A device and method for optically characterizing the relaxation process of polymer materials containing dynamic bonds

Through optical characterization devices and methods, we solve the problem of stress measurement during the reshaping process of polymer materials containing dynamic bonds, realize non-contact stress measurement and heat treatment design, support three-dimensional stress field measurement of complex structures, and improve the reshaping of materials. performance.

CN115032155BActive Publication Date: 2024-10-01XI AN JIAOTONG UNIV
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202210712899.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-06-22
Publication Date
2024-10-01
Estimated Expiration
2042-06-22

AI Technical Summary

Technical Problem

The existing technology lacks a method to measure the internal stress relaxation of the material during the reshaping process of polymer materials containing dynamic bonds, which affects the performance of the material and the reshaping process.

Method used

Optical characterization devices and methods are used to non-contactly measure the stress state inside materials containing dynamic chemical bonds. Planar parallel light sources, polarizers, transparent environmental boxes, analyzers and recording devices are used to record interference fringe information and calculate birefringence differences. and stress state, providing the design basis for heat treatment time and temperature.

Benefits of technology

It achieves non-contact measurement of the internal stress state of the material, determines the stress level during the reshaping process, provides a basis for the heat treatment of the material, and supports controllable color effects and three-dimensional stress field measurement of complex structures.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115032155B_ABST
    Figure CN115032155B_ABST
Patent Text Reader

Abstract

The present invention discloses a device and method for optically characterizing the relaxation process of a polymer material containing dynamic bonds. The device comprises a plane parallel light source, a polarizer, an opposite transparent environmental box, an analyzer and a recording device which are coaxially arranged in sequence, and a loading device arranged on the opposite transparent environmental box; the method comprises: 1) placing a polymer material sample containing dynamic chemical bonds under a linearly polarized plane parallel light environment; 2) calibrating various parameters of the sample under the linearly polarized plane parallel light environment; 3) deforming the sample by an external force and maintaining its deformation. 4) Activating the dynamic bond exchange reaction in the sample; 5) Recording the light intensity information of the interference fringes that appear after being superimposed and synthesized by the analyzer. 6) Calculating the stress relaxation state in the current sample based on the recorded light intensity information of the interference fringes. The present invention measures the stress state inside the material containing dynamic chemical bonds by a non-contact method, determines the stress level during its reshaping process, and provides a design basis for its heat treatment time and temperature.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the application field of polymers, and in particular to a device and a method for optically characterizing the relaxation process of a polymer material containing dynamic bonds. Background Art

[0002] Dynamic bond-containing polymer materials have made great progress in recent years. Due to their unique bond exchange characteristics, they exhibit the same characteristics as traditional cross-linked polymer materials when the dynamic bond exchange reaction is not activated, and have the characteristics of corrosion resistance, high temperature resistance and high strength. When the dynamic chemical bonds are excited, the topological structure of the polymer network will be rearranged, resulting in remodelable properties similar to linear polymer materials. Therefore, this type of material has been widely studied to achieve the recycling and reshaping of thermosetting materials. The entire process of its reshaping is actually the process of relaxing the stress generated by the external load, but there is currently no method to test the relaxation of the internal stress of the material during its reshaping process.

[0003] The stress distribution inside the material will significantly affect the material's performance. When the stress distribution inside the material and the magnitude of the stress can be fully detected, the material's reshaping process can be guided to achieve stable and usable reshaping of the material. Summary of the invention

[0004] In order to overcome the problem in the prior art that there is no method to test the internal stress relaxation of polymer materials containing dynamic bonds during the reshaping process, the purpose of the present invention is to provide a device and method for optically characterizing the relaxation process of polymer materials containing dynamic bonds, measure the stress state inside the material containing dynamic chemical bonds by a non-contact method, determine the stress level during the reshaping process, and provide a design basis for its heat treatment time and temperature.

