 23 wt %, or 13 wt % to 20 wt %, or 14 wt % to 20 ... %-20wt%, or 16wt%-20wt%, or 17wt%-20wt%, or 13wt%-17wt%, or 14wt%-17wt%, or 15wt%-17wt%, or 13wt%-less than 17wt%, or 14wt%-less than 17wt%, or 15wt%-less than 17wt%; and wherein the stabilizer composition comprises one or more auxiliary antioxidants, and the auxiliary antioxidant is present in an amount of 0.08wt%-0.8wt%, or 0.08wt%-0.7wt%, or 0.08wt%-0.6wt%, based on the total weight of the cellulose ester composition.
[0101] In an embodiment, the plasticizer composition comprises triacetin in an amount of 15 wt%-20 wt%, or 16 wt%-19 wt%, based on the total weight of the cellulose ester composition; and the stabilizer composition comprises one or more secondary antioxidants in an amount of 0.1 wt%-0.4 wt% or 0.1 wt%-0.3 wt%, and one or more primary antioxidants in an amount of 0.1 wt%-0.4 wt% or 0.2 wt%-0.4 wt%, wherein the wt% is based on the total weight of the cellulose ester composition. In a class of this embodiment, the one or more secondary antioxidants include phosphite compounds (e.g., Weston 705T or Doverphos S-9228T), DLTDP, or a combination thereof, and the one or more primary antioxidants include Irganox 1010, BHT, or a combination thereof. In embodiments, the cellulose ester composition has a b* value of less than 40, or less than 35, or less than 30, or less than 25, or less than 20, or less than 15 after a normal cycle time during injection molding (as described in the examples); or a b* value of less than 40, or less than 35, or less than 30, or less than 25, or less than 20 after doubling the cycle time during injection molding (as described in the examples).
[0102] In an embodiment, the plasticizer composition comprises polyethylene glycol having an average molecular weight of 300 to 500 Daltons in an amount of 13 wt%-23 wt%, or 13 wt%-20 wt%, or 13 wt%-less than 17 wt%, or 14 wt%-23 wt%, or 14 wt%-20 wt%, or 14 wt%-less than 17 wt%, or 15 wt%-23 wt%, or 15 wt%-20 wt%, or 15 wt%-less than 17 wt%, or greater than 15 wt%-23 wt%, or 17 wt%-23 wt%, or 17 wt%-20 wt%, based on the total weight of the cellulose ester composition; and the stabilizer composition comprises one or more auxiliary antioxidants in an amount of 0.01 wt%-0.8 wt%, or 0.1 wt%-0.5 wt%, or 0.1 wt%-0.3 wt%, or 0.1 wt%-0.2 wt%, based on the total weight of the cellulose ester composition. In one class of this embodiment, the one or more secondary antioxidants include phosphite compounds (e.g., Weston 705T or Doverphos S-9228T), DLTDP, or a combination thereof. In another class of this embodiment, the stabilizer composition further comprises one or more primary antioxidants (e.g., Irganox 1010 or BHT), citric acid, or a combination thereof, wherein the one or more primary antioxidants are present in an amount of 0.1 wt%-0.5 wt% or 0.1 wt%-0.4 wt% based on the total weight of the cellulose acetate composition, and wherein the citric acid is present in an amount of 0.05 wt%-0.2 wt% or 0.05 wt%-0.15 wt% based on the total weight of the cellulose acetate composition.
[0103] In an embodiment, the plasticizer composition comprises polyethylene glycol having an average molecular weight of 300 to 500 Daltons in an amount of 13 wt% to less than 17 wt%, or 14 wt% to less than 17 wt%, or 15 wt% to less than 17 wt%, based on the total weight of the cellulose ester composition; and the stabilizer composition comprises one or more auxiliary antioxidants in an amount of 0.1 wt% to 0.5 wt%, or 0.1 wt% to 0.3 wt%, or 0.1 wt% to 0.2 wt%, based on the total weight of the cellulose ester composition.
[0104] In an embodiment, the plasticizer composition comprises polyethylene glycol having an average molecular weight of 300 to 500 Daltons, in an amount of greater than 15 wt%-23 wt%, or greater than 15 wt%-20 wt%, based on the total weight of the cellulose ester composition; and the stabilizer composition comprises a first stabilizer component comprising one or more secondary antioxidants, in an amount of 0.1 wt%-0.5 wt%, or 0.1 wt%-0.3 wt%, or 0.1 wt%-0.2 wt%, based on the total weight of the cellulose ester composition; and a second stabilizer component comprising one or more primary antioxidants (e.g., Irganox 1010 or BHT), citric acid or a combination thereof, wherein the one or more primary antioxidants (if present) are present in an amount of 0.1 wt%-0.5 wt% or 0.1 wt%-0.4 wt% based on the total weight of the cellulose acetate composition, and wherein the citric acid (if present) is present in an amount of 0.05 wt%-0.2 wt% or 0.05 wt%-0.15 wt% based on the total weight of the cellulose acetate composition.
[0105] PEG / MPEG specific compositions
[0106] The present application also discloses a composition comprising: (1) cellulose acetate, wherein the acetyl substitution degree (“DS Ac ”) in the range of 2.2 to 2.6, and (2) 17 wt% to 23 wt% of a polyethylene glycol or methoxypolyethylene glycol composition having an average molecular weight of 300 to 550 Daltons, wherein the composition is melt processible, biodegradable and disintegrable.
[0107] In one embodiment or in combination with any other embodiment, the composition comprises polyethylene glycol having an average molecular weight of 300 to 500 Daltons.
[0108] In one embodiment or in combination with any other embodiment, the composition comprises polyethylene glycol having an average molecular weight of 350 to 550 Daltons.
[0109] In one embodiment or in combination with any other embodiment, the number average molecular weight ("Mn") of the cellulose acetate is in the range of 10,000 to 90,000 Daltons as measured by GPC. In one embodiment or in combination with any other embodiment, the number average molecular weight ("Mn") of the cellulose acetate is in the range of 30,000 to 90,000 Daltons as measured by GPC. In one embodiment or in combination with any other embodiment, the number average molecular weight ("Mn") of the cellulose acetate is in the range of 40,000 to 90,000 Daltons as measured by GPC.
[0110] In one embodiment or in combination with any other embodiment, when the composition is formed into a film having a thickness of 0.38 mm, according to the disintegration test protocol, as described in the specification or according to an alternative to ISO16929 (2013), the film exhibits greater than 5% disintegration after 6 weeks, and greater than 90% disintegration after 12 weeks. In one embodiment or in combination with any other embodiment, when the composition is formed into a film having a thickness of 0.38 mm, according to the disintegration test protocol, as described in the specification or according to an alternative to ISO16929 (2013), the film exhibits greater than 10% disintegration after 6 weeks, and greater than 90% disintegration after 12 weeks. In one embodiment or in combination with any other embodiment, when the composition is formed into a film having a thickness of 0.38 mm, according to the disintegration test protocol, as described in the specification or according to an alternative to ISO16929 (2013), the film exhibits greater than 20% disintegration after 6 weeks, and greater than 90% disintegration after 12 weeks. In one embodiment or in combination with any other embodiment, when the composition is formed into a film having a thickness of 0.38 mm, according to the disintegration test protocol, as described in the specification or according to an alternative to ISO16929 (2013), the film exhibits greater than 30% disintegration after 6 weeks, and greater than 90% disintegration after 12 weeks. In one embodiment or in combination with any other embodiment, when the composition is formed into a film having a thickness of 0.38 mm, according to the disintegration test protocol, as described in the specification or according to an alternative to ISO16929 (2013), the film exhibits greater than 50% disintegration after 6 weeks, and greater than 90% disintegration after 12 weeks. In one embodiment or in combination with any other embodiment, when the composition is formed into a film having a thickness of 0.38 mm, according to the disintegration test protocol, as described in the specification or according to an alternative to ISO16929 (2013), the film exhibits greater than 70% disintegration after 6 weeks, and greater than 90% disintegration after 12 weeks.
[0111] In one embodiment or in combination with any other embodiment, when the composition is formed into a film having a thickness of 0.76 mm, the film exhibits greater than 30% disintegration after 12 weeks according to a disintegration test protocol, as described in the specification or in an alternative to ISO 16929 (2013). In one embodiment or in combination with any other embodiment, when the composition is formed into a film having a thickness of 0.76 mm, the film exhibits greater than 50% disintegration after 12 weeks according to a disintegration test protocol, as described in the specification or in an alternative to ISO 16929 (2013). In one embodiment or in combination with any other embodiment, when the composition is formed into a film having a thickness of 0.76 mm, the film exhibits greater than 70% disintegration after 12 weeks according to a disintegration test protocol, as described in the specification or in an alternative to ISO 16929 (2013). In one embodiment or in combination with any other embodiment, when the composition is formed into a film having a thickness of 0.76 mm, the film exhibits greater than 90% disintegration after 12 weeks according to a disintegration test protocol, as described in the specification or in an alternative to ISO 16929 (2013). In one embodiment or in combination with any other embodiment, when the composition is formed into a film having a thickness of 0.76 mm, the film exhibits greater than 95% disintegration after 12 weeks according to a disintegration test protocol, as described in the specification or in an alternative to ISO 16929 (2013).
[0112] In one embodiment or in combination with any other embodiment, the composition further comprises at least one additional component selected from fillers, additives, biopolymers, stabilizers, or odor modifiers.
[0113] In one embodiment or in combination with any other embodiment, the composition further comprises a filler in an amount of 1 wt% to 60 wt%, based on the total weight of the composition. In a class of this embodiment, the filler is a carbohydrate, a cellulose filler, an inorganic filler, a food by-product, a desiccant, an alkaline filler, or a combination thereof.
[0114] In a subclass of this class, the filler is an inorganic filler. In a sub-subclass of this subclass, the inorganic filler is calcium carbonate.
[0115] In a subclass of this class, the filler is a carbohydrate. In a subclass of this class, the filler is a cellulosic filler. In a subclass of this class, the filler is a food byproduct. In a subclass of this class, the filler is a desiccant. In a subclass of this class, the filler is an alkaline filler.
[0116] In one embodiment or in combination with any other embodiment, the composition further comprises an odor modifying additive in an amount of 0.001 wt% to 1 wt%, based on the total weight of the composition. In a class of this embodiment, the odor modifying additive is vanillin, peppermint oil M-1178, almonds, cinnamon, spices, spice extracts, volatile organic compounds or small molecules or Plastidor. In a subclass of this class, the odor modifying additive is vanillin.
[0117] In one embodiment or in combination with any other embodiment, the composition further comprises a stabilizer in an amount of 0.01 wt% to 5 wt%, based on the total amount of the composition. In one class of this embodiment, the stabilizer is a UV absorber, an antioxidant (e.g., ascorbic acid, BHT, BHA, etc.), an acid scavenger, a free radical scavenger, an epoxidized oil (e.g., epoxidized soybean oil, epoxidized linseed oil, epoxidized sunflower oil), or a combination thereof.
[0118] The present application also discloses an article comprising a composition comprising: (1) cellulose acetate, wherein the acetyl substitution degree (“DS Ac ”) in the range of 2.2 to 2.6, and (2) 17 wt% to 23 wt% of a polyethylene glycol or methoxypolyethylene glycol composition having an average molecular weight of 300 to 550 Daltons, wherein the composition is melt processible, biodegradable and disintegrable.
[0119] In one embodiment or in combination with any other embodiment, the composition comprises polyethylene glycol having an average molecular weight of 300 to 500 Daltons. In one embodiment or in combination with any other embodiment, the composition comprises polyethylene glycol having an average molecular weight of 350 to 550 Daltons.
[0120] In one embodiment or in combination with any other embodiment, the article is formed by an orientation process, an extrusion process, an injection molding process, a blow molding process, or a thermoforming process. In a class of this embodiment, the article is formed by an orientation process. In a subclass of this class, the orientation process is a uniaxial stretching process or a biaxial stretching process.
[0121] In a class of this embodiment, the article is formed by an extrusion process. In a class of this embodiment, the article is formed by an injection molding process. In a class of this embodiment, the article is formed by a blow molding process. In a class of this embodiment, the article is formed by a thermoforming process. In a subclass of this class, the film or sheet used to form the article is 10 to 160 mils thick.
[0122] In one embodiment or in combination with any other embodiment, when the article is transparent, the article exhibits a haze of less than 10%. In one embodiment or in combination with any other embodiment, when the article is transparent, the article exhibits a haze of less than 8%. In one embodiment or in combination with any other embodiment, when the article is transparent, the article exhibits a haze of less than 6%. In one embodiment or in combination with any other embodiment, when the article is transparent, the article exhibits a haze of less than 5%. In one embodiment or in combination with any other embodiment, when the article is transparent, the article exhibits a haze of less than 4%. In one embodiment or in combination with any other embodiment, when the article is transparent, the article exhibits a haze of less than 3%. In one embodiment, when the article is transparent, the article exhibits a haze of less than 2%. In one embodiment or in combination with any other embodiment, when the article is transparent, the article exhibits a haze of less than 1%.