[0005] In order to achieve the above object, the present invention adopts the following technical solution:

[0006] A device for optically characterizing the relaxation process of a polymer material containing dynamic bonds, comprising a plane parallel light source 1, a polarizer 2, an opposite transparent environmental box 3, an analyzer 5 and a recording device 6, which are coaxially arranged in sequence, and a loading device 7 arranged on the opposite transparent environmental box 3;

[0007] The polarizer 2 filters the original natural light to form linear polarized plane parallel light. The polarizer 2 is a polarizing film, which is placed on the light-emitting side of the plane light source 1 and between the plane light source 1 and a light-transmitting surface of the opposite transparent environment box 3.

[0008] The opposite transparent environment box 3 is placed in the dynamic chemical bond polymer material sample 4, and the opposite transparent environment box 3 can provide a temperature environment, an infrared light environment and an ultraviolet light environment, which are used to stimulate the bond exchange reaction inside the dynamic chemical bond polymer material sample 4; and are also used to heat the environment temperature to reach the glass transition temperature T of the dynamic chemical bond polymer material sample 4. g The above makes the polymer material sample containing dynamic chemical bonds in a highly elastic state;

[0009] The analyzer 5 is a polarizing film. In a linearly polarized plane parallel light environment, light waves along the directions of the first principal stress and the second principal stress pass through the analyzer 5 and are superimposed and synthesized in the polarization direction of the analyzer, and interference fringes appear. The principal stress refers to the principal stress on the cross section where the shear stress is zero, and the direction is perpendicular to the cross section, and the tensile stress is positive and the compressive stress is negative. For a general stress microelement, there are three principal stresses, which are arranged in order of numerical value as the first principal stress σ1, the second principal stress σ2, and the third principal stress σ3. For a plane stress state, there are only the first principal stress σ1 and the second principal stress σ2.

[0010] The recording device 6 is used to record interference fringes.

[0011] Preferably, the plane parallel light source 1 is provided by using a point light source through a lens or using a plane LED light source; the plane parallel light source 1 is monochromatic light or polychromatic light.

[0012] Preferably, the temperature environment is provided by a heat source of the environmental box, and the heat source is an electric heating wire, a quartz lamp, a heating tube or a ceramic heating plate; the infrared light environment is provided by using an infrared lamp, and for the infrared band with a specific wavelength of 780nm to 2500nm, the infrared lamp is filtered using a filter; the ultraviolet light environment is provided by an ultraviolet lamp, and for the ultraviolet band with a specific wavelength of 400nm to 715nm, the ultraviolet lamp is filtered using a filter.

[0013] Preferably, the recording device 6 is a digital camera or a light intensity meter; the recording lens of the recording device 6 is arranged behind the analyzer 5 to record the interference fringes.

[0014] Preferably, the loading device 7 is a universal testing machine capable of recording force-displacement information or a loading device with the same function; the loading process of the loading device 7 is completed in a double-sided transparent environmental box 3 .

[0015] The method for optically characterizing the relaxation process of a polymer material containing dynamic bonds comprises the following steps:

[0016] 1): A linearly polarized plane parallel light environment is formed by a plane parallel light source 1 and a polarizer 2, and a polymer material sample 4 containing dynamic chemical bonds is placed in a transparent environment box 3 opposite to the linearly polarized plane parallel light environment;

[0017] 2): Under a linear polarization plane parallel light environment, calibrate various parameters of a polymer material sample 4 containing dynamic chemical bonds, including the tensile modulus E of the material, the cross-linking density N of the material, and the stress optical constant C of the material;

[0018] 3): Deform the polymer material sample 4 containing dynamic chemical bonds by means of the loading device 7, and maintain the deformation after loading it to a preset position;

[0019] 4): After the dynamic chemical bond polymer material sample 4 is deformed, the dynamic bond exchange reaction in the dynamic chemical bond polymer material sample 4 is activated; the light waves along the first principal stress and the second principal stress directions in the linearly polarized plane parallel light environment pass through the analyzer 5 and then are superimposed and synthesized in the polarization direction of the analyzer, and interference fringes appear.

[0020] 5): The recording device 6 records the light intensity information of the interference fringes that appear after being superimposed and synthesized by the analyzer 5;

[0021] 6): After arranging the recorded light intensity information of the interference fringes in time series, the time evolution information of the birefringence difference Δn is calculated, and at the same time, the stress state in the current dynamic chemical bond polymer material sample 4 is calculated based on the value of the birefringence difference; the birefringence difference refers to the fact that the dynamic chemical bond polymer material sample 4 has a different refractive index to the light wave in the direction of the principal stress because the internal polymer chain of the dynamic chemical bond polymer material sample 4 is oriented along the principal stress direction after being loaded. The refractive index in the first principal stress direction is n1, and the refractive index in the second principal stress direction is n, then the birefringence difference Δn=n1-n2.

[0022] Preferably, the parameters of the dynamic chemical bond-containing polymer material sample 4 in step 2) are calibrated using a uniaxial tensile test; during the test, the interference fringe information on the surface of the dynamic chemical bond-containing polymer material sample 4 and the load and displacement information recorded by the loading device 7 are simultaneously recorded;

[0023] The calibration method of the tensile modulus and crosslink density in the step 2) is to calculate the stress and stretch ratio using the load F and displacement l information recorded during the uniaxial stretching process. The stretching section of the uniaxial stretching specimen used is l0 long, w wide, and d thick. The first principal stress is calculated. The second principal stress σ2 = 0, the stretching ratio along the direction of the first principal stress Stretching ratio along the second principal stress direction Then, the first principal stress σ1 is taken as the vertical axis, and the stretching ratio λ1 along the first principal stress direction is taken as the horizontal axis. The slope K is calculated as the tensile modulus E, and the crosslinking density k is the Boltzmann constant, T is the Kelvin temperature in the double-sided transparent environmental box 3;

[0024] In the stress optical constant calibration method of the material in step 2), in the uniaxial tensile test, the principal stress difference is equal to the first principal stress, Δσ=σ1-σ2=σ1; the birefringence difference is calculated by recording the change in the intensity of the interference fringes during the loading process, with the phase at the initial measurement as the phase 0 point, and the intensity change is proportional to cos 2 ψ; ψ is the phase of the light intensity information. After obtaining the phase information, the difference in birefringence Δn under the current light intensity is inferred. Where λ is the wavelength of the light wave; after calculating the birefringence difference Δn and the principal stress difference Δσ during the stretching process, the relationship between stress and birefringence difference is plotted with the principal stress difference as the abscissa and the birefringence difference as the ordinate, and the slope K is calculated to obtain the stress optical constant C=KkT of the material, where k is the Boltzmann constant;

[0025] The method for calibrating the stress optical constant of the material in step 2) includes a method for calculating the birefringence difference from the RGB information of the monochromatic light interference fringe image; 1) reading the RGB information of the image captured by the recording device 6 into a computer storage disk, extracting the main channel of the selected monochromatic light; arranging the main channels in sequence according to the time series, and obtaining the relationship between the nominal light intensity and the time change, the nominal light intensity Changing trends meet Where I is the light intensity, A is the vector amplitude of the light wave vector, and λ is the wavelength of the light wave; 2) Extract the time series t of each peak value of the nominal light intensity. The initial phase is 0 and the nominal light intensity is the maximum. After that, the phase ψ corresponding to the i-th wave peak value is The phase ψ corresponding to the i-th trough is iπ; 3) Calculate the birefringence difference information corresponding to the peak and trough, So far, since the refractive index n1 and n2 of the polymer material along the first and second principal stress directions cannot be directly measured, they can be inferred from the interference fringes recorded by the interference fringes.