[0123] In one embodiment or in combination with any other embodiment, when the composition is formed into a film having a thickness of 0.38 mm, according to the disintegration test protocol, as described in the specification or according to an alternative to ISO16929 (2013), the film exhibits greater than 5% disintegration after 6 weeks, and greater than 90% disintegration after 12 weeks. In one embodiment or in combination with any other embodiment, when the composition is formed into a film having a thickness of 0.38 mm, according to the disintegration test protocol, as described in the specification or according to an alternative to ISO16929 (2013), the film exhibits greater than 10% disintegration after 6 weeks, and greater than 90% disintegration after 12 weeks. In one embodiment or in combination with any other embodiment, when the composition is formed into a film having a thickness of 0.38 mm, according to the disintegration test protocol, as described in the specification or according to an alternative to ISO16929 (2013), the film exhibits greater than 20% disintegration after 6 weeks, and greater than 90% disintegration after 12 weeks. In one embodiment or in combination with any other embodiment, when the composition is formed into a film having a thickness of 0.38 mm, according to the disintegration test protocol, as described in the specification or according to an alternative to ISO16929 (2013), the film exhibits greater than 30% disintegration after 6 weeks, and greater than 90% disintegration after 12 weeks. In one embodiment or in combination with any other embodiment, when the composition is formed into a film having a thickness of 0.38 mm, according to the disintegration test protocol, as described in the specification or according to an alternative to ISO16929 (2013), the film exhibits greater than 50% disintegration after 6 weeks, and greater than 90% disintegration after 12 weeks. In one embodiment or in combination with any other embodiment, when the composition is formed into a film having a thickness of 0.38 mm, according to the disintegration test protocol, as described in the specification or according to an alternative to ISO16929 (2013), the film exhibits greater than 70% disintegration after 6 weeks, and greater than 90% disintegration after 12 weeks.
[0124] In one embodiment or in combination with any other embodiment, when the composition is formed into a film having a thickness of 0.76 mm, the film exhibits greater than 30% disintegration after 12 weeks according to a disintegration test protocol, as described in the specification or in an alternative to ISO 16929 (2013). In one embodiment or in combination with any other embodiment, when the composition is formed into a film having a thickness of 0.76 mm, the film exhibits greater than 50% disintegration after 12 weeks according to a disintegration test protocol, as described in the specification or in an alternative to ISO 16929 (2013). In one embodiment or in combination with any other embodiment, when the composition is formed into a film having a thickness of 0.76 mm, the film exhibits greater than 70% disintegration after 12 weeks according to a disintegration test protocol, as described in the specification or in an alternative to ISO 16929 (2013). In one embodiment or in combination with any other embodiment, when the composition is formed into a film having a thickness of 0.76 mm, the film exhibits greater than 90% disintegration after 12 weeks according to a disintegration test protocol, as described in the specification or in an alternative to ISO 16929 (2013). In one embodiment or in combination with any other embodiment, when the composition is formed into a film having a thickness of 0.76 mm, the film exhibits greater than 95% disintegration after 12 weeks according to a disintegration test protocol, as described in the specification or in an alternative to ISO 16929 (2013).
[0125] In one embodiment or in combination with any other embodiment, according to the disintegration test protocol, as described in the specification or according to the alternative scheme of ISO16929 (2013), the product exhibits greater than 30% disintegration after 12 weeks. In one embodiment or in combination with any other embodiment, according to the disintegration test protocol, as described in the specification or according to the alternative scheme of ISO16929 (2013), the product exhibits greater than 50% disintegration after 12 weeks. In one embodiment or in combination with any other embodiment, according to the disintegration test protocol, as described in the specification or according to the alternative scheme of ISO16929 (2013), the product exhibits greater than 70% disintegration after 12 weeks. In one embodiment or in combination with any other embodiment, according to the disintegration test protocol, as described in the specification or according to the alternative scheme of ISO16929 (2013), the product exhibits greater than 80% disintegration after 12 weeks. In one embodiment or in combination with any other embodiment, according to the disintegration test protocol, as described in the specification or in an alternative to ISO16929 (2013), the product exhibits greater than 90% disintegration after 12 weeks. In one embodiment or in combination with any other embodiment, according to the disintegration test protocol, as described in the specification or in an alternative to ISO16929 (2013), the product exhibits greater than 95% disintegration after 12 weeks.
[0126] In one embodiment or in combination with any other embodiment, the article has a thickness of 0.8 mm or less. In one embodiment, the article has a thickness of 0.76 mm or less.
[0127] In one embodiment or in combination with any other embodiment, the composition further comprises at least one additional component selected from fillers, additives, biopolymers, stabilizers, or odor modifiers.
[0128] In one embodiment or in combination with any other embodiment, the composition further comprises a filler in an amount of 1 wt% to 60 wt%, based on the total weight of the composition. In a class of this embodiment, the filler is a carbohydrate, a cellulose filler, an inorganic filler, a food by-product, a desiccant, an alkaline filler, or a combination thereof.
[0129] In a subclass of this class, the filler is an inorganic filler. In a sub-subclass of this subclass, the inorganic filler is calcium carbonate.
[0130] In a subclass of this class, the filler is a carbohydrate. In a subclass of this class, the filler is a cellulosic filler. In a subclass of this class, the filler is a food byproduct. In a subclass of this class, the filler is a desiccant. In a subclass of this class, the filler is an alkaline filler.
[0131] In one embodiment or in combination with any other embodiment, the composition further comprises an odor modifying additive in an amount of 0.001 wt% to 1 wt%, based on the total weight of the composition. In a class of this embodiment, the odor modifying additive is vanillin, peppermint oil M-1178, almonds, cinnamon, spices, spice extracts, volatile organic compounds or small molecules or Plastidor. In a subclass of this class, the odor modifying additive is vanillin.
[0132] In one embodiment or in combination with any other embodiment, the composition further comprises a stabilizer in an amount of 0.01 wt% to 5 wt%, based on the total amount of the composition. In one class of this embodiment, the stabilizer is a UV absorber, an antioxidant (e.g., ascorbic acid, BHT, BHA, etc.), an acid scavenger, a free radical scavenger, an epoxidized oil (e.g., epoxidized soybean oil, epoxidized linseed oil, epoxidized sunflower oil), or a combination thereof.
[0133] The present application also discloses an article comprising a composition comprising: (1) cellulose acetate, wherein the acetyl substitution degree (“DS Ac”) in the range of 2.2 to 2.6, and (2) 13 wt% to 23 wt% of a polyethylene glycol or methoxy polyethylene glycol composition having an average molecular weight of 300 to 550 Daltons, and (3) 0.01 wt% to 1.8 wt% of an additive selected from epoxidized soybean oil, a secondary antioxidant, or a combination, wherein the composition is melt processable, biodegradable, and disintegrable.
[0134] In one embodiment or in combination with any other embodiment, the additive is present at 0.01 wt%-1 wt%, or 0.05 wt%-0.8 wt%, or 0.05 wt%-0.5 wt%, or 0.1 wt%-1 wt%.
[0135] In one embodiment or in combination with any other embodiment, the additive is epoxidized soybean oil present at 0.1 wt%-1 wt%, or 0.1 wt%-0.5 wt%, or 0.5 wt%-1 wt%, or 0.3 wt%-0.8 wt%.
[0136] In one embodiment or in combination with any other embodiment, the additive is a secondary antioxidant present at 0.01 wt%-0.8 wt%, or 0.01 wt%-0.4 wt%, or 0.4 wt%-0.8 wt%, or 0.2 wt%-0.6 wt%.
[0137] In one embodiment or in combination with any other embodiment, the composition comprises polyethylene glycol having an average molecular weight of 300 to 500 Daltons. In one embodiment or in combination with any other embodiment, the composition comprises polyethylene glycol having an average molecular weight of 350 to 550 Daltons.
[0138] In one embodiment or in combination with any other embodiment, the article is formed by an orientation process, an extrusion process, an injection molding process, a blow molding process, or a thermoforming process. In a class of this embodiment, the article is formed by an orientation process. In a subclass of this class, the orientation process is a uniaxial stretching process or a biaxial stretching process.
[0139] In a class of this embodiment, the article is formed by an extrusion process. In a class of this embodiment, the article is formed by an injection molding process. In a class of this embodiment, the article is formed by a blow molding process. In a class of this embodiment, the article is formed by a thermoforming process. In a subclass of this class, the film or sheet used to form the article is 10 to 160 mils thick.
[0140] In one embodiment or in combination with any other embodiment, when the article is transparent, the article exhibits a haze of less than 10%. In one embodiment or in combination with any other embodiment, when the article is transparent, the article exhibits a haze of less than 8%. In one embodiment or in combination with any other embodiment, when the article is transparent, the article exhibits a haze of less than 6%. In one embodiment or in combination with any other embodiment, when the article is transparent, the article exhibits a haze of less than 5%. In one embodiment or in combination with any other embodiment, when the article is transparent, the article exhibits a haze of less than 4%. In one embodiment or in combination with any other embodiment, when the article is transparent, the article exhibits a haze of less than 3%. In one embodiment, when the article is transparent, the article exhibits a haze of less than 2%. In one embodiment or in combination with any other embodiment, when the article is transparent, the article exhibits a haze of less than 1%.
[0141] In one embodiment or in combination with any other embodiment, when the composition is formed into a film having a thickness of 0.38 mm, according to the disintegration test protocol, as described in the specification or according to an alternative to ISO16929 (2013), the film exhibits greater than 5% disintegration after 6 weeks, and greater than 90% disintegration after 12 weeks. In one embodiment or in combination with any other embodiment, when the composition is formed into a film having a thickness of 0.38 mm, according to the disintegration test protocol, as described in the specification or according to an alternative to ISO16929 (2013), the film exhibits greater than 10% disintegration after 6 weeks, and greater than 90% disintegration after 12 weeks. In one embodiment or in combination with any other embodiment, when the composition is formed into a film having a thickness of 0.38 mm, according to the disintegration test protocol, as described in the specification or according to an alternative to ISO16929 (2013), the film exhibits greater than 20% disintegration after 6 weeks, and greater than 90% disintegration after 12 weeks. In one embodiment or in combination with any other embodiment, when the composition is formed into a film having a thickness of 0.38 mm, according to the disintegration test protocol, as described in the specification or according to an alternative to ISO16929 (2013), the film exhibits greater than 30% disintegration after 6 weeks, and greater than 90% disintegration after 12 weeks. In one embodiment or in combination with any other embodiment, when the composition is formed into a film having a thickness of 0.38 mm, according to the disintegration test protocol, as described in the specification or according to an alternative to ISO16929 (2013), the film exhibits greater than 50% disintegration after 6 weeks, and greater than 90% disintegration after 12 weeks. In one embodiment or in combination with any other embodiment, when the composition is formed into a film having a thickness of 0.38 mm, according to the disintegration test protocol, as described in the specification or according to an alternative to ISO16929 (2013), the film exhibits greater than 70% disintegration after 6 weeks, and greater than 90% disintegration after 12 weeks.
[0142] In one embodiment or in combination with any other embodiment, when the composition is formed into a film having a thickness of 0.76 mm, the film exhibits greater than 30% disintegration after 12 weeks according to a disintegration test protocol, as described in the specification or in an alternative to ISO 16929 (2013). In one embodiment or in combination with any other embodiment, when the composition is formed into a film having a thickness of 0.76 mm, the film exhibits greater than 50% disintegration after 12 weeks according to a disintegration test protocol, as described in the specification or in an alternative to ISO 16929 (2013). In one embodiment or in combination with any other embodiment, when the composition is formed into a film having a thickness of 0.76 mm, the film exhibits greater than 70% disintegration after 12 weeks according to a disintegration test protocol, as described in the specification or in an alternative to ISO 16929 (2013). In one embodiment or in combination with any other embodiment, when the composition is formed into a film having a thickness of 0.76 mm, the film exhibits greater than 90% disintegration after 12 weeks according to a disintegration test protocol, as described in the specification or in an alternative to ISO 16929 (2013). In one embodiment or in combination with any other embodiment, when the composition is formed into a film having a thickness of 0.76 mm, the film exhibits greater than 95% disintegration after 12 weeks according to a disintegration test protocol, as described in the specification or in an alternative to ISO 16929 (2013).
[0143] In one embodiment or in combination with any other embodiment, according to the disintegration test protocol, as described in the specification or according to the alternative scheme of ISO16929 (2013), the product exhibits greater than 30% disintegration after 12 weeks. In one embodiment or in combination with any other embodiment, according to the disintegration test protocol, as described in the specification or according to the alternative scheme of ISO16929 (2013), the product exhibits greater than 50% disintegration after 12 weeks. In one embodiment or in combination with any other embodiment, according to the disintegration test protocol, as described in the specification or according to the alternative scheme of ISO16929 (2013), the product exhibits greater than 70% disintegration after 12 weeks. In one embodiment or in combination with any other embodiment, according to the disintegration test protocol, as described in the specification or according to the alternative scheme of ISO16929 (2013), the product exhibits greater than 80% disintegration after 12 weeks. In one embodiment or in combination with any other embodiment, according to the disintegration test protocol, as described in the specification or in an alternative to ISO16929 (2013), the product exhibits greater than 90% disintegration after 12 weeks. In one embodiment or in combination with any other embodiment, according to the disintegration test protocol, as described in the specification or in an alternative to ISO16929 (2013), the product exhibits greater than 95% disintegration after 12 weeks.