[0026] Preferably, the activation method of the dynamic bond exchange reaction in the dynamic chemical bond-containing polymer material sample 4 in step 4) is consistent with the selected dynamic bond activation method, using thermal activation, infrared light irradiation activation or ultraviolet light irradiation activation.

[0027] Preferably, in step 6), the stress state in the current dynamic chemical bond-containing polymer material sample 4 is calculated, and after the birefringence difference at each position is calculated, the principal stress difference at the corresponding position is calculated as Where k is the Boltzmann constant;

[0028] The evolution law of the birefringence difference in step 6) with time t approximately satisfies the following relationship: β(λ) is the dynamic bond exchange reaction rate of polymer materials containing dynamic bonds, where w is the thermal eigenfrequency of the dynamic bond, W B is the activation energy of the dynamic chemical bond, N s is the number of Kuhn segments of the dynamic bond polymer material. Compared with the prior art, the beneficial effects of the present invention are embodied in

[0029] 1 The present invention can measure the stress state inside the material containing dynamic chemical bonds by a non-contact method, determine the stress level during the reshaping process, and provide a design basis for the heat treatment time and temperature.

[0030] 2 The present invention provides a direct correspondence between the difference in birefringence and stress, and provides a design and calculation basis for achieving controllable color effects through stress relaxation of polymer materials containing dynamic chemical bonds.

[0031] 3 The characterization method provided by the present invention can obtain the internal stress distribution level of the complex three-dimensional structure by only slicing the structure for stress testing of the complex structure. In theory, the three-dimensional stress field of any complex structure can be measured. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 Schematic diagram of the experimental setup.

[0033] Figure 2 The nominal light intensity of the interference fringes on the material surface during the loading and unloading process in Example 1 varies with time.

[0034] FIG3 a is a loading scatter plot of Example 1 during the loading process, with the stretching ratio as the horizontal axis and the stress as the vertical axis.

[0035] FIG3 b is a birefringence-stress scatter plot of Example 1 during the loading process, with the birefringence difference as the horizontal axis and the stress as the vertical axis.

[0036] Figure 3 c is a comparison diagram of the stress measured by the universal testing machine and the stress measured by the photoelastic method during the deformation retention process.

[0037] Figure 4 The nominal light intensity of the interference fringes on the material surface during the loading and unloading process in Example 2 varies with time.

[0038] FIG5 a is a loading scatter plot of Example 2 during the loading process, with the stretching ratio as the horizontal axis and the stress as the vertical axis.

[0039] FIG5 b is a birefringence-stress scatter plot of Example 2 during the loading process, with the birefringence difference as the horizontal axis and the stress as the vertical axis.

[0040] FIG5 c is a comparison diagram of the stress measured by the universal testing machine during the deformation retention process of Example 2 and the stress measured by the photoelastic method. DETAILED DESCRIPTION

[0041] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments.

[0042] Example 1 (anhydride / bisphenol A glycidyl ether epoxy resin)

[0043] 1 Raw materials: glutaric anhydride, bisphenol A glycidyl ether, zinc acetylacetonate hydrate

[0044] 2 Preparation method: Weigh 53.09 g of bisphenol A glycidyl ether, preheat at 130°C, and then add 4.11 g of zinc acetylacetonate. After stirring evenly, add 17.80 g of glutaric anhydride and stir. After stirring evenly, evacuate in a vacuum oven at 80°C until no bubbles are formed. Then pour the mixture into a steel mold preheated to 80°C and cure at 120°C for 12 hours to fully cure it. After curing and molding, demould.

[0045] 3 Calibrate various parameters: The dynamic bond activation method of the selected material is thermal activation. Cut the prepared material into samples with a length l0 of 60mm, a width w of 20mm, and a thickness d of 2mm, and put the opposite transparent environmental box 3 on the loading device 7 (universal testing machine), and use the tensile clamp to fix the sample to the universal testing machine. Use a flat LED lamp as a plane parallel light source 1, first use a blue filter film to obtain monochromatic light, and then use a polarizer 2 to convert the plane parallel light field into a linearly polarized plane parallel light field; and the analyzer 5 is the polarization lens of the recording device 6 (digital camera), and adjust the recording device 6 and the angles of the polarizer 2 and the analyzer 5. In this embodiment, the polarization direction of the two polarizers 2 is consistent with that of the analyzer 5, and the angle with the loading direction is 45°. Adjust the position of the recording device 6 so that it can clearly record the surface of the polymer material sample 4 containing dynamic chemical bonds. After adjusting the position of the polymer material sample 4 containing dynamic chemical bonds and the camera position, close the door of the transparent environmental box 3 opposite and start heating to 180°C. After the temperature of the incubator reaches the set temperature, wait for ten minutes and then load at a speed of 4mm / min. After loading to 0.8mm, keep it unchanged. Export the recorded interference fringe information and the load displacement data of the testing machine to calculate the stress. Stretch ratio l is the length of the sample during loading. Make a curve with the stretch ratio as the horizontal axis and the stress as the vertical axis, such as Figure 3a The Young's modulus of the device is calculated to be E, and the cross-linking density is N. At the same time, the values ​​of time and birefringence difference are extracted from the recorded interference fringes, and a scatter plot is drawn with birefringence difference as the vertical axis and stress as the horizontal axis, as shown in Figure 3b , calculate the slope K of the scatter distribution curve, from which the stress optical constant C=KkT can be obtained.

[0046] 4 Recording interference fringes and load displacement information of loading device 7: After the calibration experiment, keep the stretching ratio unchanged, keep the temperature unchanged at 180°C, set the recording device 6 (digital camera) to take a photo every ten seconds, and the loading device 7 (universal testing machine) to record the load and displacement information throughout the process.

[0047] 5 Calculate the stress information during the relaxation process: Arrange the collected photos in chronological order and extract the light intensity information. Figure 2 As shown; then, according to the relationship between the light intensity information and time, the value of the birefringence difference Δn is calculated. The loading method used in this embodiment is a uniaxial tensile specimen. At this time, σ1=σ, σ2=σ3=0, so it can be calculated that At the same time, the universal testing machine also recorded the information of stress changes over time, and the calculated values ​​were basically consistent with the measured values. Figure 3c A comparison chart of measured and calculated values.

[0048] Embodiment 2 (trimer acid / bisphenol A glycidyl ether epoxy resin)

[0049] 1. Raw materials: trimer acid, bisphenol A glycidyl ether, zinc acetylacetonate hydrate

[0050] 2 Preparation method: Weigh 31.71g of trimerized fatty acid, heat to 100℃, stir the heated fatty acid with a magnetic stirrer, slowly add 1.59g of zinc acetylacetonate, and stir for 30 minutes. After stirring evenly, put the mixture into a vacuum drying oven at a temperature of 100℃, gradually heat to 180℃ and maintain at 180℃, and keep the vacuum state during the period. When no bubbles are precipitated, take out the mixture and cool it to 120℃, then add 18.71g of bisphenol A glycidyl ether, continue stirring for 10 minutes, and then pour it into a steel mold preheated to 120℃. The size is 3mm×120mm×80mm, and finally cure at 130℃ for 6 hours, and demold after curing.