[0144] In one embodiment or in combination with any other embodiment, the article has a thickness of 0.8 mm or less. In one embodiment, the article has a thickness of 0.76 mm or less.
[0145] In one embodiment or in combination with any other embodiment, the composition further comprises at least one additional component selected from fillers, additives, biopolymers, stabilizers, or odor modifiers.
[0146] In one embodiment or in combination with any other embodiment, the composition further comprises a filler in an amount of 1 wt% to 60 wt%, based on the total weight of the composition. In a class of this embodiment, the filler is a carbohydrate, a cellulose filler, an inorganic filler, a food by-product, a desiccant, an alkaline filler, or a combination thereof.
[0147] In a subclass of this class, the filler is an inorganic filler. In a sub-subclass of this subclass, the inorganic filler is calcium carbonate.
[0148] In a subclass of this class, the filler is a carbohydrate. In a subclass of this class, the filler is a cellulosic filler. In a subclass of this class, the filler is a food byproduct. In a subclass of this class, the filler is a desiccant. In a subclass of this class, the filler is an alkaline filler.
[0149] In one embodiment or in combination with any other embodiment, the composition further comprises an odor modifying additive in an amount of 0.001 wt% to 1 wt%, based on the total weight of the composition. In a class of this embodiment, the odor modifying additive is vanillin, peppermint oil M-1178, almonds, cinnamon, spices, spice extracts, volatile organic compounds or small molecules or Plastidor. In a subclass of this class, the odor modifying additive is vanillin.
[0150] The present application discloses a foamable composition comprising: (1) degree of acetyl substitution (DS Ac ) cellulose acetate between 2.2 and 2.6; (2) 5 wt%-40 wt% of a plasticizer; (3) 0.1 wt%-3 wt% of a nucleating agent; and (4) 0.1 wt%-3 wt% of a chemical foaming composition comprising: (i) 25 wt%-75 wt% of a blowing agent, and (ii) 25 wt%-75 wt% of a carrier polymer having a melting point not exceeding 150°C, wherein the ratio of the blowing agent to the carrier polymer is based on the total weight of the chemical foaming composition; wherein the ratio of the cellulose acetate, plasticizer, nucleating agent and chemical foaming composition is based on the total weight of the foamable composition.
[0151] In one embodiment or in combination with any other embodiment, the foamable composition exhibits a heat distortion temperature greater than 100°C, measured using DMA at 0.45 MPa, 2% elongation, and a frequency of 1 Hz. In one embodiment or in combination with any other embodiment, the foamable composition exhibits a heat distortion temperature greater than 102°C, measured using DMA at 0.45 MPa, 2% elongation, and a frequency of 1 Hz. In one embodiment or in combination with any other embodiment, the foamable composition exhibits a heat distortion temperature greater than 104°C, measured using DMA at 0.45 MPa, 2% elongation, and a frequency of 1 Hz. In one embodiment or in combination with any other embodiment, the foamable composition exhibits a heat distortion temperature greater than 106°C, measured using DMA at 0.45 MPa, 2% elongation, and a frequency of 1 Hz. In one embodiment or in combination with any other embodiment, the foamable composition exhibits a heat distortion temperature greater than 110°C, measured using DMA at 0.45 MPa, 2% elongation, and a frequency of 1 Hz. In one embodiment or in combination with any other embodiment, the foamable composition exhibits a heat distortion temperature greater than 115° C., measured using DMA at 0.45 MPa, 2% elongation, and 1 Hz frequency.
[0152] In one embodiment or in combination with any other embodiment, the foaming agent comprises sodium bicarbonate, citric acid, or a combination thereof. In a class of this embodiment, the foaming agent comprises sodium bicarbonate. In a class of this embodiment, the foaming agent comprises citric acid.
[0153] In one embodiment or in combination with any other embodiment, the carrier polymer comprises polybutylene succinate, polycaprolactone, or a combination thereof. In a class of this embodiment, the carrier polymer comprises polybutylene succinate. In a class of this embodiment, the carrier polymer comprises polycaprolactone.
[0154] In one embodiment or in combination with any other embodiment, the plasticizer includes triacetin, triethyl citrate, or PEG400.
[0155] In a class of this embodiment, the plasticizer is present in a range of 13 wt%-23 wt%, or 17 wt%-23 wt%. In a class of this embodiment, the plasticizer is present in a range of 13 wt%-30 wt%, or 15 wt%-30 wt%.
[0156] In a class of this embodiment, the plasticizer includes triacetin.
[0157] In a subclass of this class, the plasticizer is present in the range of 13wt%-23wt%, or 15wt%-23wt%, or 17wt%-23wt%. In a subclass of this class, the plasticizer is present in the range of 13wt%-30wt%, or 15wt%-30wt%.
[0158] In a class of this embodiment, the plasticizer includes triethyl citrate. In a subclass of this class, the plasticizer exists in the scope of 13wt%-23wt%, or 15wt%-23wt%, or 17wt%-23wt%. In a subclass of this class, the plasticizer exists in the scope of 13wt%-30wt%, or 15wt%-30wt%.
[0159] In a class of this embodiment, the plasticizer includes PEG 400. In a subclass of this class, the plasticizer is present in the range of 13 wt% to less than 17 wt%, or 17 wt% to 23 wt%. In a subclass of this class, the plasticizer is present in the range of 13 wt% to 30 wt%, or 15 wt% to 30 wt%.
[0160] In one embodiment or in combination with any other embodiment, the nucleating agent comprises magnesium silicate, silicon dioxide, magnesium oxide, or a combination thereof. In a class of this embodiment, the nucleating agent comprises a particulate composition having a median particle size of less than 2 microns. In a class of this embodiment, the nucleating agent comprises a particulate composition having a median particle size of less than 1.5 microns. In a class of this embodiment, the nucleating agent comprises a particulate composition having a median particle size of less than 1.1 microns.
[0161] In a class of this embodiment, the nucleating agent comprises magnesium silicate. In a subclass of this class, the nucleating agent comprises a particulate composition having a median particle size of less than 2 microns. In a subclass of this class, the nucleating agent comprises a particulate composition having a median particle size of less than 1.5 microns. In a subclass of this class, the nucleating agent comprises a particulate composition having a median particle size of less than 1.1 microns.
[0162] In a class of this embodiment, the nucleating agent comprises silicon dioxide. In a subclass of this class, the nucleating agent comprises a particulate composition having a median particle size of less than 2 microns. In a subclass of this class, the nucleating agent comprises a particulate composition having a median particle size of less than 1.5 microns. In a subclass of this class, the nucleating agent comprises a particulate composition having a median particle size of less than 1.1 microns.
[0163] In a class of this embodiment, the nucleating agent comprises magnesium oxide. In a subclass of this class, the nucleating agent comprises a particulate composition having a median particle size of less than 2 microns. In a subclass of this class, the nucleating agent comprises a particulate composition having a median particle size of less than 1.5 microns. In a subclass of this class, the nucleating agent comprises a particulate composition having a median particle size of less than 1.1 microns.
[0164] In one embodiment or in combination with any other embodiment, the nucleating agent comprises a particulate composition having a median particle size of less than 2 microns. In one embodiment, the nucleating agent comprises a particulate composition having a median particle size of less than 1.5 microns. The nucleating agent comprises a particulate composition having a median particle size of less than 1.1 microns.
[0165] In one embodiment or in combination with any other embodiment, the foamable composition further comprises fibers. In a class of this embodiment, the fibers comprise hemp, bast, jute, flax, ramie, kenaf, sisal, bamboo, or lignocellulosic fibers. In a subclass of this class, the fibers comprise hemp.
[0166] In one embodiment or in combination with any other embodiment, the foamable composition further comprises a photodegradation catalyst. In a class of this embodiment, the photodegradation catalyst is titanium dioxide or iron oxide. In a subclass of this class, the photodegradation catalyst is titanium dioxide. In a subclass of this class, the photodegradation catalyst is iron oxide.
[0167] In one embodiment or in combination with any other embodiment, the foamable composition further comprises a pigment. In a class of this embodiment, the pigment is titanium dioxide, carbon black, or iron oxide. In a subclass of this class, the pigment is titanium dioxide. In a subclass of this class, the pigment is carbon black. In a subclass of this class, the pigment is iron oxide.
[0168] In one embodiment or in combination with any other embodiment, the foamable composition is biodegradable.
[0169] In one embodiment or in combination with any other embodiment, the foamable composition comprises two or more cellulose acetates having different degrees of acetyl substitution.
[0170] In one embodiment or in combination with any of the other embodiments, the foamable composition further comprises a biodegradable polymer other than cellulose acetate.
[0171] In one embodiment or in combination with any other embodiment, there is an article made from any of the aforementioned foamable compositions, wherein the article is a foam.
[0172] In a class of this embodiment, the article has a thickness of at most 3 mm.
[0173] In a class of this embodiment, the article has one or more skin layers. The skin layer can be located on the outer surface of the article or foam. The skin layer can also be located in the middle of the foam.
[0174] In a class of this embodiment, the article is biodegradable.
[0175] In a class of this embodiment, the density of the article is less than 0.9 g / cm3 In one class of this embodiment, the density of the article is less than 0.8 g / cm 3 In one class of this embodiment, the density of the article is less than 0.7 g / cm 3 In one class of this embodiment, the density of the article is less than 0.6 g / cm 3 In one class of this embodiment, the density of the article is less than 0.5 g / cm 3 In one class of this embodiment, the density of the article is less than 0.4 g / cm 3 In one class of this embodiment, the density of the article is less than 0.3 g / cm 3 In one class of this embodiment, the density of the article is less than 0.2 g / cm 3 In one class of this embodiment, the density of the article is less than 0.1 g / cm 3 In one class of this embodiment, the density of the article is less than 0.05 g / cm 3 In one class of this embodiment, the density of the article is 0.2-0.9 g / cm 3 within the range.
[0176] In one class of this embodiment, the article is industrially compostable or home compostable. In a subclass of this class, the article is industrially compostable. In a sub-subclass of this subclass, the article has a thickness of less than 1.1 mm. In a sub-subclass of this class, the article is home compostable. In a sub-subclass of this subclass, the article has a thickness of less than 1.1 mm. In a sub-subclass of this subclass, the article has a thickness of less than 0.8 mm. In a sub-subclass of this subclass, the article has a thickness of less than 0.6 mm. In a sub-subclass of this subclass, the article has a thickness of less than 0.4 mm.
[0177] The present application discloses a foamable composition comprising: (1) degree of acetyl substitution (DS Ac ) cellulose acetate between 2.2 and 2.6; (2) 5 wt%-40 wt% of a plasticizer; (3) 0.1 wt%-3 wt% of a nucleating agent; and (4) 0.1 wt%-15 wt% of a physical blowing agent, wherein the proportions of cellulose acetate, plasticizer, nucleating agent and physical blowing agent are based on the total weight of the foamable composition.
[0178] In one embodiment or in combination with any other embodiment, the foamable composition exhibits a heat distortion temperature greater than 100°C, measured using DMA at 0.45 MPa, 2% elongation, and a frequency of 1 Hz. In one embodiment or in combination with any other embodiment, the foamable composition exhibits a heat distortion temperature greater than 102°C, measured using DMA at 0.45 MPa, 2% elongation, and a frequency of 1 Hz. In one embodiment or in combination with any other embodiment, the foamable composition exhibits a heat distortion temperature greater than 104°C, measured using DMA at 0.45 MPa, 2% elongation, and a frequency of 1 Hz. In one embodiment or in combination with any other embodiment, the foamable composition exhibits a heat distortion temperature greater than 106°C, measured using DMA at 0.45 MPa, 2% elongation, and a frequency of 1 Hz. In one embodiment or in combination with any other embodiment, the foamable composition exhibits a heat distortion temperature greater than 110°C, measured using DMA at 0.45 MPa, 2% elongation, and a frequency of 1 Hz. In one embodiment or in combination with any other embodiment, the foamable composition exhibits a heat distortion temperature greater than 115° C., measured using DMA at 0.45 MPa, 2% elongation, and 1 Hz frequency.
[0179] In one embodiment or in combination with any other embodiment, the physical blowing agent comprises CO 2 、N 2 , unbranched or branched (C 2-6 )alkane, or any combination thereof. In one class of this embodiment, the physical blowing agent comprises CO 2 In a class of this embodiment, the physical blowing agent comprises N 2 In one class of this embodiment, the physical blowing agent comprises an unbranched or branched (C 2-6 )Alkanes.
[0180] In one embodiment or in combination with any other embodiment, the physical blowing agent is present at 0.1 wt%-0.5 wt%. In one embodiment or in combination with any other embodiment, the physical blowing agent is present at 0.5 wt%-4 wt%. In one embodiment or in combination with any other embodiment, the physical blowing agent is present at 0.3 wt%-4 wt%. In one embodiment or in combination with any other embodiment, the physical blowing agent is present at 4 wt%-10 wt%.
[0181] In one embodiment or in combination with any other embodiment, the plasticizer includes triacetin, triethyl citrate, or PEG400.