[0051] 3 Calibrate various parameters: The dynamic bond activation method of the selected material is thermal activation. Cut the prepared material into samples with a length l0 of 60mm, a width w of 20mm, and a thickness d of 2mm, and put the opposite transparent environmental box 3 on the loading device 7 (universal testing machine), and use the tensile clamp to fix the sample to the universal testing machine. Use a flat LED lamp as a plane parallel light source 1, first use a blue filter film to obtain monochromatic light, and then use a polarizer 2 to convert the plane parallel light field into a linearly polarized plane parallel light field; and the analyzer 5 is the polarization lens of the recording device 6 (digital camera), and adjust the recording device 6 and the angles of the polarizer 2 and the analyzer 5. In this embodiment, the polarization direction of the two polarizers 2 is consistent with that of the analyzer 5, and the angle with the loading direction is 45°. Adjust the position of the recording device 6 so that it can clearly record the surface of the polymer material sample 4 containing dynamic chemical bonds. After adjusting the position of the polymer material sample 4 containing dynamic chemical bonds and the camera position, close the door of the transparent environmental box 3 opposite and start heating to 180°C. After the temperature of the incubator reaches the set temperature, wait for ten minutes and then load at a speed of 4mm / min. After loading to 0.8mm, keep it unchanged. Export the recorded interference fringe information and the load displacement data of the testing machine to calculate the stress. Stretch ratio l is the length of the sample during loading. Make a curve with the stretch ratio as the horizontal axis and the stress as the vertical axis, such as Figure 5a The Young's modulus of the device is calculated to be E, and the cross-linking density is N. At the same time, the values ​​of time and birefringence difference are extracted from the recorded interference fringes, and a scatter plot is drawn with birefringence difference as the vertical axis and stress as the horizontal axis, as shown in Figure 5b , calculate the slope K of the scatter distribution curve, from which we can derive the stress optical constant C = KkT

[0052] 4 Recording interference fringes and load displacement information of loading device 7: After the calibration experiment, keep the stretching ratio unchanged, keep the temperature unchanged at 160°C, set the recording device 6 (digital camera) to take a photo every ten seconds, and the loading device 7 (universal testing machine) to record the load and displacement information throughout the process.

[0053] 5 Calculate the stress information during the relaxation process: Arrange the collected photos in chronological order and extract the light intensity information. Figure 4 As shown; then, according to the relationship between the light intensity information and time, the value of the birefringence difference Δn is calculated. The loading method used in this embodiment is a uniaxial tensile specimen. At this time, σ1=σ, σ2=σ3=0, so it can be calculated that At the same time, the universal testing machine also recorded the information of stress changes over time, and the calculated values ​​were basically consistent with the measured values. Figure 5cA comparison chart of measured and calculated values.

Claims

1. A device for optically characterizing the relaxation process of a polymer material containing dynamic bonds, characterized in that: It comprises a plane parallel light source (1), a polarizer (2), an opposite transparent environment box (3), an analyzer (5) and a recording device (6) which are coaxially arranged in sequence, and a loading device (7) arranged on the opposite transparent environment box (3); The polarizer (2) filters the original natural light to form linearly polarized plane parallel light. The polarizer (2) is a polarizing film, which is placed on the light-emitting side of the plane light source (1) and between the plane light source (1) and a light-transmitting surface of the opposite transparent environment box (3); The opposite transparent environmental box (3) is placed in a sample of a polymer material containing dynamic chemical bonds (4). The opposite transparent environmental box (3) can provide a temperature environment, an infrared light environment and an ultraviolet light environment, which are used to stimulate a bond exchange reaction inside the sample of the polymer material containing dynamic chemical bonds (4); and are also used to heat the environment temperature to reach the glass transition temperature T of the sample of the polymer material containing dynamic chemical bonds (4). g The above makes the polymer material sample containing dynamic chemical bonds in a highly elastic state; The analyzer (5) is a polarizing film. Light waves along the directions of the first principal stress and the second principal stress in a linearly polarized plane parallel light environment pass through the analyzer (5) and are superimposed and synthesized in the polarization direction of the analyzer, resulting in interference fringes. The principal stress refers to the principal stress on the cross section where the point where the shear stress is zero is located, and the direction is perpendicular to the cross section, and the tensile stress is positive and the compressive stress is negative. For a general stress microelement, there are three principal stresses, which are arranged in order of numerical value as the first principal stress σ1, the second principal stress σ2, and the third principal stress σ3. For a plane stress state, there are only the first principal stress σ1 and the second principal stress σ2. The recording device 6 is used to record interference fringes.