[0182] In a class of this embodiment, the plasticizer is present in a range of 17 wt% to 23 wt%. In a class of this embodiment, the plasticizer is present in a range of 15 wt% to 30 wt%.
[0183] In a class of this embodiment, the plasticizer includes triacetin.
[0184] In a subclass of this class, the plasticizer is present in the range of 17 wt% to 23 wt%. In a subclass of this class, the plasticizer is present in the range of 15 wt% to 30 wt%.
[0185] In a class of this embodiment, the plasticizer includes triethyl citrate. In a subclass of this class, the plasticizer is present in the range of 17wt%-23wt%. In a subclass of this class, the plasticizer is present in the range of 15wt%-30wt%.
[0186] In a class of this embodiment, the plasticizer comprises PEG 400. In a subclass of this class, the plasticizer is present in the range of 17 wt%-23 wt%. In a subclass of this class, the plasticizer is present in the range of 15 wt%-30 wt%.
[0187] In one embodiment or in combination with any other embodiment, the nucleating agent comprises magnesium silicate, silicon dioxide, magnesium oxide, or a combination thereof. In a class of this embodiment, the nucleating agent comprises a particulate composition having a median particle size of less than 2 microns. In a class of this embodiment, the nucleating agent comprises a particulate composition having a median particle size of less than 1.5 microns. In a class of this embodiment, the nucleating agent comprises a particulate composition having a median particle size of less than 1.1 microns.
[0188] In a class of this embodiment, the nucleating agent comprises magnesium silicate. In a subclass of this class, the nucleating agent comprises a particulate composition having a median particle size of less than 2 microns. In a subclass of this class, the nucleating agent comprises a particulate composition having a median particle size of less than 1.5 microns. In a subclass of this class, the nucleating agent comprises a particulate composition having a median particle size of less than 1.1 microns.
[0189] In a class of this embodiment, the nucleating agent comprises silicon dioxide. In a subclass of this class, the nucleating agent comprises a particulate composition having a median particle size of less than 2 microns. In a subclass of this class, the nucleating agent comprises a particulate composition having a median particle size of less than 1.5 microns. In a subclass of this class, the nucleating agent comprises a particulate composition having a median particle size of less than 1.1 microns.
[0190] In a class of this embodiment, the nucleating agent comprises magnesium oxide. In a subclass of this class, the nucleating agent comprises a particulate composition having a median particle size of less than 2 microns. In a subclass of this class, the nucleating agent comprises a particulate composition having a median particle size of less than 1.5 microns. In a subclass of this class, the nucleating agent comprises a particulate composition having a median particle size of less than 1.1 microns.
[0191] In one embodiment or in combination with any other embodiment, the nucleating agent comprises a particulate composition having a median particle size of less than 2 microns. In one embodiment, the nucleating agent comprises a particulate composition having a median particle size of less than 1.5 microns. The nucleating agent comprises a particulate composition having a median particle size of less than 1.1 microns.
[0192] In one embodiment or in combination with any other embodiment, the foamable composition further comprises fibers. In a class of this embodiment, the fibers comprise hemp, bast, jute, flax, ramie, kenaf, sisal, bamboo, or lignocellulosic fibers. In a subclass of this class, the fibers comprise hemp.
[0193] In one embodiment or in combination with any other embodiment, the foamable composition further comprises a photodegradation catalyst. In a class of this embodiment, the photodegradation catalyst is titanium dioxide or iron oxide. In a subclass of this class, the photodegradation catalyst is titanium dioxide. In a subclass of this class, the photodegradation catalyst is iron oxide.
[0194] In one embodiment or in combination with any other embodiment, the foamable composition further comprises a pigment. In a class of this embodiment, the pigment is titanium dioxide, carbon black, or iron oxide. In a subclass of this class, the pigment is titanium dioxide. In a subclass of this class, the pigment is carbon black. In a subclass of this class, the pigment is iron oxide.
[0195] In one embodiment or in combination with any other embodiment, the foamable composition is biodegradable.
[0196] In one embodiment or in combination with any other embodiment, the foamable composition comprises two or more cellulose acetates having different degrees of acetyl substitution.
[0197] In one embodiment or in combination with any of the other embodiments, the foamable composition further comprises a biodegradable polymer other than cellulose acetate.
[0198] In one embodiment or in combination with any other embodiment, there is an article made from any of the aforementioned foamable compositions, wherein the article is a foam.
[0199] In a class of this embodiment, the article has a thickness of at most 3 mm.
[0200] In a class of this embodiment, the article has one or more skin layers.
[0201] In a class of this embodiment, the article is biodegradable.
[0202] In a class of this embodiment, the density of the article is less than 0.9 g / cm 3 In one class of this embodiment, the density of the article is less than 0.8 g / cm3 In one class of this embodiment, the density of the article is less than 0.7 g / cm 3 In one class of this embodiment, the density of the article is less than 0.6 g / cm 3 In one class of this embodiment, the density of the article is less than 0.5 g / cm 3 In one class of this embodiment, the density of the article is less than 0.4 g / cm 3 In one class of this embodiment, the density of the article is less than 0.3 g / cm 3 In one class of this embodiment, the density of the article is less than 0.2 g / cm 3 In one class of this embodiment, the density of the article is less than 0.1 g / cm 3 In one class of this embodiment, the density of the article is less than 0.05 g / cm 3 In one class of this embodiment, the density of the article is 0.2-0.9 g / cm 3 within the range.
[0203] In one class of this embodiment, the article is industrially compostable or home compostable. In a subclass of this class, the article is industrially compostable. In a sub-subclass of this subclass, the article has a thickness of less than 6 mm. In a sub-subclass of this subclass, the article has a thickness of less than 3 mm. In a sub-subclass of this subclass, the article has a thickness of less than 1.1 mm. In a sub-subclass of this class, the article is home compostable. In a sub-subclass of this subclass, the article has a thickness of less than 6 mm. In a sub-subclass of this subclass, the article has a thickness of less than 3 mm. In a sub-subclass of this subclass, the article has a thickness of less than 1.1 mm. In a sub-subclass of this subclass, the article has a thickness of less than 0.8 mm. In a sub-subclass of this subclass, the article has a thickness of less than 0.6 mm. In a sub-subclass of this subclass, the article has a thickness of less than 0.4 mm.
[0204] In one embodiment or in combination with any other embodiment, the thickness of the article is less than 6 mm. In one embodiment or in combination with any other embodiment, the thickness of the article is less than 3 mm. In one embodiment or in combination with any other embodiment, the thickness of the article is less than 1.1 mm. In one embodiment or in combination with any other embodiment, the thickness of the article is less than 0.8 mm. In one embodiment or in combination with any other embodiment, the thickness of the article is less than 0.6 mm. In one embodiment or in combination with any other embodiment, the thickness of the article is less than 0.4 mm.
[0205] The present application discloses a method for preparing a foamable composition, the method comprising: (a) providing a non-foamable composition, the composition comprising (1) an acetyl substitution degree (DS Ac) cellulose acetate with a molecular weight between 2.2 and 2.6, (2) 5wt%-40wt% of a plasticizer, and (3) 0.1wt%-3wt% of a nucleating agent; (b) melting the non-foamable composition in an extruder to form a melt of the non-foamable composition; and (c) injecting a physical blowing agent into the melt of the non-foamable composition to prepare a molten foamable composition.
[0206] In one embodiment or in combination with any other embodiment, the physical blowing agent comprises CO 2 、N 2 , or unbranched or branched (C 2-6 )Alkanes.
[0207] CA Composition Examples
[0208] Embodiment 1. A melt-processable and biodegradable cellulose acetate composition comprising at least one cellulose acetate, at least one plasticizer, and at least one additional component selected from fillers, additives, biopolymers, stabilizers, or odor modifiers.
[0209] Embodiment 2. The composition according to embodiment 1, wherein the cellulose acetate composition comprises at least one plasticizer in an amount of 1 wt% to 40 wt%, or 5 wt% to 40 wt%.
[0210] Embodiment 3. The composition according to embodiment 1, wherein at least one plasticizer is present in an amount of 10 wt% to 25 wt% based on the total weight of the composition,
[0211] wherein the biodegradable polymer is present in an amount of 0 wt % to less than 50 wt % based on the total combined amount of the biodegradable polymer and cellulose acetate,
[0212] wherein the cellulose acetate composition is biodegradable when tested under industrial composting conditions according to ASTM D6400, and
[0213] wherein when the cellulose acetate composition is formed into a 10 mil film, the film exhibits at least 90% disintegration in not more than 12 weeks as measured according to the Disintegration Test Protocol described in the specification.
[0214] Embodiment 3. The composition of embodiment 1 or 2, wherein the DS of cellulose acetate is in the range of 1.0 to 2.5.
[0215] Embodiment 3. The composition of any of embodiments 1 or 2, wherein the Mn of the cellulose acetate is in the range of 10,000 to 90,000 as measured by GPC as discussed in the specification.
[0216] Embodiment 4. The composition of any one of embodiments 1 to 3, wherein at least one plasticizer is a food-compliant plasticizer.
[0217] Embodiment 5. The composition of any one of embodiments 1 to 4, wherein the cellulose acetate composition comprises at least one food-compliant plasticizer in an amount of 1 wt% to 40 wt%, or 5 wt% to 40 wt%, and at least one filler in an amount of 1 wt% to 60 wt%.
[0218] Embodiment 6. The composition of any one of embodiments 1 to 5, wherein the cellulose acetate composition comprises at least one plasticizer in an amount of 10 wt% to 25 wt%, or 15 wt% to 25 wt%.
[0219] Embodiment 7. The composition of any one of embodiments 1 to 6, wherein the cellulose acetate composition comprises at least one food-compliant plasticizer in an amount of 10 wt% to 25 wt%, or 15 wt% to 25 wt%, and at least one filler in an amount of 1 wt% to 60 wt%.
[0220] Embodiment 8. The composition of any one of embodiments 4 to 7, wherein the food-compliant plasticizer is triacetin.
[0221] Embodiment 9. The composition of any one of embodiments 1 to 8, wherein the cellulose acetate comprises at least one filler selected from carbohydrates, cellulose and organic fillers, mineral and inorganic fillers, food waste, desiccants, alkaline fillers, or combinations thereof.
[0222] Embodiment 10. The composition of any one of embodiments 1 to 9, wherein the filler is calcium carbonate.
[0223] Embodiment 11. The composition of any one of embodiments 1 to 10, wherein the cellulose acetate composition comprises at least one biodegradable polymer, wherein the biodegradable polymer is present in an amount less than 50 wt % based on the total combined amount of the biodegradable polymer and cellulose acetate.
[0224] Embodiment 12. The composition according to embodiment 11, wherein the at least one biodegradable polymer is selected from polyhydroxyalkanoate, polycaprolactone polymer or a combination thereof.
[0225] Embodiment 13. The composition of any one of embodiments 1 to 12, wherein the cellulose acetate composition comprises at least one odor modifying additive in an amount of 0.001 wt% to 1 wt% based on the total composition.
[0226] Embodiment 14. The composition of any one of embodiments 1 to 13, wherein the cellulose acetate composition comprises at least one stabilizer in an amount of 0.01 wt% to 5 wt% based on the total composition.
[0227] Embodiment 15. The composition of any of embodiments 1 to 14, wherein when the cellulose acetate composition is formed into a film of 0.38, or 0.51, or 0.64, or 0.76, or 0.89, or 1.02, or 1.14, or 1.27, or 1.40, or 1.52 mm (15, or 20, or 25, or 30, or 35, or 40, or 45, or 50, or 55, or 60 mils), the film exhibits at least 90% disintegration in no more than 12 weeks as measured according to the Disintegration Test Protocol as described in the instructions.
[0228] Embodiment 16. A molded article comprising the composition of any one of embodiments 1 to 15.
[0229] Embodiment 17. The molded article of embodiment 16, wherein the article is a disposable food contact article.
[0230] Embodiment 18. The molded article of embodiment 16, wherein the article is a horticultural article.
[0231] Embodiment 19. The molded article of embodiment 16, wherein the article has a maximum thickness of up to 15 mils and is certified as home compostable.
[0232] Embodiment 20. The molded article of embodiment 16, wherein the article has a maximum thickness of up to 15 mils and is non-permanent.
[0233] Example 21. A method for preparing a biodegradable cellulose acetate composition containing recycled biodegradable cellulose acetate (recycled BCA), the method comprising: (1) preparing a recycled plastic component synthesis gas by gasifying a feedstock containing at least some recycled plastic component in a synthesis gas operation; (2) using the recycled plastic component synthesis gas as a feedstock in a reaction scheme to produce at least one cellulose reactant for preparing recycled BCA; and (3) reacting the at least one cellulose reactant to prepare at least one recycled BCA.
[0234] Embodiment 22. The method of embodiment 21, wherein the at least one cellulose reactant is selected from the group consisting of acetic acid, acetic anhydride, and combinations thereof.
[0235] Embodiment 23. The method according to embodiment 21 or 22, wherein the recovered BCA is selected from cellulose acetate (CA), cellulose diacetate (CDA) or a combination thereof.
[0236] Embodiment 24. A disposable food contact article comprising the biodegradable cellulose acetate composition of any one of embodiments 21 to 23.
[0237] Foamable Example
[0238] Embodiment 1. A foamable composition comprising:
[0239] (1) Degree of acetyl substitution (DS Ac ) cellulose acetate between 2.2 and 2.6; (2) 5 wt%-40 wt% of a plasticizer; (3) 0.1 wt%-3 wt% of a nucleating agent; and (4) 0.1 wt%-3 wt% of a chemical foaming composition comprising: (i) 25 wt%-75 wt% of a blowing agent, and (ii) 25 wt%-75 wt% of a carrier polymer having a melting point not exceeding 150°C, wherein the ratio of the blowing agent to the carrier polymer is based on the total weight of the chemical foaming composition; wherein the ratio of the cellulose acetate, plasticizer, nucleating agent and chemical foaming composition is based on the total weight of the foamable composition.
[0240] Embodiment 2. The foamable composition according to any one of embodiments 1, wherein the foaming agent comprises sodium bicarbonate, citric acid or a combination thereof.
[0241] Embodiment 3. The foamable composition of any one of embodiments 1 to 2, wherein the carrier polymer comprises polybutylene succinate, polycaprolactone, or a combination thereof.
[0242] Example 4. A foamable composition comprising: (1) degree of acetyl substitution (DS Ac ) cellulose acetate between 2.2 and 2.6; (2) 5 wt%-40 wt% of a plasticizer; (3) 0.1 wt%-3 wt% of a nucleating agent; and (4) 0.1 wt%-15 wt% of a physical blowing agent, wherein the proportions of cellulose acetate, plasticizer, nucleating agent and physical blowing agent are based on the total weight of the foamable composition.
[0243] Example 5. A foamable composition comprising: (1) degree of acetyl substitution (DS Ac ) cellulose acetate between 2.2 and 2.6; (2) 5 wt%-40 wt% of a plasticizer; (3) 0.1 wt%-3 wt% of a nucleating agent; and (4) 1 wt%-15 wt% of a physical blowing agent, wherein the proportions of cellulose acetate, plasticizer, nucleating agent and physical blowing agent are based on the total weight of the foamable composition.
[0244] Embodiment 6. A foamable composition according to any one of embodiments 4 or 5, wherein the physical blowing agent comprises CO 2 、N 2 , unbranched or branched (C2-6 )alkanes, or any combination thereof.
[0245] Embodiment 7. The foamable composition of any one of embodiments 1-6, wherein the plasticizer comprises triacetin, triethyl citrate or PEG400.
[0246] Embodiment 8. The foamable composition of any one of embodiments 1 to 7, wherein the plasticizer is present at 17 wt% to 23 wt%.
[0247] Embodiment 9. The foamable composition of any one of embodiments 1 to 8, wherein the nucleating agent comprises a particulate composition having a median particle size of less than 2 microns.
[0248] Embodiment 10. The foamable composition of any one of embodiments 1 to 9, wherein the nucleating agent comprises magnesium silicate, silicon dioxide, magnesium oxide, or a combination thereof.
[0249] Embodiment 11. The foamable composition of any of embodiments 1-10, wherein the foamable composition further comprises fibers.
[0250] Embodiment 12. The foamable composition of embodiment 11, wherein the fibers are biodegradable.
[0251] Embodiment 13. The foamable composition of any of embodiments 11-12, wherein the fibers comprise hemp, bast, jute, flax, ramie, kenaf, sisal, bamboo, or lignocellulosic fibers.
[0252] Embodiment 14. The foamable composition of any one of embodiments 1-13, wherein the foamable composition further comprises a photodegradation catalyst.
[0253] Embodiment 15. The foamable composition according to embodiment 14, wherein the photodegradation catalyst is titanium dioxide or iron oxide.
[0254] Embodiment 16. The foamable composition of any one of embodiments 1 to 15, wherein the foamable composition further comprises a pigment.
[0255] Embodiment 17. The foamable composition of embodiment 16, wherein the pigment is titanium dioxide, carbon black or iron oxide.
[0256] Embodiment 18. The foamable composition of any one of embodiments 1 to 17, wherein the foamable composition is biodegradable.
[0257] Embodiment 19. The foamable composition of any of embodiments 1-18, wherein the foamable composition comprises two or more cellulose acetates having different degrees of acetyl substitution.
[0258] Embodiment 20. The foamable composition of any one of embodiments 1 to 19, wherein the foamable composition further comprises a biodegradable polymer different from the cellulose acetate.
[0259] Embodiment 21. An article prepared from the foamable composition of any one of claims 1-20, wherein the article is a foam.
[0260] Embodiment 22. The article of embodiment 21, wherein the thickness of the article is at most 6 mm.
[0261] Embodiment 23. The article of any one of embodiments 21-22, wherein the article has one or more skin layers.
[0262] Embodiment 24. The article of any one of embodiments 21-23, wherein the article is biodegradable.
[0263] Embodiment 25. The article of any one of embodiments 21-24, wherein the density of the article is less than 0.9 g / cm 3 .
[0264] Embodiment 26. The article of any one of embodiments 21-25, wherein the article is industrially compostable or home compostable.
[0265] Embodiment 27. The article of embodiment 26, wherein the thickness is less than 3 mm.
[0266] Examples
[0267] abbreviation
[0268] BHT is butylated hydroxytoluene or Tenox BHT (Eastman); bioCBA is a biodegradable chemical blowing agent; CA is cellulose acetate; CA398-30 is Eastman cellulose acetate CA398-30; CA398-10 is Eastman cellulose acetate CA398-10; CBA is a chemical blowing agent; CDA is cellulose diacetate; CAPA 6500 is polycaprolactone (Ingevity); CE41972 is Eastman cellulose acetate cellulose ester 41972; DLTDP is dilauryl thiodipropionate (Sigma Aldrich); DMA or DMTA is dynamic mechanical analysis; DS is the degree of substitution per anhydroglucose unit of the cellulose ester; EOB is elongation at break; EPSO is epoxidized soybean oil (Vikoflex 7170, Arkema); FZ 73S is Foamazol 73s (Bergen International); FZ 95 is Foamazol 95 (Bergen International); h or hr is hour; HDT is heat deformation temperature; HK40B is Hydrocerol HK40B (Clariant); PHB(6)Hx is poly(3-hydroxybutyrate-co-6 mol%-3-hydroxyhexanoate), having an average Mw of about 770,000 (measured using GPC and PS standards with dichloromethane solvent); Pz is plasticizer; TA is triacetin; TEC is triethyl citrate; ℃ is degree Celsius; wt% is weight percentage; PEG400 is polyethylene glycol having an average molecular weight of 400 Daltons. kWh / kg is kilowatt hour / kilogram; L is liter; oz is ounce; PBA is physical blowing agent; PBS is polybutylene succinate; PCL is polycaprolactone; PS is polystyrene; rpm is revolutions per minute; TGA is thermogravimetric analysis; MW is molecular weight.
[0269] Test Materials and Protocols: Cellulose Diacetate Compositions
[0270] Starting CDA materials were obtained from Eastman Chemical Company. Materials included commercially available CDAs (CA398-30 and CA398-10) having a DS of 2.5 and Mn of about 50,000 and about 40,000, and commercially manufactured CDA having a DS of 2.2. CDA compositions having a Pz were prepared. The plasticizer used in the examples was TA. The TA pre-plasticized compositions were also compounded with fillers or polymer additives into additional compositions. Cellulose acetate compositions were prepared with a polymer additive and without a TA plasticizer, the polymer additive being polyethylene glycol ("PEG-400") having an average molar mass of about 400 g / mol. Plasticized cellulose acetate resin was prepared by feeding cellulose diacetate to a twin-screw co-rotating extruder using a loss-in-weight feeder for solid and liquid feeds. The solids were fed to the feed port of the extruder, and the liquid was injected into the first heated barrel zone. The materials were compounded using an increasing temperature profile from 70°C in the first heating zone to 230°C at the die. The materials were processed under conditions sufficient to provide a relatively homogeneous resin mixture. The resulting resins were pre-plasticized cellulose acetate resins having 15 wt%, 17 wt%, or 30 wt% of TA as a plasticizer. Cellulose acetate compositions with PEG 400 were prepared in a similar manner.
[0271] In the case of compounded CDA compositions, pre-plasticized cellulose acetate resin (base resin) having 15 wt%, 17 wt% or 30 wt% of TA as a plasticizer (TA) was compounded with filler material or polymer additive. Compounding was performed on a 26 mm twin screw extruder with a side feeder. The base resin was fed into the barrel on the extruder by a loss-in-weight feeder system. The filler material or polymer additive was added by a side feeder with a loss-in-weight feeder system. The temperature of zone 1 was set to 150°C and the temperature of all subsequent zones plus the die was set to 180°C. For these compounds, the specific energy input (SEI) varied between 0.116 kWh / kg and 0.158 kWh / kg. The melt temperature was between 177°C and 181°C (measured in the die). An atmospheric vent was performed after the first kneading section and before the pumping section to remove steam from the undried base polymer and water combined with the filler material. The final product composition is produced by passing through a die to create strands, cutting the strands into pellets.
[0272] Extruded Film
[0273] The films were produced using a 1.5 inch Killion single screw extruder equipped with a Maddock mixer screw. Pellets of cellulose acetate composition were loaded into a hopper and the material was fed into a barrel where the Maddock screw transferred the material toward the die. The barrel (which houses the screw) was heated in three zones so that the pellets melted as they passed through the screw along a very narrow gap, thereby achieving high shear and highly dispersive mixing. A uniform polymer mixture was observed to form as it approached the die, and at the point where extrusion occurred, the mixture was forced through the die by the screw. When the film left the die, the extrusion formed a flat molten film, and the film solidified on a temperature controlled polished chrome roller (roller stack).
[0274] Film samples were intermittently removed after extrusion to determine film thickness. When the extruder produced the appropriate film thickness, the film was attached to a take-up roll and the film was carefully wound until the last roll was completed.
[0275] Film disintegration test protocol
[0276] The test method for disintegration is based on ISO 16929 Plastics - Determination of the degree of disintegration of plastic materials under defined composting conditions in a pilot-scale test (2013). A pilot-scale aerobic composting test was used to simulate as closely as possible a real complete composting process in a 200 L compost bin. The test material (film) was placed in a sliding frame that exposed about 8.05 cm2 of the test material on both sides of the film. These sliding frames were then mixed with biowaste and composted in two 200 L compost bins. The biowaste consisted of vegetable, garden and fruit waste (VGF), to which 11% of additional structural material was added to obtain optimal composting conditions. In line with full-scale composting, deterioration and temperature increase occurred spontaneously. The test was considered valid only if the maximum temperature during composting was above 60°C and below 75°C, and the daily temperature remained above 40°C for at least 4 weeks. The composting process was guided by air flow and moisture content. Temperature and exhaust gas composition were monitored regularly. The composting process continued until a fully stable compost was obtained (3 months). During composting, the contents of the containers were manually turned over, at which point the test objects were retrieved and visually assessed.
[0277] Solvent casting of membranes
[0278] CA398-30 was the resin for all tests (DS=2.52; mp 230-250°C, Tg 189°C). Solutions containing 12% CA398-30 in acetone were prepared. Additives were included in the solution as indicated. Some mixtures were heated to 50°C to facilitate dissolution and mixing. Thin films (~3 mils) were applied to clean glass plates using a film applicator (BYK 5351; 2" square frame, 5-50 mils). Thicker films (5-40 mils) were cast from acetone into flat-bottomed aluminum pans, and solvent evaporation was controlled by covering the pan over 16 to 24 hours. Film thickness was measured with a digital micrometer (Mitutoyo Digimatic micrometer, MDC-1" PX) with a resolution of 0.0.05 mils.
[0279] Glass transition temperature
[0280] Glass transition temperature (Tg) was estimated by differential scanning calorimetry (DSC) and DMA. DMA of the film includes a normal temperature scan under a frequency controlled oscillating strain to collect information about room temperature differences and Tg differences. For DMA, the film samples were run at 3°C / min at 0.1% strain at 1 Hz, and the Tg range was estimated based on the E' onset and the peak of the Tan (δ) curve.
[0281] Tg (DSC) of 10 mil films of PEG MW 200 to 2000
[0282] PEG with a MW between 200 and 8,000 was added at 17.0 wt% to a CA398-30 coating (12 wt% CA398-30 in acetone) and blended by heating at a temperature of up to 50°C. The film was cast at a dry thickness of 10 mils. The Tg of the CA398-30 / PEG blends was estimated by DSC second heating, and the results are summarized in Table 1. When the PEG MW was 6,000 or greater, incompatibility in the film was observed, which was a defect in the film. When the PEG MW was 2,000 or greater, no Tg was detected in the second heating of the DSC. Instead, an endotherm was detected at a temperature close to the melting point of PEG, which is a sign of immiscibility of the blend. When the PEG MW was 600 or less, a single Tg was detected in the CA / PEG blend.
[0283] Table 1. DSC of CA / PEG blends containing PEG (17.0 wt%).