2. The device for optically characterizing the relaxation process of a polymer material containing dynamic bonds according to claim 1, characterized in that: The plane parallel light source (1) uses a point light source provided through a lens or uses a plane LED light source; the plane parallel light source (1) is monochromatic light or polychromatic light.

3. The device for optically characterizing the relaxation process of a polymer material containing dynamic bonds according to claim 1, characterized in that: The temperature environment is provided by the heat source of the environmental box, and the heat source is an electric heating wire, a quartz lamp, a heating tube or a ceramic heating plate; the infrared light environment is provided by using an infrared lamp, and for the infrared band with a specific wavelength of 780nm to 2500nm, the infrared lamp is filtered using a filter; the ultraviolet light environment is provided by an ultraviolet lamp, and for the ultraviolet band with a specific wavelength of 400nm to 715nm, the ultraviolet lamp is filtered using a filter.

4. The device for optically characterizing the relaxation process of a polymer material containing dynamic bonds according to claim 1, characterized in that: The recording device (6) is a digital camera or a light intensity meter; the recording lens of the recording device (6) is arranged behind the analyzer (5) to record the interference fringes.

5. The device for optically characterizing the relaxation process of a polymer material containing dynamic bonds according to claim 1, characterized in that: The loading device (7) is a universal testing machine capable of recording force displacement information or a loading device with the same function; the loading process of the loading device (7) is completed in a double-sided transparent environmental box (3).

6. A method for optically characterizing a relaxation process of a polymer material containing dynamic bonds according to any one of claims 1 to 5, characterized in that: The following steps are involved: 1): A linearly polarized plane parallel light environment is formed by a plane parallel light source (1) and a polarizer (2), and a polymer material sample (4) containing dynamic chemical bonds is placed in a transparent environment box (3) opposite to the linearly polarized plane parallel light environment; 2): Under a linear polarized plane parallel light environment, calibrate various parameters of a polymer material sample (4) containing dynamic chemical bonds, including the tensile modulus E of the material, the cross-linking density N of the material, and the stress optical constant C of the material; 3): applying deformation to the polymer material sample (4) containing dynamic chemical bonds by means of a loading device (7), and maintaining the deformation after loading it to a preset position; 4): after the dynamic chemical bond-containing polymer material sample (4) is deformed, a dynamic bond exchange reaction in the dynamic chemical bond-containing polymer material sample (4) is activated; light waves along the directions of the first principal stress and the second principal stress in a linearly polarized plane parallel light environment pass through an analyzer (5) and then are superimposed and synthesized in the polarization direction of the analyzer, and interference fringes appear 5): The recording device (6) records the light intensity information of the interference fringes that appear after being superimposed and synthesized by the analyzer (5); 6): After arranging the recorded light intensity information of the interference fringes in time series, the time evolution information of the double refraction difference Δn is calculated, and at the same time, the stress state in the current dynamic chemical bond polymer material sample (4) is calculated based on the value of the double refraction difference; the double refraction difference refers to the fact that the dynamic chemical bond polymer material sample (4) has different refractive indices for light waves in the direction of the principal stress because the internal polymer chains of the dynamic chemical bond polymer material sample (4) are oriented along the principal stress direction after being loaded, and the refractive index in the first principal stress direction is n1, and the refractive index in the second principal stress direction is n2, then the double refraction difference Δn = n1-n2.