[0284]
[0285] Plasticizing efficiency estimated by DMA
[0286] Measuring the Tg of films plasticized with PEG and PEG derivatives is not straightforward, and it is sometimes difficult to observe a clear glass transition temperature for cellulosic materials by DSC. When a more sensitive technique is required, DMTA or DMA may be chosen.
[0287] Tables 2 and 3 provide Tg values for CA398-30) films plasticized at 23wt% and 17wt% respectively using the DMA method. Tan (δ) is used as an estimate of the Tg value of the film. At 23wt% plasticizer loading (Table 2), PEG600, MPEG165, MPEG550, and MPEG750 exhibit Tg values greater than 160°C as measured by DMA. On the other hand, PEG200, PEG300, PEG400, MPEG350, and MPEG450 exhibit Tg values of 113°C to 120°C, indicating greater plasticizing efficiency.
[0288] Table 2. DMA of CA398-30 films containing 23 wt% plasticizer.
[0289]
[0290] For a plasticizer loading of 17 wt% (Table 3), PEG400, MPEG350, and MPEG550 exhibited a Tg range of 127° C. to 132° C. However, PEG600 exhibited a Tg of 195.6° C., similar to unplasticized CA398-30.
[0291] Table 3. DMA of CA398-30 films containing plasticizer (17 wt%).
[0292]
[0293] Relative thermal stability / volatility of PEG and other plasticizers in CA398-30 films
[0294] Low MW plasticizers tend to volatilize during thermal processing, whether during compounding, extrusion or thermoforming. Isothermal volatility was tested on different film formulations. CA398-30: DS = 2.5; mp 230-250, Tg 189°C (DSC). Films (~3 mils) were cast from 12 wt% CA398-30 and plasticizer in acetone solutions onto glass plates. The solvent was evaporated and the film was equilibrated under laboratory conditions (20-23°C, 25%-30% RH). Films containing 23.0 wt% PZ (1 inch squares, equilibrated to laboratory ambient conditions, 20-23°C and ~25% RH) were accurately weighed before and after heating to 120°C for 7 minutes to 127 minutes to monitor weight loss. The results in Table 4 show that PEG200 is the most volatile plasticizer in 5 mil films, followed by TA) and TEC. The weight loss of films plasticized with PEG400, PEG600, polysorbate 20 (Tween 20) was not different from that of unplasticized CA398-30.
[0295] Table 4. Weight loss of CDA films plasticized with PZ (23 wt%) upon heating to 120°C.
[0296]
[0297] Stress whitening after biaxial stretching
[0298] The film of Example 16 was stretched to simulate thermoforming. To understand the sheet temperature effect, two oven temperatures of 165°C and 185°C were selected. The heating time was fixed at 40 seconds before stretching. To simulate the area stretch ratio of a 12-ounce clamshell, an equivalent biaxial stretch ratio of 1.5×1.5 was used. For a 12-ounce drinking cup, an equivalent biaxial stretch ratio of 2×2 was used. Two strain rates were also selected. One was 50% / s, which is essentially the same strain rate during vacuum forming at 25 inches of mercury. The other was 500% / s, which approximates high-speed stretching from a mandrel. Since stress whitening is the primary focus in this example, the key response is the haze in the sheet, which is proportional to the degree of stress whitening.
[0299] Stress whitening is formed when the CDA sheet is thermoformed into a clamshell (hinged container) or a cup. To simulate large packaging containers of different shapes and sizes, the equivalent biaxial stretch ratio is calculated by using the area stretch ratio of the container. Table 5 shows two examples. One is a 12-ounce drinking cup with an area stretch ratio of 4.45 and an approximate biaxial stretch ratio of about 2×2. The other is a 12-ounce clamshell with an area stretch ratio of 1.93 and an approximate biaxial ratio of about 1.5×1.5. The area stretch ratio is defined by the total surface area of the formed container divided by the original sheet area before forming.
[0300] Table 5. Biaxial film stretching for simulated thermoforming.
[0301] Area stretch ratio Biaxial stretching ratio 12 oz cup 4.45 ~2x2 12 ounces clam shells 1.93 ~1.5x1.5
[0302] To investigate the effect of each variable on stress whitening in biaxially stretched CDA sheets, an experimental matrix is presented in Table 6. The haze of each sample was measured by varying the thickness, stretch ratio, stretch temperature, and strain rate.
[0303] Table 6. Experimental matrix
[0304]
[0305] Haze after stretching 15 mil sample
[0306] At the lower stretch ratio of 1.5×1.5, the 15 mil Example 13 sample showed very little haze under various stretching conditions as shown in Table 7. On the other hand, the Example 15 (15 mil) sample developed some haze under the same stretching conditions, especially at 165° C. Table 7 summarizes the biaxial stretching results for the 15 mil thick samples, and even at higher stretch ratios, strain rates, and lower temperatures, Example 13 showed little haze formation, while significant haze was observed for Example 15 under the same combined stretching conditions.
[0307] Table 7. Haze results for 15 mil samples stretched under various conditions.
[0308]
[0309] Table 8 summarizes the results for the 30 mil thick samples. Even at the higher stretch ratio, strain rate, and lower temperature, Example 14 showed little haze formation, while significant haze was observed for Example 16 under the same combined stretching conditions.
[0310] Table 8. Haze results for 30 mil samples stretched under various conditions.
[0311]
[0312] In Film Examples 15 and 16, only shallow draw articles could be vacuum formed using this formulation due to stress whitening issues.
[0313] Gel counting
[0314] Gel counting protocol
[0315] Gel counts were determined by adapting ASTM D7310-11. Film samples were imaged using an Allied Vision Technologies GT2750C Ethernet-based camera. The area analyzed was 5 cm x 5 cm = 25 cm2 , take 6 images, the total imaging area is 150cm 2 . The camera is a color camera with a 2750×22001-inch pixel sensor. The camera uses default settings except that the exposure time is set to 400 microseconds. The lens used in the system is an Opto Engineering TC23080 double-sided telecentric lens. The working distance of the lens is 226.7mm. This produces a field of view of 76.5mm×64.0mm. The light used in the device is an Opto Engineering LTCLHP080-G collimated light. The light is positioned 150mm from the sample. The light and lens are set in transmission mode so that the film sample is between the light and the lens. The transmission mode layout combined with telecentric optics provides unique advantages over other illumination geometry / lens combinations. The combination of transmission mode combined with telecentric optics causes translucent gels present in translucent films to appear as dark particles on the image sensor. The gel appears as dark particles on a translucent background, enabling easy detection, counting and metering of the gel.
[0316] The images from the camera were obtained using the Measurement & Automation Explorer software of National Instruments. The images were processed using an internally developed program written in the LabVIEW programming language. Typically, the image processing program separates the individual gels in the membrane. The first step performed by the program is color plane extraction. When images are collected with a color camera, multiple images are created on different planes. The color plane extracted by this method is the HSI intensity plane because the color plane gives the best contrast between the background and the defect of interest. The next step performed in the image processing routine is image calibration. Image calibration is used to convert pixels into real-world units. This calibration is performed using an imaging standard. The saved calibration is then applied to all subsequent images in this step. The image is then thresholded using a local background correction algorithm with a local area of 32 x 32 pixels. The automatic thresholding routine performs background correction to eliminate uneven lighting effects. The intergroup variance thresholding algorithm is then applied to separate dark particles. In the intergroup variance method for thresholds, the intergroup variance is measured at each possible pixel intensity. The threshold is set at the pixel intensity that maximizes the intergroup variance. The algorithm assumes that the pixel intensity represents a bimodal distribution with 2 categories. In the processing routine, the image is a binary image at this point. Particles in the image are assigned a value of 1 and the background is assigned a value of 0. An opening function is applied to the particles. The opening function first erodes the particles and then dilates the remaining particles. Larger particles are retained, but small particles are eliminated. This step is done to eliminate sensor noise and disconnect adjacent particles that may be touching. The next step eliminates particles that touch the border of the image because these particles cannot be accurately measured. Once the border particles are eliminated, the areas of all gel particles are added. The imaged area combined with the gel area can be used to calculate the total particle / gel area of the membrane sample.
[0317] Extruded Films, Examples 17-20
[0318] CA398-30 is compounded with PEG400 or PEG600 at a desired weight percentage and then formed into pellets. The composite pellets are first prepared using a twin-screw extruder, and the conditions of the extruder are shown in Table 9. Before using the pellets to extrude a film, the pellets are dried at 140°C for 4 hours. The dried composite pellets are then extruded using an extruder with the conditions shown in Table 10.
[0319] Table 9. Extruder conditions for preparing composite pellets.
[0320] Barrel temperature ℃ Zone 1 90 Zone 2 160 Zone 3 200 Zone 4 200 Zone 5 210 Zone 6 220 Zone 7 220 Zone 8 220 Zone 9 220 Mould 225
[0321] Table 10. Extruder conditions for preparing films used for gel counting studies.
[0322] Extrusion conditions ℃ Zone 1 218 Zone 2 227 Zone 3 227 Zone 4 227 adapter 227 Mould 238 Cooling roller 93
[0323] Example 17: Film (80 wt% CA398-30, 20 wt% PEG400, 30 mil)
[0324] Example 18: Film (80 wt% CA398-30, 20 wt% PEG400, 15 mil)
[0325] Example 19: Film (80 wt% CA398-30, 20 wt% PEG600, 30 mil)
[0326] Example 20: Film (80 wt% CA398-30, 20 wt% PEG600, 15 mil)
[0327] Table 11. Gel count distribution of 15 mil and 30 mil (PEG400 / PEG600)
[0328]
[0329]
[0330] Example 1 and Example 2 - Disintegration of Filled and Unfilled Samples
[0331] Pilot scale aerobic composting tests (as described above) were conducted. In the test, the film samples were mixed with fresh organic pretreated municipal solid waste (biowaste) and introduced into an insulated compost bin where composting began spontaneously. The film samples tested included: 15 mil thick diacetate cellulose extruded film, which was plasticized with 15 wt% TA, 1 wt% EPSO, and no filler (Example 1); and 15 mil thick diacetate cellulose extruded film, which was plasticized with 15 wt% TA and composited with 1 wt% EPSO and 15 wt% calcium carbonate (Omyacarb UF-FL CaCO 3 , surface treated and with a particle size of 0.70 microns) (Example 2). Films were prepared as described above. Samples were observed after 1, 2, 3, 4, 6, 8, 10 and 12 weeks of composting. The disintegration results of Example 1 and Example 2 are summarized in Table 12.
[0332] Films made from compositions containing 15 wt% calcium carbonate had faster disintegration. Although not shown, a similar effect was observed for films containing 30 wt% TA, where the films containing 30 wt% TA disintegrated faster than otherwise similar films containing 15 wt% TA.
[0333] Examples 3 and 4 - Disintegration under the Effect of Acetyl Levels
[0334] Film samples were tested as follows: 10 mil thick cellulose diacetate extruded film, the film has an acetyl substitution degree (DS) of 2.5, Mn of 50,000, plasticized with 15wt% TA, 1wt% EPSO, and no filler (Example 3); and 10 mil thick cellulose diacetate extruded film, the film has an acetyl substitution degree (DS) of 2.2, plasticized with 15wt% TA, 1wt% EPSO, and no filler (Example 4). Films were prepared as described above. Samples were observed after 1, 2, 3, 4, 6, 8, 10, and 12 weeks of composting. The results of Example 3 and Example 4 are summarized in Table 12.
[0335] A review of the results showed that films with CDA containing lower acetyl levels disintegrated faster than similar films with CDA containing higher acetyl levels.
[0336] Example 5 - Disintegration as a Function of Molecular Weight
[0337] Film samples were tested as follows: 10 mil thick cellulose diacetate extruded film having a number average molecular weight (Mn) of 40,000 (measured by GPC as described herein), plasticized with 15 wt% TA, 1 wt% EPSO, and no filler. Films were prepared as described above. Samples were observed after 1, 2, 3, 4, 6, 8, 10, and 12 weeks of composting. The results of Example 5 are also summarized in Table 12.
[0338] The results showed that films of lower molecular weight CDA disintegrated faster than similar films of higher molecular weight CDA.
[0339] Example 6-Example 7-Disintegration of composite CDA compositions containing plasticizer and polymer additives.
[0340] The film samples tested included: a 20 mil thick cellulose diacetate extruded film, which was plasticized with 17 wt% TA and compounded with 1 wt% EPSO and 20 wt% PHB(6)Hx (Example 6); and a 20 mil thick cellulose diacetate extruded film, which was plasticized with 17 wt% TA and compounded with 1 wt% EPSO, 20 wt% PHB(6)Hx and 10 wt% CAPA 6500 (Example 7). The results are summarized in Table 12.
[0341] Example 8 - Example 11 - Disintegration of CDA Compositions Containing PEG Additives.
[0342] The film samples tested included: 15 and 30 mil thick cellulose diacetate extruded films compounded with 1 wt% EPSO and 10 wt%, 15 wt% or 20 wt% PEG-400. The results are summarized in Table 12.
[0343] Example 12 Disintegration of CDA Compositions Containing Effervescent Agents.
[0344] The film samples tested included: 20 mil thick cellulose diacetate extruded film, which was plasticized with 20 wt% TA and compounded with 1 wt% talc and 1 wt% EPSO by compounding the components in a manner similar to the above method. As described above, a single screw extruder was used to prepare the film, except that 1 wt% of a chemical blowing agent (FZ 73s) was added to the feed hopper to prepare the foamed film (Example 12). The Example 12 foam sample with a thickness of 20 mils passed the qualitative composting test after 10 weeks. The results are summarized in Table 12.
[0345] Table 12. Summary of disintegration results (industrial composting)
[0346]
[0347] OWS Home Compost
[0348] Under OWS home composting conditions, a 20 mil foam sample of Example 12 disintegrated well within 20 weeks. Under home composting conditions, Example 12 completely disappeared within 26 weeks (Table 13).
[0349] Table 13. Disintegration of Example 12 under home composting conditions.
[0350]
[0351] Disintegration and biodegradation
[0352] Usually, after degradation, parameters such as DOC (dissolved organic carbon), CO 2 There are three main methods for testing the biodegradation of materials: Sturm method, respirometry and radiolabeling 14 The C atom test method. The Sturm method accurately measures carbon dioxide production through changes in pressure. The respirometry test accurately measures oxygen consumption over a 60-day period. Finally, radiolabeling 14 C atom test determination 14 C 14 CO 2 All three methods can be used under aquatic or composting conditions if the correct equipment is used.
[0353] Carbon dioxide (CO) produced by the freshwater modified Sturm test (OECD 301B) 2 ) as a percentage of theoretical yield (based on total organic carbon analysis) is used as the basis for assessing whether a material is biodegradable. CO is measured by a sodium hydroxide trap 2 The study was run for at least 28 days and if CO 2 If production shows signs of increasing near the end of the 28-day period, it can continue.
[0354] Biodegradation Test-O 2 Consumption (OECD 301F) can be used to monitor the biodegradation of polymeric materials. OECD301F is an aquatic aerobic biodegradation test, which measures the biodegradability of materials by measuring oxygen consumption. OECD301F is most commonly used for OECD 301B tests of insoluble and volatile materials with obstacles. The purity or ratio of the main components of the test material is important for calculating the theoretical oxygen demand (ThOD). Similar to other OECD 301 test methods, the standard test duration of OECD 301F is at least 28 days, and easy biodegradability or inherent biodegradability can be measured. The solution or suspension of the test substance in a mineral culture medium is inoculated, and incubated under aerobic conditions in the dark or diffuse light. A reference compound (usually sodium acetate or sodium benzoate) is carried out in parallel to check the operation of the program.
[0355] There are three classifications of biodegradability: readily biodegradable, inherently biodegradable, and non-biodegradable. A material is readily biodegradable if it reaches ≥60% of its theoretical oxygen demand within 28 days. Inherently biodegradable materials also reach the 60% level, but only after the 28-day window has passed. Typically, testing for readily biodegradable materials lasts 28 days, while extended testing periods may be used to classify a material as inherently biodegradable.
[0356] The OxiTop method is a modification of the Sturm method to analyze biodegradation while reporting biodegradability as oxygen consumption and CO generated during the test. 2 The pressure is converted to BOD, or biological oxygen demand. The OxiTop provides accurate measurements of aquatic biodegradation in an easy to use format. The Control OC 110 Respirometer System measures the biological oxygen demand [BOD] over time. This is achieved by measuring the negative pressure created when oxygen is consumed in a closed bottle system. NaOH tablets are added to the system to collect the O 2 CO released during consumption 2 .CO 2 Reacts with NaOH to form Na 2 CO 3 , Na 2 CO 3 CO 2 The OxiTop sensor records this negative pressure and wirelessly relays the information to a controller which converts the generated CO 2Converts to BOD at a 1:1 ratio. The measured BOD can be compared to the theoretical oxygen demand for each material tested to determine the percentage of biodegradation. OxiTop can be used to screen materials for readily or inherent biodegradability.
[0357] Aquatic biodegradation of CA and CA+PEG400
[0358] The aquatic biodegradation rates of cellulose, cellulose acetate (CA), and CA blended with PEG400 were compared using the Oxitop method. Biodegradation refers to the mineralization of a substance, or its conversion into biomass, CO2, and other organic compounds through microbial metabolism. 2 and water.
[0359] Test materials included a cellulose positive control (PC) and cellulose acetate (DS 2.5), both of which were added in powder form. CA398-30 is a high viscosity, high molecular weight cellulose acetate provided as a fine, dry, free-flowing powder. The uniform particle size of the powder allows for good plasticizer distribution during blending. The average particle size is about 200-250 microns and the maximum particle size is about 500 microns. CA resin (CA398-30) was added in the form of an unmodified powder. CA resin was also uniformly mixed with a plasticizer (PEG400, 15%).
[0360] Aquatic biodegradation was assessed essentially as described in the OECD 301F test method. Eastman sludge was used as the wastewater broth, and the wastewater samples were vacuum filtered to remove solid particles. The test was extended from 28 days to 56 days. The longer duration allowed for the identification of readily biodegradable materials (materials that must pass within 28 days), as well as providing screening for inherently biodegradable materials at the longer test duration. Data were initially collected as BOD measurements (mg / LO 2 ), and then calculate the percentage of biodegradation based on the elemental composition of the substance.
[0361] Table 14. Aquatic biodegradation results for Examples 48 and 49.
[0362]
[0363] Marine biodegradation
[0364] Marine biodegradation is necessary when foam products are accidentally discharged into waterways and eventually float in the ocean. The foam itself is already favorable for photodegradation. Additional additives may be added to enhance photodegradation, especially when the article floats in a marine environment.
[0365] UV Degradation of Example 12
[0366] Accelerated UV testing shows that foams can quickly lose their molecular weight, which may be beneficial to aquatic or marine biodegradation if the product is accidentally released into a waterway or ocean. Lightweight foam products will float in water, making them easily exposed to UV during the day. The reduction in molecular weight will increase the disintegration rate of the foam, thereby increasing the rate of marine biodegradation.
[0367] The sample of Example 12 was cut into 4" x 6", and first exposed to a radiation with a peak radiation of 340 nm and an intensity of 0.89 W / m at 60°C. 2 8 hours under UV fluorescence. Then turn off the UV for 4 hours at 50°C in condensing humidity on the vertical sample. Repeat the cycle until 168 hours (14 cycles) is reached, which is equivalent to one week of UV exposure. Take out some samples for GPC molecular weight measurement. The rest will continue UV exposure for 168 hours for two weeks. Submit the original sample (0 week), the sample exposed for 1 week, and the sample exposed for two weeks for GPC molecular weight measurement. The normalized MW is the measured MW divided by the original MW, which indicates the degree of molecular decomposition due to UV degradation. The original MW is 91,000.
[0368] Table 15. UV exposure of Example 12
[0369]
[0370] Table 16 discloses additional foams made from various compositions using a small extruder (D = 1.5 inches L / D = 24). The compositions contained TA (15 wt%, 20 wt%, 25 wt%) and three types of CBA (HK40B, FZ 95 and FZ 73s) at two loadings (1 wt%, 2 wt%). All compositions contained 1% talc (ABT 1000) supplied by Barretts Minerals. All foams formed from the compositions were 20 mils thick and floated in water, indicating that the foam was 1.30 g / cm thick. 3 The initial density was reduced significantly.
[0371] Table 16. Foaming feasibility using various compositions.
[0372]
[0373]
[0374] Example 23 was used for large-scale studies on a large extruder (D = 2.5 inches, L / D = 30) to further optimize the loading level of the chemical blowing agent (0.7wt%, 1wt%, 1.3wt%), as shown in Table 17. Example 12 showed similar results to Example 23. The density of Example 12 was found to be about 0.7 (about 50% weight reduction from 1.30). The film sample of Example 12 was thermoformed into a tray using vacuum.
[0375] Table 17. 20 mil foam using three different loading levels of CBA.
[0376]
[0377] Color matching and HDT improvements
[0378] Example 34 in Table 15 is a beige CA foam, which itself is different from the ubiquitous white PS foam. For further highlight, Bayferrox 6593 iron oxide provided by Lanxess can be used to match the color of kraft paper. In addition, the texture and feel of CA foam can be changed by any natural fiber, such as hemp core fiber (hurd), as shown in Table 18, Example 35. The 1mm long hemp core fiber is provided by Centralinfiber. Hemp fiber also increases the HDT of the foam, which is about 14°C under a load of 0.45MPa and about 17°C under a load of 1.86MPa. HDT is measured by DMA at a temperature at which the sample undergoes 2% elongation under a specific tensile load.
[0379] Table 18. HDT (DMA at 2% elongation in tensile mode) of Examples 34 and 35 at two different loads.
[0380]
[0381] Hemp fiber reinforced foams also showed high Young's modulus in the machine direction (MD) and transverse direction (TD) to improve rigidity for stackability, but had lower elongation at break than the corresponding foams without fiber shown in Table 19, and were more likely to tear in home compost. Hemp fiber is expected to accelerate the overall degradation of cellulose acetate foam. Based on these results, cellulose acetate foam reinforced with hemp fiber is expected to provide heat resistance and stackability, which is more suitable for hot food applications, such as in foamed food containers. Therefore, fiber reinforced foams with higher HDT and stiffness have performance advantages compared to non-reinforced foams.
[0382] Table 19. Mechanical properties of Examples 34 and 35.
[0383]
[0384] bioCBA
[0385] Commercial CBAs typically use low melting temperature polymer carriers, such as PS or PE, so that they can be compounded with active blowing agents (such as sodium bicarbonate and citric acid) at relatively low temperatures so that the blowing agents do not thermally decompose prematurely. However, the polymer carriers are not biodegradable and may eventually form microplastics in the marine environment. In order to develop 100% biodegradable foams that do not leave microplastics when the products are accidentally discharged into the ocean, biodegradable chemical blowing agents are highly desirable. Two bioCBAs were prepared by compounding all ingredients at less than 150°C using a twin-screw extruder. Example 36: 50wt% BioPBS FD92PM / 20wt% Sodium bicarbonate / 30wt% Citric acid, and Example 37: 50wt% CAPA 6500 / 20wt% Sodium bicarbonate / 30wt% Citric acid. BioPBS FD92PM (Mitsubishi Chemical) and CAPA 6500. To ensure that the blowing agents sodium bicarbonate and citric acid were still active after compounding, the weight loss was measured using TGA in nitrogen, as Figure 1 As shown. At around 240°C, the weight loss of both BioCBAs is similar, up to 20% (from 100% to 80%). The commercial CBA FZ 73S has a different weight loss curve, losing 20% at around 230°C. Two foam samples were prepared using the two BioCBAs. The foam density of Example 36 BioPBS FD92PM CBA was 0.6 g / cm 3 , while the foam density of CAPA 6500 CBA in Example 37 is 0.4 g / cm 3 These results indicate that it is possible to produce 100% biodegradable foams by using biodegradable CBA.
[0386] Foam using physical blowing agents
[0387] For using CBA to extrude foam, it is more portable without the need for major capital investment. Injection molded foam products can also be made using CBA. However, this CBA technology is more suitable for high-density foams. For low-density foam production, such as PS foam, PBA should be used with a gas injection system.
[0388] Extrusion process of foam made from PBA
[0389] The cellulose acetate resin was dried at 60°C for 4 hours. The resin was then fed into a 2 The extrusion temperature profile is shown in the table below. 2 The melt is injected directly. Foam forms when the melt leaves the mold.
[0390] Table 20. Extruder conditions
[0391] Extruder ℃ Zone 1 200 Zone 2 205 Zone 3 210 Zone 4 210 adapter 210 Mould 200
[0392] Table 21 shows the effect of wt% of carbon dioxide on foam density. As shown, the density of the foam can be adjusted by the amount of carbon dioxide injected. The higher the carbon dioxide loading, the lower the density of the foam.
[0393] Table 21. Foaming results using carbon dioxide
[0394]
[0395] Examples of using stabilizers
[0396] Material
[0397] The cellulose acetate used was CA398-30 with a melting point of 230-250° C. and a Tg of about 189° C., or CE41972 with a melting point of 240-260° C. and a Tg of about 180° C. The plasticizer was TA (Eastman, food grade) or PEG400 (Dow Sentry Polyethylene Glycol 400).
[0398] The additives used were BHT; Irganox 1010 (pentaerythritol tetrakis(3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate from BASF); DLTDP; Weston 705T phosphite (from SI Group), Doverphos S-9228T phosphite (from Dover Chemical), EPSO and citric acid (from Sigma-Aldrich).
[0399] Solvent casting of membranes
[0400] Acetone solutions containing 12% cellulose acetate were prepared. Plasticizers and additives were included in the solution as indicated. Films (~15 mils) were cast from acetone onto flat bottom aluminum pans, and solvent evaporation was controlled by covering the pans for 48 hours. Film thickness was measured using a digital micrometer (Mitutoyo Digimatic Micrometer, MDC-1" PX) with a resolution of 0.05 mils.