7. The characterization method according to claim 6, characterized in that: The various parameters of the dynamic chemical bond-containing polymer material sample (4) in the step 2) are calibrated using a uniaxial tensile test; during the test, the interference fringe information on the surface of the dynamic chemical bond-containing polymer material sample (4) and the load and displacement information recorded by the loading device (7) are simultaneously recorded; The calibration method of the tensile modulus and the crosslink density in the step 2) is to calculate the stress and stretch ratio using the load F and displacement l information recorded during the uniaxial stretching process. The stretching section of the uniaxial stretching specimen used is l0 long, w wide, and d thick; Calculate the first principal stress The second principal stress σ2 = 0, the stretching ratio along the direction of the first principal stress Stretching ratio along the second principal stress direction Then, the first principal stress σ1 is taken as the vertical axis, and the stretching ratio λ1 along the first principal stress direction is taken as the horizontal axis. The slope K is calculated as the tensile modulus E, and the crosslinking density k is the Boltzmann constant, T is the Kelvin temperature in the double-sided transparent environmental chamber; In the stress optical constant calibration method of the material in step 2), in the uniaxial tensile test, the principal stress difference is equal to the first principal stress, Δσ=σ1-σ2=σ1; the birefringence difference is calculated by recording the change in the intensity of the interference fringes during the loading process, with the phase at the initial measurement as the phase 0 point, and the intensity change is proportional to cos 2 ψ; ψ is the phase of the light intensity information. After obtaining the phase information, the difference in birefringence Δn under the current light intensity is inferred. Where λ is the wavelength of the light wave; After calculating the birefringence difference Δn and the principal stress difference Δσ during the stretching process, the relationship between stress and birefringence difference is plotted with the principal stress difference as the horizontal coordinate and the birefringence difference as the vertical coordinate, and the slope K is calculated to obtain the stress optical constant C=KkT of the material, where k is the Boltzmann constant; The method for calibrating the stress optical constant of the material in step 2) includes a method for calculating the birefringence difference from the RGB information of the monochromatic light interference fringe image; 1) reading the RGB information of the image captured by the recording device (6) into a computer storage disk, extracting the main channel of the selected monochromatic light; arranging the main channels in sequence according to the time series, and obtaining the relationship between the nominal light intensity and the time change, the nominal light intensity Changing trends meet Where I is the light intensity, A is the vector amplitude of the light wave vector, and λ is the wavelength of the light wave; 2) Extract the time series t of each peak value of the nominal light intensity. The initial phase is 0 and the nominal light intensity is the maximum. After that, the phase ψ corresponding to the i-th wave peak value is The phase ψ corresponding to the i-th trough is iπ; 3) Calculate the birefringence difference information corresponding to the peak and trough, So far, since the refractive index n1 and n2 of the polymer material along the first and second principal stress directions cannot be directly measured, they can be inferred from the interference fringes recorded by the interference fringes.

8. The characterization method according to claim 6, characterized in that: The activation method of the dynamic bond exchange reaction in the dynamic chemical bond-containing polymer material sample (4) in step 4) is consistent with the selected dynamic bond activation method, and adopts thermal activation, infrared light irradiation activation or ultraviolet light irradiation activation.

9. The characterization method according to claim 6, characterized in that: In the step 6), the stress state in the current dynamic chemical bond-containing polymer material sample (4) is calculated. After the birefringence difference at each position is calculated, the principal stress difference at the corresponding position is calculated as: Where k is the Boltzmann constant; The evolution law of the birefringence difference in step 6) with time t approximately satisfies the following relationship: β(λ) is the dynamic bond exchange reaction rate of polymer materials containing dynamic bonds, where w is the thermal eigenfrequency of the dynamic bond, W B is the activation energy of the dynamic chemical bond, N s is the number of Kuhn segments of polymer materials containing dynamic bonds.

Citation Information

Patent Citations

  • Two-stage calibration conversion method using viscous-elastic piezoresistive material to monitor stress variation after high-speed loading

    CN102980693A

  • Tester capable of simulating plane and curved surface stress relaxation effect of thin-film materials

    CN106896022A

  • Thermoplastic vulcanizate compression stress relaxation reversible recovery behavior characterization method

    CN107024383A

  • Flexible sensing device, manufacturing method thereof and monitoring device

    CN112461409A

  • Stress display member and stress measurement method

    JP2017181155A