[0401] Screening solvent cast films
[0402] The film was cut into four equal parts and the four equal parts of four different films were placed in a single aluminum pan. A second aluminum pan was stacked on top of the film and the two aluminum pans were clamped together with a clip. The aluminum pan assembly was placed in an oven set at 200°C for one hour and then removed and allowed to cool to room temperature. The film was removed from the aluminum pan assembly and the color was measured using a CR-400 colorimeter from Konica Minolta to determine L*, a* and b*.
[0403] Composite materials
[0404] Cellulose acetate is compounded with plasticizer and optional additives to prepare pellets. The specific formulations are listed in the table below. Compounding is performed using a Leistriz 18mm twin screw extruder. The screw RPM is typically about 560, although it varies between 416 and 584 RPM. The torque range is 26.7% to 50%. The melt temperature range is 255-275°C. The melt pressure range is 412-580psi. The SEI range is 0.147-0.326. The barrel has 9 zones set with a gradient from about 64°C to about 240°C. The material is extruded through a die set set at 235-250°C.
[0405] Injection molding of panels
[0406] The plaques were injection molded using a Toyo injection molding machine to form 4"x4"x125 mil plaques. The composite pellets were first dried at 60-65°C for 1-6 hours before use. The barrel had 5 zones, set at 500-465°F in most cases (460-450°F for one set of plaques). The mold cooling was set at 120°F, or 70°F for some sets of plaques. Two different cycle times were used for most sets of plaques; a "regular" cycle time of about 39 seconds, and a "double" cycle time of about 78 seconds.
[0407] Color Measurement
[0408] The color values reported herein are CIELAB L*, a*, and b* values measured according to ASTM D 6290-98 and ASTM E308-99 using a CR-400 colorimeter from Konica Minolta. Unless otherwise noted, measurements were made on injection molded plaques having a thickness of 125 mils.
[0409] Examples of CA398-30 containing 20 wt% (Example 43) and 15 wt% PEG400 (Example 44)
[0410] CA398-30 / PEG400 formulations containing various additives were injection molded into 125 mil plates and b* values were measured with a colorimeter. Plates were made by two methods, using normal cycle times during injection molding and by doubling the cycle times during injection molding (as described above). The data are listed in Tables 22 and 23 below.
[0411] Table 22. Color (b*) of 125 mil plaques of CA398-30 containing 20% PEG400 and various additives.
[0412]
[0413]
[0414] Table 23. Color (b*) of 125 mil plaques of CA398-30 containing PEG 400 (15 wt%) and various additives.
[0415]
[0416] Review of Tables 22 and 23 shows that the presence of the acid scavenger (Vikoflex 7170) does not appear to have a large effect on color. Although not shown in the table, it was observed that Vikoflex sometimes caused an increase in haze in thicker sections. Additionally, the primary antioxidant alone (BHT or Irganox 1010) appeared to have little effect on color, with some data indicating that it may have caused a slight increase in color. However, the presence of the secondary antioxidant significantly reduced b*.
[0417] Example of CE41972 containing 17 wt% PEG400 (Example 45)
[0418] Formulations containing various additives were initially screened by preparing solvent cast films (as described above). The screening results showed that the CE41972 / PEG400 combination without additives was much more colorful than the CE41972 / TA or CA398-30 / PEG400 formulations. In addition, the addition of Vikoflex 7170 resulted in a further slight increase in b*, and the use of the primary antioxidant alone seemed to have little effect on b*. However, the use of a secondary antioxidant (DLTDP or Weston 705T) alone significantly reduced b*, citric acid alone reduced b*, and the combination of a secondary antioxidant (DLTDP or Weston 705T) with citric acid reduced b* more than each alone, the combination of DLTDP and Weston 705T reduced b* more than each alone, and the combination of DLTDP and Weston 705T with citric acid reduced b* slightly more than when only two of the three were used.
[0419] Based on the screening results, CE41972 / PEG400 formulations containing various additives were injection molded into 125 mil plaques and the b* was measured with a colorimeter. The data are listed in Tables 24 and 25 below.
[0420] Table 24. Observed color of 125 mil plaques of CE41972 containing 17 wt% PEG 400 (or 17 wt% TA as a comparison) and various additives.
[0421]
[0422] Table 25. Measured color values for Example 45.
[0423]
[0424]
[0425] Review of Tables 24 and 25 shows that the results of the plate validate the screening results and indicate that for the CE41972 / PEG400 combination, the lowest color is obtained when both the phosphite antioxidant (Doverphos S-9228T or Weston 705T) and citric acid are included, and that the color can be further slightly improved by adding DLTDP (an additional secondary antioxidant) to the phosphite antioxidant.
[0426] Example of CE41972 containing 17 wt% TA (Example 46)
[0427] CE41972 / TA formulations containing various additives were injection molded into 125 mil plaques and the b* values of the plaques made using conventional and double cycle times (as described above) were measured using a colorimeter. The data are given in Tables 26 and 27 below.
[0428] Table 26. Color (b*) of 125 mil plaques of CE41972 containing 17 wt% TA and various additives.
[0429]
[0430] A review of Table 26 shows that not all antioxidant combinations result in a reduction in b* in the formed plaques. The combination of BHT and DLTDP did not reduce b*, while the combination of Irganox 1010 and Weston 705T did reduce b*.
[0431] Table 27. Color (b*) of 125 mil plaques of CE41972 containing 17 wt% TA and various additives.
[0432]
[0433]
[0434] Review of Table 27 shows that a large reduction in b* was caused when either of the secondary phosphite antioxidants, Doverphos S-9228T or Weston 705T, was paired with the primary antioxidant, Irganox 1010. Surprisingly, the secondary antioxidants themselves did not reduce color as much as CA / PEG 400 (Table 23).
[0435] Example comparing CA398-30 with 15 wt% PEG400 and 15 wt% TA (Example 47)
[0436] A series of plaques were prepared using PEG400 or TA as plasticizers, including secondary antioxidants alone, or primary and secondary antioxidants in combination, by injection molding plaques using conventional and double cycle times (as described above). The results are listed in Table 28.
[0437] Table 28. Color (b*) of 125 mil plaques of CA398-30 containing 15 wt% plasticizer (TA or PEG400) and various additives.
[0438]
[0439] Review of Table 28 shows that there are some differences based on the plasticizer used. When the secondary antioxidant was added, the color of both combinations (CA398-30 / PEG400 and CA398-30 / TA) was significantly reduced. However, when PEG400 was used, the addition of Irganox 1010 had no benefit (Example 47-4), while when TA was used, the addition of Irganox 1010 resulted in some additional reduction in color (Example 47-8).
[0440] Example 50 - Example 57 - Disintegration of composite CA398-30 compositions containing plasticizer and polymer additives.
[0441] For each example, CA398-30 was compounded with TA, (1 wt%) EPSO and one or more biopolymers and then extruded into films or injection molded into plaques. The biopolymers used were PHB(6)Hx and CAPA 6500.
[0442] The film or sheet was prepared by a two-step process or a one-step process. For the two-step process, the material was pre-compounded on a twin-screw extruder and then extruded on a single-screw extruder or molded in an injection molding machine. For the one-step process, the material was prepared by physically blending the pellets and then completing the extrusion on a single-screw extruder. All materials were dried in a desiccant drying system at a temperature of 60°C before molding and extrusion.
[0443] Examples 50-53 films were prepared using a two-step process where the material was pre-compounded on a Leistritz 18 mm twin screw extruder at 180-200°C at a rate of 15 lbs / hr at a screw speed of 500 rpm. The material was then extruded on a 1.5" Killion extruder with a 24:1 L / D and a general purpose screw with a Maddock mixing section. The material was processed at a temperature of 200°C to 215°C on the barrel and 225 to 230°C on the die to produce 0.020 inch (20 mils or about 0.5 mm) films. Examples 56 and 57 were prepared in the same manner, except that a die was used to prepare 0.030 inch (30 mils or about 0.76 mm) films.
[0444] Example 54 films were made using a one-step process where the materials were physically blended and then extruded on a 1.5" Killion extruder with a 24:1 L / D and a general purpose screw with a Maddock mixing section. The material was processed at a temperature of 200°C to 215°C on the barrel and 225 to 230°C on the die to produce a 0.020 inch (20 mil or about 0.5 mm) film.
[0445] Example 55 Plates were prepared using a two-step process and injection molding where the material was pre-compounded on a Leistritz 18 mm twin screw extruder at 180-200°C at a rate of 15 lbs / hr at a screw speed of 500 rpm. The material was then molded on a 90 ton Toyo injection molding machine. The material was processed at a temperature of 210°C on the barrel and 20°C on the mold to produce 0.060 inch (60 mils or about 1.5 mm) plates.
[0446] Film or plaque samples were subjected to pilot scale aerobic composting testing in a manner similar to the testing described in Examples 1 and 2. The specific formulations used for each example and the disintegration test results are shown in Table 29 below.
[0447] Table 29. Formulation information for CA398-30 with triacetin and biopolymer.
[0448]
[0449] Review of Table 29 shows that a lower amount (10 wt%) of PHB(6)Hx (compared to a higher amount of 20 wt%) resulted in higher disintegration for higher TA levels (27 wt%). The combination of the two biopolymers resulted in good disintegration after 12 weeks for 17 wt% TA at 20 and 30 mil thicknesses, and greater than 50% disintegration at 60 mil thickness. Additionally, 20 wt% CAPA 6500 alone also resulted in good disintegration after 12 weeks for 17 wt% TA at 30 mil thickness.
Claims
1. A melt-processable and biodegradable cellulose acetate composition comprising at least one cellulose acetate, at least one plasticizer, a stabilizer and at least one additional component, wherein the stabilizer comprises a combination of one or more auxiliary antioxidants and citric acid, wherein the additional component is selected from a filler, an additive or a biodegradable polymer, in, The one or more auxiliary antioxidants include phosphite compounds, DLTDP or a combination thereof, the auxiliary antioxidants are present in an amount of 0.01 wt% to 0.8 wt% based on the total weight of the cellulose acetate composition, and the citric acid is present in an amount of 0.05 wt% to 0.2 wt%; wherein the at least one cellulose acetate has a degree of substitution with acetate of 1.0 to 2.5 and / or has a number average molecular weight (Mn) of 10,000 to 50,000 g / mol, measured by gel permeation chromatography (GPC) according to ASTM D6474 using NMP as solvent and a polystyrene equivalent Mn, wherein the at least one plasticizer is present in an amount of 10 wt% to 25 wt% based on the total weight of the composition, wherein if a biodegradable polymer is present, the amount of the biodegradable polymer is less than 50 wt% based on the total combined amount of the biodegradable polymer and cellulose acetate, wherein the cellulose acetate composition is biodegradable when tested under industrial composting conditions according to ASTM D6400, and wherein when the cellulose acetate composition is formed into a 0.25 mm (10 mil) film, the film exhibits at least 90% disintegration in no more than 12 weeks, as measured according to the disintegration test protocol of ISO 16929 (2013).
2. The composition according to claim 1, wherein the DS of the cellulose acetate is in the range of 1.0-2.
5.
3. The composition of claim 2, wherein the cellulose acetate has an Mn in the range of 10,000-45,000 as measured by GPC.
4. The composition of claim 3, wherein the cellulose acetate composition comprises at least one plasticizer in an amount of 15 wt% to 25 wt%.
5. The composition of claim 4, wherein the at least one plasticizer is a food-compliant plasticizer.
6. The composition of claim 5, wherein the cellulose acetate composition comprises at least one food-compliant plasticizer in an amount of 15 wt% to 25 wt%, and at least one filler in an amount of 1 wt% to 60 wt%.
7. The composition according to claim 5, wherein the food-compliant plasticizer is triacetin.
8. The composition of claim 6, wherein the cellulose acetate comprises at least one filler selected from the group consisting of an organic filler, an inorganic filler, food waste, a desiccant, an alkaline filler, or a combination thereof.
9. The composition of claim 8, wherein the filler is calcium carbonate.
10. The composition of claim 1, wherein the cellulose acetate composition comprises at least one biodegradable polymer, wherein the biodegradable polymer is present in an amount less than 50 wt % based on the total combined amount of the biodegradable polymer and cellulose acetate.
11. The composition of claim 10, wherein the at least one biodegradable polymer is selected from polyhydroxyalkanoates, polycaprolactone polymers, or combinations thereof.
12. The composition of claim 1, wherein the cellulose acetate composition comprises at least one odor modifying additive in an amount of 0.001 wt% to 1 wt%, based on the total composition.
13. The composition of claim 1, wherein the cellulose acetate composition comprises a stabilizer in an amount of 0.01 wt% to 5 wt% based on the total composition, wherein the stabilizer comprises one or more secondary antioxidants.
14. The composition of claim 1, wherein when the cellulose acetate composition is formed into a 0.51 mm (20 mil) film, the film exhibits at least 90% disintegration in not more than 12 weeks as measured according to the Disintegration Test Protocol.
15. A molded article comprising the composition according to claim 1.
16. The molded article of claim 15, wherein the article is a disposable food contact article.
17. The molded article according to claim 15, wherein the article is a horticultural article.
18. The molded article of claim 15, wherein the article is certified as home compostable for an article having a maximum thickness of up to 15 mils.
19. The molded article of claim 15, wherein the article is non-durable up to a maximum thickness of 15 mils.